A reinforced modified polypropylene cable conduit and its preparation method
By grafting aminosilanes and α,β-unsaturated amide compounds onto the surface of glass fiber, combined with nylon resin and specific molding modifiers, the problems of insufficient ring stiffness and oil resistance of polypropylene cable conduits were solved, achieving higher ring stiffness and better molding quality.
Patent Information
- Application Number
- CN202511846282.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-12-09
AI Technical Summary
Existing polypropylene cable conduits have shortcomings in terms of ring stiffness and oil resistance. In particular, the axial orientation of the glass fibers leads to insufficient circumferential compressive strength, making it difficult to meet the application requirements for high ring stiffness.
By grafting aminosilane compounds and α,β-unsaturated amide compounds onto the surface of glass fibers, strong interfacial bonds are formed, and nylon resin and specific molding modifiers are introduced to synergistically improve the ring stiffness and oil resistance of the material.
It effectively inhibits the axial orientation of glass fibers, promotes their uniform distribution in the circumferential direction of the tube, improves ring stiffness and oil resistance, and improves molding quality, solving the problems of appearance defects and poor molding that exist in traditional methods.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of polypropylene materials, and in particular to a reinforced modified polypropylene cable conduit and its preparation method. Background Technology
[0002] With the rapid development of urban underground utility tunnels and power and communication network construction, cable conduits, as core components for cable protection, are facing increasingly higher demand and performance requirements. These conduits are typically buried directly underground, enduring long-term soil pressure, surface dynamic loads, and potential chemical corrosion. Therefore, stringent requirements are placed on their ring stiffness, long-term dimensional stability, and environmental stress resistance. Polypropylene, with its low density, corrosion resistance, good insulation, and ease of processing, has found some application in this field. However, as a typical semi-crystalline polymer, polypropylene has limited intrinsic rigidity and strength, making it difficult for pure polypropylene conduits to meet the ring stiffness requirements of heavy-duty burial scenarios. Furthermore, its non-polar molecular structure results in poor oil resistance, making it prone to swelling, deformation, and even cracking in underground environments such as gas stations and factory areas where oil penetration is possible.
[0003] To improve the mechanical properties of polypropylene materials to meet ring stiffness requirements, the industry commonly employs physical blending modification methods, such as adding reinforcing fibers (especially glass fibers) to the polypropylene matrix. The introduction of glass fibers does indeed significantly improve the tensile strength and flexural modulus of the composite material. However, when this method is applied to pipe extrusion molding—that is, during the process of the melt flowing through the die and undergoing stretching and cooling—the high aspect ratio glass fibers exhibit a strong axial orientation along the melt flow direction (i.e., the pipe axis). This significant axial orientation structure, while improving the longitudinal strength of the pipe, leads to a severe deficiency in the circumferential (radial) distribution of the reinforcing phase. Consequently, when the manufactured pipe is subjected to radial pressure from external soil, the reinforcing effect of the fibers cannot be effectively utilized, and the improvement in the pipe's transverse compressive strength (ring stiffness) is far lower than theoretically expected, failing to match the improvement in axial strength and making it difficult to meet the application requirements for high ring stiffness. Summary of the Invention
[0004] This application provides a reinforced modified polypropylene cable conduit and its preparation method, which effectively overcomes the defects of existing glass fiber reinforced polypropylene cable conduits, such as poor oil resistance and insufficient circumferential compressive strength (ring stiffness) due to excessive axial orientation of glass fibers during extrusion.
[0005] In a first aspect, this application provides a reinforced modified polypropylene cable conduit, comprising the following raw materials in parts by weight: 100-120 parts polypropylene, 10-20 parts nylon resin, 5-10 parts maleic anhydride-grafted polypropylene, 15-25 parts glass fiber, and 8-12 parts molding modifier, wherein the glass fiber surface is grafted with an aminosilane compound and α,β-unsaturated amide.
[0006] In any of the above technical solutions, the method for grafting glass fibers includes: Glass fibers are coupled with aminosilane compounds to obtain amino-modified glass fibers with primary amine groups on the surface. The amino-modified glass fiber is obtained by nucleophilic addition reaction with an α,β-unsaturated amide compound; wherein the ratio of the total molar number of primary amino groups in the aminosilane compound to the molar number of the α,β-unsaturated amide compound is greater than 1.
[0007] The technical solution of this application achieves improved ring stiffness and oil resistance of cable conduits through the synergistic blending of polypropylene, nylon resin, and surface-modified glass fiber. The introduction of nylon resin plays a crucial role in improving oil resistance. The strongly polar amide groups in its molecular chain not only possess high rigidity and strength, directly contributing to the overall modulus of the material, but also effectively hinder the penetration and swelling of oily agents by repelling non-polar molecules in oily media through their polarity, thus solving the problem of insufficient oil resistance in pure polypropylene. To achieve a breakthrough in ring stiffness, the key lies in overcoming the deficiency of insufficient circumferential reinforcement caused by the axial orientation of fibers in traditional glass fiber reinforcement. To this end, this application performs surface treatment on the glass fiber. First, through the hydrolysis and condensation of aminosilane, it is firmly grafted onto the fiber surface by chemical bonds, introducing amino group reaction sites; subsequently, through nucleophilic addition reactions, the molecular chains of α,β-unsaturated amides are covalently linked to the glass fiber. This modification has several benefits. First, the grafted molecular chains create steric hindrance and lubrication, effectively inhibiting fiber agglomeration during processing and ensuring uniform dispersion in the matrix. Second, the grafted layer constructs a bridging interface between the fiber and the matrix. The residual active primary amine groups can chemically react with the anhydride groups in the maleic anhydride-grafted polypropylene to form strong covalent bonds. Third, the amide segments on the grafted layer have strong hydrogen bond interactions with the nylon resin matrix. Through chemical crosslinking and physical hydrogen bonding, a strong interfacial bond is formed, greatly enhancing the efficiency of stress transfer from the relatively flexible polypropylene / nylon matrix to the high-modulus glass fiber, thus contributing to improved ring stiffness.
[0008] More importantly, this strong interfacial interaction creates an anchoring effect during melt flow. When the melt is subjected to shearing and stretching in the mold, conventional unmodified glass fibers rotate freely and are highly oriented along the flow direction. In the system of this application, however, the chemical anchor points on the fiber surface anchor them more tightly to the surrounding matrix, significantly increasing the resistance to fiber rotation and orientation during flow. This effectively suppresses excessive axial alignment in the extrusion direction, resulting in a more random and uniform circumferential (radial) distribution in the pipe. This allows more transversely or obliquely distributed fibers to directly participate in load-bearing when the pipe is subjected to external radial soil pressure, thereby maximizing the conversion of the glass fiber reinforcement into the pipe's ring stiffness.
[0009] In any of the above technical solutions, the ratio of the total number of primary amino groups in the aminosilane compound to the number of moles of the α,β-unsaturated amide compound is 1.5 to 2.5.
[0010] The molar ratio of aminosilane to α,β-unsaturated amide should be greater than 1 to ensure that sufficient free primary amine groups are retained on the modified fiber surface for subsequent interfacial reactions. When the molar ratio is optimized to be in the range of 1.5 to 2.5:1, an interfacial layer with optimal grafting density can be constructed on the fiber surface, achieving the best balance between strong interfacial adhesion and orientation inhibition, thereby obtaining better ring stiffness test results.
[0011] In any of the above technical solutions, the mass ratio of glass fiber to aminosilane compound is 100:5 to 10.
[0012] In any of the above technical solutions, the α,β-unsaturated amide compound is one or more of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide.
[0013] In any of the above technical solutions, the length of the glass fiber is 2 to 10 mm, preferably 3 to 5 mm, and the diameter is 10 to 15 micrometers.
[0014] In any of the above technical solutions, the aminosilane compound is selected from at least one of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltrimethoxysilane, and N-2-aminoethyl-3-aminopropyltriethoxysilane.
[0015] In any of the above technical solutions, the molding modifier comprises polyα-olefin, C9 petroleum resin, and maleic anhydride-grafted EPDM rubber in a mass ratio of 1:1 to 2:1.5 to 2.5.
[0016] The specific molding modifier compound system used in this application plays a crucial role in ensuring the molding quality of the final pipe, especially corrugated pipes and other conduits with complex shapes. Glass fiber has a significant impact on melt flowability, manifesting as appearance problems such as weld lines, uneven color and gloss, and rough orange-peel texture on the inner wall. Furthermore, cable conduits often employ a corrugated design, achieving a higher moment of inertia with less material through its undulating structure, aligning with the trends of lightweighting and cost reduction. However, the irregular protrusions and corners within the mold cavity also pose challenges to pipe processing. When the melt enters the mold cavity, insufficient filling is easily generated at protrusions or corners, leading to appearance defects such as unclear contours and collapsed waveforms on the surface of the corrugated pipe product.
[0017] To address this issue, this application utilizes the synergistic effect of polyalphaolefin (PAO), C9 petroleum resin, and maleic anhydride-grafted EPDM rubber. Specifically, PAO effectively reduces melt adhesion and pressure fluctuations, ensuring stable and smooth feed. Hydrogenated C9 petroleum resin significantly improves the fluidity of the PAO melt at high temperatures, particularly helping to reduce incomplete filling when encountering abrupt changes in the mold cavity cross-section, allowing the melt to fill the complex parts of the mold cavity more smoothly. Maleic anhydride-grafted EPDM rubber enhances the intrinsic strength of the melt, effectively suppressing undesirable molding phenomena such as waveform collapse caused by uneven elastic recovery after the melt leaves the mold. It also improves the compatibility of the molding modifier with the PP matrix. These three components work synergistically to improve melt feed flow, optimize mold cavity filling, and stabilize exit molding, significantly reducing the molding defect rate.
[0018] It should be noted that conventional lubricants (such as polyethylene wax) can help with the adhesion of the melt to the inner wall of the mold, but they cannot solve the problem of insufficient filling of the melt into the cavity of the bellows mold. C9 petroleum resin has a positive effect on improving the ring stiffness of the pipe compared to other petroleum resins, while petroleum resins such as C5 are less effective. This may be because C9 petroleum resin has an aromatic ring structure, which helps to improve rigidity.
[0019] In any of the above technical solutions, the kinematic viscosity of the polyα-olefin at 100°C is 30–100 cSt.
[0020] In any of the above technical solutions, the C9 petroleum resin is selected from hydrogenated C9 petroleum resin with a softening point of 100-130℃.
[0021] Hydrogenation eliminates the unsaturated double bonds in C9 petroleum resin, preventing it from becoming brittle or sticky due to thermal and oxidative aging during processing and use, thus ensuring the long-term thermal stability required for cable conduits.
[0022] In any of the above technical solutions, the grafting rate of the maleic anhydride-grafted EPDM rubber is 0.6 to 1.0 wt%.
[0023] Secondly, this application provides a method for preparing reinforced modified polypropylene cable conduit, comprising: mixing polypropylene, nylon resin, maleic anhydride-grafted polypropylene, and molding modifier, drying to obtain a mixture, feeding the mixture into an extruder, and extruding and granulating at a temperature of 180-220°C to obtain composite material particles; adding the composite material particles and glass fiber to a corrugated pipe extrusion line for extrusion molding to obtain the final product, with an extrusion temperature of 190-220°C.
[0024] In summary, this application has the following beneficial effects: This application provides a solution to address the requirements of high ring stiffness and high oil resistance in polypropylene cable conduits. By introducing nylon resin and glass fibers grafted with aminosilane and α,β-unsaturated amide, not only is the oil resistance improved by utilizing nylon, but the strong interfacial interaction formed between the modified glass fiber and the matrix effectively suppresses the axial orientation of the fibers during processing, promoting their uniform circumferential distribution in the pipe, thereby maximizing the conversion of the fiber's reinforcing effect into ring stiffness. Simultaneously, the synergistic effect of polyα-olefin, hydrogenated C9 petroleum resin, and maleic anhydride-grafted EPDM rubber effectively solves problems such as poor molding of high-fiber-content melts in complex corrugated dies by stabilizing feed flow, improving cavity filling, and suppressing outlet deformation, ensuring the molding quality of the cable conduit. Detailed Implementation
[0025] Preparation Example
[0026] Preparation Example 1: Modified glass fiber was prepared according to the following steps: 100g of glass fiber, approximately 4mm in length and 13μm in diameter, was weighed and placed in a reaction vessel. A 200mL mixture of 90vol% ethanol and 10vol% deionized water was prepared, and the pH was adjusted to 4.5–5.0 with acetic acid. 8.0g (approximately 0.036mol) of aminopropyltriethoxysilane was added, and the mixture was stirred to allow for complete hydrolysis, yielding a pretreated solution. The pretreated solution was transferred to a reaction vessel containing the glass fiber, and the reaction was carried out under nitrogen protection in a constant temperature oil bath at 80℃ with mechanical stirring for 4 hours. After the reaction was complete, the product was filtered and washed three times with anhydrous ethanol, then dried in a vacuum oven at 90℃ for 6 hours to obtain aminated glass fiber.
[0027] The above-mentioned aminated glass fibers were redispersed in 150 mL of N,N-dimethylformamide solvent. 1.29 g (approximately 0.018 mol) of acrylamide was added under mechanical stirring, followed by 0.037 g of triethylamine as a catalyst. The reaction system temperature was raised to 60 °C, and the reaction was continuously stirred at this temperature for 8 hours. After the reaction was complete, the product was filtered, washed three times successively with DMF and deionized water, and finally dried in an 80 °C vacuum oven to constant weight, yielding modified glass fibers with aminosilane and acrylamide segments grafted onto their surface.
[0028] Preparation Example 2: Modified glass fiber was prepared according to the following steps: 100g of glass fibers, approximately 3mm in length and 10μm in diameter, were weighed and placed in a reaction vessel. A 200mL mixture of 90vol% ethanol and 10vol% deionized water was prepared, and the pH was adjusted to 4.5–5.0 with acetic acid. 5.5g (approximately 0.03mol) of aminopropyltrimethoxysilane was added, and the mixture was stirred to allow for complete hydrolysis, yielding a pretreated solution. The pretreated solution was transferred to a reaction vessel containing the glass fibers, and the reaction was carried out under nitrogen protection in a constant temperature oil bath at 80℃ with mechanical stirring for 4 hours. After the reaction was complete, the product was filtered and washed three times with anhydrous ethanol, then dried in a vacuum oven at 80℃ for 8 hours to obtain aminated glass fibers.
[0029] The above-mentioned aminated glass fibers were redispersed in 120 mL of N,N-dimethylformamide solvent. 1.42 g (approximately 0.02 mol) of acrylamide was added with stirring, followed by 0.041 g of triethylamine as a catalyst. The reaction system temperature was raised to 60 °C, and the reaction was continued with stirring at this temperature for 8 hours. After the reaction was complete, the product was filtered, washed three times successively with DMF and deionized water, and finally dried in an 80 °C vacuum oven to constant weight, yielding modified glass fibers with aminosilane and acrylamide segments grafted onto their surface.
[0030] Preparation Example 3: Modified glass fiber, prepared according to the following steps: 100g of glass fiber, approximately 5mm in length and 15μm in diameter, was weighed and placed in a reaction vessel. A 250mL solution of 90vol% ethanol and 10vol% deionized water was prepared, and the pH was adjusted to 4.5–5.0 with acetic acid. 9.6g (approximately 0.043mol) of N-2-aminoethyl-3-aminopropyltrimethoxysilane was added and stirred to allow for complete hydrolysis, yielding a pretreated solution. The pretreated solution was transferred to a reaction vessel containing the glass fiber, and the reaction was mechanically stirred in an 80℃ oil bath for 4 hours under nitrogen protection. After the reaction was complete, the product was filtered and washed three times with anhydrous ethanol, then dried in a 95℃ vacuum oven for 5 hours to obtain aminated glass fiber.
[0031] The above-mentioned aminated glass fibers were redispersed in 150 mL of N,N-dimethylformamide solvent. 1.74 g (approximately 0.017 mol) of methacrylamide was added under mechanical stirring, followed by 0.035 g of triethylamine as a catalyst. The reaction system temperature was raised to 50 °C, and the reaction was continuously stirred at this temperature for 10 hours. After the reaction was complete, the product was filtered, washed three times successively with DMF and deionized water, and finally dried in a vacuum oven at 85 °C to constant weight, thus obtaining modified glass fibers with aminosilane and acrylamide segments grafted onto their surface.
[0032] Preparation Example 4, modified glass fiber, differs from Preparation Example 1 in that the amount of acrylamide used is 2.15 g (approximately 0.036 mol), so that the ratio of the total number of moles of primary amino groups in the aminosilane compound to the number of moles of the α,β-unsaturated amide compound is 1.
[0033] Preparation Example 5, modified glass fiber, differs from Preparation Example 1 in that the amount of acrylamide used is 0.72 g (approximately 0.012 mol), so that the ratio of the total number of moles of primary amino groups in the aminosilane compound to the number of moles of the α,β-unsaturated amide compound is 3.
[0034] Preparation Example 6, modified glass fiber, differs from Preparation Example 1 in that no nucleophilic addition reaction was performed, and the resulting aminated glass fiber is the final product.
[0035] Preparation Example 7, modified glass fiber, differs from Preparation Example 1 in that it is prepared according to the following steps: 100g of glass fibers, approximately 4mm in length and 13μm in diameter, were weighed and placed in a reaction vessel. A 200mL mixture of 90vol% ethanol and 10vol% deionized water was prepared, and the pH was adjusted to 4.5–5.0 with acetic acid. 8.0g of vinyltriethoxysilane was added to the mixture, and the mixture was stirred to allow for complete hydrolysis, yielding a pretreated solution. The pretreated solution was transferred to a reaction vessel containing the glass fibers, and the reaction was carried out under nitrogen protection in a constant temperature oil bath at 80℃ with mechanical stirring for 4 hours. After the reaction was complete, the product was filtered and washed three times with anhydrous ethanol, then dried in a vacuum oven at 90℃ for 6 hours to obtain vinylated glass fibers. Example
[0036] Example 1: A reinforced modified polypropylene cable conduit was prepared according to the following process steps: Raw material preparation: Weigh 1100 g of homopolymer polypropylene resin (Shanghai Petrochemical M800E); 165 g of nylon 6 resin (BASF Ultramid B3S, Germany); weigh 82.5 g of maleic anhydride-grafted polypropylene compatibilizer (DuPont Fusabond P353, USA); 220 g of surface-modified glass fiber (prepared in Preparation Example 1); 96.8 g of molding modifier, which was prepared by premixing 22.0 g of polyα-olefin (SpectraSyn 40, kinematic viscosity at 100℃ approximately 39 cSt), 33.0 g of hydrogenated C9 petroleum resin (Tangyi Chemical D0312, softening point approximately 120℃) and 41.8 g of maleic anhydride-grafted EPDM rubber (Dow DM-7, USA, grafting rate approximately 0.8wt%) in a low-speed mixer.
[0037] Melt blending and granulation: Polypropylene, nylon resin, maleic anhydride-grafted polypropylene, and molding modifier were placed in a high-speed mixer and mixed for 5 minutes at room temperature to obtain a homogeneous matrix premix. Nylon resin and surface-modified glass fiber were separately placed in a circulating air drying oven and dried at 90°C for at least 4 hours to remove moisture. The dried matrix premix was fed into the main feed port of a twin-screw extruder (screw diameter 52mm, L / D ratio 40:1). The temperatures from the feeding section to the die head were set as follows: 185°C, 195°C, 205°C, 210°C, 210°C, 205°C (die head). The screw speed was set to 300 rpm. The melt was extruded through a die, cooled in a water bath, and pelletized to obtain reinforced modified polypropylene composite particles.
[0038] Pipe extrusion molding: Composite material particles and surface-modified glass fibers are added to a side-feed twin-screw corrugated pipe extrusion production line. The extruder temperature is set at 190℃-210℃, and the die temperature is 200℃-215℃. After shaping by the molding machine, cooling in the cooling water tank, traction by the traction machine, and fixed-length cutting by the cutting machine, a reinforced modified polypropylene cable conduit with significantly improved ring stiffness is finally produced.
[0039] Example 2: A reinforced modified polypropylene cable conduit was prepared according to the following process steps: Raw material preparation: Weigh 1050 g of homopolymer polypropylene resin (Shanghai Petrochemical M800E); 105 g of nylon 66 resin (DuPont 101L); weigh 52.5 g of maleic anhydride-grafted polypropylene compatibilizer (DuPont Fusabond P353); 157.5 g of surface-modified glass fiber (prepared in Preparation Example 2); 84.0 g of molding modifier, which was prepared by premixing 16.8 g of poly-α-olefin (SpectraSyn Elite65, kinematic viscosity at 100℃ is about 65 cSt), 25.2 g of C9 petroleum resin (CAS No. 64742-95-6, softening point is about 110℃) and 42.0 g of maleic anhydride-grafted EPDM rubber (Dow DM-7, grafting rate is about 0.8 wt%) in a low-speed mixer.
[0040] Melt blending and granulation: Polypropylene, nylon resin, maleic anhydride-grafted polypropylene, and molding modifier were placed in a high-speed mixer and mixed for 5 minutes at room temperature to obtain a homogeneous matrix premix. Nylon resin and surface-modified glass fiber were separately placed in a circulating air drying oven and dried at 90°C for at least 4 hours to remove moisture. The dried matrix premix was fed into the main feed port of a twin-screw extruder (screw diameter 52mm, L / D ratio 40:1). The temperatures from the feeding section to the die head were set as follows: 180°C, 190°C, 200°C, 205°C, 205°C, 200°C (die head). The screw speed was set to 300 rpm. The melt was extruded through a die, cooled in a water bath, and pelletized to obtain reinforced modified polypropylene composite particles.
[0041] Pipe extrusion molding: Composite material particles and surface-modified glass fiber are added to a side-feed twin-screw corrugated pipe extrusion production line. The extruder temperature is set at 190℃-210℃, and the die temperature is 195℃-210℃. After shaping by the molding machine, cooling in the cooling water tank, traction by the traction machine, and fixed-length cutting by the cutting machine, a reinforced modified polypropylene cable conduit with significantly improved ring stiffness is finally produced.
[0042] Example 3: A reinforced modified polypropylene cable conduit was prepared according to the following process steps: Raw material preparation: Weigh 1200 g of homopolymer polypropylene resin (Shanghai Petrochemical M800E); 240 g of nylon 6 resin (BASF Ultramid B3S, Germany); weigh 120 g of maleic anhydride-grafted polypropylene compatibilizer (DuPont Fusabond P353, USA); 300 g of surface-modified glass fiber (prepared in Preparation Example 3); 132 g of molding modifier, which was prepared by premixing 24.0 g of polyα-olefin (SpectraSyn 40, kinematic viscosity at 100°C approximately 39 cSt), 48.0 g of hydrogenated C9 petroleum resin (softening point approximately 120°C) and 60 g of maleic anhydride-grafted ethylene propylene diene monomer (SH-DM7, grafting rate approximately 0.6 wt%) in a low-speed mixer.
[0043] Melt blending and granulation: Polypropylene, nylon resin, maleic anhydride-grafted polypropylene, and molding modifier were placed in a high-speed mixer and mixed for 5 minutes at room temperature to obtain a homogeneous matrix premix. Nylon resin and surface-modified glass fiber were separately placed in a circulating air drying oven and dried at 90°C for at least 4 hours to remove moisture. The dried matrix premix was fed into the main feed port of a twin-screw extruder (screw diameter 52mm, L / D ratio 40:1). The temperatures from the feeding section to the die head were set as follows: 190°C, 205°C, 215°C, 220°C, 220°C, 215°C (die head). The screw speed was set to 300 rpm. The melt was extruded through a die, cooled in a water bath, and pelletized to obtain reinforced modified polypropylene composite particles.
[0044] Pipe extrusion molding: Composite material particles and surface-modified glass fibers are added to a side-feed twin-screw corrugated pipe extrusion production line. The extruder temperature is set at 195℃-220℃, and the die temperature is 210℃-220℃. After shaping by the molding machine, cooling in the cooling water tank, traction by the traction machine, and fixed-length cutting by the cutting machine, a reinforced modified polypropylene cable conduit with significantly improved ring stiffness is finally produced.
[0045] Example 4, a reinforced modified polypropylene cable conduit, differs from Example 1 in that the modified glass fiber of Example 1 is replaced with an equal amount of the modified glass fiber of Example 4.
[0046] Example 5, a reinforced modified polypropylene cable conduit, differs from Example 1 in that an equal amount of modified glass fiber from Example 5 is used to replace the modified glass fiber from Example 1.
[0047] Example 6, a reinforced modified polypropylene cable conduit, differs from Example 1 in that an equal amount of hydrogenated C9 petroleum resin (Tangyi Chemical D0312, softening point about 120°C) is used instead of poly-α-olefin (SpectraSyn 40, kinematic viscosity at 100°C about 39 cSt).
[0048] Example 7, a reinforced modified polypropylene cable conduit, differs from Example 1 in that an equal amount of hydrogenated C9 petroleum resin (Tangyi Chemical D0312, softening point approximately 120°C) is used instead of maleic anhydride-grafted EPDM rubber (Dow DM-7, grafting rate approximately 0.8 wt%).
[0049] Example 8, a reinforced modified polypropylene cable conduit, differs from Example 1 in that an equal amount of poly-α-olefin (SpectraSyn 40, kinematic viscosity at 100°C approximately 39 cSt) is used to replace hydrogenated C9 petroleum resin (Tangyi Chemical D0312, softening point approximately 120°C).
[0050] Example 9, a reinforced modified polypropylene cable conduit, differs from Example 1 in that an equal amount of hydrogenated C9 petroleum resin (softening point approximately 120°C) is used instead of hydrogenated C5 petroleum resin (Xinghai Chemical R100, softening point approximately 120°C). Comparative Example
[0051] Comparative Example 1 is a reinforced modified polypropylene cable conduit, which differs from Example 1 in that the modified glass fiber of Preparation Example 1 is replaced with an equal amount of the modified glass fiber of Preparation Example 6.
[0052] Comparative Example 2, an enhanced modified polypropylene cable conduit, differs from Example 1 in that the modified glass fiber of Preparation Example 7 is replaced with an equal amount of the modified glass fiber of Preparation Example 1.
[0053] Performance testing
[0054] Experiment 1: Ring Stiffness Test Sample preparation: Three sample segments with a length of (300±20) mm were randomly cut from the conduits prepared in each embodiment and comparative example. Each sample must contain at least 5 complete corrugation cycles. The prepared samples were conditioned in a standard laboratory environment at (23±2)℃ and (50±10)% relative humidity for no less than 24 hours.
[0055] Test Method: The test shall be conducted according to GB / T 9647-2015 "Determination of Ring Stiffness of Thermoplastic Pipes" using a ring stiffness testing machine equipped with a parallel loading plate and an inner diameter measurement system. The specimen shall be placed vertically at the center of the lower platen of the testing machine. Pressure shall be applied to the specimen at a constant compression rate (causing a relative radial deformation of 3% ± 1% per minute). The ring stiffness value of a single specimen shall be recorded. The specimen shall be rotated approximately 120° and 240° relative to the initial loading position, and the above steps shall be repeated twice. The arithmetic mean of the three measurements shall be taken as the final ring stiffness result for this batch of conduits, rounded to two decimal places. Test 2: Oil Resistance Test Sample preparation: Six standard dumbbell-shaped tensile specimens (according to GB / T 1040.2-2022) were cut from the conduits of each embodiment and comparative example to prepare sheet specimens.
[0056] Test Method: Take one sample and test its original tensile strength according to GB / T 1040.2-2022 "Determination of Tensile Properties of Plastics - Part 2: Test Conditions for Molded and Extruded Plastics". Completely immerse the remaining sample in a sealed container filled with IRM 902 oil. Place the container in a constant temperature environment of 23±2℃ and immerse for 168±2 hours. After immersion, remove the sample and quickly wipe off any residual oil with a lint-free absorbent cloth. After placing the sample in a standard laboratory environment for 24±1 hours, test its tensile strength. Compare and calculate the tensile strength retention rate of the sample before and after immersion.
[0057] Experiment 3: Molding Defect Rate Test Sampling: The raw materials for each embodiment and comparative example were continuously produced on the same small-scale corrugated pipe extrusion production line (with consistent die, screw speed, and temperature settings), with an extrusion length of 100 meters. Online Inspection: During stable extrusion, trained inspectors conducted 100% online visual inspection of the extruded pipes. Any of the following defects constituted a "defective product": surface weld lines, abnormal color gloss, obvious unclear outlines or collapses at the peaks or troughs, or a rough orange-peel texture on the inner wall. The total length of defective products detected during this production period was calculated, and the molding defect rate was calculated using the following formula: Defective molding rate = (length of defective products / total production length) × 100%.
[0058] Table 1. Performance Test Results
[0059] Analysis of experimental results: Compared to Example 1, Example 4 (glass fiber modified primary amine / amide molar ratio of 1:1) showed significantly worse ring stiffness. This indicates that when the primary amine groups are completely consumed, the fiber surface lacks sufficient free primary amine groups to chemically crosslink with the maleic anhydride-grafted polypropylene in the matrix. The direct consequence is insufficient interfacial bonding strength, leading to reduced stress transfer efficiency and weakened anchoring effect on the glass fiber during processing and its ability to inhibit axial orientation, resulting in limited improvement in ring stiffness. Example 5 (glass fiber modified primary amine / amide molar ratio of 3:1) also showed a decrease in ring stiffness. This indicates that while excessive primary amine groups ensure crosslinking points, they may lead to excessively high polarity on the fiber surface, reducing compatibility with the matrix.
[0060] Compared to Example 1, Example 6 (lacking polyalphaolefin in the molding modifier) showed a significantly worse molding defect rate. This indicates that polyalphaolefin plays an important role in reducing die adhesion and stabilizing feed pressure. Its absence leads to poor melt flow stability and increased pressure fluctuations. This unstable flow state extends to complex mold cavities, amplifying the risks of incomplete filling and poor fusion, thus significantly increasing appearance defects. Example 7 (lacking maleic anhydride-grafted EPDM rubber in the molding modifier) showed a poor molding defect rate and a slight decrease in ring stiffness. This may be because maleic anhydride-grafted EPDM rubber has the dual function of enhancing melt strength and improving compatibility. Its absence leads to insufficient melt strength, uneven elastic recovery after leaving the mold, and a greater likelihood of waveform contour changes or even collapse. Example 8 (lacking C9 petroleum resin in the molding modifier) showed poor performance in both ring stiffness and molding defect rate, especially with obvious unclear contours and waveform collapse at the peaks and troughs. This indicates that C9 petroleum resin not only acts as a flow promoter to improve cavity filling and reduce stagnation, but its aromatic ring structure also directly contributes to the material's rigidity. Its absence leads to a decrease in the melt's filling ability in complex areas of the mold, while simultaneously reducing the material's rigidity, thus negatively impacting both properties. Example 9 (using C5 petroleum resin instead of C9 petroleum resin) showed a significant decrease in ring stiffness. This directly verifies the statement in the specification that "C9 petroleum resin has a positive effect on improving the ring stiffness of pipes compared to other petroleum resins." C5 resin mainly has an aliphatic chain structure and lacks the rigid aromatic ring segments found in C9 resin; therefore, it is less effective in improving the overall modulus of the material, resulting in a lower final ring stiffness.
[0061] Compared to Example 1, Comparative Example 1 (glass fiber only aminated, without grafted amide segments) showed a severe deficiency in ring stiffness. This indicates that although glass fiber treated with aminosilane can react with PP-g-MAH, it lacks the amide chain introduced through nucleophilic addition. The absence of this segment makes it difficult for the glass fiber to form a strong hydrogen bond network with the nylon matrix, and the insufficient steric hindrance limits its ability to suppress axial orientation during melt flow. Therefore, fiber orientation is aggravated, and the effect of improving ring stiffness is deteriorated. Comparative Example 2 (glass fiber treated with vinylsilane) showed a comprehensive decline in ring stiffness, oil resistance, and molding defect rate. The reason may be that the use of silane without amino groups prevents the fiber surface from achieving the dual effects of "amino-anhydride crosslinking" and "amide-nylon hydrogen bonding," resulting in decreased compatibility between the glass fiber and the polypropylene / nylon matrix, a weak interface, failure of stress transfer, and deterioration of ring stiffness. Meanwhile, decreased compatibility leads to a tendency for glass fibers to agglomerate in the matrix, making them prone to stress concentration points and swelling. This not only weakens oil resistance but also hinders melt flow and increases the molding defect rate.
[0062] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A reinforced modified polypropylene cable conduit, characterized in that, The raw materials comprise the following parts by weight: 100-120 parts polypropylene, 10-20 parts nylon resin, 5-10 parts maleic anhydride-grafted polypropylene, 15-25 parts glass fiber, and 8-12 parts molding modifier. The glass fiber surface is grafted with aminosilane compounds and α,β-unsaturated amides. The molding modifier comprises polyα-olefin, C9 petroleum resin, and maleic anhydride-grafted EPDM rubber in a mass ratio of 1:1-2:1.5-2.
5. The method for grafting the glass fiber includes: Glass fibers are coupled with aminosilane compounds to obtain amino-modified glass fibers with primary amine groups on the surface. The amino-modified glass fiber is obtained by nucleophilic addition reaction with an α,β-unsaturated amide compound; wherein the ratio of the total molar number of primary amino groups in the aminosilane compound to the molar number of the α,β-unsaturated amide compound is greater than 1.
2. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The ratio of the total molar number of primary amino groups in the aminosilane compound to the molar number of the α,β-unsaturated amide compound is 1.5 to 2.
5.
3. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The mass ratio of the glass fiber to the aminosilane compound is 100:5 to 10.
4. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The α,β-unsaturated amide compound is one or more of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide.
5. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The kinematic viscosity of the poly-α-olefin at 100°C is 30–100 cSt.
6. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The C9 petroleum resin used is a hydrogenated C9 petroleum resin with a softening point of 100-130℃.
7. The reinforced modified polypropylene cable conduit according to claim 1, characterized in that, The grafting rate of the maleic anhydride-grafted EPDM rubber is 0.6–1.0 wt%.
8. A method for preparing a reinforced modified polypropylene cable conduit, characterized in that, include: According to the raw material ratio of any one of claims 1 to 7, polypropylene, nylon resin, maleic anhydride-grafted polypropylene, and molding modifier are mixed evenly and dried to obtain a mixture. The mixture is fed into an extruder and extruded and granulated at a temperature of 180 to 220°C to obtain composite material particles. The composite material particles and glass fiber are added to a corrugated pipe extrusion production line for extrusion molding, and the extrusion temperature is 190 to 220°C.
Citation Information
Patent Citations
High-strength polypropylene composite material for filter plate and preparation method of high-strength polypropylene composite material
CN119391086A
