A composite electrode, its preparation method and application
By employing a dual-layer structure with different porosities and compaction densities in the lithium-ion battery electrode, combined with ionic conductive polymers and interfacial coupling agents, the transmission bottleneck and weak interlayer bonding force of lithium-ion batteries during high-rate charging are solved, thereby improving the battery's fast-charging performance and cycle life.
Patent Information
- Application Number
- CN202511581248.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-10-31
AI Technical Summary
When lithium-ion battery electrodes are charged at high rates, the electron and ion transport paths compete with each other, leading to lithium metal deposition, which poses safety hazards and accelerates capacity decay. Furthermore, the existing double-layer coating technology has weak interlayer bonding and unclear functional gradient, making it impossible to effectively optimize the transport bottleneck.
By employing bottom and top layer structures with different porosities and compaction densities, combined with ionic conductive polymers and interfacial coupling agents, a clear functional gradient is formed to optimize ion and electron transport.
It significantly improves the battery's fast charging performance and cycle life, solves the problems of weak interlayer bonding and unclear functional gradient, and achieves synergistic optimization of ion and electron transport.
Smart Images

Figure CN121506860B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of secondary battery technology, and particularly relates to a composite electrode, its preparation method, and its application. Background Technology
[0002] With the rapid development of electric vehicles and portable electronic devices, the market has placed higher demands on the fast-charging capabilities of lithium-ion batteries. Currently, mainstream battery manufacturers generally use single-layer coating technology to prepare electrodes, where active materials, conductive agents, and binders are uniformly mixed. In this homogeneous structure, during high-rate charging, the transport paths of electrons and ions couple and compete, easily leading to severe polarization on the electrode side near the current collector. This results in lithium metal deposition, posing safety hazards and accelerating capacity decay.
[0003] To improve transport dynamics, existing technologies have proposed the concept of double-layer or even multi-layer coatings. However, current explorations of double-layer coating technologies still face two major challenges. First, there is the ambiguity in functional design. For example, in the scheme disclosed in Chinese patent application CN119175195A, although double-layer coating is used, the formulations of the upper and lower slurries are similar, with little difference in composition and physicochemical properties, failing to form a clear functional gradient. This structural similarity prevents it from fundamentally solving the bottleneck problem of ion / electron transport in thick electrodes, resulting in limited performance improvement. Second, there is the reliability challenge in the fabrication process. Double-layer coating involves coating two slurries with different formulations sequentially or simultaneously. Due to differences in the solvent system, solid content, and binder type used in each slurry layer, the solvent chemical potentials between the two layers may be mismatched. During the subsequent drying process, the solvent migrates from regions of high chemical potential to regions of low chemical potential. This interfacial migration disrupts the distribution of the binder, severely affecting the microstructure and bonding strength of the interlayer interface. As demonstrated in the literature (J. Power Sources, 2021, 489, 229500), weakened interlayer bonding can easily induce cracks or even interlayer delamination at the interface during drying or cycling. This not only fails to leverage the advantages of the gradient structure but also introduces new contact resistance, deteriorating the rate performance and cycle stability of the battery.
[0004] Therefore, developing a composite electrode preparation method with strong interlayer bonding, distinct functional gradients, and synergistic optimization of ion and electron transport is a technical challenge that urgently needs to be solved in this field. Summary of the Invention
[0005] One of the objectives of this invention is to provide a composite electrode, its preparation method, and its application, in order to solve the problems that weakened interlayer bonding easily induces cracks or even peeling at the interface, unclear functional gradient, and obstructed ion and electron transport.
[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a composite electrode comprising: current collector; The bottom layer is disposed on at least one surface of the current collector; the bottom layer includes a first active material, an ionic conductive polymer, a first conductive agent, and a first binder; A surface layer is disposed on the surface of the underlying layer; the surface layer includes a second active material, a second conductive agent, a second binder, and an interfacial coupling agent; The porosity φ1 of the bottom layer and the porosity φ2 of the surface layer satisfy the relationship: φ1>φ2; the compaction density ρ1 of the bottom layer and the compaction density ρ2 of the surface layer satisfy the relationship: ρ1<ρ2.
[0007] Preferably, the porosity φ1 of the bottom layer is 45% to 55%, and the porosity φ2 of the surface layer is 28% to 35%.
[0008] Preferably, the compaction density ρ1 of the bottom layer is 0.7–0.9 g / cm³. 3 The compaction density ρ2 of the surface layer is 1.5–1.7 g / cm³. 3 .
[0009] Preferably, the surface of the bottom layer is pre-cured to form an interface layer for bonding with the surface layer.
[0010] Preferably, in the bottom layer, the mass content of the first active substance is 90% to 96%, the mass content of the ionic conductive polymer is 2.5% to 5%, the mass content of the first conductive agent is 0.5% to 2%, and the mass content of the first binder is 1% to 3%.
[0011] Preferably, in the surface layer, the mass content of the second active substance is 88% to 94%, the mass content of the second conductive agent is 0.5% to 2%, the mass content of the second binder is 1% to 3%, and the mass content of the interfacial coupling agent is 0.3% to 1%.
[0012] Preferably, both the first active material and the second active material are selected from at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium olivine-structured lithium phosphate, graphite, silicon carbide, and lithium titanate.
[0013] Preferably, the ionic conductive polymer is an ionic conductive polymer formed by a polymer and a fixed anion: the polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride and its copolymers, polymethyl methacrylate, polyvinylidene chloride, and poly(β-amino ester); the fixed anion is selected from at least one of hexafluorophosphate ions and bis(trifluoromethanesulfonyl)imide ions.
[0014] Preferably, the second conductive agent comprises a one-dimensional conductive agent and a two-dimensional conductive agent, wherein the mass ratio of the one-dimensional conductive agent to the two-dimensional conductive agent is 1:1 to 1:3; the one-dimensional conductive agent is selected from at least one of carbon nanotubes and carbon nanofibers; and the two-dimensional conductive agent is graphene.
[0015] Preferably, the interface coupling agent is an inorganic substance modified and coated with an organic substance; the organic substance is selected from at least one of polydopamine, polymethyl methacrylate, and poly(β-amino ester); the inorganic substance is selected from at least one of nano-silica and nano-alumina.
[0016] Secondly, the present invention provides a method for preparing a composite electrode, comprising the following steps: (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, the first binder and the solvent are mixed and dispersed at high speed to obtain a bottom layer slurry with a solid content of 40% to 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, the interfacial coupling agent and the solvent, and disperse at high speed to obtain a surface slurry with a solid content of 48% to 55%. (2) Coating and Pre-curing: The bottom slurry is uniformly coated onto the current collector to form a wet film; the wet film is pre-cured using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: The surface slurry is then applied onto the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film is sent into a multi-temperature zone drying oven for gradient drying; after drying, the electrode is rolled to obtain the composite electrode.
[0017] Preferably, in step (2), the temperature for pre-curing the wet film is 80℃~95℃ and the time is 3~10 seconds.
[0018] Preferably, in step (4), the multi-temperature zone drying oven includes a first temperature zone, a second temperature zone, and a third temperature zone arranged sequentially; the temperature of the first temperature zone is 65℃~75℃ and the humidity is 30%~40%RH; the temperature of the second temperature zone is 95℃~105℃ and the humidity is <15%RH; the temperature of the third temperature zone is 110℃~120℃ and the humidity is <10%RH.
[0019] Thirdly, the present invention provides a lithium-ion battery comprising the aforementioned composite electrode, or comprising a composite electrode prepared by the aforementioned preparation method.
[0020] Compared with the prior art, the present invention has at least the following beneficial effects: This invention creates a distinct functionally graded structure by constructing a bottom layer and a top layer with different porosities and compaction densities on a current collector. The high porosity and low compaction density of the bottom layer provide ample space and channels for the rapid migration of lithium ions; while the low porosity and high compaction density of the top layer ensure the compact packing of active materials, increasing the energy density per unit volume and optimizing the electron transport network. This graded structure resolves the contradiction between ion and electron transport in traditional single-structure electrodes, achieving decoupling and synergistic optimization of the two transport mechanisms.
[0021] This invention introduces an ionic conductive polymer into the bottom layer, which has abundant ion-conducting groups and can form a continuous ion transport network. This design works synergistically with the high porosity structure of the bottom layer to significantly reduce the migration resistance of lithium ions inside the electrode and reduce the concentration polarization effect.
[0022] This invention optimizes the distribution of the second conductive agent in the surface layer to form a highly efficient three-dimensional electron transport network; combined with the high compaction density characteristics of the surface layer, it effectively reduces the contact impedance of electron transport and accelerates the transport speed of electrons from the active material to the current collector.
[0023] This invention adds an interfacial coupling agent to the surface layer, which can form physical anchoring and chemical hydrogen bonding with the components in the underlying layer, significantly enhancing the bonding strength between the two layers. This design fundamentally solves the problem in the prior art that double-layer electrodes are prone to interfacial cracks or even peeling during drying and use.
[0024] In summary, this invention, through innovative dual-layer gradient structure design, introduction of ionic conductive polymers, optimization of surface three-dimensional conductive network, and application of interface coupling technology, successfully solves key technical problems in traditional electrodes such as obstructed ion and electron transport, weak interlayer bonding, and unclear functional gradients, significantly improving the fast-charging performance and cycle life of the battery. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a cross-sectional view of a composite electrode structure according to an embodiment of the present invention.
[0027] In the diagram: 1. Current collector; 2. Bottom layer; 3. Surface layer; 4. Interface layer. Detailed Implementation
[0028] To make the technical problem to be solved, the technical solution, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.
[0029] In this invention, the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.
[0030] In this invention, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0031] It should be understood that in various embodiments of the present invention, the order of the above-mentioned processes does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.
[0032] According to a first aspect of the invention, see Figure 1 The present invention provides a composite electrode comprising: current collector 1; The bottom layer 2 is disposed on at least one surface of the current collector 1; the bottom layer 2 includes a first active material, an ionic conductive polymer, a first conductive agent and a first adhesive; Surface layer 3 is disposed on the surface of bottom layer 2; surface layer 3 includes a second active material, a second conductive agent, a second binder, and an interface coupling agent; Among them, the porosity φ1 of the bottom layer 2 and the porosity φ2 of the surface layer 3 satisfy the relationship: φ1>φ2; the compaction density ρ1 of the bottom layer 2 and the compaction density ρ2 of the surface layer 3 satisfy the relationship: ρ1<ρ2.
[0033] The bottom layer 2 has a higher porosity, meaning more pore space and wider ion channels. This is equivalent to creating a high-speed road for lithium ions to enter the electrode from the separator, greatly reducing the resistance to ion transport and allowing lithium ions to quickly and uniformly penetrate deep into the electrode. The top layer 3 has a lower porosity (i.e., a denser structure), meaning that the active material and conductive agent are packed more tightly. Although this slightly increases the resistance to ion transport, it greatly enhances the electronic conductivity network.
[0034] Applying a smaller rolling pressure to the bottom layer 2 maintains a lower compaction density (i.e., higher porosity), effectively fixing ion channels during the manufacturing process and ensuring they remain high-speed ion transport pathways in the final product. Applying a larger rolling pressure to the top layer 3, achieving a higher compaction density, allows for closer contact between the conductive agent and active material particles, significantly strengthening the electronic conductivity network and reducing contact resistance. By controlling the compaction density, a gradient transition in mechanical properties is created. A higher compaction density top layer 3 results in greater rigidity and a higher modulus. A lower compaction density bottom layer 2 results in greater flexibility and better toughness. This gradual mechanical structure, from current collector 1 (rigid) → top layer 3 (rigid) → bottom layer 2 (flexible), more smoothly absorbs and disperses stress generated during cycling, reducing stress concentration and thus enhancing the interlayer bonding and overall electrode structural stability, preventing cracking or delamination.
[0035] In some embodiments of the present invention, the porosity φ1 of the bottom layer 2 is 45% to 55%, and the porosity φ2 of the surface layer 3 is 28% to 35%. For example, the porosity φ1 of the bottom layer 2 can be 45%, 50%, 55%, etc., and the porosity φ2 of the surface layer 3 can be 28%, 30%, 33%, 35%, etc.
[0036] In this process, the porosity φ1 of the bottom layer 2 is controlled within the range of 45% to 55%. This range is based on the results of extensive experimental optimization: when the porosity φ1 < 45%, the electrolyte wetting is insufficient, electron conduction is limited, and rate performance is poor; when the porosity φ1 is 45% to 55%, it is conducive to electrolyte wetting and ion transport; when the porosity φ1 > 55%, electrolyte wetting is difficult, and ion transport is hindered. Similarly, the porosity φ2 of the surface layer 3 is controlled within the range of 28% to 35% in the coating roll pressing process. This range is also based on the results of extensive experimental optimization. Experiments show that controlling the porosity of both the bottom layer 2 and the surface layer 3 within this range in the coating roll pressing process results in both good mechanical strength and excellent electrochemical performance.
[0037] In some embodiments of the present invention, the compaction density ρ1 of the bottom layer 2 is 0.7–0.9 g / cm³. 3 The compaction density ρ2 of surface layer 3 is 1.5–1.7 g / cm³. 3 For example, the compaction density ρ1 of the bottom layer 2 can be 0.7 g / cm³. 3 0.8g / cm 3 0.9g / cm 3 Wait, the compaction density ρ2 of surface layer 3 can be 1.5 g / cm³. 3 1.6g / cm 3 1.7g / cm 3 etc.
[0038] In this process, the compaction density of the bottom layer 2 is controlled to be between 0.7 and 0.9 g / cm³. 3 Within this range, which is based on the results of extensive experimental optimization: density <0.7 g / cm³ 3 At this time, insufficient contact between electrode materials restricts electron conduction, resulting in poor rate performance; density 0.7–0.90 g / cm³ 3 This design ensures sufficient contact between materials, improving electron conduction, while also maintaining appropriate porosity, which is beneficial for electrolyte wetting and ion transport; density > 0.9 g / cm³ 3 When the electrode becomes excessively dense, its porosity decreases, making electrolyte wetting difficult and hindering ion transport. Similarly, it can be concluded that the compaction density of surface layer 3 should be controlled between 1.5 and 1.7 g / cm³ during the coating roll pressing process. 3 Within this range, which is based on the results of extensive experimental optimization, experiments show that controlling the compaction density of the bottom layer 2 and the top layer 3 within this range during the coating roll pressing process achieves both good mechanical strength and excellent electrochemical performance.
[0039] In some embodiments of the present invention, the surface of the bottom layer 2 is pre-cured to form an interface layer 4 for bonding with the top layer 3. By pre-curing the bottom layer 2 and bonding it with the interface coupling agent of the top layer 3, a strong physical anchoring and chemical hydrogen bonding are formed at the interface between the two layers, effectively preventing interlayer delamination.
[0040] In some embodiments of the present invention, the mass content of the first active substance in the bottom layer 2 is 90% to 96%, the mass content of the ionic conductive polymer is 2.5% to 5%, the mass content of the first conductive agent is 0.5% to 2%, and the mass content of the first binder is 1% to 3%. For example, the mass content of the first active substance can be 90%, 92%, 94%, 96%, etc., the mass content of the ionic conductive polymer can be 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., the mass content of the first conductive agent can be 0.5%, 1%, 1.5%, 2%, etc., and the mass content of the first binder can be 1%, 2%, 3%, etc.
[0041] Experiments show that when the mass content of the first active material in the bottom layer 2 is 90%–96%, the mass content of the ionic conductive polymer is 2.5%–5%, the mass content of the first conductive agent is 0.5%–2%, and the mass content of the first binder is 1%–3%, a high-quality bottom layer slurry can be obtained, thereby producing a composite electrode with excellent electrochemical performance.
[0042] In some embodiments of the present invention, the mass content of the second active material in the surface layer 3 is 88% to 94%, the mass content of the second conductive agent is 0.5% to 2%, the mass content of the second binder is 1% to 3%, and the mass content of the interfacial coupling agent is 0.3% to 1%. For example, the mass content of the second active material can be 88%, 90%, 92%, 94%, etc., the mass content of the second conductive agent can be 0.5%, 1%, 1.5%, 2%, etc., the mass content of the second binder can be 1%, 2%, 3%, etc., and the mass content of the interfacial coupling agent can be 0.3%, 0.5%, 0.7%, 1%, etc.
[0043] Experiments show that when the mass content of the second active material in the surface layer 3 is 88%–94%, the mass content of the second conductive agent is 0.5%–2%, the mass content of the second binder is 1%–3%, and the mass content of the interfacial coupling agent is 0.3%–1%, a high-quality surface layer 3 slurry can be obtained, thereby producing a composite electrode with excellent electrochemical performance.
[0044] In some embodiments of the present invention, the first active material and the second active material are both selected from at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium olivine-structured lithium phosphate, graphite, silicon carbide and lithium titanate.
[0045] In the bottom layer 2, the first active material is in close contact with ions and electrolyte, ensuring that lithium ions can quickly reach its surface and react; in the top layer 3, the second active material is tightly surrounded by a conductive agent, ensuring that the electrons generated by the reaction can be quickly conducted away.
[0046] In some embodiments of the present invention, the ionic conductive polymer is an ionic conductive polymer formed by a polymer and a fixed anion: the polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride and its copolymers, polymethyl methacrylate, polyvinylidene chloride, and poly(β-amino ester); the fixed anion is selected from at least one of hexafluorophosphate ions and bis(trifluoromethanesulfonyl)imide ions.
[0047] Among them, the ionic conductive polymer provides intrinsic ionic conductivity to compensate for insufficient electrolyte. During fast charging, the migration rate of lithium ions in the electrolyte reaches its limit, especially in the deep pores of the electrode, where the lithium ion concentration in the electrolyte drops sharply, leading to ion depletion and severe polarization. However, the polymer itself contains mobile lithium ions and molecular chain segments that promote ion migration, providing a solid-state ion transport channel even in the absence of a liquid electrolyte or when the electrolyte distribution is uneven.
[0048] Ionic conductive polymers can also optimize the active material interface and reduce interfacial impedance. The entry of lithium ions from the electrolyte / polymer into the active material particles is the rate-limiting step of the entire reaction. This interface has a high impedance, but it can be well coated on the surface of the active material to form an excellent ion-conducting interfacial layer. This greatly improves the transport kinetics of lithium ions at the solid-liquid (or solid-solid) interface, reduces charge transfer impedance, and thus improves rate performance.
[0049] In some embodiments of the present invention, the second conductive agent includes a one-dimensional conductive agent and a two-dimensional conductive agent, wherein the mass ratio of the one-dimensional conductive agent to the two-dimensional conductive agent is 1:1 to 1:3; the one-dimensional conductive agent is selected from at least one of carbon nanotubes and carbon nanofibers; and the two-dimensional conductive agent is graphene. For example, the mass ratio of the one-dimensional conductive agent to the two-dimensional conductive agent can be 1:1, 1:2, 1:3, etc.
[0050] Two-dimensional conductive agents provide a basic and broad contact and conductivity background; one-dimensional conductive agents are interspersed among them, connecting isolated particles that are not closely connected, and constructing a more robust and efficient three-dimensional conductive network; this combined composite conductive network can maximize the overall performance of the electrode.
[0051] Experiments show that when the mass ratio of one-dimensional conductive agent to two-dimensional conductive agent is 1:1 to 1:3, an electrode with excellent electrochemical performance can be obtained.
[0052] In some embodiments of the present invention, the interface coupling agent is an inorganic substance modified and coated with an organic substance; the organic substance is selected from at least one of polydopamine, polymethyl methacrylate, and poly(β-amino ester); the inorganic substance is selected from at least one of nano-silica and nano-alumina.
[0053] Interfacial coupling agents typically contain special functional groups (such as hydroxyl, carboxyl, and amino groups). These functional groups can form strong hydrogen bonds or chemical bonds with functional groups on the surface of active materials; entangle or crosslink with the molecular chains of binders; and undergo physical adsorption or π-π conjugation with the surface of conductive agents. Interfacial coupling agents can form a thin layer with a certain degree of toughness, capable of absorbing and dispersing the internal stress generated during battery cycling due to the difference in the expansion / contraction coefficients of the two layers, preventing stress concentration that could lead to interfacial cracking or delamination.
[0054] According to a second aspect of the present invention, a method for preparing a composite electrode includes the following steps: (1) Slurry preparation: Preparation of the second bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, the first binder and the solvent are mixed and dispersed at high speed to obtain the second bottom layer slurry with a solid content of 40% to 50%. Preparation of surface layer 3 slurry: Mix the second active material, the second conductive agent, the second binder, the interfacial coupling agent and the solvent, and disperse at high speed to obtain surface layer 3 slurry with a solid content of 48% to 55%; (2) Coating and Pre-curing: The bottom layer slurry 2 is uniformly coated onto the current collector 1 to form a wet film; the wet film is pre-cured using an infrared radiation device to form a semi-cured layer on its surface; (3) Overlay coating: The surface layer slurry 3 is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film is sent into a multi-temperature zone drying oven for gradient drying; after drying, the electrode is rolled to obtain the composite electrode.
[0055] In some embodiments of the present invention, in step (2), the temperature for pre-curing the wet film is 80°C to 95°C, and the time is 3 to 10 seconds. For example, the pre-curing temperature can be 80°C, 85°C, 90°C, 95°C, etc., and the time can be 3, 5, 7, 10 seconds, etc.
[0056] The curing temperature is controlled within the range of 80–95℃ based on the following considerations: When the temperature is below 80℃, the solvent evaporates slowly, and a hard shell slowly forms on the surface, preventing the internal solvent from diffusing smoothly to the outside; when the temperature is between 80 and 95℃, the solvent is completely removed, while allowing the binder molecular chains sufficient time to move and rearrange, forming a strong bond with the active materials on both sides at the interface; when the temperature is above 95℃, the solvent evaporates too quickly, the viscosity of the slurry increases sharply, and the migration of the internal solvent to the outside will drive shrinkage.
[0057] The curing time of 3 to 10 seconds is determined based on kinetic studies: when the time is less than 3 seconds, it hardens rapidly, and the vapor generated by the vaporization of the internal solvent may break through the surface layer 3, forming large and isolated pores or cracks; when the time is 3 to 10 seconds, it is conducive to the formation of a uniform, interconnected, and appropriately sized pore network; when the time is greater than 10 seconds, extending the time is uneconomical and may increase the risk of side reactions.
[0058] Experiments show that high-quality electrodes with excellent electrochemical performance can be obtained when the curing temperature is 80℃~95℃ and the curing time is 3~10 seconds.
[0059] In some embodiments of the present invention, in step (4), the multi-temperature zone drying oven includes a first temperature zone, a second temperature zone, and a third temperature zone arranged sequentially; the temperature of the first temperature zone is 65℃~75℃, and the humidity is 30%~40%RH; the temperature of the second temperature zone is 95℃~105℃, and the humidity is <15%RH; the temperature of the third temperature zone is 110℃~120℃, and the humidity is <10%RH. For example, the temperature of the first temperature zone can be 65℃, 70℃, 75℃, etc., and the humidity can be 30%RH, 35%RH, 40%RH, etc.; the temperature of the second temperature zone can be 95℃, 100℃, 105℃, etc., and the humidity can be 10%RH, 5%RH, etc.; the temperature of the third temperature zone can be 110℃, 115℃, 120℃, etc., and the humidity can be 5%RH, 2%RH, etc.
[0060] The purpose of the multi-temperature zone drying oven is to optimize the solvent evaporation process and prevent electrode cracking or bubble formation. Experiments show that electrodes prepared using multi-temperature zone drying and controlled humidity exhibit the best quality, with smooth and uniform surfaces, no cracks or bubbles, low solvent residue, and excellent electrochemical performance. In contrast, electrodes prepared by single-temperature drying without humidity control are prone to surface cracking or internal bubbles, affecting electrode quality and electrochemical performance.
[0061] According to a third aspect of the present invention, the present invention provides a lithium-ion battery comprising a composite electrode or a composite electrode prepared by a preparation method.
[0062] The preparation method of lithium-ion batteries includes the following steps: (1) The bare cell is obtained by stacking or winding the positive electrode, separator and negative electrode in sequence; (2) Place the bare cell obtained in step (1) into the outer packaging shell, dry, inject liquid, vacuum seal, stand, form, and capacity test.
[0063] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0064] Example 1: Preparation of composite electrode (1) Slurry preparation: Preparation of the bottom layer slurry: Mix artificial graphite, PEO-PAN / LiTFSI, conductive carbon black and PAA in a mass ratio of 96:2.5:0.5:1, then add deionized water and disperse at high speed to obtain a bottom layer slurry with a solid content of 50%. Preparation of surface slurry: The silicon-carbon anode, composite conductive agent (such as SWCNT+graphene), composite binder PAA+CMC (accounting for 20%), and interfacial coupling agent PDA@Al2O3 are mixed in a mass ratio of 94:0.5:1:0.3, and then added to deionized water for high-speed dispersion to obtain a surface slurry with a solid content of 55%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 10 seconds at 80°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 65℃ with a humidity of 30%RH; the second temperature zone was 95℃ with a humidity of 10%RH; and the third temperature zone was 110℃ with a humidity of 5%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 45% and the porosity φ2 of the surface layer to be 28%. The compaction density ρ1 of the bottom layer was controlled to be 0.9 g / cm³. 3 The surface compaction density ρ2 is 1.7 g / cm³. 3 Thus, a composite electrode is obtained.
[0065] Example 2: Preparation of composite electrode (1) Slurry preparation: Preparation of the bottom layer slurry: Mix the first active substance, ionic conductive polymer, first conductive agent and first binder in a mass ratio of 90:5:2:3, then add solvent and disperse at high speed to obtain a bottom layer slurry with a solid content of 40%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, and the interfacial coupling agent in a mass ratio of 88:2:3:1, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 48%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 3 seconds at 95°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 75℃ with a humidity of 40%RH; the second temperature zone was 105℃ with a humidity of 5%RH; and the third temperature zone was 120℃ with a humidity of 2%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 55% and the porosity φ2 of the surface layer to be 35%; the compaction density ρ1 of the bottom layer was controlled to be 0.7 g / cm³. 3 The surface compaction density ρ2 is 1.5 g / cm³. 3 Thus, a composite electrode is obtained.
[0066] Example 3: Preparation of composite electrode (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, and the first binder are mixed in a mass ratio of 92:4.5:1.5:2, and then a solvent is added for high-speed dispersion to obtain a bottom layer slurry with a solid content of 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, and the interfacial coupling agent in a mass ratio of 92:1:2:0.5, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 55%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 7 seconds at 85°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 70℃ with a humidity of 35%RH; the second temperature zone was 100℃ with a humidity of 5%RH; and the third temperature zone was 115℃ with a humidity of 2%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 50% and the porosity φ2 of the surface layer to be 30%. The compaction density ρ1 of the bottom layer was controlled to be 0.8 g / cm³. 3 The surface compaction density ρ2 is 1.6 g / cm³. 3 Thus, a composite electrode is obtained.
[0067] Example 4: Preparation of composite electrode (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, and the first binder are mixed in a mass ratio of 94:3.5:1:2, and then a solvent is added for high-speed dispersion to obtain a bottom layer slurry with a solid content of 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, and the interfacial coupling agent at a mass ratio of 90:1.5:2:0.7, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 55%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 5 seconds at 90°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 70℃ with a humidity of 35%RH; the second temperature zone was 100℃ with a humidity of 5%RH; and the third temperature zone was 115℃ with a humidity of 2%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 50% and the porosity φ2 of the surface layer to be 33%. The compaction density ρ1 of the bottom layer was controlled to be 0.8 g / cm³. 3 The surface compaction density ρ2 is 1.6 g / cm³. 3 Thus, a composite electrode is obtained.
[0068] Comparative Example 1: Preparation of Composite Electrode (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, and the first binder are mixed in a mass ratio of 96:2.5:0.5:1, and then a solvent is added for high-speed dispersion to obtain a bottom layer slurry with a solid content of 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, and the interfacial coupling agent in a mass ratio of 94:0.5:1:0.3, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 55%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 10 seconds at 80°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 65℃ with a humidity of 30%RH; the second temperature zone was 95℃ with a humidity of 10%RH; and the third temperature zone was 110℃ with a humidity of 5%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 40% and the porosity φ2 of the surface layer to be 25%. The compaction density ρ1 of the bottom layer was controlled to be 1 g / cm³. 3 The surface compaction density ρ2 is 1.8 g / cm³. 3 Thus, a composite electrode is obtained.
[0069] Comparative Example 2: Preparation of Composite Electrode (1) Slurry preparation: Preparation of the bottom layer slurry: Mix the first active substance, ionic conductive polymer, first conductive agent and first binder in a mass ratio of 90:5:2:3, then add solvent and disperse at high speed to obtain a bottom layer slurry with a solid content of 40%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, and the interfacial coupling agent in a mass ratio of 88:2:3:1, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 48%. (2) Coating and Pre-curing: The bottom slurry is evenly coated onto the current collector to form a wet film; the wet film is pre-cured for 3 seconds at 95°C using an infrared radiation device to form a semi-cured layer on its surface. (3) Overlay coating: A surface coating slurry is then applied over the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 75℃ with a humidity of 40%RH; the second temperature zone was 105℃ with a humidity of 5%RH; and the third temperature zone was 120℃ with a humidity of 2%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 60% and the porosity φ2 of the surface layer to be 40%; the compaction density ρ1 of the bottom layer was controlled to be 0.6 g / cm³. 3 The surface compaction density ρ2 is 1.4 g / cm³. 3 Thus, a composite electrode is obtained.
[0070] Comparative Example 3: Preparation of Composite Electrode (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, and the first binder are mixed in a mass ratio of 96:2.5:0.5:1, and then a solvent is added for high-speed dispersion to obtain a bottom layer slurry with a solid content of 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, and the second binder at a mass ratio of 94:0.5:1, then add solvent and disperse at high speed to obtain a surface slurry with a solid content of 55%. (2) Coating: The bottom layer slurry is evenly coated onto the current collector to form a wet film, and then the top layer slurry is continuously applied. (4) Gradient drying and rolling: The electrode coated with a double-layer wet film was placed in a multi-temperature zone drying oven for gradient drying. The first temperature zone was 65℃ with a humidity of 30%RH; the second temperature zone was 95℃ with a humidity of 10%RH; and the third temperature zone was 110℃ with a humidity of 5%RH. After drying, the electrode was rolled to control the porosity φ1 of the bottom layer to be 45% and the porosity φ2 of the surface layer to be 28%. The compaction density ρ1 of the bottom layer was controlled to be 0.9 g / cm³. 3 The surface compaction density ρ2 is 1.7 g / cm³. 3 Thus, a composite electrode is obtained.
[0071] Comparative Example 4: Preparation of Composite Electrode No ionic conductive polymer was added to the preparation of the bottom slurry; the rest of the preparation method was the same as in Example 1.
[0072] Comparative Example 5: Preparation of Composite Electrode In the preparation of the surface slurry, the second conductive agent was replaced with conductive carbon, and the rest of the preparation method was the same as in Example 1.
[0073] Comparative Example 6: Fabrication of a monolayer electrode (1) Slurry preparation: The first active substance, ionic conductive polymer, first conductive agent and first binder are mixed in a mass ratio of 96:2.5:0.5:1, and then a solvent is added for high-speed dispersion to obtain a slurry with a solid content of 50%.
[0074] (2) Coating: The slurry is evenly coated onto the current collector to form a wet film; (3) Gradient drying and rolling: The electrode coated with a wet film is sent into a drying oven for drying; after drying, the electrode is rolled to obtain a single-layer electrode.
[0075] Comparative Example 7: Fabrication of a monolayer electrode (1) Slurry preparation: The second active material, the second conductive agent, the second binder and the interface coupling agent are mixed in a mass ratio of 94:0.5:1:0.3, and then a solvent is added for high-speed dispersion to obtain a slurry with a solid content of 55%.
[0076] (2) Coating: The slurry is evenly coated onto the current collector to form a wet film; (3) Gradient drying and rolling: The electrode coated with a wet film is sent into a drying oven for drying; after drying, the electrode is rolled to obtain a single-layer electrode.
[0077] Performance testing of electrodes and their batteries Test method for interlayer peel strength: The testing method is the symmetrical pasting method, and the specific operating steps are as follows: 1. Sampling and Pretreatment: Cut a sample strip with a width of 25 mm and a length of approximately 100 mm from the double-coated electrode. Gently clean the surface of the sample strip (upper coating) with isopropyl alcohol to ensure it is free of dust and oil.
[0078] 2. Creating the initial peeling opening: Using a sharp scalpel blade and a steel ruler, gently draw a line along the width direction with the tip of the blade. Then, carefully and slowly use the tip of the blade to lift the upper coating into a "tongue" of about 5-10mm. This "tongue" is the starting point for subsequent clamping.
[0079] 3. Adhesion and Fixing: Place a rigid substrate horizontally and apply a sufficient amount of high-strength adhesive. Extend the end of the sample with the initial peel line beyond the substrate. Then, smoothly adhere the sample with the lower coating side to the adhesive-coated substrate, ensuring the adhesive only adheres to the back of the current collector corresponding to the lower coating and the exposed current collector; absolutely no adhesive should penetrate into the "upper-lower coating" interface to be tested. Using a standard roller, roll back and forth on the adhesive three times at approximately 10 mm / s to ensure curing. During rolling, rely solely on the roller's own weight; do not apply additional pressure. This step aims to eliminate air bubbles and ensure maximum contact area and adhesion between the adhesive and the coating. Wait for complete curing according to the adhesive instructions.
[0080] 4. Prepare the mating sample: Apply glue to another rigid substrate. Flip up the raised "top coating tongue" from the sample prepared in step 3 and smoothly attach it to this second substrate. Press it with a standard roller to ensure curing. This results in a "sandwich" structure: [Rigid Plate 1] - [Glue] - [Lower Coating + Current Collector] - [Top Coating] - [Glue] - [Rigid Plate 2]. The interface to be tested—the bonding surface between the upper and lower coatings—is located precisely between the two rigid plates.
[0081] 5. Testing: Turn on the material testing machine and computer software, and preheat for at least 15 minutes. Select the "Peel" or "T-Peel" test mode. Set the test parameters: Peel speed: 300 mm / min (this is a common industrial standard and can be adjusted according to internal specifications). Test length: at least 80 mm (effective peel segment). Sampling frequency: ≥50 Hz. Clamp the rigid plates 1 and 2 of the sample into the upper and lower clamps of the testing machine, respectively. Ensure the clamps are aligned so that the tensile force direction is 180° to the peel surface and the peel angle remains at 180° throughout the test. Click Start. The testing machine will automatically separate the two clamps to peel the coating interface, and the equipment will record the force-displacement curve in real time. From the curve, discard the initial peak (the unstable area at the start of peeling) and the end segment, and select the force value of the middle stable segment to calculate the average value (F). Peel strength σ (N / cm) = average peel force F (N) / sample width.
[0082] Test method for resistance DCR: 1. Battery State Adjustment: Allow the battery to rest at the test temperature (e.g., 25°C) for at least 24 hours to allow its internal temperature to fully equalize. Perform 1 to 3 standard charge-discharge cycles as specified by the manufacturer (e.g., constant current charging at 1C to the upper limit voltage, constant voltage charging to the cutoff current, and then constant current discharging at 1C to the lower limit voltage) to activate battery performance and ensure data stability. Adjust the battery to the specified state of charge (SOC, such as 50% SOC, at which battery characteristics are more stable and typical).
[0083] 2. Specific steps: Let it stand for 10 seconds, and record the stable voltage value V0 at the last moment; then immediately apply a constant current discharge pulse I1 (e.g., 2C) for t1 seconds (e.g., 10 seconds); record the voltage value V1 at the end of the pulse; let it stand. DCIR = |ΔV| / |ΔI|.
[0084] Test method for 5C charging capacity retention rate: 1. Battery Activation and Baseline Capacity Confirmation: Allow the battery to rest at 25°C until temperature equalization. Charge at a constant current of 0.5C to the upper limit voltage, then switch to constant voltage charging to the cutoff current (0.05C) for 1-3 standard cycles (0.5C charge / discharge is recommended) to activate the battery. Obtain the baseline capacity (C). 0.5C Let it stand for 30 minutes; then discharge at a constant current of 0.5C until the cutoff voltage. The capacity obtained from this discharge step is C. 0.5C Record this capacity; it will be used as the denominator in calculating the capacity retention rate. Let it stand again for 30 minutes.
[0085] 2.5C Charging and Capacity Confirmation: Charge the battery at 25°C with a 5C constant current to the upper limit voltage, then switch to constant voltage charging to the cutoff current (0.05C), and obtain the 5C charging capacity. 5C capacity retention rate = 5C constant current charging capacity / 0.5C constant current charging capacity.
[0086] 3C 10-minute charging SOC test method: Allow the battery to rest at 25°C until temperature equalization. Charge at a constant current of 0.5C to the upper limit voltage, then switch to constant voltage charging to the cutoff current (0.05C) for 1-3 standard cycles (0.5C charge / discharge is recommended) to activate it. Obtain the reference capacity (C). 0.5C Let stand for 30 minutes; then charge at a 3C 0.5C current for 10 minutes.
[0087] Test method for cell expansion rate after 500 cycles: 1. Initial State Recording: Allow the battery cell to stand in a standard environment (e.g., 25°C) for a sufficient time to allow its temperature to equalize. Following standard procedures, fully charge the battery cell according to standard procedures. Select at least five fixed measurement points at the center and around the perimeter of the battery cell's main body area, and mark them with a marker that will not easily come off. Use a micrometer to measure three times at each point, and take the average value as the initial thickness T at that point. 0x The average thickness at five points is calculated as the initial average thickness (T) of the battery cell. o And take initial photos of the battery cells' appearance.
[0088] 2. Record Status After 500 Cycles: Start the cyclic test step, beginning 500 cycles. It is recommended to perform a standard capacity check every 100 cycles. Pause the cyclic step after reaching the specified cycle number. Perform a standard charge-discharge test (e.g., 0.5C charge-discharge) identical to the one used to obtain the initial capacity, and record the current capacity C. n (n=100,200,...). After fully charging according to the standard procedure, cool the cell to ambient temperature, measure and record the thickness T at the marked points. nx Calculate the average thickness at 5 points as the initial average thickness (T) of the battery cell, and take a final appearance photo of the cell, comparing it with the initial photo. Overall expansion rate (%) = [(T)] 500 -T o ) / T o ]×100% The above-described embodiments and comparative examples underwent the aforementioned performance tests, and the results are shown in Table 1.
[0089] From the test results of the above embodiments and comparative examples, we can conclude that: The test results of Examples 1-4 and Comparative Examples 1-2 show that when the porosity and compaction density of the bottom layer and the surface layer satisfy the relationship and are within a certain range, the interlayer peel strength of the composite electrode is improved, the resistance DCR is reduced, the SOC of 3C 10min charging can reach 85%, and the cell expansion rate is significantly reduced after 500 cycles, indicating that the composite electrode has excellent comprehensive performance.
[0090] The test results of Example 1 and Comparative Example 3 show that the interlayer peel strength of the composite electrode after bottom layer pre-curing and the addition of interfacial coupling agent is increased from 24 N / m to 73 N / m, which effectively prevents the electrode from delamination during drying and use.
[0091] The test results of Example 1 and Comparative Example 4 show that the composite electrode with added ion-conductive polymer has significantly improved interlayer peel strength, increased the 5C charging capacity retention rate from 60% to 89.7%, reduced resistance DCR, achieved a 3C 10min charging SOC of 76%, and significantly reduced cell expansion rate after 500 cycles. This indicates that the composite electrode with added ion-conductive polymer has excellent fast charging performance.
[0092] The test results of Example 1 and Comparative Example 5 show that the composite electrode with optimized second conductive agent in the surface layer has improved interlayer peel strength, increased 5C charging capacity retention to 89.7%, reduced resistance DCR, achieved 76% SOC at 3C 10min charging, and significantly reduced cell expansion rate after 500 cycles. This indicates that the choice of conductive agent significantly affects the overall performance of the composite electrode.
[0093] The test results of Example 1 and Comparative Examples 6-7 show that the composite electrode containing both bottom and top layers has significantly improved interlayer peel strength, significantly improved 5C charging capacity retention, reduced resistance DCR, increased 3C 10min charging SOC to 76%, and significantly reduced cell expansion rate after 500 cycles. This indicates that the overall performance of the single-layer electrode failed to achieve the effect of the composite electrode.
[0094] In summary, compared with existing electrodes, the composite electrode of the present invention exhibits the following significant advantages: 1. Clear functional gradient: The introduction of high porosity and ion-conducting polymers in the bottom layer creates a high-speed channel for ion transport; the low porosity and three-dimensional carbon network in the surface layer form a "highway" for electron transport, realizing the decoupling and synergistic optimization of ion and electron transport paths.
[0095] 2. Strong interfacial bonding: Through the pre-curing of the bottom layer and the interfacial coupling agent, a strong physical anchoring and chemical hydrogen bond are formed at the interface between the two layers. The interlayer peel strength is increased from <15N / m in the traditional method to >35N / m, which effectively prevents delamination during drying and use.
[0096] 3. Excellent fast charging performance: The electrode prepared by this invention significantly reduces polarization during high-rate charging and discharging, increasing the capacity retention rate of the battery at 3C rate from 72.3% of the traditional electrode to over 89.7%, and achieving a SOC of over 76% in 10 minutes of fast charging.
[0097] 4. Strong process feasibility: The materials required for this method are all commercially available or readily available, and the core processes (pre-curing and gradient drying) can be modularly upgraded based on existing coating equipment, making it easy to carry out large-scale production.
[0098] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A composite electrode, characterized in that, include: current collector; The bottom layer is disposed on at least one surface of the current collector; the bottom layer includes a first active material, an ionic conductive polymer, a first conductive agent, and a first binder; A surface layer is disposed on the surface of the underlying layer; the surface layer includes a second active material, a second conductive agent, a second binder, and an interfacial coupling agent; The porosity φ1 of the bottom layer and the porosity φ2 of the surface layer satisfy the relationship: φ1>φ2; the compaction density ρ1 of the bottom layer and the compaction density ρ2 of the surface layer satisfy the relationship: ρ1<ρ2. The interface coupling agent is an inorganic substance modified and coated with an organic substance; the organic substance is selected from at least one of polydopamine, polymethyl methacrylate, and poly(β-amino ester); the inorganic substance is selected from at least one of nano-silica and nano-alumina.
2. The composite electrode as described in claim 1, characterized in that, The porosity φ1 of the bottom layer is 45%–55%, and the porosity φ2 of the surface layer is 28%–35%; and / or, The compacted density ρ1 of the bottom layer is 0.7–0.9 g / cm³. 3 The compaction density ρ2 of the surface layer is 1.5–1.7 g / cm³. 3 .
3. The composite electrode as described in claim 1, characterized in that, The surface of the bottom layer is pre-cured to form an interface layer for bonding with the surface layer.
4. The composite electrode as described in claim 1, characterized in that, In the underlying layer, the mass content of the first active substance is 90%–96%, the mass content of the ionic conductive polymer is 2.5%–5%, the mass content of the first conductive agent is 0.5%–2%, and the mass content of the first binder is 1%–3%; and / or, In the surface layer, the mass content of the second active substance is 88% to 94%, the mass content of the second conductive agent is 0.5% to 2%, the mass content of the second binder is 1% to 3%, and the mass content of the interfacial coupling agent is 0.3% to 1%.
5. The composite electrode as described in claim 1, characterized in that, The ionic conductive polymer is an ionic conductive polymer formed by a polymer and fixed anions: The polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride and its copolymers, polymethyl methacrylate, polyvinylidene chloride, and poly(β-amino ester); The fixed anion is selected from at least one of hexafluorophosphate ion and bis(trifluoromethanesulfonyl)imide ion.
6. The composite electrode as described in claim 1, characterized in that, The second conductive agent includes a one-dimensional conductive agent and a two-dimensional conductive agent, wherein the mass ratio of the one-dimensional conductive agent to the two-dimensional conductive agent is 1:1 to 1:3; The one-dimensional conductive agent is selected from at least one of carbon nanotubes and carbon nanofibers; The two-dimensional conductive agent is graphene.
7. A method for preparing a composite electrode as described in any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Slurry preparation: Preparation of the bottom layer slurry: The first active substance, the ionic conductive polymer, the first conductive agent, the first binder and the solvent are mixed and dispersed at high speed to obtain a bottom layer slurry with a solid content of 40% to 50%. Preparation of surface slurry: Mix the second active material, the second conductive agent, the second binder, the interfacial coupling agent and the solvent, and disperse at high speed to obtain a surface slurry with a solid content of 48% to 55%. (2) Coating and Pre-curing: The underlying slurry is uniformly coated onto the current collector to form a wet film; The wet film is pre-cured using an infrared radiation device to form a semi-cured layer on its surface; (3) Overlay coating: The surface slurry is then applied onto the semi-cured layer. (4) Gradient drying and rolling: The electrode coated with a double wet film was placed in a multi-temperature zone drying oven for gradient drying. After drying, the electrode is rolled to obtain the composite electrode.
8. The method for preparing the composite electrode as described in claim 7, characterized in that, In step (2), the temperature for pre-curing the wet film is 80℃~95℃, and the time is 3~10 seconds; and / or, In step (4), the multi-temperature zone drying oven includes a first temperature zone, a second temperature zone, and a third temperature zone arranged sequentially; the temperature of the first temperature zone is 65℃~75℃ and the humidity is 30%~40%RH; the temperature of the second temperature zone is 95℃~105℃ and the humidity is <15%RH; the temperature of the third temperature zone is 110℃~120℃ and the humidity is <10%RH.
9. A lithium-ion battery, characterized in that, The composite electrode includes any one of claims 1 to 6, or the composite electrode prepared by the preparation method according to any one of claims 7 to 8.
Citation Information
Patent Citations
Double-layer turn-back type coating machine and coating system
CN119175195A
Composite negative plate, preparation method thereof and lithium ion battery
CN117810358A
High-magnification composite electrode for semi-solid battery and preparation method of high-magnification composite electrode
CN118572024A