A method for dismantling and recycling photovoltaic modules
By combining mechanical crushing and chemical solution soaking with ultrasonic treatment, the problem of incomplete separation of the encapsulant film from other materials during photovoltaic module dismantling was solved, achieving efficient and low-cost material recycling and improving recycling purity and processing efficiency.
Patent Information
- Application Number
- CN202511878104.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-12
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-12-12
AI Technical Summary
Existing photovoltaic module dismantling and recycling processes suffer from low dismantling efficiency, high costs, and low material purity, especially incomplete separation of the encapsulant film from other materials, which affects subsequent recycling.
The method involves mechanically crushing the components and then immersing them in a decomposition solution. A mixed solution of alkali, surfactant, amine salt, or alcohol is used, combined with ultrasonic treatment, to decompose the encapsulant film in photovoltaic laminates, achieving efficient separation of materials such as solar cells, solder ribbons, and glass.
The system achieves efficient separation of the adhesive film from glass, solder ribbon, and battery cells under mild conditions, improving the purity and integrity of recycled materials, reducing energy consumption, and increasing processing efficiency.
Smart Images

Figure CN121373019B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic module recycling technology, and in particular to a method for dismantling and recycling photovoltaic modules. Background Technology
[0002] With the rapid development of the photovoltaic industry, the installed capacity of crystalline silicon photovoltaic modules is increasing day by day. By 2030, the capacity of photovoltaic modules to be scrapped and dismantled will exceed 60 million tons, and the annual amount of newly scrapped and recycled modules will reach 10 million tons. The materials used in photovoltaic modules, such as aluminum, silver, copper, glass, encapsulant film, backsheet, and junction box, can be recycled and reused.
[0003] There are two main types of existing dismantling and recycling processes. The first type is physical dismantling process, with patents such as CN116550716A, CN116274283A, and CN117505263A. The problem is that while mechanically crushing and grinding the material into fine powder particles results in high dismantling efficiency, the purity of silicon wafer powder is only 60-80%. Ethylene-vinyl acetate copolymer films (EVA films) and co-extruded polyolefin films (EPE films) contain substances such as glass, silicon powder, silver powder, and copper powder, and the purity of these substances is not high. The second type is the pyrometallurgical dismantling process, such as patent CN114505329A. This process has several problems: the high temperature burns and decomposes the film material, while the battery cells, tin-plated copper solder strips, and glass are recovered intact. The film material is mostly burned off, but unburned organic residues cover the battery cells, solder strips, and glass surfaces, affecting subsequent recycling. The process involves continuous high-temperature treatment at 200-500 degrees Celsius, resulting in high energy consumption. Currently, pyrometallurgical equipment capable of dismantling 10,000 tons annually consumes approximately 12,000 kilowatt-hours of electricity per day.
[0004] Existing two types of dismantling processes have unsatisfactory results in the recycling and reuse of materials. Patent CN114038940A discloses a method for separating the backsheet of a photovoltaic module. The photovoltaic laminate is added to an alkaline alcohol solution for reaction. After the reaction, the fluorine layer in the backsheet floats on the surface of the reaction solution, the PET layer in the fluorine-containing backsheet dissolves in the reaction solution, and the other parts of the photovoltaic laminate sink to the bottom of the solution, thus separating the backsheet from the other parts of the photovoltaic laminate. However, this method can only separate the backsheet from the other parts and cannot achieve complete separation of all components.
[0005] Therefore, there is an urgent need for a dismantling and recycling process that is highly efficient, low-cost, highly pure, and fully recoverable to meet the growing demand for material recycling and reuse and the processing of scrapped components. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a method for dismantling and recycling photovoltaic modules. This method dismantles waste photovoltaic modules based on the physical and chemical properties of the encapsulant film, achieving the goals of high recycling efficiency, low cost, high recycling purity, and complete material recovery.
[0007] The objective of this invention can be achieved through the following technical solutions: A method for dismantling and recycling photovoltaic modules, the photovoltaic modules including glass, solar cells, solder strips, encapsulant film, frames, and junction boxes, the method comprising the following steps: S1. Remove the frame and junction box of the photovoltaic module to obtain the frame, junction box and module laminate to be processed; S2. Mechanically break the glass on the surface of the component laminate to be processed to obtain a component laminate with broken surface glass; S3. Divide the component laminate with broken surface glass into several small component units; S4. The small component unit is immersed in the decomposition treatment solution and ultrasonic treatment is applied simultaneously to obtain a mixture of battery cell and solder ribbon, adhesive film and glass bonding mixture, wherein the decomposition treatment solution includes alkali, surfactant, water, and at least one of alcoholic amine salt or alcohol. S5. The mixture of battery cells and solder ribbon, and the adhesive mixture of film and glass are sorted to obtain battery cells, solder ribbon, film and glass.
[0008] Furthermore, the photovoltaic module is a crystalline silicon photovoltaic module, and the encapsulant film is an EVA encapsulant film or an EPE encapsulant film.
[0009] Furthermore, the photovoltaic module is a double-glass photovoltaic module; Alternatively, the photovoltaic module may be a single-glass photovoltaic module, which may also include a backsheet.
[0010] Furthermore, in step S2, the glass fragments in the laminated component with broken surface glass have a size of 1~10mm.
[0011] Furthermore, in step S2, a rough-faced roller press is used to mechanically break the glass on the surface of the component laminate to be processed.
[0012] Furthermore, the forward speed of the component laminate to be processed is 0.1~5m / min, and the gap between the upper and lower rollers of the roller press is 3~5mm.
[0013] Furthermore, in step S3, the component laminate with broken surface glass is divided into several small component units, which helps to improve the processing efficiency of the decomposition process.
[0014] Furthermore, the spacing of the division is 10~300mm, preferably divided according to the size of the battery cell, wherein the battery cell size is mostly 183×183mm, 210×210mm, 183mm×210mm, and can also be adjusted according to the influence of laboratory conditions, such as 100mm×100mm in the embodiment.
[0015] Further, in step S4, the alkali includes one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, sodium carbonate, sodium bicarbonate, sodium methoxide, or sodium ethoxide.
[0016] The alcohols include one or more of methanol, ethanol, isopropanol, propylene glycol, ethylene glycol, diethylene glycol, or glycerol.
[0017] Further, in step S4, the alkanolamine salt is formed by reacting an alkanolamine with an acid; the alkanolamine includes one or more of ethanolamine, diethanolamine, triethanolamine, or isopropanolamine; The acid includes organic acids and inorganic acids, wherein the organic acid includes one or more of short-chain carboxylic acids, aromatic acids, fatty acids or substituted carboxylic acids; The short-chain carboxylic acids include one or more of formic acid, acetic acid, or propionic acid; The aromatic acid includes benzoic acid or salicylic acid; The fatty acids include one or more of benzoic acid, oleic acid, linoleic acid, palmitoleic acid, palmitic acid, lauric acid, stearic acid, butyric acid, or myristic acid; and the inorganic acids include one or more of hydrochloric acid, phosphoric acid, sulfuric acid, or nitric acid. The substituted carboxylic acids include one or more of lactic acid, citric acid, or pyruvic acid.
[0018] Furthermore, the acid is a fatty acid, including one or more of oleic acid, linoleic acid, palmitoleic acid, palmitic acid, lauric acid, stearic acid, butyric acid, or myristic acid.
[0019] Furthermore, the alcoholamine salt includes one or more of the following: triethanolamine oleate, triethanolamine stearate, triethanolamine laurate, triethanolamine palmitate, diethanolamine oleate, diethanolamine linoleate, ethanolamine oleate, ethanolamine stearate, isopropanolamine oleate, triethanolamine myristate, ethanolamine hydrochloride, diethanolamine hydrochloride, isopropanolamine hydrochloride, ethanolamine sulfate, diethanolamine nitrate, or triethanolamine phosphate.
[0020] Further, in step S4, the surfactant includes one or more of sodium dodecylbenzenesulfonate, alkyl glycoside, block polyether, fatty alcohol polyoxyethylene ether, or dehydrated sorbitol fatty acid polyoxyethylene ether.
[0021] Further, in step S4, the mass concentration of the alkali is 40~500g / L, preferably 120~240g / L; When the decomposition treatment solution is a mixed solution of alkali, surfactant, water, and alcohol amine salt, the sum of the mass concentrations of the alcohol amine salt and the surfactant is 20~240 g / L, preferably 50~80 g / L; the mass ratio of the alcohol amine salt to the surfactant is 2~6:1. When the decomposition treatment solution is a mixed solution of alkali, surfactant, water, and alcohol, the sum of the mass concentrations of the alcohol and surfactant is 20~240 g / L, preferably 50~80 g / L; the mass ratio of the alcohol to the surfactant is 2~6:1. When the decomposition treatment solution is a mixed solution of alkali, surfactant, water, alcoholic amine salt, and alcohol, the sum of the mass concentrations of the alcoholic amine salt, alcohol, and surfactant is 20~240 g / L, preferably 50~80 g / L; the mass ratio of the sum of the alcoholic amine salt and alcohol to the surfactant is 2~6:1, and the mass ratio of the alcoholic amine salt to alcohol is 1:1~2.
[0022] Furthermore, in step S4, the temperature of the decomposition treatment solution is 60~100℃, preferably 70~80℃.
[0023] Furthermore, in step S4, the immersion time is 10-120 minutes, preferably 30-60 minutes.
[0024] Further, in step S4, the parameters of the ultrasound are: frequency 10~200kHz, preferably 20~40kHz; power 0.1~10W / cm. 2 Preferably, it is 0.5~1W / cm 2 .
[0025] Compared with the prior art, the present invention has the following advantages: The present invention utilizes the synergistic effect of various components in its decomposition solution to efficiently decompose key adhesive materials (encapsulants) in photovoltaic laminates. Alkali acts as the primary force in the hydrolysis reaction, targeting the ester bonds of EVA and EPE encapsulants. Surfactants, alkanolamine salts, and / or alcohol systems assist in accelerating the hydrolysis reaction, significantly improving its effectiveness and efficiency. By disrupting the ester bonds of the encapsulant, the industry challenge of completely separating the encapsulant from glass, solder ribbons, and solar cells is solved. Furthermore, the decomposition primarily affects the encapsulant at the interfaces, allowing the majority of the encapsulant to be retained for recycling. This multi-reaction synergistic mechanism enables the encapsulant to separate from glass, solder ribbons, and solar cells under mild conditions, thereby achieving high-efficiency, high-integrity, and high-purity recovery of core components such as solar cells, glass, solder ribbons, and encapsulants.
[0026] This invention creates uniform microcracks on the glass surface and between different material layers, opening channels for the decomposition solution to directly reach the internal reaction interface. This significantly increases the effective reaction area, allowing the decomposition solution to fully exert its decomposition efficiency. Compared to traditional physical methods or high-temperature pyrolysis processes, this invention represents a significant improvement in the value of recovered products, the green safety of the process, and processing efficiency.
[0027] (3) The present invention introduces ultrasonic treatment to achieve synergistic enhancement of physical stripping and chemical reaction. The cavitation effect generated by ultrasound can form high-pressure shock waves in the liquid. On the one hand, it produces mechanical tearing effect on the chemically weakened EVA bonding interface, accelerating the physical separation of each layer of material; on the other hand, ultrasonic cavitation and the accompanying strong acoustic flow effect can greatly promote the diffusion and renewal of the decomposition treatment solution to the narrow interface under the broken glass, effectively destroying the boundary layer, ensuring that the reactants are fully contacted and the degradation products are removed in time, thereby significantly shortening the overall processing time and improving the separation cleanliness of the battery cell and the glass.
[0028] (4) The amine salt and / or alcohol and surfactant system of the present invention greatly promotes the wetting and penetration depth of the decomposition treatment solution between the material layers of the component. Under mild reaction conditions, the synergistic enhancement of chemical reaction and interfacial penetration is achieved. Attached Figure Description
[0029] Figure 1 This is a flowchart of the photovoltaic module dismantling and recycling method of the present invention; Figure 2 Images of the various structures in the disassembly and recycling process of Example 3: (a) small component unit, (b) mixture of solder ribbon and battery cell, (c) adhesive mixture of film and glass, (d) solder ribbon, (e) battery cell, (f) adhesive film, (g) broken glass; Figure 3 Images of the products obtained from the disassembly and recycling in Example 3: (a) tin-plated copper strip, (b) glass, (c) battery cell, and (d) adhesive film. Figure 4 SEM images of the products obtained from the dismantling and recycling of Example 3: (a) glass, (b) tin-plated copper strip, (c) battery cell; Figure 5 Images of the products obtained from the disassembly and recycling in Example 4: (a) fluorine film, (b) unseparated PET, EVA film and glass, (c) solder ribbon and battery cell; Figure 6 The image shows the product obtained after soaking in Comparative Example 1 for 90 minutes. Figure 7 The image shows the product obtained after soaking in Comparative Example 2 for 600 minutes. Figure 8 The image shows the product obtained after soaking in Comparative Example 3 for 90 minutes. Detailed Implementation
[0030] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments. All other embodiments obtained by those skilled in the art based on the given embodiments without creative effort are within the scope of protection of this application.
[0031] Unless otherwise specified, the reagents, methods, instruments and equipment used in this invention are conventional reagents, methods, instruments and equipment in the art.
[0032] Example 1 A method for dismantling and recycling photovoltaic modules, comprising the following steps: (1) Prepare waste crystalline silicon double-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0033] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0034] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0035] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic processing.
[0036] The decomposition treatment solution is a mixture of alkali, an alcoholic amine salt, a surfactant, and water, at a temperature of 80°C, and an immersion time of 60 minutes. The alkali is sodium hydroxide with a mass concentration of 160 g / L; the alcoholic amine salt is triethanolamine oleate; and the surfactant is an alkyl glycoside. The sum of the mass concentrations of the alcoholic amine salt and the surfactant is 60 g / L, and the mass ratio of triethanolamine oleate to alkyl glycoside is 5:1. After preparing the alkali, triethanolamine oleate and alkyl glycoside are added sequentially to the alkali solution, and then the mixture is heated to 80°C before proceeding with subsequent operations.
[0037] When the decomposition treatment solution is a mixture of alkali, alcoholamine salt, surfactant and water, the sample is completely decomposed after immersion for 60 minutes.
[0038] Example 2 A method for dismantling and recycling photovoltaic modules, comprising the following steps: (1) Prepare waste crystalline silicon double-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0039] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0040] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0041] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic processing.
[0042] The decomposition treatment solution is a mixed solution of alkali, alcohol, surfactant, and water, at a temperature of 80°C, and an immersion time of 60 minutes. The alkali is sodium hydroxide with a mass concentration of 160 g / L; the alcohol is propylene glycol; and the surfactant is an alkyl glycoside, with the sum of the mass concentrations of the alcohol and surfactant being 60 g / L. The mass ratio of propylene glycol to alkyl glycoside is 5:1. After preparing the alkali, propylene glycol and alkyl glycoside are added sequentially to the alkali solution, and then the mixture is heated to 80°C before proceeding with subsequent operations.
[0043] When the decomposition treatment solution is a mixture of alkali, alcohol, surfactant and water, the sample is completely decomposed after immersion for 60 minutes.
[0044] Example 3 A method for dismantling and recycling photovoltaic modules, the photovoltaic modules including glass, solar cells, solder strips (tinned copper strips), EVA film, frames, and junction boxes, the method includes the following steps, such as... Figure 1 As shown: (1) Prepare waste crystalline silicon double-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0045] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0046] (3) Divide the broken surface glass of the module laminate into strips along the edge of the solar cell at 100mm intervals, and then divide the strips into small module units along the edge of the solar cell at 100mm intervals. See Figure 2 (a) The mass of a small component unit sample is 67.4 grams.
[0047] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic treatment. The decomposition solution is a mixture of alkali, an alcoholic amine salt, an alcohol, a surfactant, and water, at a temperature of 80°C for 30 minutes. The alkali is sodium hydroxide with a mass concentration of 160 g / L; the alcohol is propylene glycol; the alcoholic amine salt is triethanolamine oleate; and the surfactant is alkyl glycoside. The sum of the mass concentrations of the alcoholic amine salt, alcohol, and surfactant is 60 g / L, and the mass ratio of triethanolamine oleate, propylene glycol, and alkyl glycoside is 2:3:1. After preparing the alkali solution, triethanolamine oleate, propylene glycol, and alkyl glycoside are added sequentially to the alkali solution, and then the mixture is heated to 80°C before proceeding with subsequent operations.
[0048] After immersion, a mixture of adhesive film and glass binder, and a mixture of battery cells and solder ribbon can be separated, see [link to relevant documentation]. Figure 2 (b) and (c).
[0049] (5) The adhesive film and glass were manually sorted to obtain the adhesive film and glass, and the battery cell and solder ribbon mixture was manually sorted to obtain the battery cell and solder ribbon, see Figure 2 (d)~(g). This embodiment was carried out under laboratory conditions, so manual sorting was used. If it is to be applied to large-scale industrial production, mechanical separation can be used.
[0050] (6) Weighing: 54.8g glass, 7.7g EVA film, 0.8g tin-plated copper strip, 3.1g battery cell, 1.0g mixture of battery cell and glass powder, total weight: 67.4g. Photos of the surfaces of each material after processing are shown below. Figure 3 As shown. SEM tests were performed on the obtained glass, tin-plated copper strip, and solar cell. The results are as follows. Figure 4 As shown in the figure, there is no EVA residue on the surfaces of the glass, tin-plated copper strip, and battery cells, which is beneficial for subsequent recycling of these materials. However, existing physical and pyrometallurgical dismantling processes often leave EVA residue on the surfaces of the glass, tin-plated copper strip, and battery cells.
[0051] Example 4 A method for dismantling and recycling photovoltaic modules, the photovoltaic modules including glass, solar cells, solder strips (tinned copper strips), backsheets, EVA film, frames, and junction boxes, the method includes the following steps: (1) Prepare waste crystalline silicon single-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0052] (2) The photovoltaic module to be processed was mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed was 1m / min, the gap between the upper and lower rollers of the roller press was 4.0mm, and most of the broken glass was 1~10mm in size.
[0053] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0054] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic treatment. The decomposition solution is a mixture of alkali, an alcoholic amine salt, an alcohol, a surfactant, and water, at a temperature of 80°C for 30 minutes. The alkali is sodium hydroxide with a mass concentration of 160 g / L; the alcohol is propylene glycol; the alcoholic amine salt is triethanolamine oleate; and the surfactant is alkyl glycoside. The sum of the mass concentrations of the alcoholic amine salt, alcohol, and surfactant is 60 g / L, and the mass ratio of triethanolamine oleate, propylene glycol, and alkyl glycoside is 2:3:1. After preparing the alkali solution, triethanolamine oleate, propylene glycol, and alkyl glycoside are added sequentially to the alkali solution, and then the mixture is heated to 80°C before proceeding with subsequent operations.
[0055] After immersion, a mixture of polyethylene terephthalate (PET), fluorinated film, EVA film, battery cell, solder ribbon, adhesive film and glass can be separated.
[0056] (5) Separate the adhesive mixture of the film and glass to obtain the film and glass.
[0057] The dismantling and recycling method of this invention is also effective for single-glass photovoltaic modules, capable of separating PET and fluorine film, which is beneficial for the subsequent environmentally friendly treatment of the fluorine film. (See schematic diagram). Figure 5 .
[0058] Comparative Example 1 A method for dismantling and recycling photovoltaic modules is largely the same as that in Example 3, except that ultrasound is not performed in step (4). This dismantling and recycling method includes the following steps: (1) Prepare a 600W crystalline silicon double-glass photovoltaic module, mechanically remove the frame and junction box of the photovoltaic module to obtain the frame, junction box and module laminate to be processed.
[0059] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0060] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0061] (4) Immerse the weighed small component unit sample in the decomposition treatment solution. The decomposition treatment solution is a mixture of alkali, an alcoholic amine salt, an alcohol, a surfactant, and water, at a temperature of 80°C. The alkali is sodium hydroxide with a mass concentration of 160 g / L; the alcohol is propylene glycol; the alcoholic amine salt is triethanolamine oleate; and the surfactant is alkyl glycoside. The sum of the mass concentrations of the alcoholic amine salt, alcohol, and surfactant is 60 g / L, and the mass ratio of triethanolamine oleate, propylene glycol, and alkyl glycoside is 2:3:1. After preparing the alkali solution, add triethanolamine oleate, propylene glycol, and alkyl glycoside sequentially to the alkali solution, then heat to 80°C to begin subsequent operations.
[0062] When the immersion time is 90 minutes, the adhesive mixture of the film and glass, part of the battery cell, and the solder ribbon are separated. Figure 6 As shown, the small component units were not completely decomposed. Further immersion for 150 minutes resulted in complete decomposition of the small component units. This demonstrates the effectiveness of ultrasonic treatment in improving component separation efficiency.
[0063] Comparative Example 2 A method for dismantling and recycling photovoltaic modules is largely the same as that in Example 3, except that no alkali is added to the decomposition solution in step (4). This dismantling and recycling method includes the following steps: (1) Prepare waste crystalline silicon double-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0064] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0065] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0066] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic treatment. The decomposition solution is a mixture of an alkanolamine salt, an alcohol, a surfactant, and water, at a temperature of 80°C. The alcohol is propylene glycol; the alkanolamine salt is triethanolamine oleate; and the surfactant is an alkyl glycoside. The sum of the mass concentrations of the alkanolamine salt, alcohol, and surfactant is 60 g / L, and the mass ratio of triethanolamine oleate, propylene glycol, and alkyl glycoside is 2:3:1. Triethanolamine oleate, propylene glycol, and alkyl glycoside are added sequentially to water, and then the mixture is heated to 80°C to begin subsequent operations.
[0067] The sample did not decompose after immersion for 120 minutes. Immersion was continued for 600 minutes. Figure 7 As shown, the sample has not decomposed, indicating that there is no hydrolytic effect from the alkaline solution, and the film cannot be separated from the glass, solder ribbon, and battery cell.
[0068] Comparative Example 3 A method for dismantling and recycling photovoltaic modules is largely the same as that in Example 3, except that the decomposition solution in step (4) is an aqueous sodium hydroxide solution. This dismantling and recycling method includes the following steps: Figure 1 As shown: (1) Prepare waste crystalline silicon double-glass photovoltaic modules, mechanically remove the frame and junction box of the photovoltaic modules to obtain the frame, junction box and module laminate to be processed.
[0069] (2) The photovoltaic module to be processed is mechanically crushed using a roller press with a concave-convex interface to obtain a module laminate with broken glass on the surface. The forward speed of the photovoltaic module to be processed is 1m / min, the gap between the upper and lower rollers of the roller press is 5.0mm, and most of the broken glass is 1~10mm in size.
[0070] (3) Divide the broken surface glass of the module laminate into small strips along the edge of the cell at a spacing of 100mm, and divide the small strips into small module units along the edge of the cell at a spacing of 100mm.
[0071] (4) Immerse the weighed small component unit sample in the decomposition treatment solution, and simultaneously use 20KHZ, 0.5W / cm 2 Ultrasonic synergistic treatment. The decomposition solution is a 160 g / L sodium hydroxide aqueous solution, at a temperature of 80°C, and an immersion time of 90 min.
[0072] After soaking for 90 minutes, as Figure 8As shown, the sample decomposition reaction was not fully completed within 90 minutes. After immersion for 300 minutes, the sample was completely decomposed. This indicates that although the alkaline solution can play a decomposition role, it is difficult to achieve high-efficiency decomposition and is not the optimal technical solution.
[0073] Although the present invention has been described in detail above with general descriptions, specific embodiments, and experiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.
Claims
1. A method for dismantling and recycling photovoltaic modules, characterized in that, Photovoltaic modules include glass, solar cells, solder ribbons, encapsulant film, frames, and junction boxes. This dismantling and recycling method includes the following steps: S1. Remove the frame and junction box of the photovoltaic module to obtain the frame, junction box and module laminate to be processed; S2. Mechanically break the glass on the surface of the component laminate to be processed to obtain a component laminate with broken surface glass; S3. Divide the component laminate with broken surface glass into several small component units; S4. Immerse the small component unit in the decomposition treatment solution and simultaneously use ultrasound to obtain a mixture of battery cell and solder ribbon, and a bonding mixture of adhesive film and glass. The decomposition treatment solution includes alkali, surfactant, water, and at least one of alcoholic amine salt or alcohol. The mass concentration of the alkali is 40~500g / L. The alkali includes one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, sodium carbonate, sodium bicarbonate, sodium methoxide or sodium ethoxide. S5. The mixture of solar cells and solder ribbon, and the adhesive mixture of film and glass are sorted to obtain solar cells, solder ribbon, adhesive film and glass; In step S2, the glass fragments in the laminated component with broken surface glass have a size of 1~10mm. In step S2, a concave-convex interface roller press is used to mechanically break the glass on the surface of the component laminate to be processed. The forward speed of the component laminate to be processed is 0.1~5m / min, and the gap between the upper and lower rollers of the roller press is 3~5mm. In step S4, the temperature of the decomposition treatment solution is 60~100℃; In step S4, the parameters of the ultrasound are: frequency 10~200kHz, power 0.1~10W / cm. 2 .
2. The method for dismantling and recycling photovoltaic modules according to claim 1, characterized in that, In step S4, the alcohols include one or more of methanol, ethanol, isopropanol, propylene glycol, ethylene glycol, diethylene glycol, or glycerol.
3. The method for dismantling and recycling photovoltaic modules according to claim 1, characterized in that, In step S4, the alkanolamine salt is formed by the reaction of an alkanolamine with an acid; The alkanolamine includes one or more of ethanolamine, diethanolamine, triethanolamine, or isopropanolamine; The acid includes organic acids and inorganic acids, wherein the organic acid includes one or more of short-chain carboxylic acids, aromatic acids, fatty acids or substituted carboxylic acids; The short-chain carboxylic acids include one or more of formic acid, acetic acid, or propionic acid; The aromatic acid includes benzoic acid or salicylic acid; The fatty acids include one or more of benzoic acid, oleic acid, linoleic acid, palmitoleic acid, palmitic acid, lauric acid, stearic acid, butyric acid, or myristic acid; and the inorganic acids include one or more of hydrochloric acid, phosphoric acid, sulfuric acid, or nitric acid. The substituted carboxylic acids include one or more of lactic acid, citric acid, or pyruvic acid.
4. The method for dismantling and recycling photovoltaic modules according to claim 1, characterized in that, The alcoholamine salts include one or more of the following: triethanolamine oleate, triethanolamine stearate, triethanolamine laurate, triethanolamine palmitate, diethanolamine oleate, diethanolamine linoleate, ethanolamine oleate, ethanolamine stearate, isopropanolamine oleate, triethanolamine myristate, ethanolamine hydrochloride, diethanolamine hydrochloride, isopropanolamine hydrochloride, ethanolamine sulfate, diethanolamine nitrate, or triethanolamine phosphate.
5. A method for dismantling and recycling photovoltaic modules according to claim 1, characterized in that, In step S4, the surfactant includes one or more of sodium dodecylbenzenesulfonate, alkyl glycoside, block polyether, fatty alcohol polyoxyethylene ether, or dehydrated sorbitol fatty acid polyoxyethylene ether.
6. A method for dismantling and recycling photovoltaic modules according to claim 1, characterized in that, In step S4, when the decomposition treatment solution is a mixed solution of alkali, surfactant, water, and alcohol amine salt, the sum of the mass concentrations of the alcohol amine salt and the surfactant is 20~240 g / L, and the mass ratio of the alcohol amine salt to the surfactant is 2~6:
1. When the decomposition treatment solution is a mixed solution of alkali, surfactant, water, and alcohol, the sum of the mass concentrations of the alcohol and surfactant is 20~240g / L, and the mass ratio of the alcohol to the surfactant is 2~6:
1. When the decomposition treatment solution is a mixed solution of alkali, surfactant, water, alcoholic amine salt, and alcohol, the sum of the mass concentrations of the alcoholic amine salt, alcohol, and surfactant is 20~240 g / L, the mass ratio of the sum of the alcoholic amine salt and alcohol to the surfactant is 2~6:1, and the mass ratio of the alcoholic amine salt to alcohol is 1:1~2.
Citation Information
Patent Citations
Method for separating back plate of photovoltaic module
CN114038940A
Mixture separation equipment after disassembly of photovoltaic module
CN116274283A
Decommissioned photovoltaic module disassembling and recycling method and production line
CN116550716A
Cascade sorting equipment and method for disassembly fragments of scrapped photovoltaic module
CN117505263A
Method for efficiently separating and recycling waste photovoltaic module by using composite solvent
CN118847685A