Environment-friendly water-soluble aerosol spray paint and preparation method thereof

By modifying hollow glass microspheres and combining them with specific photoinitiators and thickeners, the contradiction between heat insulation performance and drying speed in water-soluble aerosol paints has been resolved, achieving rapid drying, strong adhesion, and efficient heat insulation.

CN121136602APending Publication Date: 2025-12-16GUANGDONG HOSEN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511558049.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-29
Publication Date
2025-12-16

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve synergistic optimization of heat insulation performance, drying speed, and film strength in water-soluble aerosol paints, and suffer from problems such as poor filler compatibility, weak interfacial bonding, slow drying, and poor initial water resistance.

Method used

By modifying hollow glass microspheres, hydrophilic polyethylene glycol segments and acrylate double bonds that can participate in photocuring are introduced. Combined with a specific ratio of composite photoinitiator and thickener system, a synergistic effect is formed, achieving rapid drying, strong adhesion and efficient heat insulation.

Benefits of technology

It achieves a balance between rapid drying, strong adhesion, and high-efficiency heat insulation performance of water-soluble aerosol paint, solving the problems of instability and insufficient performance in traditional technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the field of water-based spray paint, and particularly relates to environment-friendly water-soluble aerosol spray paint and a preparation method thereof. The spray paint is prepared from the following components: water-based resin, modified hollow glass microspheres, a coloring agent, a thickening agent, a composite photoinitiator, a multifunctional monomer and water. The modified hollow glass microspheres are modified and prepared through a two-step method: firstly, 3-aminopropyltriethoxysilane is adopted for surface amination, then polyethylene glycol diacrylate is grafted, and hydrophilic chain segments and cross-linkable double bonds are introduced to the surface of the modified hollow glass microspheres at the same time. Through the synergistic effect of the components, the drying speed and the adhesive force of the product are remarkably improved while the excellent heat insulation performance of the product is maintained, and the technical problems that a traditional heat insulation coating is slow in drying and poor in adhesive force are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water-based spray paint, specifically an environmentally friendly water-soluble aerosol spray paint and its preparation method. Background Technology

[0002] With increasingly stringent global environmental regulations and rising consumer awareness of environmental protection, the coatings industry is undergoing a profound transformation from traditional solvent-based products to water-based, environmentally friendly products. Against this backdrop, water-soluble aerosol paints, due to their advantages such as requiring no specialized equipment, convenient application, and extremely low volatile organic compound (VOC) content, are demonstrating enormous market potential in fields such as architectural decoration, automotive repair, industrial maintenance, and DIY projects. Simultaneously, the demand for building energy conservation and industrial equipment insulation continues to grow, opening up broad application opportunities for functional coatings with thermal insulation properties. Developing a thermally insulating and environmentally friendly water-soluble aerosol paint by combining thermal insulation performance with the convenience and environmental friendliness of water-soluble aerosol paint is undoubtedly an innovative direction that aligns with market development trends, with promising application prospects, such as energy-saving renovations of building exteriors, convenient insulation of storage tanks and pipelines, and on-site construction of complex structural components requiring thermal insulation.

[0003] However, those skilled in the art face several long-standing technical contradictions and challenges in the development of such products, which severely restrict their industrialization and performance improvement:

[0004] Firstly, to achieve thermal insulation, lightweight functional fillers such as hollow glass microspheres and ceramic microspheres are typically introduced. However, these fillers, especially hollow glass microspheres, have closed surfaces, are chemically inert, and have poor compatibility with water-based resins. This not only causes the fillers to float or settle during storage and application, affecting stability, but more importantly, their dispersion in the paint film blocks the path of moisture evaporation, creating numerous dead ends in a maze, significantly prolonging the drying time of the paint film. This contradicts the requirements of aerosol spraying for rapid surface drying and ease of operation.

[0005] Secondly, traditional thermal insulation fillers and water-based resin matrices are mainly bonded through physical adsorption, resulting in weak interfacial adhesion. This leads to a series of problems: First, the mechanical properties of the paint film (such as hardness and abrasion resistance) decrease; second, adhesion is impaired, especially on smooth substrates such as metals or plastics, where the paint film is prone to peeling; finally, microscopic defects at the interface become channels for the penetration of moisture and corrosive media, affecting the durability and protective performance of the paint film.

[0006] Finally, water-based paints inherently suffer from slow drying and poor initial water resistance. While ultraviolet (UV) curing technology can significantly improve curing speed and film performance, its application in water-based systems faces challenges. Moisture's absorption and scattering of UV light reduces curing efficiency and exacerbates oxygen inhibition, leading to incomplete surface curing and stickiness. Simply introducing heat-insulating fillers further hinders UV light penetration and moisture escape, making deep curing difficult and hindering the formation of a strong, uniform cross-linked network, ultimately affecting the product's practicality and reliability.

[0007] In summary, existing technologies lack a comprehensive solution that can simultaneously satisfy the requirements of rapid drying, excellent adhesion, efficient thermal insulation, and environmental friendliness. How to overcome these technical bottlenecks and achieve synergistic optimization of various performance indicators through innovative formulation design and material modification has become a key technical problem urgently needing to be solved in this field. Summary of the Invention

[0008] To address the shortcomings of existing technologies, this invention provides an environmentally friendly water-soluble aerosol paint and its preparation method.

[0009] An environmentally friendly water-soluble aerosol spray paint is composed of the following components: water-based resin, modified hollow glass microspheres, colorant, thickener, composite photoinitiator, multifunctional monomer, and water.

[0010] Preferably, the environmentally friendly water-soluble aerosol spray paint is composed of the following components by weight:

[0011] 30-50 parts water-based resin, 10-20 parts modified hollow glass microspheres, 5-10 parts colorant, 2-4 parts thickener, 1-2 parts composite photoinitiator, 1-2 parts multifunctional monomer, and 5-10 parts water.

[0012] More preferably, the environmentally friendly water-soluble aerosol paint may also contain functional additives such as silane coupling agents, defoamers, water-based dispersants, preservatives, organosilicon wetting agents, zirconium-based drying accelerators, and corrosion inhibitors, wherein the amount of the functional additives added is 10-20 wt% of the water-based resin.

[0013] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of (2-3):1.

[0014] The colorant is an environmentally friendly inorganic pigment; preferably, the environmentally friendly inorganic pigment is at least one of cobalt green GT705 and cobalt blue PB28.

[0015] The thickener is at least one of waterborne nonionic associative polyurethane and hydroxyethyl cellulose; preferably, the thickener is a mixture of waterborne nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of (1-2):1.

[0016] The composite photoinitiator is at least one of Irgacure 2959 and Irgacure 369; preferably, the composite photoinitiator is a mixture of Irgacure 2959 and Irgacure 369 in a mass ratio of 1:(1-2).

[0017] The multifunctional monomer is at least one of polyethylene glycol diacrylate and trimethylolpropane triacrylate; preferably, the multifunctional monomer is a mixture of polyethylene glycol diacrylate and trimethylolpropane triacrylate in a mass ratio of 1:(1-2).

[0018] The method for preparing the modified hollow glass microspheres includes the following steps:

[0019] S1. By mass, 1-2 parts of 3-aminopropyltriethoxysilane are mixed with 40-50 parts of anhydrous ethanol, and the pH is adjusted to 5-6 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution; 150-200 parts of anhydrous ethanol and 9-10 parts of hollow glass microspheres are mixed, and the mixture is stirred continuously while adding the above 3-aminopropyltriethoxysilane / ethanol solution. The mixture is then refluxed at 74-76℃ for 8-12 hours, filtered, washed, and dried to obtain aminated hollow glass microspheres;

[0020] S2. By weight, mix 4-5 parts of polyethylene glycol diacrylate and 90-100 parts of anhydrous ethanol, and add 0.1-0.2 parts of dibutyltin tetralaurate to obtain a polyethylene glycol diacrylate / ethanol solution. Disperse the aminated hollow glass microspheres obtained in step S1 in 90-100 parts of anhydrous ethanol, and add the polyethylene glycol diacrylate / ethanol solution dropwise through a constant pressure dropping funnel at a rate of 3-5 ml / min. Under nitrogen protection, stir and react in a water bath at 58-60℃ for 10-12 h in the dark. Filter, wash, and dry in the dark to obtain the modified hollow glass microspheres.

[0021] This invention also provides a method for preparing an environmentally friendly water-soluble aerosol spray paint, comprising the following steps:

[0022] (1) Mix 5-10 parts of colorant and 5-10 parts of water by weight, and grind them for 1-2 hours using a basket mill to obtain component A;

[0023] (2) Under light-protected conditions, mix and stir 30-50 parts of water-based resin, 2-4 parts of thickener, 1-2 parts of multifunctional monomer, and 10-20 parts of modified hollow glass microspheres for 20-30 minutes. Then add component A obtained in step (1) and continue stirring for 30-60 minutes. Finally, add 1-2 parts of composite photoinitiator and stir for 5-10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. Pack the slurry into a container and inject 10-15 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0024] The spindle speed of the basket grinder in step (1) is 1500-2000 r / min, and the grinding media is zirconia beads.

[0025] The beneficial effects of this invention are:

[0026] This invention aims to synergistically resolve the inherent contradiction between heat insulation performance, drying speed, and film strength that has long existed in existing water-soluble aerosol spray paint technologies. Its core breakthrough lies in the successful transformation of functional fillers from traditional inert components into multifunctional active components through precise surface modification, thereby generating a synergistic effect with a carefully designed resin-curing system.

[0027] The modified hollow glass microspheres, prepared through a two-step modification process, play a crucial role. Their surface simultaneously incorporates hydrophilic polyethylene glycol segments and acrylate double bonds capable of participating in photocuring. This innovative design allows the modified microspheres to construct a highly efficient moisture-conducting network within the paint film via the PEG chains, actively guiding water molecules to the surface. This effectively overcomes the inherent limitation of hollow glass microspheres in hindering moisture evaporation, laying a solid foundation for rapid surface drying. Simultaneously, the terminal acrylate double bonds can copolymerize with the resin system under UV irradiation, connecting the microspheres to the resin network through strong covalent bonds. This represents a fundamental shift from traditional physical adsorption to chemical bonding, completely resolving the problems of weak interfacial bonding and poor paint film adhesion caused by filler introduction. Crucially, this mild surface modification process fully preserves the hollow structure of the microspheres, ensuring their core thermal insulation function is fully utilized.

[0028] Building upon this foundation, a composite photoinitiator system, combining Irgacure 2959 and Irgacure 369 in a specific ratio, further enhances the coating film performance. Irgacure 2959 primarily absorbs short-wave UVB, rapidly generating a high concentration of free radicals on the coating film surface. This achieves rapid surface curing while effectively consuming surface oxygen to overcome oxygen inhibition. Meanwhile, Irgacure 369, with its strong absorption capacity for long-wave UVA, can penetrate deep into the coating film to initiate polymerization, ensuring thorough cross-linking of the underlying resin. The synergistic effect of these two components enables simultaneous and complete curing of the coating film from the surface to the deeper layers, providing crucial assurance for obtaining a coating film with high hardness, high adhesion, and excellent chemical resistance.

[0029] Furthermore, the composite thickener system, a blend of hydroxyethyl cellulose and waterborne nonionic associative polyurethane, provides ideal application performance through rheological synergy. Hydroxyethyl cellulose primarily offers low shear viscosity, effectively preventing filler sedimentation and ensuring storage stability; while the waterborne nonionic associative polyurethane contributes excellent high shear thinning and leveling properties, ensuring effective spray atomization and film smoothness. The organic combination of these two components guarantees the product's stability and applicability throughout the entire process, from storage and application to film formation.

[0030] In terms of the preparation process, this invention employs a stepwise grinding and mixing process. First, the colorant and water are subjected to high-shear grinding to ensure sufficient pigment dispersion, achieving optimal tinting strength and hiding power, and preventing subsequent pigment agglomeration from affecting the paint film performance. A light-protected and sequential feeding method is used to formulate the paint under light-protected conditions, with the photoinitiator added in the final step. This effectively prevents pre-polymerization of the active components during storage, ensuring the product's storage stability and curing efficiency during use. Simultaneously, a mild modification process controlling parameters such as reaction pH, temperature, and time ensures the integrity and structural stability of the hollow glass microspheres while achieving a high grafting rate, thus fully preserving their thermal insulation function.

[0031] In summary, this invention, by endowing hollow glass microspheres with dual functions of hydrophilicity, moisture conductivity, and crosslinking capability, and organically combining them with a photoinitiation system and a rheological system of a thickener, successfully achieves a unified set of technical objectives—rapid drying, strong adhesion, efficient heat insulation, and excellent workability—within a water-based UV-curing water-soluble aerosol spray paint system. This technical solution, which simultaneously meets multiple requirements in the field of environmentally friendly water-soluble aerosol spray paint, is difficult to achieve with conventional techniques in this field, fully demonstrating the innovation and technological advancement of this invention. Detailed Implementation

[0032] The acrylic polysiloxane emulsion is made by mixing acrylic polysiloxane and water at a mass ratio of 8:1. The acrylic polysiloxane is purchased from Quark New Materials Co., Ltd., model: SH-309.

[0033] Water-based acrylic emulsion, model: Xinlian 1025, Yingde Xinlian Chemical Co., Ltd.

[0034] Cobalt Blue PB28, Model: PB28, Foshan Dachangshun Materials Technology Co., Ltd.

[0035] Waterborne nonionic associative polyurethane, model: SHYT 800, Jining Tangyi Chemical Co., Ltd.

[0036] Hydroxyethyl cellulose, model: 01, molecular weight: 30000, Jinan Shenglong Chemical Co., Ltd.

[0037] Polyethylene glycol diacrylate, item number: 455008, average molecular weight: 700, Merck Life Sciences Ltd.

[0038] Trimethylolpropane triacrylate, CAS No.: 15625-89-5.

[0039] 3-Aminopropyltriethoxysilane, CAS No.: 919-30-2. Example 1

[0040] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0041] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0042] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0043] The colorant is cobalt blue PB28.

[0044] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0045] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0046] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0047] The method for preparing the modified hollow glass microspheres includes the following steps:

[0048] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0049] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0050] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0051] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0052] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0053] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads. Example 2

[0054] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0055] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0056] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0057] The colorant is cobalt blue PB28.

[0058] The thickener is a water-based nonionic associative polyurethane.

[0059] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0060] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0061] The method for preparing the modified hollow glass microspheres includes the following steps:

[0062] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0063] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0064] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0065] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0066] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0067] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads. Example 3

[0068] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0069] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0070] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0071] The colorant is cobalt blue PB28.

[0072] The thickener is hydroxyethyl cellulose.

[0073] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0074] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0075] The method for preparing the modified hollow glass microspheres includes the following steps:

[0076] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0077] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0078] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0079] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0080] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0081] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads. Example 4

[0082] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0083] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0084] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0085] The colorant is cobalt blue PB28.

[0086] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0087] The composite photoinitiator is Irgacure 2959.

[0088] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0089] The method for preparing the modified hollow glass microspheres includes the following steps:

[0090] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0091] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0092] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0093] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0094] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0095] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads. Example 5

[0096] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0097] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0098] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0099] The colorant is cobalt blue PB28.

[0100] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0101] The composite photoinitiator is Irgacure 369.

[0102] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0103] The method for preparing the modified hollow glass microspheres includes the following steps:

[0104] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0105] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0106] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0107] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0108] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0109] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads.

[0110] Comparative Example 1

[0111] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0112] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0113] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0114] The colorant is cobalt blue PB28.

[0115] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0116] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0117] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0118] The method for preparing the modified hollow glass microspheres includes the following steps:

[0119] By weight, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the mixture was stirred continuously while adding the above 3-aminopropyltriethoxysilane / ethanol solution. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, the modified hollow glass microspheres were obtained.

[0120] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0121] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0122] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0123] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads.

[0124] Comparative Example 2

[0125] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0126] 50 parts water-based resin, 20 parts hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0127] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0128] The colorant is cobalt blue PB28.

[0129] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0130] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0131] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0132] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0133] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0134] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0135] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads.

[0136] Comparative Example 3

[0137] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0138] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 1.5 parts composite photoinitiator, 1.5 parts multifunctional monomer, and 10 parts water.

[0139] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0140] The colorant is cobalt blue PB28.

[0141] The composite photoinitiator is composed of Irgacure 2959 and Irgacure 369 mixed in a mass ratio of 1:2.

[0142] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0143] The method for preparing the modified hollow glass microspheres includes the following steps:

[0144] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0145] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0146] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0147] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0148] (2) Under light-protected conditions, 50 parts of water-based resin, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes. Finally, 1.5 parts of composite photoinitiator are added and stirred for 10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and injected with 12 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0149] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads.

[0150] Comparative Example 4

[0151] An environmentally friendly water-soluble aerosol spray paint, by weight, consists of the following components:

[0152] 50 parts water-based resin, 20 parts modified hollow glass microspheres, 7 parts colorant, 3 parts thickener, 1.5 parts multifunctional monomer, and 10 parts water.

[0153] The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of 2:1.

[0154] The colorant is cobalt blue PB28.

[0155] The thickener is a mixture of water-based nonionic associative polyurethane and hydroxyethyl cellulose in a mass ratio of 2:1.

[0156] The multifunctional monomer is composed of polyethylene glycol diacrylate and trimethylolpropane triacrylate mixed in a mass ratio of 1:1.

[0157] The method for preparing the modified hollow glass microspheres includes the following steps:

[0158] S1. By mass, 2 parts of 3-aminopropyltriethoxysilane and 50 parts of anhydrous ethanol were mixed, and the pH was adjusted to 5.5 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution. 200 parts of anhydrous ethanol and 10 parts of hollow glass microspheres were mixed, and the above 3-aminopropyltriethoxysilane / ethanol solution was added while stirring continuously. The mixture was then refluxed at 75°C for 10 hours. After filtration, washing, and drying, aminated hollow glass microspheres were obtained.

[0159] S2. By mass, 5 parts of polyethylene glycol diacrylate and 100 parts of anhydrous ethanol are mixed, and 0.15 parts of dibutyltin tetralaurate are added to obtain a polyethylene glycol diacrylate / ethanol solution. The aminated hollow glass microspheres obtained in step S1 are dispersed in 100 parts of anhydrous ethanol, and the polyethylene glycol diacrylate / ethanol solution is added dropwise to it through a constant pressure dropping funnel at a rate of 4 ml / min. Under nitrogen protection, the mixture is stirred and reacted in a water bath at 60°C for 12 h in the dark. After filtration, washing, and drying in the dark, the modified hollow glass microspheres are obtained.

[0160] The preparation method of the environmentally friendly water-soluble aerosol spray paint includes the following steps:

[0161] (1) Mix 7 parts colorant and 10 parts water by weight, and grind them for 2 hours using a basket mill to obtain component A;

[0162] (2) Under light-protected conditions, 50 parts of water-based resin, 3 parts of thickener, 1.5 parts of multifunctional monomer and 20 parts of modified hollow glass microspheres are mixed and stirred for 30 minutes. Then, component A obtained in step (1) is added and stirred for another 40 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. The slurry is then bottled and 12 wt% of compressed nitrogen gas is injected as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.

[0163] The spindle speed of the basket grinder in step (1) is 1600 r / min, and the grinding media is zirconia beads.

[0164] Test Example 1

[0165] The surface drying time was determined according to the national standard GB / T 1728-2020, "Determination of Drying Time of Paint Film and Putty Film". Specifically, under standard conditions of 23℃ and 50% relative humidity, the sample was sprayed onto a clean tinplate, with a wet film thickness of 100μm. The finger-touch method was used; the paint film surface was lightly touched with a finger at specific intervals until the paint film felt initially dry and no longer sticky to the finger. The time elapsed is the surface drying time, expressed in minutes (min). The results are shown in Table 1.

[0166] Table 1: Results of Surface Drying Time Detection

[0167]

[0168] As shown in Table 1, Example 1 of the present invention achieved the shortest surface drying time (15 min), and its drying efficiency was significantly better than all comparative examples and modified examples. This fully demonstrates that the modified hollow glass microspheres prepared by the surface modification process and the composite photoinitiator system produced a synergistic effect. Specifically, the hydrophilic PEG chains grafted onto the surface of the modified microspheres effectively constructed moisture conduction channels, overcoming the inherent defect of hollow glass microspheres in hindering moisture escape; while the combination of Irgacure 2959 and Irgacure 369 synergistically solved the problems of surface oxygen inhibition and insufficient deep curing. The data comparison between Comparative Example 1 and Comparative Example 2 particularly highlights the key and irreplaceable role of the polyethylene glycol diacrylate grafting step in promoting moisture evaporation, an effect that cannot be expected by those skilled in the art based on conventional silane coupling agent modification.

[0169] Test Example 2

[0170] The adhesion was determined according to the international standard ISO 2409:2020, "Paints and varnishes—Cross-cut test". Specifically, a special cross-cutting tool (1mm blade spacing) was used to create six parallel cuts on the dried paint film, followed by six more cuts perpendicular to the blades, forming 25 squares of 1mm x 1mm size. Debris was gently brushed away with a soft brush, and then special pressure-sensitive adhesive tape (3M #610) was applied, pressed firmly, and then quickly peeled off at a 60° angle within 0.5-1.0 seconds. The adhesion was rated according to the number of squares that detached from the substrate, referring to the grading chart in the standard. Grade 0 represents a completely smooth cut edge with no squares detached, the best grade; Grade 5 represents a detachment rate greater than 65%, the worst grade. The results are shown in Table 2.

[0171] Table 2: Adhesion Test Results

[0172]

[0173] As shown in Table 2, Example 1 of the present invention achieved the optimal Grade 0 adhesion. This indicates that the two-step modification imparts crosslinkability to the hollow glass microspheres, and the modified microspheres, acting as active crosslinking points, are introduced into the polymer network, fundamentally strengthening the interfacial bonding strength. Although the adhesion of Comparative Example 1 (aminated only) is better than that of Comparative Example 2 (unmodified), it is far from reaching the level of Example 1, which strongly proves that the introduction of the polymerizable double bonds is the decisive factor in obtaining the ultimate adhesion.

[0174] Test Example 3

[0175] Thermal insulation performance test: A test panel (100mm×100mm×1mm aluminum plate, dry film thickness 50μm) coated with the sample was placed on the surface of a constant-temperature hot stage, with the stage temperature set at 60℃. Two calibrated type K thermocouple temperature sensors were used: one was placed directly against the center of the uncoated back of the test panel, denoted as T1; the other was placed in a still air layer 10mm above the coating film, denoted as T2. After the system reached thermal equilibrium (approximately 30 minutes), stable readings of T1 and T2 were recorded. The thermal insulation temperature difference ΔT was calculated using the formula ΔT = T1 - T2, in degrees Celsius (℃). A larger ΔT value indicates better thermal insulation performance of the coating film. The results are shown in Table 3.

[0176] Table 3: Results of Thermal Insulation Performance Tests

[0177]

[0178] The data from Test Example 3 shows that, while endowing hollow glass microspheres with novel interfacial properties and functions, the present invention perfectly preserves and even slightly improves their core thermal insulation performance (Example 1, ΔT = 8.0℃). This confirms the mildness and effectiveness of the modification method, without damaging the hollow structure of the microspheres. Meanwhile, the comparison between Example 1 and Comparative Example 2 illustrates that good interfacial bonding helps form a denser coating film, reducing heat loss due to interfacial defects, thereby more fully realizing the thermal insulation potential. Furthermore, the comprehensive performance degradation in Comparative Examples 3 and 4, conversely demonstrating the indispensability of the thickening system and photocuring system described in this invention for ensuring the basic storage stability, workability, and final film formation of the product.

[0179] In summary, this invention, through the combination of specific modified hollow glass microspheres and a carefully selected formulation system, successfully and synergistically resolves the long-standing contradictions among multiple technical objectives such as high thermal insulation performance, rapid drying, strong adhesion, and environmental friendliness.

Claims

1. An environmentally friendly water-soluble aerosol spray paint, characterized in that, It is composed of the following components: water-based resin, modified hollow glass microspheres, colorant, thickener, composite photoinitiator, multifunctional monomer, and water.

2. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, By weight, it consists of the following components: 30-50 parts water-based resin, 10-20 parts modified hollow glass microspheres, 5-10 parts colorant, 2-4 parts thickener, 1-2 parts composite photoinitiator, 1-2 parts multifunctional monomer, and 5-10 parts water.

3. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, The water-based resin is composed of acrylic polysiloxane emulsion and water-based acrylic emulsion mixed in a mass ratio of (2-3):

1.

4. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, The thickener is at least one of water-based nonionic associative polyurethane and hydroxyethyl cellulose.

5. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, The composite photoinitiator is at least one of Irgacure 2959 and Irgacure 369.

6. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, The multifunctional monomer is at least one of polyethylene glycol diacrylate and trimethylolpropane triacrylate.

7. The environmentally friendly water-soluble aerosol spray paint as described in claim 1, characterized in that, The method for preparing the modified hollow glass microspheres includes the following steps: S1. By mass, 1-2 parts of 3-aminopropyltriethoxysilane are mixed with 40-50 parts of anhydrous ethanol, and the pH is adjusted to 5-6 with glacial acetic acid to obtain a 3-aminopropyltriethoxysilane / ethanol solution; 150-200 parts of anhydrous ethanol and 9-10 parts of hollow glass microspheres are mixed, and the mixture is stirred continuously while adding the above 3-aminopropyltriethoxysilane / ethanol solution. The mixture is then refluxed at 74-76℃ for 8-12 hours, filtered, washed, and dried to obtain aminated hollow glass microspheres; S2. By weight, mix 4-5 parts of polyethylene glycol diacrylate and 90-100 parts of anhydrous ethanol, and add 0.1-0.2 parts of dibutyltin tetralaurate to obtain a polyethylene glycol diacrylate / ethanol solution. Disperse the aminated hollow glass microspheres obtained in step S1 in 90-100 parts of anhydrous ethanol, and add the polyethylene glycol diacrylate / ethanol solution dropwise through a constant pressure dropping funnel at a rate of 3-5 ml / min. Under nitrogen protection, stir and react in a water bath at 58-60℃ for 10-12 h in the dark. Filter, wash, and dry in the dark to obtain the modified hollow glass microspheres.

8. A method for preparing an environmentally friendly water-soluble aerosol spray paint as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) Mix 5-10 parts of colorant and 5-10 parts of water by weight, and grind them for 1-2 hours using a basket mill to obtain component A; (2) Under light-protected conditions, mix and stir 30-50 parts of water-based resin, 2-4 parts of thickener, 1-2 parts of multifunctional monomer, and 10-20 parts of modified hollow glass microspheres for 20-30 minutes. Then add component A obtained in step (1) and continue stirring for 30-60 minutes. Finally, add 1-2 parts of composite photoinitiator and stir for 5-10 minutes to obtain an environmentally friendly water-soluble aerosol spray paint slurry. Pack the slurry into a container and inject 10-15 wt% of compressed nitrogen as a propellant to obtain the environmentally friendly water-soluble aerosol spray paint.