Chemically amplified positive photoresist as well as preparation method and application thereof

By using a mixed resin system of acid-dissociable (meth)acrylic resin and mercapto-containing resin, the balance between the footing size of the non-exposed area of ​​the photoresist and its resistance to electroplating solutions was solved, achieving high precision and electroplating resistance of the photoresist pattern.

CN121142906APending Publication Date: 2025-12-16FUYANG SINEVA MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511518163.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-23
Publication Date
2025-12-16

AI Technical Summary

Technical Problem

Existing chemically amplified photoresists struggle to balance the size of the footing at the bottom of the non-exposed area and the photoresist film's tolerance to the electroplating solution when forming resist patterns, resulting in poor-shaped electroplated products.

Method used

A mixed resin system comprising acid-dissociable (meth)acrylic resin, alkali-soluble resin and mercapto-containing resin is used. The size of the non-exposed area footing is controlled by introducing mercapto resin, and the resistance of the photoresist film to electroplating solution is improved.

Benefits of technology

It achieves good morphology of photoresist patterns, excellent resistance of photoresist films to electroplating solutions, and controllable footing size in non-exposed areas, ensuring the precision and controllability of electroplated products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121142906A_ABST
    Figure CN121142906A_ABST
Patent Text Reader

Abstract

The invention provides a chemically amplified positive photoresist as well as a preparation method and application thereof, and relates to the technical field of photoresists. The chemically amplified positive photoresist provided by the invention comprises mixed resin and sulfydryl-containing resin, wherein the mixed resin is composed of acid dissociation (methyl) acrylic resin and alkali-soluble resin; due to the addition of the (methyl) acrylic resin with the acid dissociation property, the photoresist shows excellent tolerance to an electroplating solution, so that an electroplating forming product with excellent collapse margin is obtained. And meanwhile, sulfydryl is introduced into a resin system, so that the size of the footing in a non-exposure area can be effectively controlled, and the balance between the size of the footing and the electroplating-resistant liquid is realized. After the chemical amplification type positive photoresist is exposed, a photoresist pattern with relatively good morphology can be formed.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the photoresist technical field, especially relates to a kind of chemical amplification type positive photoresist and preparation method and application thereof. BACKGROUND

[0002] In recent years, with the miniaturization of electronic equipment, semiconductor packaging technology has also achieved the results of high-density development, in these high-density packaging technologies, such as bump or metal column is led out at the edge of wafer and connected with terminal to realize rewiring, are arranged on the surface of substrate with high precision. Bump, metal column, wiring are often formed by electroplating treatment, which requires that the photoresist line of mask plate can not only ensure the appearance, but also can resist the erosion of electroplating solution well.

[0003] When using conventional chemical amplification photoresist to form a resist pattern that can be used as a metal surface electroplating template, the electroplating solution is easy to penetrate into the contact area between the photoresist film and the metal substrate during the electroplating process, and the shape of the electroplating formed product obtained in this case is often poor. At this time, the line in the non-exposed area has a proper size footing, which is beneficial to prevent the penetration of the electroplating solution in the above area. Therefore, we believe that there is a certain balance between inhibiting the size of the footing of the non-exposed area of the photoresist and improving the resistance of the photoresist film to the electroplating solution. SUMMARY

[0004] The present application aims to provide a kind of chemical amplification type positive photoresist and preparation method and application thereof, to solve the problem that the size of the footing of the non-exposed area and the resistance of the photoresist film to the electroplating solution cannot reach a balance when using conventional chemical amplification photoresist to form a resist pattern.

[0005] To achieve the above purpose, the present application provides a kind of chemical amplification type positive photoresist, comprising, by weight fraction: 30-70 parts of mixed resin, 0.1-1.5 parts of photoacid generator, 0.05-1 parts of acid diffusion inhibitor, 0.3-1 parts of thiol-containing resin, 0.05-1 parts of additive and solvent. The mixed resin comprises, by weight fraction: 20-50 parts of acid dissociation (methyl) acrylic acid resin and 10-40 parts of alkali-soluble resin.

[0006] The weight fraction of the mixed resin may be, for example, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, or any value between 30 and 70 parts; the weight fraction of the photoacid generator may be, for example, 0.1 part, 0.5 part, 1 part, 1.2 parts, 1.5 parts, or any value between 0.1 and 1.5 parts; the weight fraction of the acid diffusion inhibitor may be, for example, 0.05 part, 0.1 part, 0.2 part, 0.3 part, 0.5 part, 0.7 part, 0.9 part, 1 part, or any value between 0.05 and 1 part; the weight fraction of the thiol-containing resin may be, for example, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, or any value between 0.3 and 1 part; and the weight fraction of the additive may be, for example, 0.05 part, 0.1 part, 0.2 part, 0.3 part, 0.5 part, 0.7 part, 0.9 part, 1 part, or any value between 0.05 and 1 part.

[0007] The weight fraction of the acid-dissociable (meth)acrylic resin may be, for example, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, or any value between 20 and 50 parts; and the weight fraction of the alkali-soluble resin may be, for example, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, or any value between 10 and 40 parts.

[0008] In some embodiments, the acid-dissociable (meth)acrylic resin has a structural formula as shown below: .

[0009] In some embodiments, the acid-dissociable (meth)acrylic resin has a weight average molecular weight between 10,000 and 300,000, for example, 10,000, 20,000, 30,000, 40,000, 50,000, 80,000, 100,000, 130,000, 150,000, 200,000, 250,000, 300,000, or any value between 10,000 and 300,000, and a polydispersity between 1 and 10, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or any value between 1 and 10.

[0010] In some embodiments, the alkali-soluble resin comprises a phenolic hydroxyl structural unit; Preferably, the alkali-soluble resin comprises at least one of a phenol-formaldehyde resin and a polyhydroxystyrene resin; Preferably, the phenol-formaldehyde resin has a weight average molecular weight between 1,000 and 40,000, and the polyhydroxystyrene resin has a weight average molecular weight between 2,000 and 30,000; Preferably, the phenol-formaldehyde resin is obtained by addition condensation of a phenolic substance and an aldehyde substance in the presence of an acidic catalyst. Preferably, the phenolic substances include any one of phenol, o-cresol, m-cresol, p-cresol, m-ethylphenol, o-ethylphenol, o-butylphenol, m-butylphenol, p-ethylphenol, p-butylphenol, 2,3-xylenol, 2,4-xylenol, 2,6-xylenol, 3,4-xylenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, p-phenylphenol, resorcinol, hydroquinone, and hydroquinone monomethyl ether; the aldehyde substances include any one of formaldehyde, benzaldehyde, acetaldehyde, and nitrobenzaldehyde. Preferably, the acidic catalyst includes any one of hydrochloric acid, nitric acid, sulfuric acid, formic acid, oxalic acid, and acetic acid.

[0011] In some embodiments, the general structural formula of the thiol-containing resin is as follows: ; Wherein, R is a thiol monomer; Preferably, R is selected from any of the following structures: , , , , .

[0012] In some embodiments, the weight-average molecular weight of the thiol-containing resin is between 2000 and 4000, for example, it can be any value between 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900, 4000 or 2000-4000.

[0013] In some embodiments, the photoacid-generating agent is selected from any of the following structures: , , , .

[0014] In some embodiments, the acid diffusion inhibitor is selected from any of the following structures: , , .

[0015] This application also provides a method for preparing the above-mentioned chemically amplified positive photoresist, comprising: mixing and dissolving the raw materials to obtain the chemically amplified positive photoresist.

[0016] This application also provides the application of the above-described chemically amplified positive photoresist in the preparation of resist patterns.

[0017] Compared with the prior art, the beneficial effects of this application include: The chemically amplified positive photoresist provided in this application comprises a mixed resin consisting of an acid-dissociable (meth)acrylic resin, an alkali-soluble resin, and a mercapto-containing resin. The addition of the acid-dissociable (meth)acrylic resin enables the photoresist to exhibit excellent resistance to electroplating solutions, thereby obtaining electroplated products with excellent collapse margin. Simultaneously, the introduction of mercapto groups into the resin system can effectively control the size of the non-exposed footing, thus achieving a balance between footing size and electroplating solution resistance.

[0018] The chemically amplified positive photoresist provided in this application can form a photoresist pattern with good morphology after exposure. The photoresist film exhibits excellent resistance to electroplating solution. Large footing defects in the non-exposed area can lead to the detachment of plated metal pillars and wiring, affecting the accuracy and controllability of the pattern. By introducing mercapto monomers into the resin system, the size of the footing in the non-exposed area can be effectively improved, achieving a balance between footing size and resistance to electroplating solution. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation on the scope of this application.

[0020] Figure 1 The footing dimension (W) required to be measured for the exposure films of the embodiments and comparative examples. f A schematic diagram of ( ); Figure 2 This is a schematic diagram showing the electroplating resistance of the exposed films in the examples and comparative examples. Figure 3 This is a schematic diagram showing the electroplating resistance (no) results in the exposed films of the examples and comparative examples. Detailed Implementation

[0021] As used in this article: "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0022] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1–5” is disclosed, the described range should be interpreted as including ranges “1–4”, “1–3”, “1–2”, “1–2 and 4–5”, “1–3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0023] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.

[0024] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has "a" parts by mass and component B has "b" parts by mass, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it can mean that the mass of component A is aK and the mass of component B is bK (where K is any number representing a multiplier). It is important to understand that, unlike parts by mass, the sum of the mass parts of all components is not limited to 100 parts.

[0025] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0026] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0027] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased commercially.

[0028] Example 1 Example 1 provides a chemically amplified positive photoresist, comprising, by weight: 60 parts of mixed resin, 1.3 parts of photoacid generator, 0.2 parts of acid diffusion inhibitor, 0.8 parts of mercapto-containing resin, 0.2 parts of leveling agent DFX-18, and solvent PGMEA, with the solid content adjusted to 37 wt%.

[0029] The mixed resin comprises 24 parts of acid-dissociable (meth)acrylic resin A and 36 parts of alkali-soluble resin B. The structural formula of acid-dissociable (meth)acrylic resin A is shown below: Weight-average molecular weight Mw = 23000, polydispersity PDI = 1.75; Alkali-soluble resin B comprises: 24 parts of B-1 and 12 parts of B-2, wherein the structural formula of B-1 is: m / p=60 / 40, Mw=8000; the structural formula of B-2 is: Mw=3600, PDI=1.16.

[0030] The structural formula of the photoacid-producing agent is: .

[0031] The structural formula of the acid diffusion inhibitor is: .

[0032] The structural formula of the mercapto-containing resin E-1 is: .

[0033] The preparation method of the thiol-containing resin used in Example 1 includes the following steps: 75.00 g of tert-butyl acrylate and 25.00 g of mercaptoacrylate were weighed into a 500 ml dry three-necked flask. 1.60 g of azobisisobutyronitrile (AIB) initiator and 150.00 g of methanol solvent were also weighed into the same flask. The mixture was stirred at room temperature to dissolve the initiator. The flask was then connected to a reflux condenser, and nitrogen gas was purged through it for 10 min with stirring to replace the air. Nitrogen gas was then continuously purged, and the reaction mixture was heated to 65–70 °C and reacted under reflux for 8–12 hours. The reaction mixture was cooled to room temperature and slowly added dropwise to 2.5 L of mechanically stirred n-heptane. Precipitation was observed, and the solid product was collected by filtration. This product was dried under vacuum at 45 °C to obtain the copolymer. The molecular weight of the copolymer was determined by Shimadzu gel permeation chromatography: Mw = 2800.

[0034] Example 1 also provides a method for preparing a chemically amplified positive photoresist, comprising: adding the above-mentioned components into a container in proportion, mixing thoroughly, and shaking on a shaker for more than 48 hours to ensure that the components are completely dissolved and uniform. Subsequently, the photoresist solution is filtered using a 2μm filter membrane to remove impurities or particles, so as to ensure the purity of the photoresist solution and the quality of the final film layer.

[0035] Example 2 The only difference between Example 2 and Example 1 is that the structural formula of the mercapto-containing resin E-2 is: .

[0036] Example 3 The only difference between Example 3 and Example 1 is that the structural formula of the mercapto-containing resin E-3 is: .

[0037] Example 4 The only difference between Example 4 and Example 1 is that the structural formula of the mercapto-containing resin E-4 is: .

[0038] Example 5 The only difference between Example 5 and Example 1 is that the structural formula of the mercapto-containing resin E-5 is: .

[0039] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that the thiol-containing resin is replaced with the corresponding thiol monomer, and the structural formula of the thiol monomer E-1-1 is: .

[0040] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that the thiol-containing resin is replaced with the corresponding thiol monomer. The structural formula of the thiol monomer E-2-1 is: .

[0041] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that the thiol-containing resin is replaced with the corresponding thiol monomer. The structural formula of the thiol monomer E-3-1 is: .

[0042] Comparative Example 4 The only difference between Comparative Example 4 and Example 1 is that the thiol-containing resin is replaced with the corresponding thiol monomer. The structural formula of the thiol monomer E-4-1 is: .

[0043] Comparative Example 5 The only difference between Comparative Example 5 and Example 1 is that the thiol-containing resin is replaced with the corresponding thiol monomer. The structural formula of the thiol monomer E-5-1 is: .

[0044] Comparative Example 6 The only difference between Comparative Example 6 and Example 1 is that no mercapto-containing resin is added.

[0045] Comparative Example 7 The only difference between Comparative Example 7 and Example 1 is that acid-dissociative (meth)acrylic resin A is not added.

[0046] The formulations of the chemically amplified positive photoresists for each embodiment and comparative example are shown in Table 1.

[0047] Table 1. Formulations (parts) of chemically amplified positive photoresists for each embodiment and comparative example.

[0048] The chemically amplified positive photoresists of each embodiment and comparative example were applied to an 8-inch copper-plated silicon wafer substrate using spin coating (pre-speed + main speed), followed by heat treatment to remove the solvent (PAB: 120°C, 120s) to form a photoresist film with a thickness of 8 μm. The photoresist was then selectively exposed using a Nikon I-line stepper exposure machine through a mask at an exposure energy of 135 mJ / cm². 2 The mask was then exposed and baked on a hot plate at 110°C (PEB: 100°C, 90s); immediately after that, a 2.38 wt% tetramethylammonium hydroxide (TMAH) alkaline development was performed at 23°C for 60s using the developing device Track 8, and finally rinsed with deionized water for 60s to obtain the corresponding L / S pattern of the mask.

[0049] The exposed films prepared by the above operations were observed for their cross-sectional morphology using CD-SEM, SEM, and other equipment, and the footing dimensions (W) were measured. f A diagram illustrating the measurement of footing dimension (Wf) is shown below. Figure 1As shown. The photoresist silicon wafer prepared by the above operation was cut into 5cm*5cm pieces, and then immersed in a copper acid plating solution at room temperature for 1 hour. After that, it was taken out and observed by OM to see if the morphology of the photoresist changed, thus verifying the photoresist's resistance to the plating solution. The morphology did not change, indicating that it was OK. Figure 2 As shown; lines that are missing or deformed indicate an unacceptable shape (no), such as... Figure 3 As shown.

[0050] The performance test results of each embodiment and comparative example are shown in Table 2.

[0051] Table 2 Performance test results of each embodiment and comparative example

[0052] As can be seen from the test data in Table 2, the acid-dissociable (meth)acrylic resin with a specific structural unit (A0) introduced into the chemically amplified positive photoresist system of this application exhibits excellent resistance to electroplating solutions, thereby obtaining electroplated molded products with excellent collapse margin; at the same time, the addition of a mercapto-containing acrylic resin component that satisfies the structural unit (E0) can effectively control the size of the photoresist footing on the substrate surface. The combination of the two achieves a balance between controllable footing and resistance to electroplating solutions.

[0053] Based on the results of the embodiments and comparative examples, it is evident that adding a mercapto-containing resin in the embodiments reduces the footing size, but not to the point of making it too small, as an excessively small footing size would easily lead to a decrease in electroplating resistance. However, in the comparative examples, adding the corresponding mercapto monomers resulted in an excessively small footing size, thus deteriorating electroplating resistance. Therefore, the solution in this application achieves a good balance between footing size and electroplating resistance by adding an acid-dissociable (meth)acrylic resin and a mercapto-containing resin.

[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

[0055] Furthermore, those skilled in the art will understand that although some embodiments herein include certain features included in other embodiments but not others, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the foregoing claims, any of the claimed embodiments can be used in any combination. The information disclosed in this background section is intended only to enhance the understanding of the general background of this application and should not be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

Claims

1. A chemically amplified positive photoresist, characterized in that, By weight, it includes: 30-70 parts of mixed resin, 0.1-1.5 parts of photoacid-generating agent, 0.05-1 parts of acid diffusion inhibitor, 0.3-1 parts of mercapto-containing resin, 0.05-1 parts of additives and solvent; The mixed resin, by weight, comprises: 20-50 parts of acid-dissociable (meth)acrylic resin and 10-40 parts of alkali-soluble resin.

2. The chemically amplified positive photoresist according to claim 1, characterized in that, The structural formula of the acid-dissociable (meth)acrylic resin is shown below: 。 3. The chemically amplified positive photoresist according to claim 2, characterized in that, The weight-average molecular weight of the acid-dissociable (meth)acrylic resin is between 10,000 and 300,000, and the polydispersity is between 1 and 10.

4. The chemically amplified positive photoresist according to claim 1, characterized in that, The alkali-soluble resin includes phenolic hydroxyl structural units; Preferably, the alkali-soluble resin includes at least one of phenolic resin and polyhydroxystyrene resin; Preferably, the weight-average molecular weight of the phenolic resin is between 1,000 and 40,000, and the weight-average molecular weight of the polyhydroxystyrene resin is between 2,000 and 30,000. Preferably, the phenolic resin is obtained by addition condensation of phenolic substances and aldehyde substances in the presence of an acidic catalyst; Preferably, the phenolic substances include any one of phenol, o-cresol, m-cresol, p-cresol, m-ethylphenol, o-ethylphenol, o-butylphenol, m-butylphenol, p-ethylphenol, p-butylphenol, 2,3-xylenol, 2,4-xylenol, 2,6-xylenol, 3,4-xylenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, p-phenylphenol, resorcinol, hydroquinone, and hydroquinone monomethyl ether; the aldehyde substances include any one of formaldehyde, benzaldehyde, acetaldehyde, and nitrobenzaldehyde. Preferably, the acidic catalyst includes any one of hydrochloric acid, nitric acid, sulfuric acid, formic acid, oxalic acid, and acetic acid.

5. The chemically amplified positive photoresist according to claim 1, characterized in that, The general structural formula of the mercapto-containing resin is shown below: ; Wherein, R is a thiol monomer; Preferably, R is selected from any of the following structures: 、 、 、 、 。 6. The chemically amplified positive photoresist according to claim 5, characterized in that, The weight-average molecular weight of the mercapto-containing resin is between 2000 and 4000.

7. The chemically amplified positive photoresist according to claim 1, characterized in that, The photoacid-generating agent is selected from any of the following structures: 、 、 、 。 8. The chemically amplified positive photoresist according to claim 1, characterized in that, The acid diffusion inhibitor is selected from any of the following structures: 、 、 。 9. A method for preparing a chemically amplified positive photoresist according to any one of claims 1 to 8, characterized in that, include: The raw materials are mixed and dissolved to obtain the chemically amplified positive photoresist.

10. The use of a chemically amplified positive photoresist according to any one of claims 1 to 8 in the preparation of resist patterns.