A high-efficiency flexible electronic transfer paper and its preparation method
By introducing a directional arrangement of magnetic and photothermal nanoparticles into the transfer paper and combining it with near-infrared laser irradiation, the problems of low transfer efficiency and device damage are solved, achieving a high-efficiency and rapid transfer effect suitable for flexible electronics manufacturing.
Patent Information
- Application Number
- CN202511839334.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-12-08
AI Technical Summary
Existing transfer paper or transfer process suffers from low transfer efficiency, easy damage to micro and nano devices, and difficulty in achieving selective, non-contact local triggering, which limits roll-to-roll continuity and precise alignment of complex patterns.
Magnetic nanoparticles and photothermal nanoparticles are introduced into the polyvinyl alcohol-based functional layer. They are then oriented and arranged in a magnetic framework using an external magnetic field. Combined with near-infrared laser irradiation, rapid local photothermal conversion is achieved, reducing transfer energy consumption and time, and improving transfer efficiency.
It achieves selective high-throughput transfer with low energy consumption and short time, reduces thermal/mechanical damage to micro/nano devices, improves transfer efficiency and product yield, and is suitable for roll-to-roll fabrication.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of papermaking technology, and in particular to a flexible electronic transfer paper with high-efficiency transfer printing and its preparation method. Background Technology
[0002] With the rapid development of flexible electronics, wearable devices, thin-film sensors, and printed electronics, the efficient and precise transfer of microelectronic components and functional patterns from donor substrates to flexible carrier substrates has become a key step in flexible electronics manufacturing. Transfer printing technology, as an important process for connecting chip-level devices to flexible substrates and enabling roll-to-roll production, directly determines the yield and industrialization feasibility of flexible electronic products based on its processing speed, energy consumption, positional accuracy, and damage control.
[0003] Existing transfer paper or transfer process generally suffers from low transfer efficiency: to obtain reliable peeling and bonding, high overall heating temperature, long heating time or high pressure are often required. This not only reduces production throughput, but also easily leads to thermal / mechanical damage to micro and nano devices. At the same time, it is difficult to achieve selective, non-contact local triggering, thus limiting roll-to-roll continuity and precise alignment of complex patterns.
[0004] Therefore, there is an urgent need for a flexible electronic transfer paper and its preparation method that can achieve selective and high-throughput transfer in a short time with low energy consumption. Summary of the Invention
[0005] In view of the above-mentioned shortcomings in the prior art, the purpose of this application is to provide a flexible electronic transfer paper with high-efficiency transfer and its preparation method.
[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows: By introducing and utilizing an external magnetic field to orient magnetic nanoparticles in a polyvinyl alcohol-based functional layer to form a magnetic framework structure, and coordinating dispersed photothermal nanoparticles to achieve rapid local photothermal conversion under near-infrared laser irradiation, the overall heating and time required for transfer are significantly reduced while maintaining the flexibility and reusability of the material, thereby achieving rapid, accurate, and efficient transfer of electronic components, compatible with roll-to-roll preparation, and improving product yield.
[0007] In a first aspect, embodiments of this application provide a flexible electronic transfer paper with high-efficiency transfer capability. The transfer paper includes: a flexible substrate; at least one polyvinyl alcohol-based functional layer disposed on at least a portion of the surface of the flexible substrate; and a release layer disposed on at least the surface of the polyvinyl alcohol-based functional layer on the side opposite to the flexible substrate. The polyvinyl alcohol-based functional layer comprises polyvinyl alcohol and magnetic nanoparticles and photothermal nanoparticles dispersed therein. The magnetic nanoparticles are oriented and arranged in a magnetic framework structure in the dry film of the polyvinyl alcohol-based functional layer by an applied magnetic field.
[0008] In one alternative embodiment, the flexible substrate includes at least one of polyethylene terephthalate film, polyimide film, and polyethylene naphthalate film; the release layer includes a fluorosilane release layer.
[0009] In one alternative embodiment, the magnetic nanoparticles include carboxylated iron oxide, wherein the dry weight of carboxylated iron oxide accounts for 15-25% of the dry weight of polyvinyl alcohol; and the photothermal particles include reduced graphene oxide, wherein the dry weight of reduced graphene oxide accounts for 1-3% of the dry weight of polyvinyl alcohol.
[0010] In one alternative embodiment, the thickness of the flexible substrate is 40-60 μm; the thickness of the polyvinyl alcohol-based functional layer dry film is 4.5-5.5 μm; and the thickness of the release layer dry film is 40-60 nm.
[0011] Secondly, embodiments of this application provide a method for preparing a flexible electronic transfer paper with high-efficiency transfer capability. The preparation method includes the following steps: S100, dissolving polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol aqueous solution, and then cooling the polyvinyl alcohol aqueous solution after heat preservation to obtain a polyvinyl alcohol-based liquid; S200, dispersing a water-based surface-modified magnetic nanoparticle dispersion, a photothermal nanoparticle dispersion, and a dispersant to obtain a nanofunctional slurry; S300, homogenizing the polyvinyl alcohol-based liquid and the nanofunctional slurry, and then adjusting the pH of the mixing system. H to 7.2-7.8, after degassing treatment, a composite slurry is obtained; S400, the composite slurry is coated on a flexible substrate to form a wet film; the wet film is dried in multiple sections, and when the solid content is 60-70%, a magnetic field of not less than 200mT is applied to make the magnetic nanoparticles oriented to form a magnetic skeleton, and then the drying process is continued to obtain an intermediate product with a polyvinyl alcohol functional layer dry film; S500, a fluorosilane release agent is coated on the surface of the intermediate product with a polyvinyl alcohol functional layer dry film, and after drying treatment, a release layer is formed to obtain transfer paper.
[0012] In an optional embodiment, in step S100, the dissolution temperature of polyvinyl alcohol in deionized water is 93-97°C; the mass concentration of the polyvinyl alcohol aqueous solution is 8-12%; the heat preservation and dissolution time is 50-70 min; and the temperature after cooling is 30-50°C.
[0013] In an optional embodiment, in step S200, the dispersant includes at least one of polyvinylpyrrolidone, sodium dodecyl sulfate, and Triton X-100; the dispersion treatment speed is 8000-12000 rpm and the time is 10-20 min.
[0014] In an optional implementation, in step S300, the homogenization temperature is 30-50°C and the rotation speed is 8000-10000 rpm.
[0015] In an optional implementation, prior to step S400, the process further includes: applying a corona treatment to the flexible substrate.
[0016] In an optional implementation, in step S400, the multi-section includes a preheating zone, a critical drying zone, and a curing zone; the temperature of the preheating zone is 48-52°C; the temperature of the critical drying zone is 53-57°C, and a magnetic field of not less than 200mT is applied in this zone for 10-30s; the temperature of the curing zone is 68-72°C.
[0017] The beneficial effects of this application include at least the following: 1. The photothermal particles used in this application serve as a highly efficient local heat source, generating millisecond-level instantaneous high temperatures under near-infrared laser irradiation; the magnetic skeleton serves as a highly efficient heat conduction pathway, rapidly and uniformly diffusing this heat to the entire functional layer interface. The synergistic effect of the two enables the transfer paper to achieve a dramatic change in interface adhesion in a short time with low energy consumption, thereby completing the rapid release and reliable reception of electronic components, improving transfer efficiency, and reducing the risk of damage to thermal components.
[0018] 2. This application fundamentally enhances the mechanical properties of the functional layer by constructing an oriented magnetic skeleton in the PVA matrix. This skeleton structure not only significantly improves the mechanical strength, tear resistance and durability of the dry film, enabling it to withstand the tensile and bending stresses in roll-to-roll production, but also realizes the self-alignment and precise positioning functions in the transfer process through magnetism. Detailed Implementation
[0019] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are only for explaining this application, but the implementation of this application is not limited thereto.
[0020] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art to which this application pertains. Unless otherwise specified, the experimental reagents used in the following embodiments are conventional biochemical reagents; the amounts of experimental reagents used are, unless otherwise specified, the amounts used in conventional experimental operations; and the experimental methods used are, unless otherwise specified, conventional methods.
[0021] In a first aspect, embodiments of this application provide a flexible electronic transfer paper with high-efficiency transfer capability. The transfer paper includes: a flexible substrate; at least one polyvinyl alcohol-based functional layer disposed on at least a portion of the surface of the flexible substrate; and a release layer disposed on at least the surface of the polyvinyl alcohol-based functional layer on the side opposite to the flexible substrate. The polyvinyl alcohol-based functional layer comprises polyvinyl alcohol and magnetic nanoparticles and photothermal nanoparticles dispersed therein. The magnetic nanoparticles are oriented and arranged in a magnetic framework structure in the dry film of the polyvinyl alcohol-based functional layer by an applied magnetic field.
[0022] Preferably, the transfer paper of this application comprises a three-layer composite structure consisting of a flexible substrate, a polyvinyl alcohol (PVA)-based functional layer, and a release layer. The PVA-based functional layer utilizes PVA's excellent film-forming properties, flexibility, and water solubility as a temporary and reliable adhesion substrate, while simultaneously carrying selected magnetic nanoparticles and photothermal nanoparticles. During film formation or curing, the magnetic nanoparticles are oriented and aligned by an external magnetic field, constructing a magnetic framework. This macroscopically endows the functional layer with anisotropic mechanical strength and thermal conductivity pathways, significantly improving the mechanical strength and tear resistance of the dry film and facilitating magnetic alignment and positioning. Photothermal nanoparticles efficiently absorb near-infrared light and instantaneously convert light energy into heat energy, while the magnetic framework provides a directional and rapid conduction pathway for heat, avoiding local overheating and allowing heat energy to spread rapidly and uniformly throughout the functional layer. Under this thermo-magnetic coupling, the functional layer can generate controlled stress concentration or local adhesion energy reduction at the interface under relatively low global temperature and short-term irradiation conditions. This results in a dramatic change in interfacial adhesion force within milliseconds under near-infrared laser irradiation, thereby achieving rapid and reliable adhesion and release switching between the donor substrate and the transfer paper.
[0023] Preferably, carboxylated Fe3O4 is used as the magnetic nanoparticle in the functional layer. The carboxylation treatment endows the Fe3O4 surface with abundant carboxyl groups, which can form stable hydrogen bonds or coordination with the hydroxyl groups on the PVA chain, thereby significantly improving the dispersion of magnetic particles in the PVA matrix and preventing agglomeration, strengthening the particle-matrix interface bonding, and making the magnetic skeleton more firmly oriented under the action of an external magnetic field. Controlling the dry weight of carboxylated Fe3O4 within the range of 15-25% of the dry weight of PVA can reach or approach the particle connectivity threshold in the dry film, thereby constructing a continuous and effective thermal and mechanical load-bearing pathway. Below 15%, it is difficult to form a continuous skeleton, and the thermal and mechanical reinforcement is insufficient, while above 25%, the slurry viscosity will increase significantly, film formation will be difficult, and the film flexibility will be reduced.
[0024] Preferably, reduced graphene oxide (rGO) is used as photothermal nanoparticles. Due to its extremely high absorption coefficient and excellent photothermal conversion efficiency in the near-infrared band, rGO accounts for 1-3% of the dry weight of PVA. This ratio can generate instantaneous high temperatures sufficient to trigger local softening or molecular structure changes in PVA under laser irradiation, while avoiding the impact on the light transmittance, uniformity, or manufacturing cost of the film due to excessive addition. At the same time, it can inhibit rGO self-aggregation and maintain good film-forming properties.
[0025] Furthermore, when magnetic nanoparticles and photothermal nanoparticles work together, carboxylated Fe3O4 constructs a highly efficient thermal conduction pathway, providing a directional and rapid heat conduction pathway and enhancing the magnetic responsiveness and mechanical strength of the functional layer. rGO, acting as a local heat source, rapidly heats up after absorbing near-infrared light and transfers heat to the surrounding PVA and adjacent magnetic framework, generating controllable local high-temperature patches. Under the thermo-magnetic coupling effect, local thermal energy diffuses rapidly and uniformly through the magnetic framework, generating controlled stress concentration or a decrease in adhesion energy at the interface. This allows for rapid and controllable changes in interfacial adhesion energy under relatively low overall temperature and short-term irradiation conditions, thereby facilitating reliable adhesion and release switching between the donor substrate and the transfer paper.
[0026] Preferably, the flexible substrate serves as the support for the entire transfer paper, providing mechanical support and overall flexibility. This allows the transfer paper to adapt to high-speed continuous production processes such as roll-to-roll and is suitable for applications involving curved surfaces or wearable devices. The flexible substrate includes at least one of polyethylene terephthalate (PET), polyimide (PI), and polyethylene naphthalate (PEN) films. These polymer materials possess excellent mechanical properties, good chemical stability, a smooth surface, and moderate thermal stability, enabling them to withstand the thermal stress during the preparation and transfer of the functional layer. Specifically, PET is inexpensive and has good transparency, making it suitable for mass production requiring light transmission or low cost; PI's high-temperature resistance is suitable for higher-temperature processes; and PEN is superior to PET in terms of heat resistance and barrier properties, making it suitable for applications with higher requirements for dimensional stability and gas and humidity barrier properties.
[0027] Preferably, the release layer directly contacts the electronic components to be transferred, undertaking controllable and reversible adhesion and release functions. This application selects fluorosilane materials as the release layer. Fluorosilane molecules contain fluorinated groups with low surface energy, which can form a dense monolayer or ultrathin coating on the surface of the PVA functional layer, significantly reducing surface energy. At room temperature, the van der Waals forces and adhesion provided by the PVA matrix are sufficient to fix the device. However, when near-infrared laser or photothermal stimulation causes a local instantaneous temperature rise in the functional layer, the mobility of the PVA chain segments increases and softens, resulting in a rapid weakening of the interaction force between the PVA chain and the fluorosilane layer and the device. At the same time, the low surface energy, chemical inertness, contamination resistance, and wear resistance of the fluorosilane layer itself are conducive to preferential detachment of the interface at a controlled location without damaging the device. Since the fluorosilane layer can form an ultrathin and chemically stable film through solution self-assembly or low-temperature vapor phase coating, this thin layer will not significantly hinder the near-infrared laser from reaching the underlying photothermal particles, and can provide long-term release performance and reusability durability.
[0028] Furthermore, the thickness of the flexible substrate in this application is 40-60μm. This range takes into account both the processing rigidity and overall flexibility required for roll-to-roll processing. If it is thinner than 40μm, it is prone to wrinkles, dimensional drift or breakage under high-speed winding or tension control. If it is thicker than 60μm, it will significantly increase rigidity and reduce the ability to fit small curved surfaces, which is not conducive to flexible applications. In addition, this thickness achieves a good balance between mechanical strength, heat capacity and cost, and is suitable for most flexible electronics production lines. The polyvinyl alcohol-based functional layer dry film has a thickness of 4.5-5.5 μm. This thickness is sufficient to accommodate 15-25% carboxylated Fe3O4 magnetic particles and form a magnetic framework within the dry film, thus ensuring mechanical reinforcement and directional thermal conduction pathways. Simultaneously, it is thin enough to maintain a low heat capacity, enabling rapid local heating and rapid thermal conduction during photothermal excitation, ensuring millisecond-level response and good microscale adhesion. If the thickness is less than 4.5 μm, it may lead to particle exposure or surface roughness and uneven release. If the thickness is greater than 5.5 μm, it increases the heating energy requirement and prolongs the response time. The release layer dry film has a thickness of 40-60 nm. This thickness significantly reduces the interfacial surface energy for reliable room-temperature gripping, while remaining thin enough not to become a significant thermal barrier, ensuring effective penetration of near-infrared light and triggering localized high-temperature release of the underlying photothermal particles. A thickness below 40 nm may result in uneven coverage, while a thickness above 60 nm will waste material, increase internal stress, and potentially reduce thermal conduction and alignment accuracy.
[0029] Secondly, embodiments of this application provide a method for preparing a flexible electronic transfer paper with high-efficiency transfer capability, the method comprising the following steps: S100. Dissolve polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol aqueous solution. After dissolving the polyvinyl alcohol aqueous solution at a constant temperature, cool it to obtain a polyvinyl alcohol-based liquid. S200. The water-based surface-modified magnetic nanoparticle dispersion, the photothermal nanoparticle dispersion and the dispersant are dispersed to obtain a nanofunctional slurry. S300: Polyvinyl alcohol base liquid and nano-functional slurry are homogenized, and then the pH of the mixture is adjusted to 7.2-7.8. After degassing, composite slurry is obtained. S400. The composite slurry is coated onto a flexible substrate to form a wet film. The wet film is dried in multiple sections. When the solid content is 60-70%, a magnetic field of not less than 200mT is applied to make the magnetic nanoparticles oriented to form a magnetic skeleton. Then the drying process is continued to obtain an intermediate product with a polyvinyl alcohol functional layer. S500: A fluorosilane release agent is coated onto the surface of an intermediate product with a polyvinyl alcohol functional layer dry film, and after drying, a release layer is formed to obtain transfer paper.
[0030] Preferably, in step S100, dissolving PVA in deionized water at 93-97℃ and maintaining the temperature for 50-70 minutes allows the PVA molecular chains to fully expand and the intermolecular hydrogen bonds to be effectively opened, thereby increasing the dissolution rate and avoiding undissolved particles, ensuring the uniformity of the base solution. The solution concentration is controlled at 8-12%. Below 8%, the dry film thickness is difficult to maintain and drying shrinkage stress increases, potentially leading to discontinuous film formation or peeling. Above 12%, the solution viscosity is too high, which is detrimental to homogeneous mixing, degassing, and continuous coating. After dissolution and temperature maintenance, the solution is cooled to 30-50℃ to avoid excessive water evaporation, dispersant failure, or nanoparticle agglomeration caused by high temperatures. In summary, step S100, through the synergistic effect of high-temperature dissolution, appropriate concentration control, and controlled cooling, provides a stable and controllable base solution system for the uniform dispersion of nanoparticles, the quality of functional layer film formation, and the control of dry film thickness, significantly improving the uniformity and repeatability of the final transfer paper.
[0031] Preferably, in step S200, water-based surface-modified magnetic nanoparticles and photothermal nanoparticles are mixed with a suitable dispersant and subjected to high-shear dispersion at 8000-12000 rpm for 10-20 min to prepare a highly dispersed and stable nanofunctional slurry. The magnetic particles are carboxylated and otherwise surface-modified in the aqueous phase to enhance their affinity with the PVA matrix and inhibit agglomeration; simultaneously, dispersants such as polyvinylpyrrolidone (PVP), sodium dodecyl sulfate (SDS), and Triton X-100 are introduced to achieve stable coating of the particles. High-speed shear treatment utilizes intense shear and turbulence to break up soft agglomerates, fully exposing monodisperse particles and coating them with the dispersant, thereby obtaining a slurry with small particle size, narrow distribution, and stable suspension. Using an aqueous system ensures good compatibility between the nanoslurry and the PVA-based liquid, avoiding immediate flocculation caused by solvent mismatch, and facilitating the subsequent formation of a continuous or nearly connected magnetic framework under an applied magnetic field, achieving efficient directional heat conduction.
[0032] Preferably, in step S300, the nanofunctional slurry and PVA base liquid are homogenized at 30-50℃ and 8000-10000rpm. The combination of a mild thermal environment and strong mechanical shear force fully disperses the nanoparticles and coats them with PVA molecular chains, forming isolated and uniformly distributed microscale particle clusters. This lays the foundation for the subsequent formation of a magnetic framework and photothermal layer under an external magnetic field. Subsequently, the pH of the mixture is adjusted to a weakly alkaline state of 7.2-7.8 so that the carboxyl groups on the surface of carboxylated Fe3O4 and other particles are ionized into negatively charged carboxylate groups. This enhances the electrostatic repulsion between particles, improves the storage and handling stability of the composite slurry, and inhibits sedimentation or flocculation, while taking into account the chemical stability of PVA and the effective working range of the dispersant. Finally, a degassing treatment is performed to remove the entrained free air bubbles and prevent pinholes, bulges, or uneven thickness during coating and drying.
[0033] Preferably, in step S400, by coating the composite slurry into a wet film on a flexible substrate, and combining multi-segment gradient drying with a controlled magnetic field, in-situ oriented assembly of magnetic nanoparticles and immobilization of the magnetic framework are achieved. The wet film is first gently heated in a preheating zone to remove low-boiling solvents and avoid surface skinning. When the solid content of the wet film rises to 60-70% and enters the critical drying zone, the PVA matrix exhibits a viscoelastic solid-like state, and the Brownian motion of the particles is restricted but not yet completely fixed. This is the key window for the migration and oriented alignment of magnetic particles. During this window period, a strong magnetic field of not less than 200 mT is applied and maintained for about 10-30 s, which magnetizes the magnetic nanoparticles and drives them to rapidly flip, aggregate, and arrange into chain or network structures along the magnetic field direction under the drive of the magnetic torque. The chain structures are interconnected to form a three-dimensional interconnected magnetic framework. Subsequently, the film enters the curing zone to quickly remove residual moisture and fix the formed magnetic framework in the matrix, resulting in a dry film with a complete structure, uniform particle distribution, and well-defined functions.
[0034] Furthermore, pre-treatment with corona on the flexible substrate can significantly improve the polarity and surface energy of the substrate surface. By oxidizing the substrate surface and introducing oxygen-containing functional groups, the wettability and initial adhesion of the PVA-based paste are improved, thereby achieving better spreadability and adhesion during the coating stage and reducing the risk of delamination, edge curling, or pattern misalignment. In addition, surface activation is beneficial for interfacial bonding control during release layer deposition and improves the smoothness and uniformity during the transition from wet film to dry film, thereby improving the dimensional stability and product yield of the transfer paper.
[0035] Preferably, in step S500, a fluorosilane release agent is coated onto the surface of the intermediate product with the PVA dry film and dried to form a release layer. The fluorosilane release agent forms a low surface energy coating on the film surface and self-assembles on the substrate by solvent evaporation or low-temperature curing to form a continuous 40-60 nm release layer. This release layer effectively reduces the interfacial adhesion between the donor substrate and the transfer paper during the transfer process, allowing for controlled peeling of the interface under photothermal triggering or magneto-thermal coupling rather than device damage. In addition, the chemical stability and abrasion resistance of fluorosilane are beneficial for multiple transfers or repeated use.
[0036] In summary, each step from S100 to S500 controls the chemical composition, dispersion state, interfacial energy, and microstructure of the material in situ, so that the final transfer paper has both a rapid, localized photothermal response under near-infrared laser and a magnetic field-induced directional thermal and mechanical channel. At the same time, corona pretreatment and multi-zone drying treatment ensure the flatness of the film and the interfacial bonding.
[0037] This application has undergone multiple experiments, and some of the test results are presented here for reference to further describe the invention in detail. The following is a detailed description in conjunction with specific embodiments.
[0038] Example 1 This embodiment provides a high-efficiency flexible electronic transfer paper and its preparation method, including the following steps: S100. In a jacketed reactor with a stirrer, PVA is dissolved in deionized water at 95°C to prepare a 10wt% polyvinyl alcohol aqueous solution. The solution is kept at this temperature for 60 minutes and then cooled to 40°C to obtain a polyvinyl alcohol-based solution. S200, In a high-speed dispersion vessel, carboxylated iron oxide (20% of PVA dry weight), reduced graphene oxide (2% of PVA dry weight) and polyvinylpyrrolidone are added in proportion, and homogenized at 10,000 rpm for 15 min to obtain nano-functional slurry. S300: PVA base liquid and nano-functional slurry are mixed at 40℃ and homogenized at 9000rpm. Then, the pH is adjusted to 7.5 and degassing is performed to obtain composite slurry. S400, the polyethylene terephthalate film is corona treated, and the composite slurry is coated onto the corona-treated polyethylene terephthalate film by a doctor blade to form a wet film; the wet film is dried in multiple sections, passing through a preheating zone of 50°C, and when the solid content of the wet film rises to 65% and enters the critical drying zone of 55°C, a magnetic field of not less than 200mT is applied and held for 20s to cause the magnetic nanoparticles to align and form a magnetic framework, and then it enters the curing zone of 70°C to obtain an intermediate product with a polyvinyl alcohol functional layer dry film; S500: A fluorosilane release agent is coated onto the surface of an intermediate product with a polyvinyl alcohol functional layer dry film, and after drying, a release layer is formed to obtain transfer paper.
[0039] Example 2 This embodiment provides a high-efficiency flexible electronic transfer paper and its preparation method, including the following steps: S100. In a jacketed reactor with a stirrer, PVA is dissolved in deionized water at 93°C to prepare an 8wt% polyvinyl alcohol aqueous solution. The solution is kept at this temperature for 50 minutes and then cooled to 30°C to obtain a polyvinyl alcohol-based solution. S200, in a high-speed dispersion vessel, add carboxylated iron oxide (15% of PVA dry weight), reduced graphene oxide (1% of PVA dry weight) and sodium dodecyl sulfate in the specified ratio, and homogenize at 8000 rpm for 20 min to obtain nano-functional slurry. S300: PVA base liquid and nano-functional slurry are mixed at 30℃ and homogenized at 8000rpm. Then, the pH is adjusted to 7.2 and degassing is performed to obtain composite slurry. S400. The polyimide film is corona treated. The composite slurry is coated onto the corona-treated polyimide film by a doctor blade to form a wet film. The wet film is dried in multiple sections. After passing through the preheating zone at 48°C, when the solid content of the wet film rises to 53% and enters the critical drying zone at 55°C, a magnetic field of not less than 200mT is applied and held for 10s to make the magnetic nanoparticles oriented to form a magnetic skeleton. Then it enters the curing zone at 68°C to obtain an intermediate product with a dry film containing a polyvinyl alcohol functional layer. S500: A fluorosilane release agent is coated onto the surface of an intermediate product with a polyvinyl alcohol functional layer dry film, and after drying, a release layer is formed to obtain transfer paper.
[0040] Example 3 This embodiment provides a high-efficiency flexible electronic transfer paper and its preparation method, including the following steps: S100. In a jacketed reactor with a stirrer, PVA is dissolved in deionized water at 97°C to prepare a 12wt% polyvinyl alcohol aqueous solution. The solution is kept at this temperature for 70 minutes and then cooled to 50°C to obtain a polyvinyl alcohol-based solution. S200, in a high-speed dispersion vessel, add carboxylated iron oxide (25% of PVA dry weight), reduced graphene oxide (3% of PVA dry weight) and Triton X-100 in the specified ratio, and homogenize at 12000 rpm for 10 min to obtain nano-functional slurry. S300: PVA base liquid and nano-functional slurry are mixed at 50℃ and homogenized at 10000rpm. Then, the pH is adjusted to 7.8 and degassing is performed to obtain composite slurry. S400. A corona treatment is performed on a polyethylene naphthalate film. A composite slurry is applied to the corona-treated polyethylene naphthalate film using a doctor blade to form a wet film. The wet film is then subjected to multi-segment drying. After passing through a preheating zone at 52°C, when the solid content of the wet film rises to 65% and enters the critical drying zone at 57°C, a magnetic field of not less than 200mT is applied and maintained for 30s to orient the magnetic nanoparticles to form a magnetic framework. Subsequently, the film enters a curing zone at 72°C to obtain an intermediate product with a polyvinyl alcohol functional layer. S500: A fluorosilane release agent is coated onto the surface of an intermediate product with a polyvinyl alcohol functional layer dry film, and after drying, a release layer is formed to obtain transfer paper.
[0041] Example 4 This embodiment provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that in step S400, the polyethylene terephthalate film is not corona treated, that is, the composite slurry is coated on the polyimide film by a doctor blade to form a wet film.
[0042] Comparative Example 1 This comparative example provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that in step S200, carboxylated iron oxide dispersion is not added, and only reduced graphene oxide and polyvinylpyrrolidone are retained.
[0043] Comparative Example 2 This comparative example provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that in step S200, the reduced graphene oxide dispersion is not added, and only carboxylated iron tetroxide and polyvinylpyrrolidone are retained.
[0044] Comparative Example 3 This comparative example provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that: in step S400, during the multi-segment drying process, no magnetic field is applied in the critical drying zone.
[0045] Comparative Example 4 This comparative example provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that in step S400, during the multi-segment drying process, a magnetic field with an intensity of less than 50mT is applied in the critical drying zone.
[0046] Comparative Example 5 This comparative example provides a flexible electronic transfer paper with high-efficiency transfer and its preparation method. The specific steps are as shown in Example 1, except that in step S200, a dispersion of ordinary iron oxide nanoparticles without carboxylation surface modification is used.
[0047] Test data The paper samples from Examples 1-4 and Comparative Examples 1-5 were measured as follows, and the results are shown in Tables 1 and 2.
[0048] The thickness measurement methods for each layer are shown in Table 1. (1) Thickness of flexible substrate: According to the national standard GB / T 6672-2001 "Mechanical measurement method for determination of thickness of plastic film and sheet".
[0049] (2) Thickness of the polyvinyl alcohol-based functional layer dry film: The thickness of the functional layer is obtained by measuring the difference between the total thickness of the substrate and the functional layer and the thickness of the substrate. The thickness of the blank flexible substrate is accurately measured and recorded as D1. On the same roll, the thickness of the intermediate product with PVA functional layer dry film obtained after completing step S400 is accurately measured and recorded as D2. The thickness of the PVA functional layer dry film = D2 - D1.
[0050] (3) Release layer dry film thickness: The thickness was measured using an ellipsometry in the wavelength range of 400-800nm and calculated by software modeling.
[0051] Table 1 Grasping rigidity modulus: Using a micro mechanical testing instrument, after applying a 150mT magnetic field to the back of the transfer paper to activate the magnetic skeleton, the maximum bending stress when lifting the micro LED chip is measured, and its equivalent rigidity modulus (MPa) is calculated.
[0052] Transfer success rate: The percentage of successful transfers (%) was calculated by repeating the pick-up and release transfer operation of the micro-device 100 times on a 1cm×1cm donor substrate.
[0053] Release energy threshold: Using an 808nm near-infrared laser, the minimum energy density required for reliable release of the device was determined by gradually increasing the irradiation energy.
[0054] Coating adhesion: According to the national standard GB / T 9286-1998, the cross-cut test was conducted to evaluate the bonding strength between the PVA functional layer and the flexible substrate (0-5 level, with 0 being the best, indicating no peeling).
[0055] Table 2 As shown in Table 1, Comparative Example 1 lacks magnetic nanoparticles, resulting in a reduction in film-forming material and a thinner functional layer. Comparative Examples 4 and 5 have insufficient magnetic field strength or particle agglomeration, which disrupts the uniformity and density of the film formation, requiring a thicker wet film to form a continuous dry film, resulting in a thicker functional layer.
[0056] Table 2 shows that Comparative Example 1 exhibits extremely low gripping rigidity modulus and a transfer success rate of less than 50%, demonstrating that magnetic nanoparticles and a magnetic framework are the core components for achieving high-rigidity gripping. Comparative Example 2's release energy threshold far exceeds the normal range, failing to achieve efficient release, proving that photothermal nanoparticles are a necessary condition for near-infrared triggered selective release. Comparative Examples 3 and 4 show significantly lower gripping rigidity than Example 1, demonstrating that magnetic field orientation greater than 200 mT is a key process for forming an effective magnetic framework. Comparative Example 5 suffers from particle agglomeration, resulting in decreased magnetic framework order and gripping rigidity, proving that carboxylation surface modification is crucial for ensuring nanoparticle dispersion and the final framework. Example 4 shows decreased coating adhesion, leading to localized coating peeling during gripping and a significantly reduced transfer success rate, demonstrating the importance of substrate pretreatment for ensuring product reliability.
[0057] In summary, this invention produces a flexible electronic transfer paper with strong gripping rigidity, high transfer success rate, and rapid and precise release, whose overall performance is far superior to that of the comparative examples.
[0058] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application, and should all be included within the protection scope of this application.
Claims
1. A flexible electronic transfer paper with high-efficiency transfer capability, characterized in that, The transfer paper includes: Flexible substrate; At least one polyvinyl alcohol (PVA) functional layer is disposed on at least a portion of the surface of the flexible substrate; and A release layer is disposed on at least one surface of the polyvinyl alcohol-based functional layer on the side opposite to the flexible substrate; The polyvinyl alcohol-based functional layer comprises polyvinyl alcohol and magnetic nanoparticles and photothermal nanoparticles dispersed therein; the magnetic nanoparticles are oriented and arranged in the dry film of the polyvinyl alcohol-based functional layer by an external magnetic field to form a magnetic framework structure. The magnetic nanoparticles include carboxylated iron oxide, wherein the dry weight of the carboxylated iron oxide accounts for 15-25% of the dry weight of polyvinyl alcohol. The photothermal nanoparticles include reduced graphene oxide, wherein the dry weight of the reduced graphene oxide accounts for 1-3% of the dry weight of polyvinyl alcohol; The dry film thickness of the polyvinyl alcohol-based functional layer is 4.5-5.5 μm.
2. The transfer paper according to claim 1, characterized in that, The flexible substrate includes at least one of polyethylene terephthalate film, polyimide film, and polyethylene naphthalate film; The release layer includes a fluorosilane release layer.
3. The transfer paper according to claim 1, characterized in that, The thickness of the flexible substrate is 40-60 μm; The thickness of the release layer dry film is 40-60 nm.
4. A method for preparing a flexible electronic transfer paper with high-efficiency transfer capability, characterized in that, The preparation method is used to prepare the transfer paper according to any one of claims 1-3, and the preparation method includes the following steps: S100. Polyvinyl alcohol is dissolved in deionized water to obtain a polyvinyl alcohol aqueous solution. The polyvinyl alcohol aqueous solution is dissolved under heat and then cooled to obtain a polyvinyl alcohol base liquid. S200. The water-based surface-modified magnetic nanoparticle dispersion, the photothermal nanoparticle dispersion and the dispersant are dispersed to obtain a nanofunctional slurry. S300. The polyvinyl alcohol-based liquid and the nano-functional slurry are homogenized, and then the pH of the mixture is adjusted to 7.2-7.
8. After degassing, a composite slurry is obtained. S400. The composite slurry is coated onto a flexible substrate to form a wet film. The wet film is dried in multiple sections. When the solid content is 60-70%, a magnetic field of not less than 200mT is applied to make the magnetic nanoparticles oriented to form a magnetic skeleton. Then, the drying process is continued to obtain an intermediate product with a polyvinyl alcohol functional layer. S500: A fluorosilane release agent is coated onto the surface of the intermediate product with a polyvinyl alcohol functional layer dry film, and after drying, the release layer is formed to obtain the transfer paper.
5. The preparation method according to claim 4, characterized in that, In step S100, The polyvinyl alcohol dissolves in deionized water at a temperature of 93-97°C. The mass concentration of the polyvinyl alcohol aqueous solution is 8-12%; The heat preservation and dissolution time is 50-70 minutes; The temperature after cooling is 30-50℃.
6. The preparation method according to claim 4, characterized in that, In step S200, The dispersant includes at least one of polyvinylpyrrolidone, sodium dodecyl sulfate, and Triton X-100; The dispersion process is carried out at a speed of 8000-12000 rpm for 10-20 min.
7. The preparation method according to claim 4, characterized in that, In step S300, The homogenization process is carried out at a temperature of 30-50℃ and a rotation speed of 8000-10000 rpm.
8. The preparation method according to claim 4, characterized in that, Before step S400, the method further includes: performing a corona treatment on the flexible substrate.
9. The preparation method according to claim 4, characterized in that, In step S400, the multi-section includes a preheating zone, a critical drying zone, and a curing zone; The temperature in the preheating zone is 48-52℃; The temperature of the critical drying zone is 53-57℃, and a magnetic field of not less than 200mT is applied in this zone for 10-30s; the temperature of the curing zone is 68-72℃.
Citation Information
Patent Citations
Application of diamagnetic ink in glass
CN106634166A
Light-to-heat conversion layer, method for producing same, and donor sheet using said light-to-heat conversion layer
CN110741287A