High-surface-capacity capacitive electrochemical capacitor electrode and preparation method thereof
By designing a Ni3N/MoO3 core-shell heterostructure, the problems of low energy density and poor cycling stability of traditional electrodes are solved, and an electrochemical capacitor electrode with high specific capacity and long-term cycling stability is realized, which is suitable for new energy vehicles and industrial high-power energy storage systems.
Patent Information
- Application Number
- CN202511897972.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-16
- Publication Date
- 2026-03-03
AI Technical Summary
Traditional activated carbon electrode supercapacitors have low energy density, while nickel-based compound battery-type electrodes suffer from slow reaction kinetics, limited ion diffusion, and insufficient structural stability, resulting in poor cycle stability and making it difficult to meet the application scenarios that require both high energy and high power.
By adopting a Ni3N/MoO3 core-shell heterostructure design, MoO3 is deposited on the surface of a nickel hydroxide precursor through in-situ atomic layer deposition and high-temperature nitriding treatment to form a Ni3N/MoO3 electrode. This process modulates the electronic structure and suppresses volume expansion, thereby improving the conductivity and surface activity of the material.
The specific capacity and cycle stability of the electrode are significantly improved. The Ni3N/MoO3 electrode retains 80% of its capacity after 7000 cycles of high-rate charge and discharge, making it suitable for new energy vehicles and industrial high-power energy storage systems.
Smart Images

Figure CN121601457A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical energy storage materials technology, and in particular to a high areal capacity electrochemical capacitor electrode and its preparation method. Background Technology
[0002] With the widespread application of new energy storage systems in electric transportation, smart grids, and high-power equipment, energy storage devices are facing an urgent need to simultaneously improve energy density, power density, and cycle stability. While traditional activated carbon electrode supercapacitors possess excellent power characteristics, their energy density is generally below 10 Wh·kg⁻¹ due to their surface physical adsorption energy storage mechanism. -1 It is difficult to meet the application scenarios that require both high energy and high power.
[0003] Hybrid capacitors combine pseudocapacitive and battery-type electrodes, achieving synergistic coupling between surface capacitance processes and bulk Faraday reactions, providing a feasible path to overcome the energy-power imbalance. However, battery-type electrodes generally suffer from slow reaction kinetics, limited ion diffusion, and insufficient structural stability, becoming the core bottleneck restricting their performance improvement.
[0004] Among various battery materials, nickel-based compounds (Ni(OH)2, NiO, Ni3S4, Ni3N) have attracted widespread attention due to their tunable valence state, abundant resources, and low cost. Ni3N, in particular, possesses a metal-like band structure and excellent electron transport performance, which can significantly improve bulk reaction rates and rate performance. However, its pure-phase structure is prone to volume expansion and structural degradation during charge and discharge, leading to poor cycle stability and rapid capacity decay. Summary of the Invention
[0005] The main objective of this invention is to provide a high areal capacitance electrochemical capacitor electrode and its preparation method, aiming to solve at least one of the above-mentioned technical problems.
[0006] To achieve the above objectives, the present invention provides a method for preparing a high areal capacitance electrochemical capacitor electrode, comprising the following steps: (1) Preparation of precursors Ni(NO3)3, NH4F and urea were dissolved in deionized water, and then nickel foam was added. After hydrothermal reaction treatment, Ni(OH)2 / nickel foam precursor was obtained. (2) Deposition of MoO3 The Ni(OH)2 / nickel foam precursor was washed and dried, and then a MoO3 thin layer was deposited on the Ni(OH)2 / nickel foam precursor by atomic layer deposition to obtain the composite precursor. (3) Nitriding treatment The composite precursor was annealed in a mixed atmosphere of NH3 and Ar to obtain a high areal capacitance electrochemical capacitor electrode.
[0007] Furthermore, in step (1), the ratio of Ni(NO3)3, NH4F, urea and deionized water is 1.5 mmol: 0.0925 g: 0.3 g: 18 mL.
[0008] Furthermore, in step (1), the hydrothermal reaction treatment temperature is 120 ℃ and the time is 6 hours.
[0009] Furthermore, in step (2), the thickness of the MoO3 thin layer is 2~4 nm.
[0010] Furthermore, in step (2), the volume ratio of NH3 to Ar is 30:70, and the gas flow rate is 100 sccm.
[0011] Furthermore, in step (2), the specific process of annealing is as follows: anneal at 350°C for 2 hours with a heating rate of 2°C / min, and then naturally cool to room temperature.
[0012] The present invention also provides a high areal capacitance electrochemical capacitor electrode, which is prepared according to the above preparation method.
[0013] The design principle of this invention is as follows: This invention proposes a Ni3N / MoO3 core-shell heterostructure design strategy, constructing a stable biphase electrode structure through in-situ atomic layer deposition (ALD) to achieve synergistic control of electronic structure and reaction kinetics. Specifically, this invention deposits MoO3 on the surface of a nickel hydroxide precursor using atomic layer deposition and then performs high-temperature nitriding treatment to form a MoO3 / Ni3N core-shell heterostructure. This not only allows for the control of the electronic structure of Ni3N but also enhances the conductivity and surface activity of the material. The Ni3N core provides high conductivity and bulk Faraday storage capacity, while the MoO3 shell effectively suppresses volume expansion and maintains structural integrity. Simultaneously, spontaneous charge migration induced by the Fermi level difference between the two phases can reconstruct electronic states at the interface, generating more surface active sites and significantly enhancing pseudocapacitance contribution and ion transport efficiency. The resulting Ni3N / MoO3 electrode exhibits excellent overall performance: specific capacity increased to 469.5 C·g. -1 (2.7 times that of pure Ni3N), and still retains 80.8% capacity after 7000 cycles.
[0014] The beneficial effects of this invention are reflected in: The electrode prepared by this invention exhibits high specific capacitance, excellent rate performance, and long-term cycle stability in aqueous hybrid capacitors. After 7000 cycles under high-rate charge-discharge conditions, it retains approximately 80% of its capacity and maintains stable output performance under high-power instantaneous discharge. The electrode's high power and excellent long-cycle stability make it suitable for applications with stringent requirements for high power density and long lifespan, such as new energy metallurgical vehicles, electric logistics vehicles, and industrial high-power energy storage systems.
[0015] This invention provides a new theoretical basis and structural design ideas for the application of transition metal nitrides in high-power hybrid capacitors through in-situ interface construction and bandgap modulation, laying a technical foundation for the industrialization of next-generation high-energy-density energy storage systems. Attached Figure Description
[0016] Figure 1 Scanning electron microscope images of a) Ni3N and b) Ni3N / MoO3.
[0017] Figure 2 This is the elemental distribution diagram of Ni3N / MoO3.
[0018] Figure 3 The X-ray diffraction patterns are for Ni3N and Ni3N / MoO3.
[0019] Figure 4 The images show the Raman spectra of Ni3N and Ni3N / MoO3.
[0020] Figure 5 The cyclic voltammetry curves for Ni3N and Ni3N / MoO3 are shown.
[0021] Figure 6 The charge-discharge curves of Ni3N / MoO3 and a comparison of its specific capacity with that of Ni3N are shown.
[0022] Figure 7 The diagram shows the cyclic stability of Ni3N / MoO3. Detailed Implementation
[0023] To enable those skilled in the art to more clearly understand the technical solutions described in this invention, the following embodiments are provided for illustration. It should be noted that the following embodiments do not constitute a limitation on the scope of protection claimed by this invention.
[0024] Unless otherwise specified, the raw materials, reagents or devices used in the following embodiments can be obtained from conventional commercial sources or by existing known methods; unless otherwise specified, the methods used in the embodiments of the present invention are methods mastered by those skilled in the art.
[0025] Example 1 Preparation of electrodes for high areal capacitance electrochemical capacitors (1) Preparation of precursors The nickel foam was ultrasonically cleaned in ethanol and dilute hydrochloric acid solutions and then air-dried to remove the oil and oxide layers on its surface. Subsequently, 1.5 mmol of Ni(NO3)3·6H2O, 0.0925 g of NH4F and 0.3 g of urea ((NH2)2CO) were dissolved in 18 mL of deionized water and stirred thoroughly to form a homogeneous hydrothermal reaction solution. The resulting solution and a cleaned nickel foam (2 cm × 3 cm) were transferred to a PTFE-lined reactor (50 mL) and sealed with a stainless steel shell. The reactor was then hydrothermally reacted at 120 °C for 6 hours to obtain the Ni(OH)2 / nickel foam precursor. (2) Deposition of MoO3 The Ni(OH)2 / nickel foam precursor obtained in step (1) was taken out, thoroughly washed with deionized water and ethanol, and dried. Subsequently, an atomic layer deposition (ALD) technique was used to controllably deposit a thin layer of MoO3 on the surface of the obtained precursor, with 150 deposition cycles, to obtain the composite precursor. The specific process is as follows: The Ni(OH)₂ / nickel foam precursor was placed in the ALD reaction chamber. After evacuation, the ALD reaction was initiated. A single cycle consisted of the following steps: First, Mo(CO)₆ was introduced into the reaction chamber as precursor 1, undergoing pulse adsorption with surface groups on the substrate. The Mo(CO)₆ was uniformly adsorbed onto the substrate surface and purged with nitrogen for 60 seconds to remove excess reactants and byproducts. Second, ozone was used as precursor 2 to react with the surface Mo(CO)₆, forming an amorphous MoO₃ compound. Simultaneously, nitrogen purging was used for cleaning. In the third step, water vapor was introduced into the reaction chamber as precursor 3, introducing new Mo(CO)₆ adsorption sites, followed by a corresponding cleaning step. These steps were repeated 150 times, with the deposition temperature controlled at 220℃. Furthermore, N₂ (99.99% purity) was used as the power source (for valve opening and closing, etc.) and precursor delivery gas throughout the deposition process. The entire deposition process used 99.9% pure oxygen (O2) as the ozone source, with the supply pressure maintained at 0.2-0.25 MPa. Mo(CO)6 was used as the molybdenum source, placed in a foaming flask, and foamed at room temperature. The reaction time between the molybdenum source precursor and the matrix was 0.35 s, the reaction time of the ozone precursor was 5 s, and the reaction time of the water vapor precursor was 0.03 s, ultimately forming a 3 nm thick MoO3 thin layer.
[0026] (3) Nitriding treatment The composite precursor was placed in a mixed atmosphere of NH3 / Ar (volume ratio 30:70) and annealed at 350 °C for 2 hours at a gas flow rate of 100 sccm and a heating rate of 2 °C / min. After natural cooling to room temperature, a Ni3N / MoO3 heterostructure array was obtained. The mass loading of its active materials (Ni3N and MoO3) was measured to be approximately 2 mg·cm³. -2 This is the electrode of a high-area-capacitance electrochemical capacitor, hereinafter referred to as Ni3N / MoO3.
[0027] Experimental Example 1 Performance testing of electrodes for high areal capacitance electrochemical capacitors The structure and performance of Ni3N (prepared according to the method of Example 1, omitting step (2)) and the Ni3N / MoO3 prepared in Example 1 were analyzed and tested for electrochemical performance, as follows: I. Structural and Performance Analysis like Figure 1 As shown in Figure a, Ni3N exhibits a structural characteristic of transforming from smooth nanosheets to nanoparticles, indicating that the nanosheets break down into particles during the nitriding process. However, after coating the Ni(OH)2 surface with a MoO3 layer, the nanosheet structure can be better preserved (…). Figure 1 (b) This structural feature facilitates rapid ion diffusion and enhances structural stability, thereby endowing the material with excellent rate performance and cycle stability.
[0028] The elemental distribution diagram of Ni3N / MoO3 is as follows: Figure 2 As shown, Mo, Ni, O, and N elements are uniformly distributed on the sample surface, confirming the successful coating of MoO3.
[0029] X-ray diffraction patterns of Ni3N and Ni3N / MoO3 are as follows: Figure 3 As shown, the strong diffraction peaks at 30.3°, 38.9°, 41.8°, 44.5°, 58.5°, 70.5°, 78.3°, 85.5°, and 87.3° correspond to the (101), (110), (002), (111), (112), (300), (203), (302), and (221) crystal planes of Ni3N (JCPDS: 89-5144), respectively. The main difference between the diffraction patterns of the two materials is that the Ni3N / MoO3 heterostructure exhibits a relatively broad diffraction peak between 20° and 30°, which can be attributed to the poorly crystallinized MoO3 phase.
[0030] Raman spectroscopy further confirmed the MoO3 coating; both characterization methods primarily focus on the structural information of the material surface. For Raman spectroscopy, 123 cm⁻¹... -1 161 cm-1 200 cm -1 230 cm -1 and 533 cm -1 The peak at that point corresponds to a typical vibrational mode of Ni3N. Figure 4 After recombination with MoO3, the Raman peak intensity of Ni3N significantly decreased. A new 681 cm⁻¹ peak appeared. -1 (B) 2g B 3g ) and 820 cm -1 (A) g B 1g The characteristic peak can be attributed to α-MoO3, while the 574 cm⁻¹ peak... -1 and 755 cm -1 The peak originates from the Mo-O-Mo vibrational mode in reduced MoO3. Furthermore, the 1084 cm⁻¹ peak... -1 The peak at 1358 cm⁻¹ is attributed to the stretching vibration of the Ni-O bond, indicating slight oxidation of the Ni₃N surface in air. However, no NiO diffraction peaks were observed in the XRD patterns of Ni₃N nanosheets and Ni₃N / MoO₃ core-shell arrays, suggesting that NiO is not the dominant phase in the material and therefore does not significantly affect the electrochemical performance of the samples. Correspondingly, the peak at 1358 cm⁻¹ is... -1 and 1579 cm -1 The peaks at these locations can be attributed to the symmetric and asymmetric stretching vibrations of the NO bond, which may indicate the possibility of chemical bonding between MoO3 and Ni3N.
[0031] II. Electrochemical Performance Testing Electrochemical performance was tested using an electrochemical workstation in a three-electrode system. The Ni3N and Ni3N / MoO3 electrodes were used as working electrodes in KOH electrolyte, the Ag / AgCl electrode was used as the reference electrode, and the Pt electrode was used as the counter electrode.
[0032] The cyclic voltammetry curves of Ni3N and Ni3N / MoO3 are as follows: Figure 5 As shown, both exhibit strong redox peaks, indicating that their energy storage mechanism depends on the reversible redox of Ni. The cyclic voltammetry curve area of Ni3N / MoO3 is larger than that of Ni3N, indicating that constructing the Ni3N / MoO3 heterostructure effectively improves the specific capacity.
[0033] The specific capacity of pure Ni3N electrode and Ni3N / MoO3 electrode was tested, such as... Figure 6 As shown. The results indicate that the Ni3N / MoO3 electrode at 1 A·g -1 It exhibits excellent specific capacitance of 469.5 C·g at current density. -1(130.4 mAh·g) -1 ), significantly superior to pure Ni3N electrode (175.8 C·g). -1 When the current density increases by 30 times (to 30 A·g) -1 Even at this stage, the prepared heterostructure can still maintain a high capacity of 237.6 C·g. -1 The corresponding capacity retention rate is 50.6%, which is better than the 76.5 C·g of the pure Ni3N electrode. -1 (Retention rate 43.5%).
[0034] Cyclic performance testing, such as Figure 7 As shown, the results indicate that the Ni3N / MoO3 electrode performs well at high rates (30 A·g). -1 After 7000 cycles under certain conditions, it still retains 80.8% of its initial capacity, demonstrating excellent cycle stability.
[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a high-area-capacitance electrochemical capacitor electrode, characterized in that, Includes the following steps: (1) Preparation of precursors Ni(NO3)3, NH4F and urea were dissolved in deionized water, and then nickel foam was added. After hydrothermal reaction treatment, Ni(OH)2 / nickel foam precursor was obtained. (2) Deposition of MoO3 The Ni(OH)2 / nickel foam precursor was washed and dried, and then a MoO3 thin layer was deposited on the Ni(OH)2 / nickel foam precursor by atomic layer deposition to obtain the composite precursor. (3) Nitriding treatment The composite precursor was annealed in a mixed atmosphere of NH3 and Ar to obtain a high areal capacitance electrochemical capacitor electrode.
2. The method for preparing the high areal capacitance electrochemical capacitor electrode as described in claim 1, characterized in that, In step (1), the ratio of Ni(NO3)3, NH4F, urea and deionized water is 1.5 mmol: 0.0925 g: 0.3 g: 18 mL.
3. The method for preparing the high areal capacitance electrochemical capacitor electrode as described in claim 1 or 2, characterized in that, In step (1), the hydrothermal reaction treatment temperature is 120 ℃ and the time is 6 hours.
4. The method for preparing the high areal capacitance electrochemical capacitor electrode as described in claim 1 or 2, characterized in that, In step (2), the thickness of the MoO3 thin layer is 2~4 nm.
5. The method for preparing the high areal capacitance electrochemical capacitor electrode as described in claim 1 or 2, characterized in that, In step (2), the volume ratio of NH3 to Ar is 30:70, and the gas flow rate is 100 sccm.
6. The method for preparing the high areal capacitance electrochemical capacitor electrode as described in claim 1 or 2, characterized in that, In step (2), the specific process of annealing is as follows: anneal at 350 °C for 2 hours with a heating rate of 2 °C / min, and then naturally cool to room temperature.
7. A high areal capacitance type electrochemical capacitor electrode, characterized in that, Prepared according to the preparation method described in any one of claims 1 to 6.
Citation Information
Patent Citations
NF@molybdenum oxide@nickel cobalt-LDH composite material, and preparation method and application thereof
CN113130214A
Preparation method and application of carbon nanotube / molybdenum oxide integrated array electrode material
CN113299924A
Composite material and preparation method thereof, electrode containing composite material and application
CN115739148A
Preparation method and application of molybdenum-doped nickel nitride electrode material
CN115995352A