Device and method for controlling warpage compensation of wafer in X / Y direction

By depositing films with different internal stresses and non-uniform thickness profiles on the back side of the wafer, the problems of improper clamping and process inhomogeneity caused by wafer bending are solved, wafer planarization is achieved, and the stability and efficiency of semiconductor manufacturing are improved.

CN121241420APending Publication Date: 2025-12-30LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480036199.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-07-27
Filing Date
2024-05-30
Publication Date
2025-12-30

AI Technical Summary

Technical Problem

During semiconductor processing, wafer bending can lead to problems such as improper electrostatic chuck clamping, uneven processing, and photolithography misalignment, affecting equipment performance and yield.

Method used

Films with different internal stresses and non-uniform thickness profiles are deposited on the back side of the wafer. The bending of the wafer in the X and Y directions is compensated by alternately forming curved strip and curved channel profile films, forming complementary film stacks to achieve a flat surface.

Benefits of technology

Effectively reduce or eliminate wafer bending, ensure stable clamping and uniform process conditions for wafers in subsequent processing steps, and improve equipment performance and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121241420A_ABST
    Figure CN121241420A_ABST
Patent Text Reader

Abstract

Methods, apparatus, and structures for mitigating wafer bending of a semiconductor wafer are provided herein. Deposition of the backside layer stack may mitigate wafer bending that varies in an orthogonal direction. Each backside layer may be deposited by a backside deposition device. It thus provides a substantially flat surface on the back side of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] References merged The PCT application form is filed together with this specification as part of this application. Each application listed in the concurrently filed PCT application form that claims a benefit or priority from this application is incorporated herein by reference in its entirety for all purposes. Background Technology

[0002] In semiconductor processing, it may be desirable for wafers to remain substantially flat. However, during normal operation, wafers may experience wafer bending. Wafer bending can cause several problems, such as improper electrostatic chuck clamping, wafer transporter failure to hold, non-uniform process conditions, misalignment and / or pattern transfer issues during lithography, etc. These problems degrade or damage equipment performance and reduce yield and productivity. Devices and processes have been developed to manage wafer bending by keeping the wafer flat within process tolerances. One process involves depositing a film on the back side of the wafer to counteract any stresses that may cause wafer bending.

[0003] The background description provided herein is for the purpose of presenting the general context of this disclosure. The work of the currently designated inventor, within the scope described in this background section and in aspects of the specification that could not be identified as prior art at the time of filing, neither expressly nor impliedly acknowledges that it is prior art to this disclosure. Summary of the Invention

[0004] This document discloses methods and systems for depositing films. In one aspect of the embodiments herein, a method for reducing curvature in a substrate is provided, the method comprising: receiving a substrate having a front side and a back side, wherein the substrate has a first curvature in an X direction and a second curvature in a Y direction; performing one or more cycles of: (a) forming a first back side layer on the back side of the substrate, wherein the first back side layer compensates for the first curvature more than compensates for the second curvature, or compensates for the second curvature more than compensates for the first curvature, and wherein the first back side layer has a first type of internal stress and a first non-uniform thickness profile; and (b) forming a second back side layer on the back side of the substrate, wherein the second back side layer compensates for the smaller of the first curvature or the second curvature compensated by the first back side layer, wherein the second back side layer has a second type of internal stress opposite to the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile are complementary to each other, such that when the first back side layer and the second back side layer are formed, they provide a complementary film stack having a substantially flat surface on the back side of the substrate.

[0005] In some embodiments, the substrate is a semiconductor wafer having a partially fabricated integrated circuit on the front side. In some embodiments, the substrate has a saddle-shaped bend. In some embodiments, the method further includes determining, before forming the first back side layer, that the amplitude of the first bend is greater than the amplitude of the second bend. In some embodiments, the method further includes rotating the substrate based on determining that the amplitude of the first bend is greater than the second bend before forming the first back side layer. In some embodiments, the first non-uniform thickness profile is a curved strip whose thickness toward the center of the substrate is greater than the thickness at the edge of the substrate. In some embodiments, the curved strip has a longitudinal axis substantially parallel to the Y direction. In some embodiments, the curved strip has a generally parabolic shape, the thickness of which varies as a function of the X direction away from the back side of the substrate in the Z direction perpendicular to both the X and Y directions. In some embodiments, the second non-uniform thickness profile is a curved channel whose thickness toward the edge of the substrate is greater than the thickness at the center of the substrate. In some embodiments, the curved channel has a parabolic shape, the thickness of which varies in the Z direction as a function of the X direction away from the back surface of the substrate. In some embodiments, the first type of internal stress is tensile stress. In some embodiments, the first type of internal stress is compressive stress. In some embodiments, the method further includes forming a third back surface layer on the back surface of the substrate, wherein the third back surface layer has a uniform shape and either the first type of internal stress or the second type of internal stress. In some embodiments, the type and magnitude of the internal stress of the third back surface layer are based on the curvature of the substrate after the formation of the first and second back surface layers. In some embodiments, the method further includes identifying the values ​​of the first and second curvatures, and wherein the first and second back surface layers are formed based on the values ​​of the first and second curvatures. In some embodiments, the method further includes identifying the values ​​of the first and second curvatures, and wherein the magnitude of the internal stress of the first and second back surface layers is based on the values ​​of the first and second curvatures. In some embodiments, the one or more cycles are two or more cycles. In some embodiments, the total thickness of the layers deposited during the one or more cycles is at least about 2 µm. In some embodiments, the first backing layer and the second backing layer share a first thickness, and each cycle of (a) and (b) deposits a complementary profile layer of the first thickness. In some embodiments, the first thickness is less than about 1 µm.In some embodiments, the change in wafer bending compensation between the first back layer and the second back layer after annealing is less than about 20%. In some embodiments, the method further includes forming a third back layer on the back side of the substrate after performing the one or more cycles, wherein the third back layer increases the flatness of the back side of the substrate. In some embodiments, the method further includes performing plasma treatment after forming the first back layer, performing plasma treatment after forming the second back layer, or both, wherein the plasma treatment improves the adhesion of the first back layer and the second back layer.

[0006] In another aspect of the embodiments herein, a substrate is provided, the substrate comprising: one or more front layers on a front side of the substrate, wherein the substrate has a first curvature in the X direction and a second curvature in the Y direction of the substrate; a first back layer on a back side of the substrate, wherein the first back layer compensates for the first curvature more than it compensates for the second curvature, or compensates for the second curvature more than it compensates for the first curvature, and wherein the first back layer has a first type of internal stress and a first non-uniform thickness profile; a second back layer on the back side of the substrate, wherein the second back layer compensates for the smaller of the first curvature or the second curvature compensated by the first back layer, wherein the second back layer has a second type of internal stress opposite to the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile are complementary to each other, such that when the first back layer and the second back layer are formed, they provide a complementary film stack having a substantially flat surface on the back side of the substrate.

[0007] In some embodiments, if the first back layer does not compensate for the thickness of the one or more front layers, the substrate has a first or second bend of about 300 μm or greater. In some embodiments, the first non-uniform thickness profile is a curved strip whose thickness towards the center of the substrate is greater than the thickness at the edge of the substrate. In some embodiments, the curved strip has a longitudinal axis substantially parallel to the Y direction. In some embodiments, the curved strip has a generally parabolic shape, and the thickness of the generally parabolic shape varies away from the back of the substrate as a function of the X direction in the Z direction, which is perpendicular to both the X and Y directions. In some embodiments, the second non-uniform thickness profile is a curved channel whose thickness towards the edge of the substrate is greater than the thickness towards the center of the substrate. In some embodiments, the curved channel has a parabolic shape, and the thickness of the parabolic shape varies away from the back of the substrate as a function of the X direction in the Z direction. In some embodiments, the first type of internal stress is tensile stress. In some embodiments, the first type of internal stress is compressive stress. In some embodiments, the substrate further includes a third back-side layer on the back side of the substrate, wherein the third back-side layer has a uniform shape and either the first type of internal stress or the second type of internal stress. In some embodiments, the type and magnitude of the internal stress in the third back-side layer are based on the curvature of the substrate after the formation of the first and second back-side layers. In some embodiments, the substrate further includes additional complementary film stacks. In some embodiments, the complementary film stacks and the additional complementary film stacks alternate together between the first and second back-side layers. In some embodiments, the total thickness of all complementary film stacks is at least about 2 µm. In some embodiments, the thickness of each complementary film stack is less than about 1 µm. In some embodiments, after annealing, the change in total wafer curvature compensation of all complementary film stacks is less than about 20%. In some embodiments, the substrate further includes a third back-side layer deposited on the back side of the substrate after all complementary film stacks, wherein the third back-side layer increases the flatness of the back side of the substrate.

[0008] In another aspect of the embodiments herein, an apparatus is provided, the apparatus comprising: a processing chamber; and a controller including a memory and a processor, configured to: receive a substrate having a front side and a back side, wherein the substrate has a first curvature in an X direction and a second curvature in a Y direction; perform one or more cycles of: (a) forming a first back side layer on the back side of the substrate, wherein the first back side layer compensates for the first curvature more than compensates for the second curvature, or compensates for the second curvature more than compensates for the first curvature, and wherein the first back side layer has a first type of internal stress and a first non-uniform thickness profile; (b) forming a second back side layer on the back side of the substrate, wherein the second back side layer compensates for the smaller of the first curvature or the second curvature compensated by the first back side layer, wherein the second back side layer has a second type of internal stress opposite to the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile are complementary to each other, such that when the first back side layer and the second back side layer are formed, they provide a complementary film stack having a substantially flat surface on the back side of the substrate.

[0009] These and other features of the disclosed embodiments will be described in detail below with reference to the accompanying drawings. Attached Figure Description

[0010] Figures 1A and 1B show examples of unbent and bent semiconductor wafers on an electrostatic chuck.

[0011] Figure 2 shows exemplary isometric views of various wafer bending shapes.

[0012] Figure 3A shows an exemplary region on the back side of a wafer deposited with a curved strip profile and a curved channel profile according to various embodiments herein.

[0013] Figures 3B and 3C show side views and exploded side views of a wafer with a back surface layer having a curved strip profile and a curved channel profile according to various embodiments of the present invention.

[0014] Figure 3D-3G shows a side view of a wafer with alternating stacks of back layers according to various embodiments of the present invention, the alternating stacks of back layers having curved strip profiles and curved channel profiles.

[0015] Figures 4A-B are diagrams showing the internal stresses of various tensile and compressive membranes and stacked membranes according to various embodiments described herein.

[0016] Figure 4C is an isometric view of a bent wafer according to various embodiments described herein.

[0017] Figure 5 is a process flow diagram showing some operations during semiconductor wafer processing.

[0018] Figures 6A and 6B show block diagrams of an exemplary substrate processing system.

[0019] Figure 7A shows an exemplary cross-section of the edge of the spray-base.

[0020] Figure 7B shows a top view of an exemplary carrier ring.

[0021] Figure 8 shows a schematic diagram of an exemplary process system that can be used to perform the methods described herein. Detailed Implementation

[0022] the term The following terms are used throughout this specification: The terms “semiconductor wafer,” “wafer,” “substrate,” “wafer substrate,” and “partially fabricated integrated circuit” are used interchangeably. Those skilled in the art will understand that the term “partially fabricated integrated circuit” can refer to a silicon wafer during any of the many stages of integrated circuit manufacturing thereon. Wafers or substrates used in the semiconductor device industry typically have diameters of 200 mm, 300 mm, or 450 mm. Examples of wafer materials include silicon (Si), gallium arsenide (GaAs), and silicon germanium (SiGe). Besides semiconductor wafers, other artifacts that can utilize the disclosed embodiments include various articles of manufacture, such as printed circuit boards, magnetic recording media, magnetic recording sensors, mirrors, optical elements, display devices or components, such as backplanes for pixelated display devices, flat panel displays, micromechanical devices, and the like. Artifacts can have a wide variety of shapes, sizes, and materials.

[0023] As used herein, “semiconductor device manufacturing operations” refers to operations performed during the manufacture of semiconductor devices. Typically, the entire manufacturing process comprises multiple semiconductor device manufacturing operations, each performed in its own specific semiconductor manufacturing tooling, such as plasma reactors, electroplating baths, chemical mechanical planarization tools, wet etching tools, and the like. Categories of semiconductor device manufacturing operations include subtractive processes, such as etching and planarization processes, and additive processes, such as deposition processes (e.g., physical vapor deposition, chemical vapor deposition, atomic layer deposition, electrochemical deposition, electroless deposition). In the context of etching processes, substrate etching processes include processes that etch mask layers, or more generally, processes that etch any layers of material previously deposited on and / or otherwise left on the substrate surface. Such etching processes can etch stacks of layers within a substrate.

[0024] A "manufacturing apparatus" is an apparatus in which a manufacturing process is performed. A manufacturing apparatus typically has a processing chamber in which workpieces reside during processing. Typically, in use, a manufacturing apparatus performs one or more semiconductor device manufacturing operations. Examples of manufacturing apparatuses for semiconductor device manufacturing include deposition reactors, such as electroplating tanks, physical vapor deposition reactors, chemical vapor deposition reactors, and atomic layer deposition reactors, as well as subtractive process reactors, such as dry etching reactors (e.g., chemical and / or physical etching reactors, wet etching reactors, and ashing tanks).

[0025] As used herein, “wafer bending” can refer to the deformation of a wafer. This deformation may have radial and / or azimuth components. Examples of wafer bending types include dome shapes, bowl shapes, and saddle shapes. Wafer bending can occur during manufacturing, for example, due to stress on the wafer during material deposition on its active surfaces. Wafer bending can occur during various manufacturing processes, such as when depositing large amounts of stacked material. Wafer bending can complicate subsequent processing steps. For example, if the bending is too great, the wafer may not be properly clamped, subjecting it to uneven heating and / or other process conditions. Furthermore, performing processing steps (such as photolithography) on an over-bent wafer can produce poor results.

[0026] In some embodiments, wafer curvature can be measured as the deviation of the average or median distance from the wafer surface to a reference plane. In some embodiments, the median point on the wafer surface can be the center point (e.g., in the case of concave or dome curvature), or an edge point of the wafer and / or the average edge point of the wafer (e.g., in the case of warp or convex curvature). In some embodiments, wafer curvature can be measured from the reference plane such that when the edge point of the wafer is below the reference plane, the edge point is considered to have negative curvature, and when the edge point of the wafer is above the reference plane, the edge point is considered to have positive curvature. In some embodiments, positive or negative curvature can be measured along a Z-axis perpendicular to the reference plane.

[0027] In some implementations, wafer bending can vary between two principal planar directions of the substrate (referred to as the x and y directions). For example, wafer bending along the x direction can be a positive Z-direction, while wafer bending along the y direction can be a negative Z-direction (the Z-axis is perpendicular to the plane formed by the x and y directions). Figure 2 shows eight shapes that can be formed based on bending in the x and y directions. When bending along the x and y axes is positive, a bowl shape is formed, while when bending along the x and y axes is negative, an umbrella or dome shape is formed. Other shapes include a "halfpipe" or "taco" shape when there is essentially no wafer bending in one direction but positive or negative bending in the direction perpendicular to the plane. A "saddle" or "potato chip" shape is formed when wafer bending is positive in one direction and negative in the other.

[0028] Wafer bending can be characterized by x-bending and y-bending values. A positive x-bending value corresponds to wafer bending in the positive z-direction, located at wafer coordinates with a large x-value and a small or zero y-value; for example, an x-value greater than approximately 100 mm or approximately 150 mm (for a 300 mm wafer), and a y-value of approximately 0 mm (with the reference point at the wafer center). Similarly, a negative x-bending value corresponds to wafer bending in the negative z-direction, located at wafer coordinates with a large x-value and a small or zero y-value. Conversely, positive and negative y-bending correspond to wafer bending along the positive or negative z-direction, respectively, at wafer coordinates with a large y-value and a small or zero x-value.

[0029] In some implementations, wafer bending can be characterized by a single value. In some implementations, wafer bending can be described as a “delta bow.” When referring to the wafer bending of a saddle-shaped wafer, the wafer delta bow can be represented by the difference between a negative bending in one direction (e.g., along the x-axis) and a positive bending in another direction (e.g., along the y-axis). For example, a 200µm wafer bending might result from a -25µm x-bending and a +175µm y-bending. For wafers with tucker-shaped, bowl-shaped, or dome-shaped wafer bending, the wafer bending can refer to the difference between the maximum bending and the aforementioned reference plane.

[0030] A "bent strip profile" is characterized by a two-dimensional shape whose thickness varies along one of the two principal planar dimensions of the substrate, namely the x and y directions. While the thickness varies in one of these directions, it remains essentially unchanged in the other. Furthermore, a bent strip profile means that the layer thickness is generally thicker at the center of the substrate than at the substrate edges. Therefore, the structure appears as a strip or "speed bump" on the back side of the substrate. In some cases, the bent strip profile varies as a function of the x-axis position in the direction away from the substrate plane (z-direction), but does not vary significantly in the y-axis position. In other cases, the bent strip profile varies as a function of the y-axis position in the z-direction, but does not vary significantly in the x-axis position. In some embodiments, the bent strip is positioned along the principal axis of the substrate such that the centerline of the strip passes through the origin (center point) of the substrate. Therefore, a characteristic of a bent strip profile may be that the film thickness at the center of the substrate is greater than the thickness at the substrate edges. The bent shape can generally be rounded, such as circular, parabolic, Gaussian, etc.

[0031] The "curved channel profile" is characterized by a two-dimensional shape whose thickness varies along one of the x and y directions of the substrate. While the thickness varies in one of these directions, it remains essentially unchanged in the other. Furthermore, the curved strip profile implies that the layer thickness is generally thicker towards the substrate edge than towards the substrate center. Therefore, this structure appears as a channel or indentation on the back side of the substrate. In some cases, the curved channel profile varies as a function of the x-axis position in the direction away from the substrate plane (z-direction), but does not show a significant change in the y-axis position. In other cases, the curved channel profile varies as a function of the y-axis position in the z-direction, but does not show a significant change in the x-axis position. In some embodiments, the curved channel is positioned along the principal axis of the substrate, such that the centerline of the channel passes through the origin (center point) of the substrate. Therefore, the curved channel profile may be characterized by a film thickness greater at the substrate edge than at the substrate center. The curved shape can generally be rounded, such as circular, parabolic, Gaussian, etc.

[0032] Generally, curved strip profiles and curved channel profiles refer to the geometries of membranes with different properties. Typically, the membrane property is its thickness, but other properties can similarly constitute the profile. These properties may include membrane density, membrane composition, and internal stress. Examples of curved strip profiles and curved channel profiles are shown in Figures 3B and 3C. Membrane 308 is an example of a curved strip profile, while membrane 307 is an example of a curved channel profile. Curved strip profile membranes and curved channel profile membranes can also be referred to as non-uniform thickness profile membranes. Non-uniform thickness profile membranes can refer to either curved strip profile membranes or curved channel profile membranes.

[0033] A "uniform thickness profile" is characterized by a two-dimensional shape whose thickness is substantially constant along any planar direction of the substrate (e.g., the x and y directions). In some embodiments, a combination of a curved channel profile film and a curved strip profile film can be a uniform thickness film. In some embodiments, the curved channel profile film and the curved strip profile film have complementary shapes, which together can form a profile bilayer film with substantially uniform thickness. In some embodiments, a combination of a curved strip profile film and a curved channel profile film can be referred to as a stack of complementary profile films. In some embodiments, a non-uniform thickness profile can refer to one or both of a curved channel profile and a curved strip profile. In some embodiments, a stacked film composed of a layer having a curved channel profile and a layer having a curved strip profile may be substantially flat, for example, having a flatness similar to a single uniform thickness profile film, and a deposition thickness similar to that of a combined non-uniform thickness profile film.

[0034] Bending wafers Semiconductor device manufacturing typically involves depositing stacks of layers or films on a wafer. Generally, most of the deposition and other processes for forming the device occur on one side of the wafer, often referred to as the front side or front face. As the deposited layers accumulate, they introduce stress into the wafer. Large net tensile or compressive stresses can cause the wafer to bend (and in cases of excessive tensile stress, may crack), which is undesirable.

[0035] Bending is particularly likely to occur when depositing large amounts of stacked material, such as in 3D-NAND devices, or when depositing thick front-side layers. Significant bending can adversely affect subsequent processing steps. For example, if the bending is too large, the wafer may not be properly clamped. Figures 1A and 1B show wafers on electrostatic chucks, which typically have flat surfaces. Figure 1A shows wafer 102 on electrostatic chuck 110. When wafer 102 is substantially flat for a specific process operation purpose, for example, with a bending of about 100 μm or less, the wafer can be properly clamped, thus securing it for subsequent processing steps. Figure 1B shows a bent wafer 104 on electrostatic chuck 110. Wafer 104 is shown as having negative wafer bending (i.e., a dome shape where the center point of the wafer is higher than the edge). This is likely due to compressive internal stress in the front-side layer. A front-side layer with tensile internal stress can cause the wafer to bend in the opposite way, forming a bowl shape.

[0036] Significant bending can cause a variety of manufacturing problems. In some cases, the wafer may not be properly secured to the electrostatic chuck. This can lead to various non-uniformity issues, such as uneven heating of the wafer, uneven application of process gases across the wafer surface, and / or the distance between the wafer and the nozzle and / or nozzle base may not remain uniformly parallel (i.e., parallelism may be compromised). Wafer bending can cause other problems. For example, some processing steps (such as photolithography) are highly precise, and significant wafer irregularities can produce undesirable results. This problem may manifest as photolithography defocusing. Cracks may also occur, which can introduce additional defects and reduce yield.

[0037] An exemplary stack that could cause these problems is one with alternating oxide and nitride layers (e.g., silicon oxide / silicon nitride / silicon oxide / silicon nitride, etc.). Another example of a stack type that could cause bending includes alternating oxide and polysilicon layers (e.g., silicon oxide / polysilicon / silicon oxide / polysilicon, etc.). Other examples of potentially problematic stack materials include, but are not limited to, tungsten and titanium nitride.

[0038] Material in the stack can be deposited using chemical vapor deposition (CVD) techniques, such as plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), metal-organic chemical vapor deposition (MOCVD), atomic layer deposition (ALD), or plasma-enhanced atomic layer deposition (PEALD), or by direct metal deposition (DMD). These examples are not intended to be limiting. Some of the disclosed embodiments may be useful whenever wafer stress and / or bending occurs due to the presence of material on the front side of the wafer.

[0039] The front-side stack can be deposited as any number of layers and thickness. In one example, the stack may include about 20 or more layers, with a total thickness of about 2 μm to about 4 μm. In some cases, the multi-layer stack may include about 100 or more layers. In some embodiments, the multi-layer stack may include about one hundred or more layers. In some embodiments, the multi-layer stack may have about five hundred or more layers. In some embodiments, the multi-layer stack may have about one thousand or more layers. For example, such a stack may have a thickness of about 4 μm to 12 μm.

[0040] The stress induced in the wafer by stacked components or other front-side deposits can range from about -500 MPa to about +500 MPa. In some embodiments, the resulting bending is about 150 μm or greater, for example, about 300 μm or more, about 400 μm or more, or about 200 μm to about 400 μm (for a 300 mm wafer).

[0041] Another cause of wafer warping may be the front-side processing, which uses a thick hard mask with limited etch selectivity. In these embodiments, at least one of one or more front-side layers is a hard mask. Thick hard masks may have internal stresses similar to those described above, such as ranging from 0 MPa to approximately 500 MPa. The stresses caused by the hard mask can be tensile or compressive stresses. A thick hard mask can result in significant wafer warping, for example, approximately 150 μm or greater.

[0042] Several techniques have been devised to eliminate bending. When bending is severe, the deposition process can be adjusted to reduce or counteract the internal stress in the deposited layer. However, any such adjustments should not interfere with the process requirements of the manufacturing equipment. A common technique for counteracting bending is to deposit a layer on the back side of the wafer.

[0043] Backside deposits can be intentionally formed on the back side of a wafer to control overall wafer stress and warping. If the backside layer has the same type of internal stress (tensile or compressive) and is comparable in magnitude to the internal stress generated on the front side of the wafer, the backside film effectively counteracts and reduces wafer warping.

[0044] Examples of back-side films used to counteract warping include amorphous silicon, silicon oxide, silicon nitride, and silicon oxynitride. Variations of these films, such as doped amorphous silicon, doped silicon oxide, doped silicon nitride, and doped silicon oxynitride, can be used, and these films can be formed under different deposition conditions to tune and optimize their material properties. Furthermore, other types of films that may be introduced during semiconductor processing can be used in combination with and / or as alternatives to these exemplary films. Current back-side films have high internal stress and can alleviate the stress exerted on the wafer by the front-side layer, thereby reducing or eliminating wafer warping. While not mandatory, the back-side layer is generally made of a high-stress film deposited on the silicon wafer. High-stress films are often preferred because they can more effectively compensate for wafer warping.

[0045] In some implementations, the back-side film thickness is relatively uniform because the bending caused by the front-side deposition material is relatively symmetrical, forming a bowl or dome shape based on uniform anisotropic internal stress. Therefore, depositing a uniformly thick profile film under tensile or compressive internal stress can alleviate the stress generated by the front-side layer on the wafer, as the back-side film will produce a similarly symmetrical, opposite wafer bending. However, some front-side deposition techniques can lead to anisotropic stress, causing the internal stress on the wafer's front side and the resulting bending to change in the principal planar directions (compared to another principal planar direction), such as the x and y directions. In such implementations, the wafer may have x-bends and y-bends, which may differ in size and orientation (or sign). A uniform back-side layer may not be sufficient to resolve such saddle-shaped wafer bending.

[0046] Figure 2 shows eight different shapes that can be formed based on different combinations of positive or negative curvature along the x and y axes or directions. Bowl, umbrella, semi-tubular, or saddle shapes can be formed depending on whether the wafer curvature along the x and y axes is positive, negative, or essentially nonexistent. When the wafer curvature shape is bowl or umbrella, a uniform thickness profile film with uniformly tensile or compressive internal stresses in all directions can appropriately alleviate the stress exerted on the wafer by the front layer. However, when the wafer curvature shape is different, such as saddle or semi-tubular, the uniformly tensile internal stresses in all directions will over- or under-compensate for the wafer curvature, or may exaggerate it. For example, an uniformly stretched back film deposited on a wafer with negative x-curvature and positive y-curvature (i.e., saddle shape) will alleviate the wafer curvature along the y direction but will increase the wafer curvature along the x direction.

[0047] This document discloses a technique for depositing a film on the back side of a wafer that generates anisotropic stresses across the wafer, allowing control over overall wafer curvature. When viewed along the x-direction, such a film may exhibit internal compressive stress near the wafer center and internal tensile stress near the wafer edge, and vice versa. When viewed along the y-direction, such a film may exhibit either internal compressive stress from the center to the edge or internal tensile stress from the center to the edge. When deposited on the back side of a wafer, such a film can reduce wafer curvature unequal along the x and y directions. While such a technique is obviously applicable to wafers with positive y-curvature and negative x-curvature, or vice versa, the technique disclosed herein can be applied to wafers with various types of wafer curvature (where the magnitude or sign of curvature differs in one principal direction from that in another principal direction) or without curvature. For example, the technique disclosed herein can be applied to wafers with a specific curvature shape caused by front-side deposition. As another example, the back side of a bare wafer without a front-side deposition layer, or a wafer with no curvature or minimal curvature, can be pre-treated with the technique disclosed herein before curvature is generated by front-side deposition.

[0048] Anisotropic internal stress can be achieved by depositing curved strip profile films and curved channel profile films on the wafer. The curved strip profile films and curved channel profile films may have different internal stresses, resulting in a stacked film with anisotropic internal stress, i.e., the internal stress varies based on direction. As an example, Figures 3A-3C show curved strip profile films and curved channel profile films. Figure 3A is a bottom surface view of a wafer 306 having a central region 304 and an edge region 302. Figures 3B and 3C present a side view and an exploded side view, respectively, showing a curved strip profile film 308 and a curved channel profile film 307 along the x-direction of the wafer 306. A front layer 305 can be deposited on the front (or top) side of the wafer 306, causing the wafer to bend, which is compensated by films 307 and 308 deposited on the back (or bottom) side of the wafer 306. The films can be deposited on the back side of the wafer, such that the films are deposited substantially in the central region 304 or the edge region 302. This can be achieved via a nozzle configured to deposit the film substantially in the central region 304 or the edge region 302. In some embodiments, a nozzle base (or shopped) may be used for such deposition. In some embodiments, the shopped spacer may be configured to deposit in these regions, for example, by controlling the reactant flow in the regions of the shopped spacer corresponding to the regions in Figure 3A. These regions are schematically shown in Figure 3A for reference only; the shopped spacer or wafer may be considered in any different configuration of number, shape, and regions.

[0049] Referring back to Figures 3B and 3C, the film substantially deposited in the central region 304 may have a curved strip profile 308, while the film substantially deposited in the edge region 302 may have a curved channel profile 307. That is, for example, a compressive stress film (307) may be deposited more extensively (e.g., thicker) in the edge region 302 compared to the central region 304, while a tensile stress film (308) may be deposited more extensively (e.g., thicker) in the central region 304 compared to the edge region 302. While the films may be substantially deposited in either the central region 304 or the edge region 302, it should be understood that some deposition may occur within the wafer and in other regions. Furthermore, the shapes of the curved strip profile and the curved channel profile are merely examples, and the profile shapes may vary. In some embodiments, the central region 304 may also be referred to as a curved strip profile deposition region. In some embodiments, the edge region 302 may also be referred to as a curved channel profile deposition region. In some other embodiments, the central region 304 may be referred to as a curved strip profile deposition region, and the edge region 302 may be referred to as a curved channel profile deposition region.

[0050] The curved strip profile film 308 has a decreasing thickness along the x-direction from the center to the edge of the wafer 306, and a uniform or substantially uniform thickness along the y-direction of the wafer. Conversely, the curved channel profile film 307 has an increasing thickness along the x-direction from the center to the edge of the wafer 306, and a uniform or substantially uniform thickness along the y-direction of the wafer. The curved strip profile film 308 and the curved channel profile film 307 can together form a profile film of uniform thickness.

[0051] Since films 307 and 308 are deposited independently, each film can be deposited under conditions with different internal stresses. For example, the curved strip profile film 308 may have compressive internal stress, while the curved channel profile film 307 may have tensile internal stress, and vice versa. Because film stresses can be superimposed, the stacked films may have compressive internal stress in regions of films with small x / large y coordinates (i.e., corresponding to the central region 304), while the stacked films may also have tensile internal stress in regions of films with large x / small y coordinates (i.e., corresponding to the edge region 302), and vice versa. As mentioned above, the wafer center can be considered the origin, for example, x=0 and y=0. Anisotropic internal stresses are further explained with reference to Figures 4A-B.

[0052] Although the films 307 and 308 discussed herein have opposite types of internal stress—for example, one film has compressive internal stress and the other has tensile internal stress—in some embodiments, both films may have either tensile or compressive internal stress, but with different magnitudes. This can address wafer problems where the amplitudes of x-bend and y-bend are different, or even where both bends are positive or negative. In some embodiments, depositing films of the same type of stress can increase yield.

[0053] In some implementations, the film thickness can also be increased as wafer warp compensation by the back-side layer increases, since a thicker film can typically compensate for greater wafer warp. However, a thicker film also increases the risk of cracking. Back-side films with internal tensile stress are more prone to cracking because they are typically brittle. Therefore, in some implementations, a stretch film is deposited first, followed by a compression film, because the compression film deposited on the stretch film partially offsets the internal tensile stress and reduces the risk of cracking. However, with a large back-side film thickness, internal stress can still cause film cracking. For example, cracking may occur in a single stack of complementary profile films when the total film thickness is 1.25 µm. Cracking is undesirable because it can reduce wafer warp compensation of the layers, lead to defects and potential etching during subsequent manufacturing operations, and even contaminate and / or damage the processing chamber.

[0054] To address this issue, alternating stacked films can be used, which offer a higher crack resistance margin compared to single stacked films of equal thickness. In some embodiments, alternating stacked films can be deposited, wherein each layer has a curved channel profile or a curved strip profile. Figures 3D-3G show various embodiments of alternating back-side film stacks having complementary profiles on a substrate 306 having one or more front-side layers 305. In Figure 3D, films 307 and 308 are alternately formed as alternating stacked films 340 having films 308-1, 308-2, 308-3, and 308-N, and films 307-1, 307-2, 307-3, and 307-M. In some embodiments, N=M, meaning the alternating stack has the same number of curved strip profile films and curved channel profile films. In other embodiments, N=M, such that there are more or fewer curved strip profile films than curved channel profile films.

[0055] Compared to compensation provided by single-stacked curved channel profile films and curved strip profile films, alternating stacked films 340 can compensate for larger wafer warpage from the front-side layer. For example, a single-stacked complementary profile film, at a thickness of about 1.25 µm, may crack, but it can compensate for about 250 µm of wafer warpage. An alternating stacked film with a total thickness of 1.25 µm can similarly compensate for about 250 µm of wafer warpage, but with a reduced risk of cracking. Alternating stacked films may have lower yield due to the deposition of multiple complementary layer stacks rather than single complementary layer film stacks, and are therefore generally desirable. However, the improved material properties of alternating stacked films provide several benefits discussed herein, including higher crack tolerance and improved thermal stability. In some embodiments, alternating stacked films 340 may include two or more sets of complementary profile films, such as two or more sets of curved strip profile films 308 and curved channel profile films 307.

[0056] In some embodiments, each curved strip profile membrane 308-1-N and curved channel profile membrane 307-1-M has the same profile. In other embodiments, the profiles of one or more non-uniform thickness profile membranes may differ from those of the other non-uniform thickness profile membranes. In some embodiments, the complementary profile membrane stack may be defined by a thickness 350, which refers to the thickness of the complementary profile membrane stack (e.g., a combination of curved strip profile membranes and curved channel profile membranes). The thickness 350 of the complementary profile membrane stack may be less than about 1 µm or between about 0.5 µm and about 1 µm. In some embodiments, each complementary membrane stack in an alternating membrane stack may have the same thickness, which, for the four-layer stack shown in FIG. 3D, may have a total thickness between about 2 µm and about 4 µm. In some embodiments, each complementary profile membrane stack in an alternating stack may have a different thickness.

[0057] Figure 3D shows a diagram of depositing a curved strip profile film 308 after the curved channel profile film 307 is deposited, and then repeated four times to provide an alternating stack of four complementary profile films. Figure 3E shows a similar stack, except that the curved strip profile film 308-1 is deposited before, rather than after, the curved channel profile film 307-1. As mentioned above, the number of layers and thickness profiles shown in these figures are merely exemplary. More or fewer than four pairs of complementary films can be deposited to optimize the overall curvature of the wafer. Furthermore, as shown in Figures 3F and 3G, additional stretch or compressive layers can be added between a pair of complementary films or as a final layer.

[0058] Figures 3F and 3G show depositable capping or filler layers. In Figure 3F, a capping layer 342 with a uniform or substantially uniform thickness is deposited. As will be discussed further below, capping layer 342 can be a uniform thickness profile film with tensile internal stress, compressive internal stress, or zero or negligible internal stress. A uniform thickness profile film can be deposited after a stack of one or more complementary profile films is deposited. In some embodiments, a uniform thickness profile film can be deposited between stacks of complementary profile films. For example, the complementary profile films described herein can be used to compensate for saddle-shaped wafer curvature, such as positive x-curvature and negative y-curvature. While complementary profile films reduce the difference in wafer curvature between the x and y directions, the wafer curvature may still be relatively large, such as 200 µm or more, when viewed from a reference plane (e.g., an xy plane intersecting the wafer). For example, a saddle-shaped wafer may have a backside deposition layer that changes its shape to a bowl-shaped or dome-shaped wafer. The difference between x-curvature and y-curvature is reduced, but the wafer is still curved. A contour capping layer of uniform thickness can compensate for such wafer curvature by having uniform tensile or compressive internal stress. Since the x-curvature and y-curvature have been significantly balanced by complementary contour films, the uniform thickness contour film can compensate for the remaining wafer curvature.

[0059] Figure 3G shows a schematic diagram of the filler layer 344. During the deposition of the curved strip profile film 308, the curved strip profile film may exhibit a "center drop," meaning that the film thickness has two maximum values ​​deviating from the film center position at or near the radius zero (i.e., at or near the wafer center), and at the radius zero, the film thickness is less than the maximum value. For complementary profile films with small thicknesses, such as less than about 1 µm, such thickness differences may not be significant. However, for complementary profile films with large overall thicknesses or alternatingly stacked complementary profile films, such as greater than about 2 µm or greater than about 2.5 µm, the center drop may become significant and affect the flatness of the film. Therefore, a filler layer 344 can be deposited to fill the gaps formed in the curved strip profile film. In some embodiments, a filter layer 344 can be deposited to fill the gaps formed in the curved channel profile film, for example, in the case where the alternatingly stacked film 340 is formed similarly to that in Figure 3D. The filler layer 344 can be deposited using a technique similar to that of the curved strip profile 344, with its thickness forming a sharper cone as a function of radius.

[0060] Compared to single-stacked films, alternating-stacked films may offer several advantages. As mentioned above, alternating-stacked films have a higher crack resistance margin. This is likely because the compressive stress film applies compressive stress to the tensile stress film, reducing the internal tensile stress at the outer edge of the tensile stress film and thus reducing the risk of cracking.

[0061] Alternating stacked films can also improve thermal stability. Under thermal annealing conditions, such as during manufacturing processes at approximately 600°C or higher, the back layer of silicon nitride can exhibit stress shift. Stress shift is a change in internal stress within the film, typically occurring after annealing, and is generally undesirable as it can reduce the film's ability to compensate for wafer warping or increase the risk of cracking. Such stress shift can originate from unreacted substances in the film, such as hydrogen and nitrogen, which may be present in Si-H or NH bonds from precursors and reactants such as silanes and NH3. Under annealing conditions, these bonds may react, and hydrogen and / or nitrogen may diffuse to the surface, leaving the film and altering the internal stress. For a single bilayer of a complementary profile film, increasing the overall thickness increases the percentage of stress shift after annealing. However, alternating stacked films may not increase the percentage of stress shift. This is likely because the alternating layers restrict the diffusion of substances from the film, where each interface of the compressed and stretched film may restrict the diffusion of hydrogen and other substances, and thus limit the stress shift of the film.

[0062] For example, after annealing at 800°C for 30 minutes, a 0.5 µm thick complementary profile film stack may exhibit stress offset, resulting in approximately 20% reduction in wafer warp compensation. A 2.5 µm thick complementary profile film stack may exhibit approximately 38% stress offset under the same operation, which is undesirable because a larger stress offset requires a thicker film to properly compensate for wafer warp after annealing, thus reducing yield. However, the alternating stacked films disclosed herein, with an overall thickness between approximately 1 µm and approximately 2.5 µm, can exhibit approximately 20% or less wafer warp compensation loss (derived from internal stress offset), where each complementary bilayer can have a thickness of approximately 0.5 µm. Therefore, in some embodiments, the stress offset depends not on the overall thickness of the alternating stack, but on the thickness of the individual non-uniform thickness profile films, allowing the alternating stack to compensate for larger wafer warp without resulting in a large wafer warp compensation loss after annealing. In various embodiments, annealing can be performed at temperatures above about 650°C, above about 700°C, above about 800°C, above about 900°C, or between about 650°C and about 900°C. The alternating stacked films described herein may have stress shifts after annealing, which cause a change of about 20% or less in wafer bending compensation.

[0063] Figures 4A-B provide graphs of the internal stress multiplied by the thickness of the two films measured along the x-axis from the wafer center to the edge. In Figure 4A, the stretched film deposition has a curved channel profile, while the compressed film deposition has a curved strip profile. The internal stress of the stacked films is based on the combination of the two films, and therefore exhibits compressive stress (negative in Figure 4A) for small x-values ​​(e.g., along the x-axis from the center to 100 mm), and tensile stress (positive) for large x-values ​​(e.g., along the x-axis from approximately 100 mm to the wafer edge).

[0064] Figure 4B shows different film combinations, where stretched film deposition has a curved strip profile and compressed film deposition has a curved channel profile. The internal stress of the stacked films is based on the combination of the two films, and therefore has tensile stress (positive values ​​in Figure 4B) for small x values ​​(e.g., along the x-axis from the center to 100 mm) and compressive stress (negative values) for large x values ​​(e.g., along the x-axis from about 100 mm to the wafer edge). As shown by the x-axis in Figures 4A and 4B, the result of stacked films is anisotropic internal stress, which varies in the x- and y-axis directions of the films.

[0065] In various embodiments, the two films can be deposited according to the diagrams in Figure 4A or Figure 4B. In some embodiments, an additional back layer can be deposited. The diagrams in Figures 4A and 4B are merely examples, and the deposited films may have different stress profiles than those shown in the figures. For example, as discussed further herein, the internal stress of the two films can be controlled based on identified wafer bending / internal stress forces.

[0066] Figure 4C provides an isometric view of wafer curvature based on back-side deposition of stacked films, which have an internal stress profile similar to that shown in Figure 4B. Stretched film deposition has a curved stripe profile, while compressed film deposition has a curved channel profile. The internal stress of the stacked films is based on the combination of the two films, and therefore exhibits tensile stress for small x-values ​​and compressive stress for large x-values. In other words, the wafer in Figure 4C has positive x-curvature caused by internal compressive stress along the x-direction, and negative y-curvature caused by internal tensile stress along the y-direction.

[0067] It should be understood that the wafer bending shown in Figure 4C is for a substantially flat wafer on which the back-side layer corresponding to that in Figure 4B is deposited. In common applications, incoming wafers are bent based on the internal stress of the front-side layer, and the wafer bending shown in Figure 4C will counteract the existing bending to achieve a relatively flat shape. For example, the stacked films shown in Figures 4B and 4C can be used to counteract the -X / +Y wafer bending shape shown in Figure 2.

[0068] As shown in Figure 4C, for small y-values, the compressive internal stress in the central region causes the wafer to have positive x-curvature, while for large y-values, the tensile internal stress in the edge region causes the wafer to have negative y-curvature. This anisotropic internal stress allows stacked films to mitigate the curvature of the saddle-shaped wafer, resulting in a substantially flat wafer.

[0069] Figure 5 illustrates an exemplary process using a back-side layer structure deposition, which includes two or more films with non-uniform thickness profiles. The process in Figure 5 begins with measuring and / or identifying wafer curvature (502). One or more front-side layers may be deposited on the wafer, as well as the one or more back-side layers, resulting in wafer curvature. Measuring and / or identifying wafer curvature may include measuring or determining the shape of the wafer and which dimensions have greater curvature. In some embodiments, measuring and / or identifying wafer curvature may include measuring and / or identifying x-curvature values ​​and y-curvature values. In some embodiments, measuring and / or identifying wafer curvature may include measuring and / or identifying whether the x-curvature is greater than or less than the y-curvature.

[0070] After measuring and / or identifying wafer curvature, the wafer is received into the processing chamber (504). In some embodiments, measuring and / or identifying wafer curvature may be performed as part of receiving the wafer into the processing chamber or after receiving the wafer into the processing chamber. In some embodiments, optionally, as part of receiving the wafer into the processing chamber or after receiving the wafer into the processing chamber, the wafer (506) may be rotated. Rotation may be performed to orient the wafer such that the wafer curvature aligns with the deposition area of ​​the processing chamber, as described above in conjunction with FIG. 3A. For example, the processing chamber may be configured to deposit a stretch film in the central region and a compression film in the edge regions. Thus, the incoming wafer may be rotated such that the positive dimensional curvature between the x-axis and y-axis of the wafer aligns with the central region of the processing chamber (because the tensile internal stress film deposited on the back side of the wafer alleviates the positive curvature). In some embodiments, the incoming wafer may be rotated such that the positive wafer curvature aligns with the central region of the processing chamber. In some embodiments, the processing chamber may be configured to deposit a curved strip profile stretch film and a curved channel profile compression film. For example, compared to other combinations of non-uniform thickness profile films and internal stress, the processing chamber can deposit curved strip profile stretched films and curved channel profile compressed films with better material properties (e.g., better non-uniformity). Therefore, rotating the wafer to align the wafer bends with the deposition area of ​​the processing chamber can improve yield and reduce non-uniformity compared to performing different formulations on wafers with +X / -Y bends and wafers with -X / +Y bends.

[0071] For example, returning to Figure 2, if the processing chamber is configured to deposit a curved strip profile stretched film in the central region and a curved channel profile compressed film in the edge region, then the -X / +Y saddle shape will not require rotation, while the +X / -Y saddle shape will require rotation. Rotation will ensure that the positive bend aligns with the curved strip profile stretched film and the negative bend aligns with the curved channel profile compressed film. In fact, rotating a wafer with a +X / -Y curved saddle shape by 90° will result in a wafer with a -X / +Y curved saddle shape, assuming the coordinates are relative to the deposition apparatus rather than the wafer itself.

[0072] As discussed further below, in some embodiments, rotation may be optional because the processing chamber can deposit curved strip profile films and curved channel profile films with compressive or tensile internal stresses. Therefore, depending on the x-bend and y-bend of the wafer, the internal stress of the deposited film can be varied to appropriately compensate for the x-bend and y-bend. However, it is worth noting that in some embodiments, the processing chamber may not be azimuthally symmetrical; the curved strip profiles and curved channel profiles may not rotate but have a fixed orientation, as shown in Figure 3A.

[0073] A first back-side layer (508) with a first type of internal stress and a first non-uniform thickness profile is deposited. The first type of internal stress can be compressive or tensile. The non-uniform thickness profile can be a curved strip profile or a curved channel profile discussed herein, or any other variation or combination of such profiles. The type of internal stress and profile of the film can be based on wafer curvature. For example, a curved channel profile stretched film or a curved strip profile compressed film can be deposited on a +X / -Y wafer-curved saddle-shaped wafer to compensate for positive X-curvature or negative Y-curvature, respectively.

[0074] Alternatively, the wafer can be rotated 90°, effectively giving it a -X / +Y wafer bending saddle shape. In this embodiment, a curved channel profile compression film or a curved strip profile stretching film can be deposited thereon to compensate for (current) negative X-bending or positive Y-bending, respectively.

[0075] A second back layer (510) is deposited having a second type of internal stress and a second non-uniform thickness profile (which is complementary to the first non-uniform thickness profile). In some embodiments, the second type of internal stress is the opposite type of the first type of internal stress, i.e., compressive or tensile stress. The second non-uniform thickness profile may be complementary to the first non-uniform thickness profile; that is, if the first non-uniform thickness profile is a curved strip profile, then the second non-uniform thickness profile is a curved channel profile. In some embodiments, the second back layer may not be complementary to the first back layer, or may be partially complementary to the first back layer.

[0076] Generally, stretching films pull positive bends into a more planar shape, while compression films push negative bends into a more planar shape. Furthermore, as shown in Figure 3A, curved strip profile films compensate for Y-bends, while curved channel profile films compensate for X-bends, because the curved strip profile films are deposited primarily in the central region, and the curved channel profile films are deposited primarily in the edge regions. Therefore, based on the x-bends and y-bends of the incoming wafer, complementary films can be deposited to properly handle both x-bends and y-bends. Depending on the wafer bends handled by the first back layer, a second back layer can be formed to handle another wafer bend, such as an x-bend or a y-bend.

[0077] In some embodiments, an optional plasma treatment may be performed to improve the adhesion of the back layer to the substrate (511). Plasma treatment can improve the adhesion of curved strip profile and curved channel profile films to the underlying layer and / or substrate. This operation may be performed between the deposition of the first and second back layers, after the deposition of the first back layer, or after the deposition of the second back layer, or may not be performed at all or may be performed more than once. In some embodiments, an inert gas (such as argon, xenon, N2, etc.) may be used for plasma treatment. In some embodiments, plasma treatment is performed using an inert gas and substantially without the use of other gases. Plasma treatment can bombard the surface, improving adhesion without etching the layer.

[0078] In some embodiments, operations 508 and 510, and optional operation 511, may be repeated once or multiple times. Optionally, operation 511 may be performed for any one or more of each cycle of depositing complementary profile films. These operations may be repeated to deposit alternating layer stacks as shown in Figures 3D-G. In some embodiments, each pair of complementary profile films may have a thickness of less than about 1 µm, wherein the alternating stack films may have a total thickness greater than about 1 µm, greater than about 2 µm, greater than about 3 µm, or between about 1 µm and about 3 µm. Alternating stack films typically reduce throughput compared to complementary profile films in a single stack. However, alternating stack films may have improved material properties, including crack tolerance, thermal stability, adhesion, substrate surface protection, and film uniformity.

[0079] Optionally, in some embodiments, a third layer (512) is deposited, having a uniform thickness profile, a curved channel profile, or a curved strip profile. In some embodiments, the first and second back layers can balance x-bends and y-bends, however some bends may still be present. In such embodiments, the wafer may have a bowl or umbrella shape. Therefore, depositing a film with a uniform thickness profile can help further reduce wafer bends. In some embodiments, an isotropic internal stress film, such as a stretching film or a compression film, is deposited to further mitigate wafer bends. The type and magnitude of the internal stress can be based on wafer bends. Positive wafer bends or bowl shapes can be mitigated using a stretching film, while negative wafer bends or dome / umbrella shapes can be mitigated using a compression film.

[0080] In some implementations, the wafer warpage may be relatively large after the deposition of the first and second back-side layers, so a third film can be deposited to mitigate such warpage. For example, the incoming wafer may have an x-warpage of 400 μm and a y-warpage of -400 μm, and the x-warpage and y-warpage after the deposition of the first and second back-side layers may be -300 μm. Although the x-warpage and y-warpage are still large, they have been balanced and can therefore be mitigated by depositing a back-side layer with a uniform thickness profile. Thus, the first and second back-side layers can balance the x-warpage and y-warpage, but cannot mitigate the warpage within acceptable tolerances.

[0081] In some embodiments, the internal stress of the deposited first and second back layers may be less than that of the deposited front layer; that is, the first and second back layers cannot fully compensate for the bending caused by the front layer. In some embodiments, the stacking of the first and second back layers can reduce wafer bending to about 200 μm or less.

[0082] In some embodiments, a capping layer or filler layer (collectively referred to as cap-fill layer) is deposited in step 512. The cap-fill layer can be deposited to improve the flatness of the back side of the substrate and / or the overall wafer curvature. As mentioned above, curved strip profile films may exhibit a “center drop,” where the film thickness has two maximum values ​​at the film center location away from zero radius, and at zero radius, the film thickness is less than the maximum value. For complementary profile films with small thicknesses, such as less than about 1 µm, such thickness differences may not be noticeable. However, for complementary profile films with larger thicknesses or alternating stacks of complementary profile films with a large total thickness, such as greater than about 2.5 µm or greater than about 3 µm, the center drop may become significant and affect the film flatness.

[0083] Therefore, in some embodiments, a curved strip profile film is deposited in 512 as a cap fill layer. The cap fill layer can be any material disclosed herein, including silicon nitride or silicon oxide. In some embodiments, the cap fill layer can have neutral or substantially neutral internal stress. Cap fill layers can be deposited to improve the flatness of the back-side layer stack, and therefore neutral or zero internal stress may be desirable, as it does not affect the internal stress of the back-side layer and the overall wafer curvature.

[0084] In some embodiments, operation 512 is not performed. In these embodiments, since the wafer is substantially flat after the deposition of the first and second back layers, a uniform back film is not deposited. This may be due to the adjustment of the first and second back layers based on the wafer's x-bend and y-bend. Therefore, the first and second back layers can fully compensate for wafer bending without a third uniform layer. For example, the magnitude of the tensile and / or compressive stresses of the back layers can be controlled by adjusting deposition conditions such as RF power (including high-frequency and low-frequency power), temperature, pressure, precursor flow, reactive gas flow, precursor flow ratio, dopant, and the thickness of the deposited film. In some embodiments, process conditions can be varied to adjust the magnitude of the tensile or compressive stresses of the back layers, thereby significantly reducing the x-bend and y-bend of the incoming wafer. Therefore, depositing the first and second back layers as described above can significantly reduce all wafer bending. In these embodiments, a uniform third back layer may not be necessary to reduce the bending of the incoming wafer.

[0085] In some implementations, operation 512 may not be performed based on the shape of the incoming wafer. For example, a Tucker roll or semi-tubular wafer may have minimal or no curvature in the x or y direction. Therefore, only the curvature in the x or y direction needs to be mitigated, rather than both. In such implementations, the curved strip profile film and the curved channel profile film can be adjusted to compensate for either x-curvature or y-curvature. These two non-uniform thickness profile films can balance the curvature by mitigating either x-curvature or y-curvature, while not causing curvature in the other substantially flat direction.

[0086] The back-side layer can be deposited using CVD, PECVD, ALD, epitaxy, PVD, or other deposition processes. The back-side layer can be deposited using a dedicated back-side deposition apparatus. In some embodiments, the wafer switches between operating chambers 508, 510, and / or 512. The back-side deposition apparatus can be a different deposition apparatus than that used to deposit one or more front-side layers.

[0087] The curvature induced by the first, second, and third back layers can be the sum of the individual induced curvatures. In some embodiments, the combined curvature amplitude of the back layers can be approximately the same as the curvature amplitude of one or more front layers. In some embodiments, the combined x-curvature and y-curvature amplitude of the back layers can be approximately the same as the x-curvature and y-curvature amplitude of one or more front layers. In some embodiments, the curvature contributions of all front and back layers can be combined to minimize the total curvature of the wafer (i.e., less than about 100 μm). In some embodiments, after performing the method of FIG. 5, the wafer can be substantially flat, for example, the wafer can have a curvature of about 200 μm or less, about 150 μm or less, about 100 μm or less, about 50 μm or less, or about 30 μm or less. Flatness can depend on the specific downstream operation to be performed. For example, deposition or etching operations can be performed within tolerances, with wafer curvature of about 200 μm or less, about 150 μm or less, or about 100 μm or less. However, photolithography operations may have tighter tolerances, and the flatness can be approximately 50 μm or less, or approximately 30 μm or less.

[0088] Note that when referring to the bending values ​​caused or resulting from each back layer, it is assumed that the bending is not compensated by other layers. For example, when referring to the magnitude of the bending caused by the first back layer, we assume that the bending would occur in the absence of other layers on the substrate, such as the absence of a front layer. The magnitude of the layer-induced bending depends on the internal stress of the material in the layer and the thickness of the layer.

[0089] Compensation of the back layer refers to the bending contribution of the back layer, which can be combined with the bending contribution of the front layer to reduce or balance x-bending and y-bending. As described above, the bending contributions of all front and back layers can be combined. Positive bending (forming a bowl shape) caused by the front layer can be reduced by a back layer with tensile internal stress, which causes negative bending. The negative bending caused by the back layer compensates for the positive bending caused by the front layer, thereby making the total wafer bending smaller and / or more uniform than without a back layer. Bending strip profile films and bending channel profile films can compensate for x-bending or y-bending, depending on the orientation of the processing chamber and the wafer. For example, assuming the back layer is deposited according to the region of FIG. 3A, the bending strip profile film can compensate for y-bending, for example, reducing the total y-bending, while the bending channel profile film can compensate for x-bending, for example, reducing the total x-bending. In some embodiments, compensation may include partial mitigation of wafer bending. As described above, the first and second back layers can partially compensate for wafer bending, and a third or more back layers can be deposited to compensate for any remaining wafer bending. In other embodiments, the first and second back layers having the non-uniform thickness profile described herein can fully compensate for wafer curvature, for example, reducing wafer curvature to less than about 100 μm or less than about 30 μm.

[0090] In some embodiments, the back layer disclosed herein comprises a material having an internal stress of at least about 100 MPa or from about 100 to about 2000 MPa. These values ​​can be tensile or compressive internal stresses, depending on the type and properties of the back material required to counteract the bending caused by the front layer. The aforementioned internal stress values ​​can be applied to any one or more back layers in a multilayer back stack. Any two back layers can have the same or different internal stress values.

[0091] Exemplary materials used to fabricate a back layer with tensile internal stress include silicon nitride (SiN), silicon oxynitride, and a polymer layer. As an example, a tensile film can be deposited using CVD or PECVD techniques. To eliminate wafer warping caused by a front layer with compressive internal forces, a compression film can be used for the host back layer. The compression film can be formed using specific materials and / or processing conditions. Materials used to fabricate the compression film include silicon oxide (SiO2). x Materials include silicon nitride, aluminum oxide, aluminum nitride, and polycrystalline silicon. The compressed film can be deposited using CVD or PECVD techniques. The above materials and deposition techniques are applicable to any one or more back layers of a multilayer back stack. Any two back layers can be formed using the same or different techniques.

[0092] Deposition via PECVD involves flowing reactants (optionally along with co-reactants) into a processing chamber while exposing a bent semiconductor substrate to plasma. The plasma drives a gas-phase reaction, resulting in film deposition. PECVD reactions typically involve continuously feeding reactants to the semiconductor substrate while it is exposed to plasma. In some embodiments, depositing a nitride film on the back side of a substrate includes exposing the back side of a flat and / or bent semiconductor substrate to a silicon-containing precursor and a nitrogen-containing reactant, and exposing the back side of the semiconductor substrate to plasma to drive a reaction between the silicon-containing precursor and the nitrogen-containing reactant, thereby depositing a nitride film. To protect the front side of the semiconductor substrate (on which circuitry, transistors, and other device components are patterned in back-side processes), the front side is protected from exposure to plasma and / or reactants or process gases, for example, by maintaining a gap between the front side of the semiconductor substrate and the nozzle smaller than the plasma sheath, and / or by allowing an inert gas to flow toward the front side of the semiconductor substrate. By depositing on the back side of the semiconductor substrate, nitride film deposition on circuitry, transistors, and other device components on the front side of a bent semiconductor substrate can be avoided.

[0093] In some embodiments, the curved strip profiles and curved channel profiles described herein can be achieved by controlling the precursor concentration near the curved semiconductor substrate during deposition. In this disclosure, the precursor concentration adjacent to the curved semiconductor substrate can be controlled by design features of the nozzle base. Such design features can affect the hemodynamics of the precursor flowing out of the nozzle base. In some embodiments, the nozzle base can be divided into multiple regions, as shown in Figure 3A. For example, precursor gas can be delivered to a first region, and dilution gas can be delivered to a second region, and / or precursor and dilution gases of different flow rates or concentrations can be delivered to different regions to control the thickness and / or properties of the deposited film in different regions. This regulates the concentration of precursor gas near the curved semiconductor substrate. In some embodiments, the precursor gas can be delivered via a first supply pipe, and the dilution gas can be delivered via a second supply pipe.

[0094] Device Figure 6A is a block diagram illustrating a substrate processing system 632 for performing processing on wafer 602 according to some embodiments. As shown, the substrate processing system may include a processing chamber (or cell) 634. A central pillar may be configured to support a base when the top surface (or front side) of wafer 602 is being processed (e.g., a film is being formed on the top surface of wafer 602 or the back side of wafer 602). According to some embodiments disclosed herein, the base may refer to a nozzle base (“ShoPed”) 606. A nozzle 636 may be disposed above the ShoPed 606.

[0095] In some embodiments, nozzle 636 may be electrically coupled to power supply source 638 via mating network 640. Power supply source 638 may be controlled by control module 642, such as a controller. In some embodiments, power may be provided to nozzle 606 instead of nozzle 636, or power may be provided to both nozzle 606 and nozzle 636. Control module 642 may be configured to operate substrate processing system 632 by executing process inputs and controls for a specific process recipe. Depending on whether the top surface of wafer 602 is receiving a deposited layer or layer stack, or whether the bottom surface of wafer 602 is receiving a deposited layer or layer stack, controller module 642 may set various operational inputs for the process recipe, such as power level, timing parameters, process gases, mechanical movement of wafer 602, and / or height of wafer 602 relative to nozzle 606 (and distance between wafer 602 and nozzle 636).

[0096] In some embodiments, the center post may also include lifting pins controlled by a lifting pin controller. These lifting pins can be used to lift the wafer 602 from the nozzle 606 to allow an end effector (not shown) to pick up the wafer and lower it after the end effector has placed it. The end effector can also position the wafer 602 above the spacer 644. As will be described below, the spacer 644 may be sized to provide controlled separation of the wafer 602 between the bottom surface of the nozzle 636 (facing the wafer) and the top surface of the nozzle 606 (facing the wafer).

[0097] In some embodiments, the substrate processing system 632 may further include a first gas manifold 646 connected to a first gas source 648 (e.g., a gaseous chemical and / or inert gas supplied from a facility). Depending on the purpose and the processing being performed on the top surface of the wafer 602, the control module 642 may control the delivery of the first gas source 648 via the first gas manifold 646. The selected gas may then flow into the nozzle 636 and be distributed within a space defined between the surfaces of the nozzle 636 facing the wafer 602 when the wafer is placed above the substrate or spray holder.

[0098] In some embodiments, the substrate processing system 632 may further include a second gas manifold 650 connected to a second gas source 652 (e.g., a gaseous chemical and / or inert gas supplied from the facility). Depending on the processing performed on the bottom surface of the wafer 602, the control module 642 can control the delivery of the second gas source 652 via the second gas manifold 650. The selected gas can then flow into the nozzle 636 and be distributed within a spatial volume defined between the surfaces of the nozzle 606 facing the lower surface or lower side (back side) of the wafer 602 when the wafer is positioned above the nozzle 606 and / or spacer 644. The spacer 644 provides separation optimized for deposition on the lower surface of the wafer 602 and reduces deposition above the top surface of the wafer 602. In some embodiments, when the deposition target is the lower surface of wafer 602, an inert gas can flow through nozzle 636 across the top surface of wafer 602, which can push the reactant gas away from the top surface and allow the reactant gas supplied from nozzle 606 to be guided to the lower surface of wafer 602. Spacer 644 and / or other similar substrate support features can be used to provide controlled separation between the wafer and the nozzle and nozzle. Spacer 644 and / or other similar substrate support features can be connected or supported by the nozzle so that the wafer (or its reference plane, when the wafer is bent) can maintain a uniform and / or parallel distance from the top surface of the nozzle, even in cases of undesirable movement or vibration at the system or chamber level.

[0099] In some embodiments, nozzle 636 or nozzle 606, or both, may have a partitioned deposition design similar to that shown in FIG. 3A. For example, gas manifold 650 may be fluidly connected to control the gas delivery to region 302 or region 304. By controlling the gas flow to region 302 or region 304, a film may be deposited as shown in FIGS. 3B and 3C. In some embodiments, nozzle 636 or nozzle, or both, may have a different partitioned deposition design than that shown in FIG. 3A. For example, referring to FIG. 5, when measuring or identifying wafer curvature (502), a film may be deposited on the back side of the wafer using a nozzle and / or nozzle with a partitioned deposition design corresponding to that particular wafer, or the airflow through the nozzle and / or nozzle may be adjusted to correspond to the contour of the wafer curvature.

[0100] Furthermore, the gas may or may not be premixed. Appropriate valves and mass flow control mechanisms can be employed to ensure the correct gas delivery during the deposition and plasma treatment phases of the process. The process gas may exit chamber 634 via one or more exhaust ports or outlets. A vacuum pump (e.g., a first- or second-stage mechanical dry pump and / or a turbomolecular pump) can extract the process gas and maintain an appropriate low pressure within the reactor via a closed-loop controlled flow limiter (e.g., a throttle valve or pendulum valve).

[0101] In some embodiments, the carrier ring 654 may surround an outer region of the spray holder 606. When processing the top surface of the wafer 602, for example, when material is being deposited thereon, the carrier ring 654 may be configured to be positioned above a carrier ring support region that forms a step downward from the wafer support region at the center of the spray holder 606. The top surface of the carrier ring 654 is substantially coplanar with the top surface of the wafer 602. The carrier ring 654 may include an outer edge side (e.g., outer radius) of its disk structure and a wafer edge side (e.g., inner radius) of its disk structure, which is closest to the location of the wafer 602. The carrier ring 654 may be associated with an inner diameter (ID). The inner diameter may extend to the inner periphery of the carrier ring and generally surround the substrate (e.g., the wafer 602) in the processing chamber. The wafer edge side of the carrier ring 654 may also include a plurality of contact support structures or "tabs" that are configured to raise the wafer 602 when the carrier ring 654 is held by spacers 644. The carrier ring 654 may include a plurality of tabs, the number of which is selected from the range of supporting the wafer 602 during processing. Additional details regarding the tab implementation will be provided below. In some implementations, the wafer may be placed directly on spacers or other similar substrate support features, or directly supported by spacers or other similar substrate support features, without the need for a carrier ring.

[0102] Figure 6B is a block diagram illustrating another version of a substrate processing system 632 for performing processing on wafer 602 according to some embodiments. In some embodiments, a spoke fork 656 may be used to raise and hold a carrier ring 654 at its process height, for example, to allow deposition on the lower surface (back side) of wafer 602. Thus, the carrier ring 654 can be raised together with wafer 602. In some embodiments, the carrier ring 654 may be rotated to another station, such as in a multi-station system. In some embodiments, the wafer may be raised or moved directly using a spoke fork or any other transfer mechanism without a carrier ring.

[0103] Broadly speaking, the embodiments disclosed herein are systems for depositing PECVD films on selected sides (front and / or back) of a wafer via dynamic control. Some embodiments may include dual-flow electrodes for defining a capacitively coupled PECVD system. This system may include a flow nozzle (e.g., nozzle 636) and a nozzle holder 606. In some embodiments, the flow holder (i.e., the nozzle holder) is a combination of the nozzle and the holder, where deposition is performed on the back side of the wafer. The electrode geometry combines features of the nozzle (e.g., gas mixing chamber, orifices, orifice patterns, anti-gas spray baffles) with features of the holder. Examples of features of the holder or nozzle holder include an embedded controlled heater (or a distributed heater or heater element), a wafer lifting mechanism, the ability to maintain a plasma suppression ring, and mobility. This allows wafer transfer and gas handling to be performed with or without RF power from the holder.

[0104] In some implementations, the system may have a wafer lifting mechanism that tightly controls the parallelism of the substrate relative to the "spray holder," the nozzle, and / or the electrodes. In one example, this can be achieved by setting a lifting mechanism (e.g., a mandrel or lifting pin mechanism) parallel to the two electrodes and controlling manufacturing tolerances. In another example, lifting can be achieved by raising the wafer lifting component. This option may not allow for dynamic control of the side where deposition is performed.

[0105] In some configurations, the lifting mechanism allows for dynamic control of the substrate position during processing (before, during, and after plasma) to control the side on which deposition occurs, the deposition profile, and the properties of the deposited film. The system can further allow for selective activation / deactivation of the reactant flow on that side. Reactants can flow on one side, while an inert gas can flow on the other to suppress deposition and plasma flow.

[0106] In some implementations, the gap between the sides of the wafer where plasma / deposition is not required can be tightly controlled. This distance can be controlled to suppress plasma. If the distance is not controlled, the wafer may be susceptible to plasma damage. For example, the system may allow a minimum gap of about 2 mm to about 0.5 mm, while in another implementation it may allow about 1 mm to about 0.05 mm (limited by wafer bending), and such gaps can be controlled. This gap can be controlled according to process conditions.

[0107] In some implementations, the airflow base (i.e., the nozzle) may achieve, but is not limited to: (a) thermally stabilizing the wafer to the processing temperature prior to processing; (b) selectively designing the aperture pattern on the nozzle to selectively deposit films in different regions on the back side of the wafer; (c) attaching replaceable rings to achieve appropriate plasma confinement and aperture patterning; (d) an in-chamber stabilized wafer transfer mechanism for transferring the wafer outward to another chamber or boat – e.g., lift pins, RF coupling features, minimum contact arrays; (e) implementing gas mixing features, e.g., internal gas chambers, baffles, and manifold line openings; and (f) providing compartments in the airflow base (i.e., the nozzle) to allow selective airflow to flow to different regions on the back side of the wafer, and controlling the flow rate via a flow controller and / or multiple gas chambers.

[0108] In another embodiment, dynamic gap control of the wafer lifting mechanism is used to achieve: (a) controlling the distance from the deposition or reactant flow electrode to the side or middle of the wafer to be deposited, allowing deposition on both sides; and (b) the lifting mechanism dynamically controlling the distance during the process (before plasma, during plasma, after plasma) to control the side to be deposited, the deposition profile, and the characteristics of the deposited film. In another embodiment, for deposition modes used on the back side of the wafer, edge exclusion control is highly desirable to avoid lithography-related overlay issues. The lifting mechanism used in this system is accomplished via a carrier ring 654, which has design features for shielding deposition on the edges. This edge exclusion control is specified through the design and shape of the carrier ring.

[0109] Figure 7A shows a cross-sectional view of the edge region of the spray nozzle 606. This view provides a cross-sectional representation of the support ring 654, which has an inner radius 654a and an outer radius 654b. In some embodiments, the support ring 654 includes a support extension 654c that extends below a substantially flat surface of the support ring 654.

[0110] The support extension 654c is configured to mate and reside within a support surface defined in the top surface of the spacer 644. The support surface provides a complementary mating surface to the support extension 654c, thereby preventing the carrier ring 654 from sliding or moving when supported by the spacers 644. Although three spacers 644 are shown in FIG. 7B, it is conceivable that any number of spacers can be provided, as long as the carrier ring can be supported substantially parallel to the surface of the nozzle 606 and the spacing is defined to support the wafer 602 at a distance from the top surface of the base 606.

[0111] Further illustration shows that the top surface of the spray holder 606 will include a perforation pattern 606a distributed across the entire surface to provide uniform gas distribution and output during operation. In one embodiment, the perforation pattern 606a is distributed in a plurality of concentric rings, which begin at the center of the top surface of the spray holder 606 and extend to the outer periphery of the spray holder 606. At least one perforation pattern 606a is disposed at an edge perforation region 607 of the perforation pattern, and the orifice defined in the edge perforation region 607 is preferably angled to provide gas without being perpendicular to the surface of the spray holder 606.

[0112] In one example, the angle or tilt of the orifice in the edge hole region 607 is defined as tilted or angled away from the center of the nozzle 106. In one embodiment, this angle is approximately 45° to the horizontal. In other embodiments, this angle may vary between 20° and approximately 80° to the horizontal. In one embodiment, by providing angled orifices in the edge hole region 607, additional distribution of process gases can be provided during backside deposition of the wafer 602. In one embodiment, the remaining orifices 606d of the hole pattern 606a are oriented substantially perpendicular to the surface of the nozzle 106 and pointing towards the underside of the wafer 602.

[0113] Figure 7B shows that when wafer 602 is held by carrier ring 654, the edge of wafer 602 will be located on the edge region of the carrier ring inner radius 654a, which is closer to carrier ring 654. When positioning with spacer 644, the surface of nozzle 636 facing the top surface of wafer 602 can be substantially close enough to prevent deposition from occurring during the deposition mode on the back side of wafer 602.

[0114] For example, the distance between the top of wafer 602 and the surface of nozzle 636 is preferably between about 2 mm and about 0.5 mm, and in some embodiments about 1 mm to about 0.5 mm, depending on wafer curvature. That is, if the wafer is significantly curved, the gap will be about 0.5 mm or more. If the wafer is not significantly curved, the gap may be less than about 0.5 mm. In one embodiment, it is preferable to minimize the gap to prevent deposition on the top side of the substrate when a material layer is being deposited on the back side of the substrate. In some embodiments, nozzle 636 is configured to supply an inert gas flow over the top side of wafer 602 during deposition on the back side of the substrate and supply of deposition gas through nozzle 606.

[0115] Any suitable chamber may be used to implement the disclosed embodiments. Exemplary deposition apparatuses include a variety of systems, such as ALTUS® and ALTUS®Max available from Lam Research Corp. (Fremont, California), or any other variety of other commercially available processing systems.

[0116] Figure 8 is a schematic diagram of a processing system suitable for a deposition process (e.g., a front-side deposition process) according to an embodiment. System 800 includes a transfer module 803. Transfer module 803 provides a clean, pressurized environment to minimize the risk of contamination of the substrate being processed as it moves between various reactor modules. Mounted on transfer module 803 is a multi-station reactor 809 capable of performing ALD, processing, and CVD according to various embodiments. Multi-station reactor 809 may include multiple stations 811, 813, 815, and 817, which may operate sequentially according to the disclosed embodiments. A station may include a heating base or substrate support, one or more gas inlets or nozzles or distribution plates.

[0117] One or more single-station or multi-station modules 807 capable of performing plasma or chemical (non-plasma) pre-cleaning, other deposition operations, or etching operations may also be mounted on transfer module 803. This module can also be used for various processes, such as preparing substrates for deposition processes. System 800 also includes one or more wafer source modules 801, where wafers are stored before and after processing. An atmospheric robot (not shown) in atmospheric transfer chamber 819 can first move wafers from source modules 801 to loading locks 821. Wafer transfer devices (typically robotic arm units) in transfer module 803 move wafers from loading locks 821 to modules mounted on transfer module 803 and move wafers between these modules.

[0118] In various implementations, a system controller 842 is used to control the process conditions during the deposition process. The controller 842 will typically include one or more memory devices and one or more processors. The processor may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, etc.

[0119] The controller 842 controls all activities of the deposition apparatus. The system controller 842 runs system control software, which includes a set of instructions for controlling timing, gas mixing, chamber pressure, chamber temperature, wafer temperature, radio frequency (RF) power levels, wafer chuck or pedestal position, and other parameters specific to the process. In some embodiments, additional computer programs stored on memory devices associated with the controller 842 may be used.

[0120] The described implementation includes a user interface associated with controller 842. The user interface may include a display screen, a graphical software display of the device and / or process conditions, and user input devices such as pointing devices, keyboards, touchscreens, microphones, etc.

[0121] The system control logic can be configured in any suitable manner. Generally, this logic can be designed or configured in hardware and / or software. Instructions for controlling the drive circuitry can be hard-coded or provided as software. These instructions can be provided through "programming." Such programming is understood to include any form of logic, including hard-coded logic in digital signal processors, application-specific integrated circuits (ASICs), and other devices with specific algorithms implemented in hardware. Programming is also understood to include software or firmware instructions executable on a general-purpose processor. The system control software can be encoded in any suitable computer-readable programming language.

[0122] Computer program code used to control processes in a process sequence can be written in any conventional computer-readable programming language: for example, assembly language, C, C++, Pascal, Fortran, or others. The compiled object code or script is executed by a processor to perform the tasks identified in the program. Also, as indicated, the program code can be hard-coded.

[0123] The controller parameters relate to process conditions such as, for example, process gas composition and flow rate, temperature, pressure, cooling gas pressure, substrate temperature, and chamber wall temperature. These parameters are provided to the user in the form of a recipe and can be entered using a user interface.

[0124] Signals used for process monitoring can be provided via analog and / or digital input connections to system controller 842. Signals used for process control are output via analog and digital output connections to device 800.

[0125] The system software can be designed or configured in different ways. For example, multiple chamber assembly subroutines or control targets can be written to control the operation of the chamber assembly required to perform the deposition process according to the disclosed embodiments. Examples of programs or program segments used for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.

[0126] In some implementations, system controller 842 is part of a system, which may be part of the examples described above. Such a system may include semiconductor processing apparatus, which includes one or more processing tools, one or more chambers, one or more platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after the processing of semiconductor wafers or substrates. The electronics may be referred to as a “controller”, which can control various components or sub-components of one or more systems. Depending on the processing requirements and / or system type, system controller 842 may be programmed to control any process disclosed herein, including the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer tools and other transfer tools, and / or loading locks that are connected to or docked with a specific system.

[0127] System Controller In a broad sense, a controller can be defined as an electronic device having various integrated circuits, logic, memory, and / or software for receiving instructions, issuing instructions, controlling operations, enabling cleaning operations, enabling endpoint measurements, etc. Such a controller can be used in or with any of the devices described herein. Integrated circuits can include chips in the form of firmware storing program instructions, digital signal processors (DSPs), chips defined as application-specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). Program instructions can be instructions sent to the controller in the form of various individual settings (or program files) that define operating parameters for performing a specific process on or for a semiconductor wafer or system. In some embodiments, operating parameters can be part of a recipe defined by a process engineer to complete one or more processing steps during the fabrication of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or wafer dies.

[0128] A system controller may be part of or coupled to a computer integrated with, coupled to, or otherwise networked to the system, or a combination thereof. For example, the controller may be in the “cloud” or be all or part of a fab host system, allowing remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of manufacturing operations, examine the history of past manufacturing operations, examine trends or performance criteria of multiple manufacturing operations, change parameters of the current process, set processing steps to follow the current process, or initiate a new process. In some examples, a remote computer (e.g., a server) may provide process recipes to the system via a network (which may include a local network or the Internet). The remote computer may include a user interface that enables the input or programming of parameters and / or settings, which are then transmitted from the remote computer to the system. In some examples, the controller receives instructions in the form of data specifying parameters for each processing step to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process to be performed and the type of tool to which the controller is configured to interface with or control the tool. Therefore, as described above, a controller can be distributed, for example, by comprising one or more discrete controllers networked together and operating toward a common purpose (such as the process and control described herein). An example of a distributed controller for such a purpose is one or more integrated circuits on-site communicating with one or more integrated circuits remotely (e.g., at the platform level or as part of a remote computer), which together control the process on-site.

[0129] Exemplary systems may include, but are not limited to, plasma etching chambers or modules, deposition chambers or modules, rotary rinsing chambers or modules, metal plating chambers or modules, cleaning chambers or modules, chamfering edge etching chambers or modules, physical vapor deposition (PVD) chambers or modules, CVD chambers or modules, ALD chambers or modules, atomic layer etching (ALE) chambers or modules, ion implantation chambers or modules, developing (track) chambers or modules, and any other semiconductor processing systems that may be associated with or used for the fabrication and / or preparation of semiconductor wafers.

[0130] As described above, depending on one or more processing steps to be performed by the tool, the controller may communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the plant, a host computer, another controller, or tools used in the transport of materials to and from the tool location and / or loading port in the semiconductor manufacturing plant.

[0131] The system controller may include various programs. A substrate positioning program may include program code for controlling a chamber assembly used to load the substrate onto a pedestal or chuck and controlling the spacing between the substrate and other chamber components, such as gas inlets and / or targets. A process gas control program may include code for controlling gas composition, flow rate, pulse duration, and optionally, for allowing gas to flow into the chamber prior to deposition to stabilize the pressure within the chamber. A pressure control program may include code for controlling the pressure within the chamber by adjusting, for example, a throttle valve in the chamber's exhaust system. A heater control program may include code for controlling the current of a heating unit used to heat the substrate. Alternatively, the heater control program may control the delivery of a heat transfer gas, such as helium, to the wafer chuck.

[0132] Examples of chamber sensors that can be monitored during the deposition process include mass flow controllers, pressure sensors such as pressure gauges, and thermocouples located in a base or chuck. Appropriately programmed feedback and control algorithms, along with data from these sensors, can be used to maintain the desired process conditions.

[0133] The foregoing describes implementations of the present invention in single-chamber or multi-chamber semiconductor processing tools. The apparatus and processes described herein can be used in conjunction with photolithography patterning tools or processes, for example, for fabricating or manufacturing semiconductor devices, displays, LEDs, photovoltaic panels, etc. Typically, although not necessarily required, these tools / processes will be used or operated together in a common manufacturing facility. Photolithographic patterning of a film typically involves some or all of the following steps, each step employing multiple feasible tools: (1) applying a photoresist to the workpiece, i.e., the substrate, using a spin coater or spray coater; (2) curing the photoresist using a hot plate or oven or a UV curing tool; (3) exposing the photoresist to visible light or UV or X-rays using a tool such as a wafer stepper; (4) developing the photoresist to selectively remove it and thus pattern it using a tool such as a wet cleaning station; (5) transferring the photoresist pattern onto the underlying film or workpiece using a dry or plasma-assisted etching tool; and (6) removing the photoresist using a tool such as an RF or microwave plasma stripper.

[0134] in conclusion While the above embodiments have been described in detail to a certain extent for clarity of understanding, it will be apparent that certain variations and modifications may be implemented within the scope of the appended claims. The embodiments disclosed herein may be implemented without some or all of these specific details. In other instances, known process operations have not been described in detail to avoid unnecessarily obscuring the disclosed embodiments. Furthermore, although the disclosed embodiments are described in conjunction with specific embodiments, it should be understood that these specific embodiments are not intended to limit the disclosed embodiments. It should be noted that there are many alternative processes, systems, and apparatuses for implementing embodiments of the invention. Therefore, embodiments of the invention should be considered illustrative rather than restrictive, and these embodiments are not limited to the details given herein.

Claims

1. A method of reducing warpage in a substrate, the method comprising: receiving a substrate having a front side and a back side, wherein the substrate has a first warpage in an X direction of the substrate and a second warpage in a Y direction of the substrate; performing one or more cycles of: (a) forming a first backside layer on the back side of the substrate, wherein the first backside layer compensates for the first warpage more than the second warpage or the second warpage more than the first warpage, and wherein the first backside layer has a first type of internal stress and a first non-uniform thickness profile; (b) forming a second backside layer on the back side of the substrate, wherein the second backside layer compensates for the lesser of the first warpage or the second warpage compensated for by the first backside layer, wherein the second backside layer has a second type of internal stress opposite the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile complement each other such that when the first backside layer and the second backside layer are formed, they provide a complementary stack of films on the back side of the substrate having a substantially planar surface.

2. The method of claim 1, wherein the substrate is a semiconductor wafer having a partially fabricated integrated circuit on the front side.

3. The method of claim 1, wherein the substrate has a saddle-shaped warpage.

4. The method of claim 1, further comprising, prior to forming the first backside layer, determining that the first warpage has a greater magnitude than the second warpage.

5. The method of claim 4, further comprising, prior to forming the first backside layer, rotating the substrate based on the determination that the first warpage has a greater magnitude than the second warpage.

6. The method of claim 1, wherein the first non-uniform thickness profile is a curved strip having a thickness toward a center of the substrate that is greater than a thickness of an edge of the substrate.

7. The method of claim 6, wherein the curved strip has a longitudinal axis substantially parallel to the Y direction.

8. The method of claim 6, wherein the curved strip has a generally parabolic shape having a thickness as a function of the X direction that changes away from the back side of the substrate in a Z direction perpendicular to the X direction and the Y direction.

9. The method of claim 1, wherein the second non-uniform thickness profile is a curved channel having a thickness toward an edge of the substrate that is greater than a thickness of a center of the substrate.

10. The method of claim 9, wherein the curved channel has a parabolic shape having a thickness as a function of the X direction that changes away from the back side of the substrate in a Z direction.

11. The method of claim 1, wherein the first type of internal stress is a tensile stress.

12. The method of claim 1, wherein the first type of internal stress is a compressive stress.

13. The method of claim 1, further comprising forming a third backside layer on the backside of the substrate, wherein the third backside layer has a uniform shape and either the first type of internal stress or the second type of internal stress.

14. The method of claim 13, wherein the type and magnitude of internal stress of the third backside layer is based on a bow of the substrate after forming the first backside layer and the second backside layer.

15. The method of claim 1, further comprising identifying a value of the first bow and a value of the second bow, and wherein the first backside layer is formed and the second backside layer is formed based on the value of the first bow and the value of the second bow.

16. The method of claim 1, further comprising identifying a value of the first bow and a value of the second bow, and wherein the magnitude of internal stress of the first backside layer and the magnitude of internal stress of the second backside layer is based on the value of the first bow and the value of the second bow.

17. The method of claim 1, wherein the one or more cycles is two or more cycles.

18. The method of claim 1, wherein a total thickness of layers deposited during the one or more cycles is at least about 2 pm.

19. The method of claim 1, wherein the first backside layer and the second backside layer collectively have a first thickness, and each cycle of (a) and (b) deposits a complementary profile layer having the first thickness.

20. The method of claim 19, wherein the first thickness is less than about 1 pm.

21. The method of claim 1, wherein a variation in wafer bow compensation after annealing of the first backside layer and the second backside layer is less than about 20%.

22. The method of claim 1, further comprising forming a third backside layer on the backside of the substrate after performing the one or more cycles, wherein the third backside layer increases a flatness of the backside of the substrate.

23. The method of claim 1, further comprising performing a plasma treatment after forming the first backside layer, performing a plasma treatment after forming the second backside layer, or both, wherein the plasma treatment improves adhesion of the first backside layer and the second backside layer.

24. A substrate, comprising: one or more frontside layers on a frontside of the substrate, wherein the substrate has a first bow in an X-direction of the substrate and a second bow in a Y-direction of the substrate; a first backside layer on a backside of the substrate, wherein the first backside layer compensates for the first bow more than the second bow or the second bow more than the first bow, and wherein the first backside layer has a first type of internal stress and a first non-uniform thickness profile; a second backside layer on the backside of the substrate, wherein the second backside layer compensates for a lesser of the first bow or the second bow that is not compensated for by the first backside layer, wherein the second backside layer has a second type of intrinsic stress opposite the first type of intrinsic stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile complement each other such that when the first backside layer and the second backside layer are formed, they provide a complementary film stack on the backside of the substrate having a substantially flat surface.

25. The substrate of claim 24, wherein the substrate has the first bow or the second bow of about 300 pm or greater if neither of the one or more frontside layers is compensated for by the first backside layer.

26. The substrate of claim 24, wherein the first non-uniform thickness profile is a curved strip having a thickness toward a center of the substrate that is greater than a thickness of an edge of the substrate.

27. The substrate of claim 26, wherein the curved strip has a longitudinal axis substantially parallel to the Y direction.

28. The substrate of claim 26, wherein the curved strip has a generally parabolic shape having a thickness as a function of the X direction that changes away from a backside of the substrate in a Z direction perpendicular to the X direction and the Y direction.

29. The substrate of claim 24, wherein the second non-uniform thickness profile is a curved channel having a thickness toward an edge of the substrate that is greater than a thickness of a center of the substrate.

30. The substrate of claim 29, wherein the curved channel has a parabolic shape having a thickness as a function of the X direction that changes away from a backside of the substrate in a Z direction.

31. The substrate of claim 24, wherein the first type of intrinsic stress is a tensile stress.

32. The substrate of claim 24, wherein the first type of intrinsic stress is a compressive stress.

33. The substrate of claim 24, further comprising a third backside layer on the backside of the substrate, wherein the third backside layer has a uniform shape and either of the first type of intrinsic stress or the second type of intrinsic stress.

34. The substrate of claim 33, wherein a type of intrinsic stress and a magnitude of the intrinsic stress of the third backside layer are based on a bow of the substrate after the first backside layer and the second backside layer are formed.

35. The substrate of claim 24, further comprising an additional complementary film stack.

36. The substrate of claim 35, wherein the complementary film stack and the additional complementary film stack alternate together between the first backside layer and the second backside layer.

37. The substrate of claim 35, wherein a total thickness of all of the complementary film stacks is at least about 2 pm.

38. The substrate of claim 35, wherein a thickness of each of the complementary film stacks is less than about 1 pm.

39. The substrate of claim 35, wherein a variation in total wafer bow compensation of all complementary film stacks after annealing is less than about 20%.

40. The substrate of claim 35, further comprising a third backside layer deposited on the backside of the substrate after all complementary film stacks, wherein the third backside layer increases flatness of the backside of the substrate.

41. An apparatus for semiconductor processing, the apparatus comprising: a process chamber; and a controller comprising a memory and a processor configured to: receive a substrate having a frontside and a backside, wherein the substrate has a first bow in an X-direction of the substrate and a second bow in a Y-direction of the substrate; perform one or more cycles of: (a) forming a first backside layer on the backside of the substrate, wherein the first backside layer compensates for the first bow more than the second bow or the second bow more than the first bow, and wherein the first backside layer has a first type of internal stress and a first non-uniform thickness profile; (b) forming a second backside layer on the backside of the substrate, wherein the second backside layer compensates for the lesser of the first bow or the second bow compensated by the first backside layer, wherein the second backside layer has a second type of internal stress opposite the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile are complementary to each other such that when the first backside layer and the second backside layer are formed, they provide a complementary film stack having a substantially flat surface on the backside of the substrate.

42. A method for semiconductor processing, the method comprising: receiving a substrate having a frontside and a backside, wherein the substrate has a first bow in an X-direction of the substrate and a second bow in a Y-direction of the substrate; performing one or more cycles of: (a) forming a first backside layer on the backside of the substrate, wherein the first backside layer compensates for the first bow more than the second bow or the second bow more than the first bow, and wherein the first backside layer has a first type of internal stress and a first non-uniform thickness profile; (b) forming a second backside layer on the backside of the substrate, wherein the second backside layer compensates for the lesser of the first bow or the second bow compensated by the first backside layer, wherein the second backside layer has a second type of internal stress opposite the first type of internal stress and a second non-uniform thickness profile; and wherein the first non-uniform thickness profile and the second non-uniform thickness profile are complementary to each other such that when the first backside layer and the second backside layer are formed, they provide a complementary film stack having a substantially flat surface on the backside of the substrate.