A low-temperature, high-pressure resistant lithium iron phosphate cathode material, its preparation method and battery
By preparing lithium iron phosphate cathode materials with a particle size distribution of large, medium and small through gradient sintering, the problems of slowed lithium-ion diffusion rate and increased interfacial impedance in lithium iron phosphate cathode materials at low temperatures were solved, achieving a balance between high actual density and low-temperature performance, thus improving battery performance and preparation efficiency.
Patent Information
- Application Number
- CN202511381397.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-09-25
AI Technical Summary
Existing lithium iron phosphate cathode materials suffer from slower lithium-ion diffusion rates and increased interfacial impedance at low temperatures, leading to decreased capacity and a lower discharge voltage plateau, making it difficult to balance high real density and low-temperature performance.
Different precursor powders were prepared using different iron sources. Gradient sintering technology was used to control the primary particle size and nucleation growth, forming a gradation of large, medium and small particles. Combined with nano-sized particles, the lithium-ion diffusion path was shortened and ion transport was optimized.
It achieves a balance between high actual density and low-temperature performance, improves the volumetric energy density and low-temperature capacity retention of the battery, simplifies the manufacturing process, and reduces costs.
Smart Images

Figure CN121180969B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium iron phosphate materials technology, and in particular to a low-temperature, high-pressure resistant lithium iron phosphate cathode material, its preparation method, and a battery thereof. Background Technology
[0002] The statements herein provide only background information in relation to this invention and do not necessarily constitute prior art.
[0003] Lithium iron phosphate (LFP) cathode materials are widely used in the electric vehicle field due to their high safety, low cost, and long lifespan. As the range requirements for electric vehicles increase, higher demands are placed on volumetric energy density. Furthermore, the significant temperature differences between northern and southern my country limit the application range of LFP due to its poor low-temperature performance. Therefore, LFP products with high compaction and excellent low-temperature performance are needed.
[0004] Compacted density refers to the mass per unit volume of an electrode sheet after it has been compressed under a specific pressure. Increasing compacted density means packing more active material into a limited battery casing, thereby significantly improving the battery's volumetric energy density. Using a gradation of large, medium, and small particles to increase compacted density is a feasible method. A commonly used method is to first prepare lithium iron phosphate particles of different sizes, and then mix them in a specific ratio. However, since the particles are only bonded through contact, there are issues with large interfacial gaps and weak bonding forces. During rolling, particles may slip or break, making it difficult to fully eliminate voids and resulting in limited improvement in compacted density.
[0005] The poor low-temperature performance of lithium iron phosphate cathode materials is mainly manifested in a sharp decrease in capacity and a reduction in discharge voltage plateau at low temperatures. The root cause is the slowed diffusion rate of lithium ions in the solid phase and the decrease in electrolyte conductivity and increase in interfacial impedance at low temperatures. One of the most effective methods to improve its low-temperature performance is to scale the active material to the nanoscale, shortening the diffusion path of lithium ions in the solid phase, and utilizing the agglomeration of nanoscale primary particles to obtain micron-sized spherical secondary particles. However, this method struggles to effectively eliminate the voids between nanoscale primary particles during rolling, making it difficult to achieve a high compaction density. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the purpose of this invention is to provide a low-temperature, high-pressure resistant lithium iron phosphate cathode material, its preparation method, and a battery thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides a method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material, comprising the following steps: Iron source, lithium source, phosphorus source, carbon source, dopant and dispersant are wet-mixed in proportion to obtain slurry. The slurry is then ground and dried to obtain precursor powder. By replacing the iron source, at least two precursor powders can be prepared; After the different precursor powders are mixed evenly in proportion, they are subjected to gradient sintering in an inert atmosphere to obtain the final product.
[0008] Secondly, the present invention provides a low-temperature, high-pressure lithium iron phosphate cathode material, which is prepared by the aforementioned preparation method.
[0009] Thirdly, the present invention provides a battery in which the active material of the positive electrode is the low-temperature resistant, high-pressure lithium iron phosphate positive electrode material.
[0010] The beneficial effects achieved by one or more embodiments of the present invention described above are as follows: To prepare lithium iron phosphate cathode materials with excellent high-pressure, low-temperature performance, this invention utilizes different precursors to prepare lithium iron phosphate, fully leveraging the performance advantages of each precursor. Furthermore, the sintering method is optimized to produce high-pressure, high-pressure lithium iron phosphate products with well-proportioned particle sizes, rounded particle shapes, and excellent coating.
[0011] Gradient sintering precisely controls the particle size by adapting the nucleation / growth temperature of different precursors through multiple temperature segments, achieving multi-level gradation of large, medium and small particles (increasing compaction density); at the same time, it utilizes nanoscale particles to shorten the lithium-ion diffusion path, spherical particles to optimize ion transport, and the advantages of composite precursors to reduce interfacial impedance (improving low-temperature performance), ultimately balancing high compaction and low-temperature resistance, while solving the problems of long processing flow, high equipment requirements and high preparation cost. Attached Figure Description
[0012] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0013] Figure 1 It is the TG-DTA curve of the ferrous oxalate system mixture; Figure 2 It is the TG-DSC curve of the iron oxide system mixture; Figure 3 It is the TG-DTA curve of the iron phosphate system mixture; Figure 4 This is a SEM image of the lithium iron phosphate cathode material in Example 3 of the present invention. Detailed Implementation
[0014] It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0015] In a first aspect, the present invention provides a method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material, comprising the following steps: Iron source, lithium source, phosphorus source, carbon source, dopant and dispersant are wet-mixed in proportion to obtain slurry. The slurry is then ground and dried to obtain precursor powder. By replacing the iron source, at least two precursor powders can be prepared; After the different precursor powders are mixed evenly in proportion, they are subjected to gradient sintering in an inert atmosphere to obtain the final product.
[0016] like Figure 1 As shown, in the ferrous oxalate system, the formation and crystallization process of lithium iron phosphate only begins after 400℃; after about 390℃, the TG curve basically stops changing, but there is an endothermic peak at 400℃ and an exothermic peak at 450~500℃, indicating that the formation of lithium iron phosphate should be between 400~500℃.
[0017] like Figure 2 As shown in the thermogravimetric curves, in the iron oxide red system, significant mass loss occurs in the sample at temperatures of 200℃ and 600℃, accompanied by endothermic reactions. Before 200℃, Fe2O3 is reduced to a mixture of divalent and trivalent Fe3O4; from 200℃ to 600℃, Fe3O4 is further reduced to FeO; from 600℃ to 800℃, LiFePO4 / C begins to form, and the reaction is completed at 800℃.
[0018] like Figure 3 As shown, in the ferric phosphate system, the weight loss of the mixture mainly occurs in the 200~500℃ range, due to the decomposition of glucose and the reduction of Fe by carbon. 3+ The appearance of a small exothermic peak on the DTA curve at around 510℃, along with a rapid decrease in sample mass, indicates that LiFePO4 / C has begun to form, and the lost mass is caused by the loss of carbon from lithium carbonate. After 700℃, the sample mass hardly changes anymore, and the DTA curve also tends to flatten out, indicating that the reaction for synthesizing the LiFePO4 / C composite material has been completed.
[0019] The thermogravimetric curves of lithium iron phosphate prepared by ferrous oxalate, iron oxide red, and iron phosphate show that the nucleation and growth temperatures required for different precursors vary significantly. The size of primary lithium iron phosphate particles can be controlled by a one-step multi-stage sintering method (i.e., gradient sintering). This method can be used to prepare lithium iron phosphate materials with different primary particle sizes, achieve multi-level gradation of materials, and prepare high-pressure compaction lithium iron phosphate products.
[0020] Nanoscale primary particles generated by gradient sintering, such as small particles generated at lower temperatures in the iron phosphate system, can significantly shorten the diffusion distance of lithium ions in the solid phase and alleviate the problem of slowed lithium ion diffusion rate at low temperatures.
[0021] If multiple iron sources are directly mixed to prepare a single precursor, the reaction temperature requirements of different iron sources will interfere with each other during sintering, which may lead to insufficient reaction of some iron sources or excessive grain growth, making it impossible to accurately control the primary particle size. Moreover, even if gradient sintering is used during the sintering process, it is difficult to generate multi-level particles with significant size differences, thus failing to effectively improve the compaction density.
[0022] In this invention, different precursor powders are first prepared using different iron sources. After the different precursor powders are mixed evenly, gradient sintering is carried out. The reaction conditions of each iron source can be optimized independently to ensure that each precursor has specific particle morphology and size potential before mixing.
[0023] Existing technologies that "prepare particles of different sizes and then mix them" involve physical mixing, where particles are only bonded through contact. This often results in large interfacial gaps and weak bonding forces, leading to particle slippage or breakage during rolling and making it difficult to fully eliminate voids. This invention, through "gradient sintering after mixing different precursors," allows different iron sources to nucleate and grow in situ during the same sintering process. The three types of particles form a composite structure of "chemical bonding and mechanical interlocking" through sintering, resulting in tighter interfacial bonding between particles. This facilitates more efficient stacking during rolling, with small particles filling the gaps between medium particles and medium particles filling the gaps between large particles, significantly improving compaction density.
[0024] Furthermore, existing technologies require independent control of multiple sets of synthesis parameters (such as sintering temperature, time, and raw material ratio) to prepare particles of different sizes in batches, resulting in high process complexity and significant batch-to-batch variations. In this invention, only the type of iron source needs to be adjusted for different precursors, and pretreatment parameters such as grinding and spray drying can be uniformly optimized, avoiding the cost accumulation of multiple processes. Gradient sintering, with its "one-step forming," replaces the cumbersome steps of "batch sintering + mixing," reducing the risk of particle contamination or breakage caused by intermediate steps and improving product consistency.
[0025] In some embodiments, the iron source is selected from ferrous sulfate, ferric nitrate, ferrous chloride, ferrous oxalate, iron oxide red, or ferric phosphate.
[0026] Preferably, the iron source is at least two of ferrous oxalate, iron oxide red, and ferric phosphate.
[0027] More preferably, the iron source is ferrous oxalate, iron oxide red, and ferric phosphate.
[0028] The precursor prepared from ferrous oxalate generates gas during thermal decomposition, reducing particle agglomeration and making the primary particles more spherical with good roundness. This results in shorter electron migration channels and ion diffusion paths, reducing polarization. The material prepared from iron oxide red has a dense structure, excellent rate performance, and a stable discharge plateau. The material prepared from iron phosphate has good processability, a smooth interface, and reduced interfacial impedance at low temperatures. Gradient sintering combines the advantages of various materials, synergistically improving capacity retention and voltage plateau at low temperatures.
[0029] Preferably, the drying process during the preparation of precursor powder is carried out using a spray drying method.
[0030] Further preferred embodiments show that the precursor powder prepared with ferrous oxalate as the iron source has a D50 of 60-70 μm, the precursor powder prepared with ferric phosphate as the iron source has a D50 of 20-25 μm, and the precursor powder prepared with iron oxide red as the iron source has a D50 of 6-8 μm.
[0031] By employing spray drying and strictly controlling the spray drying parameters during the drying process, the particle size of precursor powders prepared from different iron sources is controlled within a specific range. For example, the precursor powder of ferrous oxalate has a larger particle size, while the precursor powders of iron phosphate and iron oxide red have smaller particle sizes. After mixing, a primary particle gradation is formed, which, in conjunction with subsequent gradient sintering, produces a well-graded lithium iron phosphate product and effectively improves its compaction.
[0032] More preferably, when mixing, the mass ratio of the precursor powder prepared from ferrous oxalate, iron oxide red, and ferric phosphate is 6-8:0.8-1.2:1-3, preferably 7:1:2. According to the Furnas theoretical model, the powder bulk density is optimal when the volume ratio of large, medium, and small particles is 73.5:19.3:7.2. However, iron oxide red has the highest density, followed by ferric phosphate, and ferrous oxalate has the lowest density. Therefore, this ratio is adopted.
[0033] Preferably, the gradient sintering process includes at least the following steps: first, heating to 350-450℃ and holding for 1.5-2.5 hours; then heating to 700-800℃ and holding for 2-10 hours.
[0034] More preferably, the gradient sintering procedure is as follows: first, heat to 350-450℃ and hold for 1.5-2.5 hours; then heat to 500-600℃ and hold for 1.5-2.5 hours; then heat to 700-800℃ and hold for 2-4 hours; finally, heat to 810-850℃ and hold for 2-4 hours.
[0035] Further preferably, after sintering, the sintered material is rapidly cooled with ice water. Rapid cooling with ice water after sintering can inhibit excessive growth of primary particles, maintain the dispersibility and structural stability of nano-sized particles, and further maintain short diffusion paths and good ion transport capabilities.
[0036] More preferably, the gradient sintering procedure is as follows: first, heat to 350-450℃ and hold for 1.5-2.5 hours; then heat to 550-600℃ and hold for 1.5-2.5 hours; then heat to 740-780℃ and hold for 2-4 hours; finally, heat to 820-840℃ and hold for 2-4 hours.
[0037] Gradient sintering amplifies the gradation effect. In the low-temperature section (350-450℃), under oxygen-deficient conditions of the carbon source, thermal decomposition promotes the nucleation of ferrous oxalate precursor into nanoparticles. In the medium-temperature section (500-600℃), the ferric phosphate precursor is driven to grow into small particles, and the ferrous oxalate nanoparticles gradually grow. In the high-temperature section (700-850℃), the iron oxide red precursor forms dense small particles, and the ferrous oxalate system further grows into large particles, while the ferric phosphate system grows into medium-sized particles.
[0038] The temperature range is refined to suit the nucleation-growth requirements of different iron sources, avoiding insufficient reaction or excessive growth. Specifically: At 350-450℃ (low temperature range), the nucleation of ferrous oxalate precursor is preferentially promoted, generating nanoscale particles (according to the thermogravimetric curve, iron phosphate starts to react at 510℃, the low temperature range mainly provides the necessary conditions for the nucleation of the ferrous oxalate system, and subsequent sintering mainly controls the growth of lithium iron phosphate crystal nuclei of ferrous oxalate. This invention controls the growth rate in the high temperature range by doping with an appropriate amount of TiO2 to prevent subsequent abnormal growth).
[0039] At 550-600℃ (medium temperature range), the iron phosphate precursor is specifically driven to grow into lithium iron phosphate crystal nuclei; the ferrous oxalate system has better crystallinity at this temperature, and the medium temperature range further controls its slow grain growth, ensuring the roundness of the particles while avoiding agglomeration.
[0040] The crystallization reaction of the iron phosphate system is completed at 740-780℃ (the reaction is completed after 700℃), and the crystals grow. The growth rate is controlled by adding an appropriate amount of NH4VO3. During this process, the iron oxide red system begins to form crystal nuclei. Further heating to 820-840℃ promotes the formation of dense small particles of iron oxide red precursor (iron oxide red requires 600~800℃ to react; the high temperature range ensures its crystal form integrity and improves rate performance), avoiding the problem of incomplete crystal growth and low phase purity caused by a single high temperature range (700-800℃).
[0041] The nanoparticles (ferrous oxalate source) generated in the low-temperature section are isolated by medium and large particles in the medium and high-temperature sections to avoid agglomeration and coarsening; the iron oxide red in the high-temperature section generates well-crystallized nanoparticles, which grow slowly under the action of ferrous oxalate and iron phosphate dopants, avoiding the problem of "small particles disappearing and large particles growing excessively" caused by high temperature alone, and ensuring the long-term stability of multi-level gradation.
[0042] Therefore, this gradient sintering process can generate large, medium and small particles with more significant size differences, which can more effectively reduce the packing porosity and make it easier to eliminate voids during rolling, thereby improving the compaction density.
[0043] The nanoparticles (iron oxide source) generated in the high-temperature section and the rounded medium-sized particles (iron phosphate source) in the medium-temperature section can shorten the lithium-ion diffusion distance and alleviate the problem of slowed diffusion rate at low temperature. Segmented temperature control reduces particle agglomeration, maintains the smooth interface characteristics of the iron phosphate source, and avoids the destruction of carbon coating caused by long-term sintering in a single high-temperature section, thereby reducing interface polarization at low temperature.
[0044] In some embodiments, different precursor powders are thoroughly mixed evenly using a ribbon mixer.
[0045] In some embodiments, the phosphoric acid is selected from at least one of phosphoric acid, sodium monohydrogen phosphate, sodium dihydrogen phosphate, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, lithium monohydrogen phosphate, or lithium dihydrogen phosphate. Alternatively, the carbon source is selected from at least one of glucose, sucrose, polyethylene glycol, citric acid, or starch; Alternatively, the dopant is selected from at least one of titanium dioxide, ammonium metavanadate, niobium pentoxide, magnesium oxide, or aluminum oxide; Alternatively, the dispersant may be selected from water and / or ethanol.
[0046] In some embodiments, the pulverization is air jet pulverization, with an air pressure of 0.3-0.5 MPa and a grading frequency of 30-40 Hz.
[0047] Secondly, the present invention provides a low-temperature, high-pressure lithium iron phosphate cathode material, which is prepared by the aforementioned preparation method.
[0048] Thirdly, the present invention provides a battery in which the active material of the positive electrode is the low-temperature resistant, high-pressure lithium iron phosphate positive electrode material.
[0049] The present invention will be further described below with reference to the embodiments.
[0050] Example 1 A method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material includes the following steps: 1. Ferrous oxalate and lithium dihydrogen phosphate were mixed in a molar ratio of 1:1.02 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide were then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate was 9%, the weight ratio of polyethylene glycol to ferrous oxalate was 5%, and the weight ratio of titanium dioxide to ferrous oxalate was 0.4%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0051] 2. Slurry A is milled to control the milling particle size at 0.55~0.75μm to obtain nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 60-70μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0052] 4. Grind slurry C to control the particle size to 0.15~0.25μm to obtain nano-sized slurry; spray dry the nano-sized slurry to control the inlet air temperature to 240℃, the outlet air temperature to 90℃, and the atomization frequency to 35Hz to obtain spray powder D with a spray particle size D50 = 20-25μm. 5. Spray powder B and spray powder D are fully physically mixed at a mass ratio of 7:3 using a ribbon mixer to obtain spray powder E.
[0053] 6. Place the spray powder E in a roller kiln and sinter it under a nitrogen atmosphere. The heating rate is 3℃ / min. Sinter to 400℃ and hold for 2 hours. Then, the heating rate is 5℃ / min. The sintering temperature is 760℃ and the sintering time is 9 hours. The sintered material is then obtained by water cooling. The sintered material was pulverized using an air jet mill, with the air pressure controlled at 0.32 MPa and the classification frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm. Finally, further impurity removal (removal of magnetic foreign matter such as that introduced by equipment wear), mixing, and packaging yield the finished lithium iron phosphate product.
[0054] Example 2 A method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material includes the following steps: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.02 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to the mixture to obtain a mixture in which the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.4%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0055] 2. Slurry A is milled to control the milling particle size at 0.55~0.75μm to obtain nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 60-70μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry C with a solid content of 45-55%.
[0056] 4. The slurry C is sand-milled, and the sand-milling particle size is controlled at 0.15~0.25μm to obtain nano-sized sand-milled slurry; the nano-sized sand-milled slurry is spray-dried, and the inlet air temperature is controlled at 230℃, the outlet air temperature at 90℃, and the atomization frequency at 33Hz to obtain spray powder D with a spray particle size D50 = 20-25μm. 5. Add 98% pure iron oxide red, ammonium dihydrogen phosphate and lithium carbonate to the reaction vessel in a molar ratio of 1:1:1.02. Add glucose and polyethylene glycol to obtain a mixture. The weight ratio of glucose to iron oxide red is 9:100 and the weight ratio of polyethylene glycol to iron oxide red is 5:100. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0057] 6. Grind slurry E to control the particle size of 0.1~0.15μm to obtain nano-sized slurry; spray dry the nano-sized slurry to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 47Hz to obtain spray powder F with a spray particle size D50=6-8μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a weight ratio of 7:1:2 to obtain spray powder G.
[0058] 8. Place the above sprayed material in a roller kiln and sinter it under a nitrogen atmosphere. The heating rate is 3℃ / min, and the sintering temperature is 400℃. Hold the temperature for 2 hours, then the heating rate is 5℃ / min, the sintering temperature is 760℃, and the sintering time is 9 hours. Finally, the sintered material is obtained by water cooling.
[0059] The sintered material is pulverized using an air jet mill, with the air pressure controlled at 0.35 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further purified, mixed, and packaged to obtain the finished lithium iron phosphate product.
[0060] Example 3 A method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material includes the following steps: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.03 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.45%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0061] 2. Slurry A is milled to control the milling particle size at 0.55~0.75μm to obtain nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 60-70μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0062] 4. Grind slurry C to control the particle size of 0.15~0.25μm to obtain nano-sized slurry; spray dry the nano-sized slurry to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 35Hz to obtain spray powder D with a spray particle size D50 = 20~25μm. 5. Iron oxide red with a purity of 98%, ammonium dihydrogen phosphate, and lithium carbonate are added to a reaction vessel in a molar ratio of 1:1:1.02. Glucose and polyethylene glycol are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron oxide red is 9% and the weight ratio of polyethylene glycol to iron oxide red is 5%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0063] 6. The above mixed slurry E is milled to control the milling particle size of 0.1~0.15μm to obtain nano-milled slurry; the nano-milled slurry is spray-dried to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 43Hz to obtain spray powder F with a spray particle size D50=6-8μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a mass ratio of 7:1:2 to obtain spray powder G.
[0064] The above-mentioned sprayed powder G was placed in a roller kiln and sintered under a nitrogen atmosphere. The heating rate was 3℃ / min, and the sintering temperature was 400℃. The temperature was held for 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 570℃. The holding time was 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 760℃. The holding time was 3 hours. Then the temperature was increased to 830℃ at a heating rate of 5℃ / min and held for 3 hours. Finally, the sintered material was obtained by rapid cooling with chilled water.
[0065] Since the three precursors require different sintering temperatures, lithium iron phosphate materials with three particle sizes (large, medium, and small) are prepared by controlling the nucleation and growth time through a three-stage sintering method.
[0066] The final sintering material was pulverized using an air jet mill, with the air pressure controlled at 0.35 MPa and the classification frequency at 30-40 Hz, to obtain pulverized material with particle sizes of D10 ≥ 0.15, D50 = 0.7-1.8 μm, D90 < 10 μm, and D100 < 25 μm. Finally, further impurity removal, mixing, and packaging were performed to obtain the finished lithium iron phosphate product, the SEM image of which is shown below. Figure 4As shown, it can be seen that the individual particles have good roundness and there are three particle sizes: large, medium and small.
[0067] Comparative Example 1 The only difference from Example 1 is that ferrous oxalate in step 1 of Example 1 is replaced with ferric phosphate; all other aspects are the same as in Example 1. The specific preparation method is as follows: 1. Iron phosphate with an iron-to-phosphorus ratio of 0.96 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and titanium dioxide are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of titanium dioxide to iron phosphate is 0.45%. Add an appropriate amount of pure water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0068] 2. Slurry A is sand-milled, and the sand-milling particle size is controlled at 0.55~0.75μm to obtain nano-sized sand-milled slurry; the nano-sized sand-milled slurry is spray-dried, and the inlet air temperature is controlled at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25~30Hz to obtain spray powder B with a spray particle size D50=60-70μm; 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0069] 4. Grind slurry C to control the particle size of 0.15~0.25μm to obtain nano-sized slurry; spray dry the nano-sized slurry to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 50Hz to obtain spray powder D with a spray particle size D50 = 10~30μm. 5. Spray powder B and spray powder D are fully physically mixed at a mass ratio of 2:1 using a ribbon mixer to obtain spray powder E.
[0070] The above-mentioned sprayed material was placed in a roller kiln and sintered under a nitrogen atmosphere at a heating rate of 3℃ / min to 400℃ and held for 2 hours. Then, the heating rate was increased to 5℃ / min, the sintering temperature was 760℃, and the sintering time was 9 hours. The sintered material was then obtained by water cooling.
[0071] The sintered material is pulverized using an air jet mill, with the air pressure controlled at 0.32 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further purified, mixed, and packaged to obtain the finished lithium iron phosphate product.
[0072] Comparative Example 2 The difference from Example 3 is that the D50 of both spray powder B and spray powder D prepared in step 2 is 6-8 μm, while all other aspects are the same as in Example 3. The specific preparation method is as follows: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.03 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.45%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0073] 2. Slurry A is sand-milled, and the sand-milling particle size is controlled at 0.55~0.75μm to obtain nano-sized sand-milled slurry; the nano-sized sand-milled slurry is spray-dried, and the inlet air temperature is controlled at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50=6-8μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0074] 4. The slurry C is sand-milled, and the sand-milling particle size is controlled at 0.15~0.25μm to obtain nano-sized sand-milled slurry; the nano-sized sand-milled slurry is spray-dried, and the inlet air temperature is controlled at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 35Hz to obtain spray powder D with a spray particle size D50=6-8μm. 5. Iron oxide red with a purity of 98%, ammonium dihydrogen phosphate, and lithium carbonate are added to a reaction vessel in a molar ratio of 1:1:1.02. Glucose and polyethylene glycol are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron oxide red is 9% and the weight ratio of polyethylene glycol to iron oxide red is 5%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0075] 6. The above mixed slurry E is milled to control the milling particle size of 0.1~0.15μm to obtain nano-milled slurry; the nano-milled slurry is spray-dried to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 43Hz to obtain spray powder F with a spray particle size D50=6-8μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a mass ratio of 7:1:2 to obtain spray powder G.
[0076] The above-mentioned sprayed powder G was placed in a roller kiln and sintered under a nitrogen atmosphere. The heating rate was 3℃ / min, and the sintering temperature was 400℃. The temperature was held for 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 570℃. The holding time was 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 760℃. The holding time was 3 hours. Then the temperature was increased to 830℃ at a heating rate of 5℃ / min and held for 3 hours. Finally, the sintered material was obtained by rapid cooling with chilled water.
[0077] Since the three precursors require different sintering temperatures, lithium iron phosphate materials with three particle sizes (large, medium, and small) are prepared by controlling the nucleation and growth time through a three-stage sintering method.
[0078] The final sintering material is pulverized by an air jet mill, with the air pressure controlled at 0.35 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further impurity removed and mixed.
[0079] Comparative Example 3 The difference from Example 3 is that the D50 of the spray powders B, D, and F prepared in step 2 are all 20-25 μm; otherwise, they are the same as in Example 3. The specific preparation method is as follows: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.03 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.45%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0080] 2. Slurry A is sand-milled, and the sand-milling particle size is controlled at 0.55~0.75μm to obtain nano-sized sand-milled slurry; the nano-sized sand-milled slurry is spray-dried, and the inlet air temperature is controlled at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 20~25μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0081] 4. Grind slurry C with sand to control the sand particle size at 0.15~0.25μm to obtain nano-sized sand-milled slurry; spray dry the nano-sized sand-milled slurry with the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 30-35Hz to obtain spray powder D with a spray particle size D50 = 20~25μm. 5. Iron oxide red with a purity of 98%, ammonium dihydrogen phosphate, and lithium carbonate are added to a reaction vessel in a molar ratio of 1:1:1.02. Glucose and polyethylene glycol are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron oxide red is 9% and the weight ratio of polyethylene glycol to iron oxide red is 5%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0082] 6. The above mixed slurry E is milled to control the milling particle size at 0.1~0.15μm to obtain a nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 43Hz to obtain a spray powder F with a spray particle size D50 of 20~25μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a mass ratio of 7:1:2 to obtain spray powder G.
[0083] The above-mentioned sprayed powder G was placed in a roller kiln and sintered under a nitrogen atmosphere. The heating rate was 3℃ / min, and the sintering temperature was 400℃. The temperature was held for 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 570℃. The holding time was 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 760℃. The holding time was 3 hours. Then the temperature was increased to 830℃ at a heating rate of 5℃ / min and held for 3 hours. Finally, the sintered material was obtained by rapid cooling with chilled water.
[0084] Since the three precursors require different sintering temperatures, lithium iron phosphate materials with three particle sizes (large, medium, and small) are prepared by controlling the nucleation and growth time through a three-stage sintering method.
[0085] The final sintering material is pulverized by an air jet mill, with the air pressure controlled at 0.35 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further sieved and mixed.
[0086] Comparative Example 4 The difference from Example 3 is that the D50 of the spray powders B, D, and F prepared in step 2 are all 60-70 μm, while all other aspects are the same as in Example 3. The specific preparation method is as follows: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.03 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.45%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0087] 2. Slurry A is milled to control the milling particle size at 0.55~0.75μm to obtain nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 60-70μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0088] 4. Grind slurry C to control the particle size to 0.15~0.25μm to obtain nano-sized slurry; spray dry the nano-sized slurry to control the inlet air temperature to 240℃, the outlet air temperature to 90℃, and the atomization frequency to 30-35Hz to obtain spray powder D with a spray particle size D50=60-70μm. 5. Iron oxide red with a purity of 98%, ammonium dihydrogen phosphate, and lithium carbonate are added to a reaction vessel in a molar ratio of 1:1:1.02. Glucose and polyethylene glycol are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron oxide red is 9% and the weight ratio of polyethylene glycol to iron oxide red is 5%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0089] 6. The above mixed slurry E is milled to control the milling particle size of 0.1~0.15μm to obtain nano-milled slurry; the nano-milled slurry is spray-dried to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 43Hz to obtain spray powder F with a spray particle size D50 of 60-70μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a mass ratio of 7:1:2 to obtain spray powder G.
[0090] The above-mentioned sprayed powder G was placed in a roller kiln and sintered under a nitrogen atmosphere. The heating rate was 3℃ / min, and the sintering temperature was 400℃. The temperature was held for 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 570℃. The holding time was 2 hours. Then the heating rate was 5℃ / min, and the sintering temperature was 760℃. The holding time was 3 hours. Then the temperature was increased to 830℃ at a heating rate of 5℃ / min and held for 3 hours. Finally, the sintered material was obtained by rapid cooling with chilled water.
[0091] Since the three precursors require different sintering temperatures, lithium iron phosphate materials with three particle sizes (large, medium, and small) are prepared by controlling the nucleation and growth time through a three-stage sintering method.
[0092] The final sintering material is pulverized by an air jet mill, with the air pressure controlled at 0.35 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further impurity removed and mixed.
[0093] Comparative Example 5 The difference from Example 3 is that in step 7, during the sintering process, the phrase "then the heating rate is 5℃ / min, the sintering temperature is 760℃, the holding time is 3h, and then the temperature is increased to 830℃ at a heating rate of 5℃ / min, and held for 3h" is replaced with "then the heating rate is 5℃ / min, the temperature is increased to 830℃, and held for 6h". All other steps are the same as in Example 3. The specific preparation method is as follows: 1. Ferrous oxalate and lithium dihydrogen phosphate are mixed in a molar ratio of 1:1.03 and added to a reaction vessel. Glucose, polyethylene glycol, and titanium dioxide are then added to obtain a mixture. In the mixture, the weight ratio of glucose to ferrous oxalate is 9%, the weight ratio of polyethylene glycol to ferrous oxalate is 5%, and the weight ratio of titanium dioxide to ferrous oxalate is 0.45%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 60 minutes to obtain a uniformly mixed slurry A with a solid content of 35%.
[0094] 2. Slurry A is milled to control the milling particle size at 0.55~0.75μm to obtain nano-sized milled slurry; the nano-sized milled slurry is spray-dried to control the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 25Hz to obtain spray powder B with a spray particle size D50 of 60-70μm. 3. Iron phosphate with an iron-to-phosphorus ratio of 0.98 and lithium carbonate are added to a reaction vessel at a molar ratio of 1:1.02. Glucose, polyethylene glycol, and ammonium metavanadate are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron phosphate is 9%, the weight ratio of polyethylene glycol to iron phosphate is 5%, and the weight ratio of ammonium metavanadate to iron phosphate is 0.15%. Add an appropriate amount of water to the mixture and stir at high speed in a reactor for 60 minutes to obtain a slurry C with a solid content of 50% that is uniformly mixed.
[0095] 4. Grind slurry C with sand to control the sand particle size at 0.15~0.25μm to obtain nano-sized sand-milled slurry; spray dry the nano-sized sand-milled slurry with the inlet air temperature at 240℃, the outlet air temperature at 90℃, and the atomization frequency at 30-35Hz to obtain spray powder D with a spray particle size D50 = 20~25μm. 5. Iron oxide red with a purity of 98%, ammonium dihydrogen phosphate, and lithium carbonate are added to a reaction vessel in a molar ratio of 1:1:1.02. Glucose and polyethylene glycol are then added to the mixture to obtain a mixture in which the weight ratio of glucose to iron oxide red is 9% and the weight ratio of polyethylene glycol to iron oxide red is 5%. Add an appropriate amount of ethanol to the mixture and stir at high speed in a reactor for 90 minutes to obtain a uniformly mixed slurry E with a solid content of 50%.
[0096] 6. The above mixed slurry E is milled to control the milling particle size of 0.1~0.15μm to obtain nano-milled slurry; the nano-milled slurry is spray-dried to control the inlet air temperature of 240℃, the outlet air temperature of 90℃, and the atomization frequency of 43Hz to obtain spray powder F with a spray particle size D50=6-8μm. 7. Spray powders B, D and F are fully physically mixed by ribbon mixing at a mass ratio of 7:1:2 to obtain spray powder G.
[0097] The above-mentioned sprayed powder G was placed in a roller kiln and sintered under a nitrogen atmosphere. The heating rate was 3℃ / min, and the sintering temperature was 400℃. The temperature was held for 2 hours. Then the heating rate was 5℃ / min, the sintering temperature was 570℃, and the holding time was 2 hours. Then the temperature was increased to 830℃ at a heating rate of 5℃ / min and held for 6 hours. Finally, the sintered material was obtained by rapid cooling with chilled water.
[0098] Since the three precursors require different sintering temperatures, lithium iron phosphate materials with three particle sizes (large, medium, and small) are prepared by controlling the nucleation and growth time through a three-stage sintering method.
[0099] The final sintering material is pulverized by an air jet mill, with the air pressure controlled at 0.35 MPa and the grading frequency at 30~40 Hz, to obtain pulverized material with particle sizes of D10≥0.15, D50=0.7~1.8μm, D90<10μm, and D100<25μm; finally, it is further impurity removed and mixed.
[0100] In Table 1, the test method for powder compaction is as follows: first, weigh about 1.0g of powder and put it evenly into the mold, apply a pressure of 30Mpa, hold the pressure for 10s, and after the pressure is applied, calculate the overall thickness of the powder compaction based on the mold and the upper and lower pressure heads / plates.
[0101] The test method for 1C capacity retention is as follows: A 3.2Ah soft pack was prepared using lithium iron phosphate prepared in the examples and comparative examples. The specific steps are as follows: 1. Capacity calibration: Let stand at 25℃ for 60 minutes, first charge with constant current and constant voltage to 3.65V, then discharge with 1C rate to the cutoff voltage of 2.0V. Repeat the above steps until the capacity difference between two consecutive discharges is less than 3%, and record it as the initial capacity C0. 2. Constant current and constant voltage charging: Adjust the temperature to 25℃ and charge to 3.65V using constant current and constant voltage. 3. 0℃ 1C capacity retention rate: Adjust the temperature to 0℃, let it stand for 60 minutes after reaching 0℃, then discharge at a rate of 1C, record the discharge capacity C1, and finally calculate the 0℃ 1C capacity retention rate. Repeat step 2 above; 4. -20℃ 1C Capacity Retention Rate: Adjust the temperature to -20℃, let it stand for 60 minutes after reaching 0℃, then discharge at a rate of 1C and record the discharge capacity C. 2, Finally, the capacity retention rate at -20℃ 1C was calculated.
[0102] 5. In Table 1, D50 particle size distribution refers to the D50 particle size distribution of lithium iron phosphate powder after sintering and pulverization.
[0103] Table 1. Performance comparison of lithium iron phosphate products prepared in the examples and comparative examples.
[0104] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a low-temperature, high-pressure resistant lithium iron phosphate cathode material, characterized in that: Includes the following steps: Iron source, lithium source, phosphorus source, carbon source, dopant and dispersant are wet-mixed in proportion to obtain slurry. The slurry is then ground and dried to obtain precursor powder. By replacing the iron source, at least two precursor powders can be prepared; After the different precursor powders are mixed evenly in proportion, they are subjected to gradient sintering in an inert atmosphere to obtain the final product. The iron source is ferrous oxalate, iron oxide red, and ferric phosphate; The precursor powder prepared with ferrous oxalate as the iron source has a D50 of 60-70 μm, the precursor powder prepared with ferric phosphate as the iron source has a D50 of 20-25 μm, and the precursor powder prepared with iron oxide red as the iron source has a D50 of 6-8 μm. The gradient sintering procedure is as follows: first, heat to 350-450℃ and hold for 1.5-2.5 hours; then heat to 500-600℃ and hold for 1.5-2.5 hours; then heat to 700-800℃ and hold for 2-4 hours; finally, heat to 810-850℃ and hold for 2-4 hours.
2. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: When mixing, the mass ratio of the precursor powder prepared from ferrous oxalate, iron oxide red, and ferric phosphate is 6-8:0.8-1.2:1-3.
3. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: After sintering, the sintered material is rapidly cooled with ice water.
4. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: The gradient sintering procedure is as follows: first, heat to 350-450℃ and hold for 1.5-2.5 hours; then heat to 550-600℃ and hold for 1.5-2.5 hours; then heat to 740-780℃ and hold for 2-4 hours; finally, heat to 820-840℃ and hold for 2-4 hours.
5. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: Different precursor powders were thoroughly mixed using a ribbon mixer.
6. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: The phosphoric acid is selected from at least one of phosphoric acid, sodium monohydrogen phosphate, sodium dihydrogen phosphate, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, lithium monohydrogen phosphate, or lithium dihydrogen phosphate. Alternatively, the carbon source is selected from at least one of glucose, sucrose, polyethylene glycol, citric acid, or starch; Alternatively, the dopant is selected from at least one of titanium dioxide, ammonium metavanadate, niobium pentoxide, magnesium oxide, or aluminum oxide; Alternatively, the dispersant may be selected from water and / or ethanol.
7. The method for preparing the low-temperature, high-pressure resistant lithium iron phosphate cathode material according to claim 1, characterized in that: The drying process for preparing precursor powders was carried out using spray drying.
8. A low-temperature, high-pressure resistant lithium iron phosphate cathode material, characterized in that: It is prepared by any of the preparation methods described in claims 1-7.
9. A battery, characterized in that: The active material of its positive electrode is the low-temperature, high-pressure lithium iron phosphate positive electrode material as described in claim 8.
Citation Information
Patent Citations
A lithium iron phosphate with high compact density and a preparation method thereof
CN109192948A
Method for preparing high-compaction lithium iron phosphate material and application
CN119706781A