Flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber resistant to high-temperature thermo-oxidative aging and preparation method thereof

By introducing vinyl-modified M/CeO2 nanoparticles into silicone rubber, the problems of ALSR flammability and low efficiency of traditional flame retardant methods are solved. This achieves improved flame retardant properties and heat and oxygen aging resistance of silicone rubber with low filler content, making it suitable for high temperature and high humidity environments.

CN121628385APending Publication Date: 2026-03-10SHENYANG INSTITUTE OF CHEMICAL TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610010022.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-06
Publication Date
2026-03-10

AI Technical Summary

Technical Problem

Existing addition-cured liquid silicone rubber (ALSR) is flammable, and traditional flame-retardant improvement methods suffer from low efficiency, large filler content, and damage to mechanical properties, making it difficult to maintain electrical insulation reliability in high temperature and high humidity environments.

Method used

M/CeO2 nanoparticles were prepared by using oxygen-vacancy cerium-based fillers and vinyl grafting modification. These nanoparticles were then introduced into silicone rubber at low content to form a highly efficient free radical scavenging and catalytic char formation layer, thereby improving flame retardant properties and heat and oxygen aging resistance.

Benefits of technology

It significantly improves the flame retardancy and heat and oxygen aging resistance of silicone rubber at low filler content, while maintaining good mechanical properties and processing performance, making it suitable for high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses high-temperature-resistant thermo-oxidative-aging-resistant flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber and a preparation method thereof, and relates to a silicone rubber-containing composite material and a preparation method thereof. The silicone rubber composite material comprises a silicone rubber matrix and a cerium-based composite filler dispersed in the silicone rubber matrix, the filler is M / CeO2 nanoparticles, and the M / CeO2 nanoparticles are prepared through coprecipitation and calcination; optionally, vinyl-containing siloxane is used for modifying the surface of the Vinyl-M / CeO2 material, and a vinyl-grafted Vinyl-M / CeO2 material is obtained; and finally, mixing and vulcanizing the filler with vinyl silicone oil, hydrogen-containing silicone oil, an inhibitor, a platinum catalyst, white carbon black and other components. The cerium-based filler is subjected to transition metal doping and surface modification, so that the compatibility of the cerium-based filler with a silicone rubber matrix and the participation degree of the cerium-based filler in a curing system are remarkably improved. The material shows excellent thermal stability, flame retardance and thermo-oxidative aging resistance, keeps good mechanical properties and processing fluidity, and has wide application prospects in the high-end fields of electronic packaging, new energy batteries and the like.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a kind of high molecular silicone rubber material and its preparation method, in particular to a kind of high-temperature thermal oxygen aging and flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber and its preparation method. BACKGROUND

[0002] Addition type liquid silicone rubber (ALSR) is widely used in electronic packaging, new energy battery components and aerospace fields due to its excellent weather resistance, electrical insulation performance and flexibility. However, the molecular backbone of ALSR is mainly composed of Si-O bonds and organic side chains such as methyl and phenyl groups, and its limiting oxygen index (LOI) is usually between 18% and 24%, indicating that the material is inherently flammable. Under high temperature or open flame conditions, ALSR is easily ignited and releases a large amount of heat, which poses a serious safety hazard. Therefore, improving the thermal stability and flame retardant performance of ALSR is crucial to broaden its practical application fields.

[0003] Traditional flame-retardant modification methods mainly rely on the addition of metal hydroxides such as Al(OH)3 and Mg(OH)2. This type of filler plays a flame-retardant role by decomposing heat and releasing water vapor. However, this type of flame-retardant system has obvious shortcomings: the flame-retardant efficiency is low, and more than 50 wt% is often required to achieve ideal flame-retardant effect. Such a high filling amount can severely damage the mechanical properties, processing flowability and transparency of ALSR, and also leads to increased material density and cost, limiting its application in precision packaging fields.

[0004] To overcome the limitations of traditional flame-retardant systems, researchers have developed various functional modification schemes. For example, Chinese patent application CN202511123789.4 discloses a flame-retardant tracking-resistant silicone rubber and its preparation method, which introduces nitrogen-containing organosilicon boron compounds modified layered nanomaterials to construct a composite flame-retardant system with a core-shell structure. This material maintains the good mechanical properties and processing performance of ALSR while significantly improving the flame-retardant effect and tracking-resistant performance. However, the nitrogen-containing compounds used in this technical solution may cause the hydrophobicity of the silicone rubber to decrease due to their inherent polarity, affecting the electrical insulation reliability of the material in high temperature and high humidity environments, and limiting its application in certain scenarios with strict requirements for water resistance.

[0005] In recent years, rare earth metal oxides have shown unique advantages in the field of polymer flame retardation. In particular, cerium-based materials, due to their special 4f electronic structure and controllable oxygen vacancy concentration, exhibit excellent performance in catalyzing charring and scavenging free radicals. By precisely controlling the doping ratio of transition metals, the electronic structure and surface activity can be further adjusted to enhance the interfacial interaction with the polymer matrix. The introduction of such functional fillers into the ALSR system is expected to significantly improve the flame retardation performance at very low addition levels, while maintaining the original processing performance and mechanical properties of the matrix.

[0006] Therefore, under the premise of considering processing performance and comprehensive performance, a new ALSR composite material based on oxygen vacancy-containing cerium-based fillers is developed, which simultaneously has excellent high-temperature resistance, heat-oxidation resistance, high flame retardation, and good mechanical properties. It not only has important scientific research value, but also has broad market prospects in high-end fields such as electric vehicle battery packaging, high-power integrated circuit protection, aerospace sealing systems, etc. This technical route, which realizes material performance breakthrough through nanoscale interface engineering and flame retardation mechanism innovation, will provide new ideas and directions for the development of the next generation of high-performance silicone rubber materials. SUMMARY

[0007] The present application aims to provide a high-temperature and heat-oxidation resistant and flame-retardant oxygen vacancy-containing cerium-based filler silicone rubber and a preparation method thereof. The oxygen vacancy-containing cerium-based filler has high efficiency in absorbing free radicals and catalyzing charring, and a small amount of introduction can significantly improve the high-temperature resistance, heat-oxidation resistance, and flame retardation performance of the silicone rubber. It can achieve the effect of improving the performance of ALSR without sacrificing the flowability of ALSR.

[0008] The purpose of the present application is achieved by the following technical solutions: A high-temperature and heat-oxidation resistant and flame-retardant oxygen vacancy-containing cerium-based filler silicone rubber, the material comprising a silicone rubber matrix and a cerium-based composite filler dispersed in the silicone rubber matrix, the cerium-based composite filler being M / CeO2 nanoparticles with oxygen vacancies, wherein M is at least one metal selected from Mn, Fe, Co, Ni, Zr, Hf, Cu, and La; the theoretical molar ratio of M to Ce in the M / CeO2 nanoparticles is 0.05:1 to 2:1; the surface of the M / CeO2 nanoparticles is modified with a silane coupling agent containing an unsaturated bond.

[0009] The high-temperature and heat-oxidation resistant and flame-retardant oxygen vacancy-containing cerium-based filler silicone rubber, the silane coupling agent containing an unsaturated bond is selected from at least one of vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltris(2-methoxyethoxy)silane.

[0010] The high-temperature thermal oxidation aging resistant and flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber, the silicone rubber matrix is any one of addition type silicone rubber, condensation type silicone rubber or peroxide vulcanized type silicone rubber.

[0011] The high-temperature thermal oxidation aging resistant and flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber, when the silicone rubber matrix is addition type silicone rubber, components of the composite material are as follows in mass fraction: vinyl terminated polysiloxane 100 mass fraction; reinforcing filler 20-40 mass fraction; hydrogen-containing silicone oil 0.5-10 mass fraction; platinum catalyst 0.1-5 mass fraction; and cerium-based composite filler 0.5-2 mass fraction.

[0012] The high-temperature thermal oxidation aging resistant and flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber, the content of the cerium-based composite filler in the composite material is 0.1-10 mass fraction, based on 100 mass fraction of raw silicone rubber.

[0013] A high-temperature thermal oxidation aging resistant and flame-retardant oxygen-containing vacancy cerium-based filler silicone rubber preparation method, the method comprises the following preparation steps: (1) the molar ratio of fixed transition metal M and cerium (Ce) is 0.1-1:1, wherein M is one of Mn, Fe, Co, Ni, Zr, Hf, Cu and La; the transition metal salt solution is mixed with the cerium nitrate solution, continuously stirred at room temperature for 1 h; in the stirring process, a certain concentration of alkali solution is slowly added, after the addition is completed, the reaction is continued for 3 h, and then it is left for 2-5 h; after the reaction is completed, the mixture is suction filtered, washed until the filtrate is neutral (pH=7), the obtained solid is dried in a blast drying oven at 80 ℃ for 12 h, and then calcined at 400-700 ℃ for 2-3 h, to obtain M / CeO2 nanoparticles; (2) the M / CeO2 nanoparticles obtained in step (1) are dispersed in an alcohol solvent, ultrasonic treatment is carried out for 0.5-1 h to make them uniformly dispersed; at the same time, vinyl-containing siloxane, alcohol solvent, deionized water and catalyst are placed in a three-necked flask, hydrolysis is carried out at 40 ℃ for 1-1.5 h; then, the dispersed M / CeO2 nanoparticle alcohol solution is added to the three-necked flask, under the protection of inert gas, the temperature is raised to 90 ℃ and the reaction is carried out for 2-4 h, after the reaction is completed, it is left for 30 min; the product is suction filtered, washed until neutral, then washed with alcohol solvent for 3-5 times, and finally dried in a blast drying oven at 70 ℃ for 12 h, to obtain vinyl grafted Vinyl-M / CeO2 material; (3) mixing the vinyl silicone oil (100 phr), the hydrogen-containing silicone oil (1-3 phr), the inhibitor (0.1-1 phr), the organic platinum catalyst (0.1-1 phr), the white carbon black (20-40 phr) and the Vinyl-M / CeO2 material obtained in step (2) (0.5-2 phr) in a three-roll mill at room temperature for 0.5-1.5 h; placing the mixed rubber in a flat vulcanizing machine for one-stage vulcanization, and then transferring the sample into a blast oven for two-stage vulcanization to obtain the silicone rubber containing the oxygen vacancy cerium-based filler.

[0014] In step (1), the suitable transition metal salt includes but is not limited to the following water-soluble salts: manganese (such as manganese chloride, manganese sulfate, manganese acetate), iron (such as ferrous sulfate, ferrous chloride, iron nitrate), cobalt (such as cobalt chloride, cobalt nitrate, cobalt acetate), nickel (such as nickel sulfate, nickel nitrate, nickel chloride), zirconium (such as zirconium oxychloride, zirconyl nitrate), hafnium (such as hafnium sulfate, hafnium nitrate), copper (such as copper sulfate, copper nitrate, copper chloride) and lanthanum (such as lanthanum chloride, lanthanum nitrate, lanthanum acetate); The alkali solution is one of sodium hydroxide, sodium carbonate and sodium bicarbonate; The concentration of the transition metal salt solution and the cerium nitrate solution is independently 0.1-1.0 mol / L; The concentration of the sodium hydroxide solution is 1-3 mol / L; The concentration of the sodium hydroxide solution is 1.2-2 mol / L.

[0015] In step (1), the calcination process is carried out in an air atmosphere or a nitrogen atmosphere; the heating rate of calcination is 1-5 ℃ / min.

[0016] In step (2), the alcohol solvent is at least one of methanol, ethanol and isopropanol; the mass ratio of the M / CeO2 nanoparticles to the alcohol solvent is 1:(8-15); The vinyl-containing siloxane is at least one of vinyltrimethoxysilane, vinyltriethoxysilane and vinyltris(2-methoxyethoxy)silane; The catalyst is an acidic catalyst; the acidic catalyst is at least one of hydrochloric acid, nitric acid, sulfuric acid, acetic acid (glacial acetic acid) and formic acid; the acidic catalyst is acetic acid (glacial acetic acid); The mass ratio of the M / CeO2 nanoparticles, the vinyl-containing siloxane, the alcohol solvent, the deionized water and the catalyst is 1: (0.01-0.05): (8-12): (0.2-0.5): (0.0005-0.002); the mass ratio of the M / CeO2 nanoparticles, the vinyl-containing siloxane, the alcohol solvent, the deionized water and the catalyst is 1: (0.013-0.02): (9-11): (0.3-0.4): (0.0007-0.001); the pH value of the hydrolysis process is controlled between 4 and 5; and the inert gas is nitrogen or argon.

[0017] The inhibitor in step (3) is one of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol and 3,5-dimethyl-1-hexyn-3-ol. The organic platinum catalyst is defined as a commercial dilute solution with a platinum content of about 3000 ppm, and the types thereof include a divinyltetramethyldisiloxane platinum complex or a 3-methyl-1-butyn-3-ol platinum complex. The mixing process is carried out in two steps: first, the vinyl silicone oil, the hydrogen-containing silicone oil, the inhibitor, the white carbon black and the Vinyl-M / CeO2 material are premixed for 5-10 min, and then the organic platinum catalyst is added for mixing for 0.5-1.5 h. The vulcanization process adopts two-stage vulcanization: the first stage is hot pressing at 120-150 DEG C and 8 MPa for 10-30 min (one-stage vulcanization); and then the sample is placed in a blast drying oven at 150-200 DEG C for baking for 1-2 h (two-stage vulcanization).

[0018] The present application has the following advantages: The oxygen-containing vacancy cerium-based filler silicone rubber provided by the present application has excellent processing performance, outstanding high-temperature resistance, excellent heat-oxygen aging resistance, significant flame retardation effect and high mechanical property retention rate, and has broad application prospects in high-temperature, heat-oxygen aging and flame retardation related application fields.

[0019] Specifically: (1) The present application modifies the oxygen-containing vacancy cerium-based filler by vinyl grafting, and introduces it into the ALSR curing system, thereby effectively improving the compatibility and interface bonding force between the filler and the matrix. The filler has multiple functions of removing free radicals, adsorbing gaseous decomposition products and catalyzing the formation of a dense carbon layer, thereby fully playing a synergistic protection role in the ALSR system.

[0020] (2) The functional filler in the silicone rubber is introduced in a very low amount (only 1-2 parts), and significant performance improvement can be achieved, which embodies high functional efficiency, is an effective strategy to achieve a good balance between material performance and processing fluidity, and greatly expands the applicability of ALSR in high temperature and flame retardant fields.

[0021] (3) The preparation method provided by the application has simple process, easily available raw materials, controllable operation conditions, good potential for large-scale production, and is suitable for industrialization promotion and application. BRIEF DESCRIPTION OF DRAWINGS

[0022] Figure 1 XRD spectra of Co / CeO2 in Example 1 and CeO2 in Comparative Example 2; Figure 2 FTIR spectra of Co / CeO2 and Vinyl-Co / CeO2 in Example 1; Figure 3 Filler dispersion comparison photos of silicone rubber in Example 1 and Comparative Example 3; Figure 4 Actual photos of silicone rubber in Example 1, Comparative Example 1 and Comparative Example 2 after cone calorimeter test. DETAILED DESCRIPTION

[0023] The application will be described in detail below in combination with specific drawings and examples. It is necessary to point out here that the following examples are only used to further illustrate the application, and the implementation of the application is not limited by the following examples. Any changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and principles of the application shall be equivalent replacement methods and shall be included in the protection scope of the application.

[0024] The raw materials used in the examples are all conventional commercially available raw materials. The test analysis methods used in the following examples are as follows: X-ray diffractometer was used to perform powder X-ray diffraction (XRD) characterization of the sample. The specific experimental parameters are as follows: (1) Cu-Ka1 target was selected; (2) the incident wavelength was l=0.154 nm; (3) the tube voltage was 40 kV; (4) the tube current was 40 mA; (5) the scanning range was 20°-90°.

[0025] FT-IR analysis: The sample was mixed with potassium bromide at a ratio of 1:10, and a spectrometer was used for analysis.

[0026] Cone calorimeter was used for cone calorimeter test, and 100mmx100mmx4mm sample was determined according to ISO5660 standard, and the external heat radiation intensity used was 45 kW / m2.

[0027] TG test (conventional, prior art general): under nitrogen atmosphere, initial equilibrium temperature 30°C, temperature ramp to 800°C at 10°C / min.

[0028] The thermal aging performance of the material was tested as follows: the sample was aged at 250°C for 60 hours, and then its mechanical properties were tested in accordance with ISO 37.

[0029] Example 1: (1) 0.5 mol / L Co(NO3)2·6H2O solution (50 mL) and 0.5 mol / L Ce(NO3)3·6H2O aqueous solution (100 mL) were mixed to establish a theoretical Co / Ce molar ratio of 0.5:1. Subsequently, the mixture was continuously stirred at room temperature for 1 h. While continuing to stir vigorously, 134 mL of 1.5 mol / L NaOH solution was gradually added to the mixture. After the addition was completed, the stirring was continued for 3 h, and then the mixture was allowed to stand for 2 h. The resulting mixture was filtered through a vacuum filtration system and washed thoroughly until the solution pH reached 7. The resulting sample was then dried at 80°C for 12 h and calcined at 600°C for 2 h to obtain Co / CeO2 nanoparticles.

[0030] (2) 3 g of Co / CeO2 nanoparticles were ultrasonically treated in 30 mL of anhydrous ethanol at room temperature for 30 min. Meanwhile, vinyltrimethoxysilane (0.05 g), anhydrous ethanol (30 g), deionized water (0.7 g), and glacial acetic acid (0.02 g) were placed in a three-necked flask and hydrolyzed at 40°C for 1 h, with the pH controlled between 4-5 throughout the process; then the dispersed Co / CeO2 nanoparticle ethanol solution was added to the three-necked flask, which was heated to 90°C under nitrogen protection and reacted for 3 h. After the reaction was completed, the mixture was allowed to stand for 30 min; the product was suction filtered, washed to neutral, and then washed with anhydrous ethanol for 3 times. Finally, the product was dried in a 70°C air-draft drying oven for 12 h to obtain a vinyl-grafted Vinyl-Co / CeO2 material.

[0031] (3) First, the vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1.4 phr), 1-ethynyl-1-cyclohexanol (0.5 phr), white carbon black (40 phr), and Vinyl-Co / CeO2 material obtained in step (2) (1 phr) were pre-mixed on a three-roll mill for 10 min, and then divinyltetramethyldisiloxane platinum complex (0.5 phr) was added and mixed for 0.5 h; the mixed rubber was placed in a flat vulcanizing machine and vulcanized at 140°C and 8 MPa for 20 min, and then the sample was transferred to an air-draft oven and baked at 180°C for 1 h to obtain the Vinyl-Co / CeO2 filler-containing silicone rubber.

[0032] Example 2: The difference between this example and Example 1 is that in step (2), ethenyltris(2-methoxyethoxy)silane is used instead of ethenyltrimethoxysilane for the hydrolysis and grafting reaction.

[0033] The specific steps are as follows: 3 g of Co / CeO2 nanoparticles were ultrasonically treated in 30 mL of anhydrous ethanol at room temperature for 30 min. Meanwhile, ethenyltris(2-methoxyethoxy)silane (0.095 g), anhydrous ethanol (57 g), deionized water (1.3 g), and glacial acetic acid (0.03 g) were placed in a three-necked flask and hydrolyzed at 40 °C for 1 h, with the pH controlled between 4 and 5 throughout the process; then the dispersed Co / CeO2 nanoparticle ethanol solution was added to the three-necked flask, which was heated to 90 °C under nitrogen protection and reacted for 3 h, after which it was allowed to stand for 30 min; the product was suction filtered, washed to neutral, washed with anhydrous ethanol three times, and finally dried in a 70 °C blast drying oven for 12 h to obtain the vinyl-grafted Vinyl-Co / CeO2 material.

[0034] The remaining steps, including the preparation of the filler in step (1) and the silicone rubber compounding in step (3), are the same as in Example 1.

[0035] Example 3: The difference between this example and Example 1 is that in step (3), the amount of Vinyl-Co / CeO2 material obtained in step (2) introduced is increased from 1 phr to 2 phr.

[0036] Specifically, first, the vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1.4 phr), 1-ethynyl-1-cyclohexanol (0.5 phr), white carbon black (40 phr), and Vinyl-Co / CeO2 material obtained in step (2) (2 phr) were pre-mixed on a three-roll mill for 10 min, then divinyltetramethyldisiloxane platinum complex (0.5 phr) was added and mixed for 0.5 h; the mixed rubber was placed in a flat vulcanizing machine and vulcanized at 140 °C and 8 MPa for 20 min, then the sample was transferred to a blast oven and baked at 180 °C for 1 h to obtain the silicone rubber containing high content of Vinyl-Co / CeO2 filler.

[0037] The remaining steps, including the preparation of the filler in step (1) and the surface modification in step (2), are the same as in Example 1.

[0038] Example 4: The difference between this example and Example 1 is that in step (3), the amount of Vinyl-Co / CeO2 material obtained in step (2) introduced is reduced from 1 phr to 0.5 phr.

[0039] Specifically, first, vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1.4 phr), 1-ethynyl-1-cyclohexanol (0.5 phr), white carbon black (40 phr), and the Vinyl-Co / CeO2 material obtained in step (2) (0.5 phr) were placed on a three-roll mill for premixing for 10 min, then divinyltetramethyldisiloxane platinum complex (0.5 phr) was added and mixed for 0.5 h; the mixed rubber was placed in a flat vulcanizing machine and vulcanized at 140 ℃ and 8 MPa for 20 min, then the sample was transferred to a blast oven and baked at 180 ℃ for 1 h, thereby obtaining the silicone rubber containing a high content of the Vinyl-Co / CeO2 filler.

[0040] The remaining steps, including the preparation of the filler in step (1) and the surface modification in step (2), were the same as in Example 1. Example 5

[0041] The difference between this example and Example 1 is that in step (1), the 0.5 mol / L Co(NO3)2·6H2O solution (50 mL) was replaced with a 0.1 mol / L Co(NO3)2·6H2O solution (50 mL) to establish a theoretical Co / Ce molar ratio of 0.1:1. The amount of the 1.5 mol / L NaOH solution was adjusted to 117 mL to maintain the alkalinity required for coprecipitation.

[0042] The remaining steps, including the vinyl grafting in step (2) and the silicone rubber compounding in step (3), were the same as in Example 1. Example 6

[0043] The difference between this example and Example 1 is that in step (1), the 0.5 mol / L Co(NO3)2·6H2O solution (50 mL) was replaced with a 0.1 mol / L Co(NO3)2·6H2O solution (50 mL) to establish a theoretical Co / Ce molar ratio of 0.1:1. The amount of the 1.5 mol / L NaOH solution was adjusted to 117 mL to maintain the alkalinity required for coprecipitation.

[0044] Step (2) was exactly the same as in Example 1, using vinyltrimethoxysilane for grafting, and finally obtaining a Vinyl-Mn / CeO2 material.

[0045] Step (3) was exactly the same as in Example 1, using 1 phr of the Vinyl-Mn / CeO2 material to prepare silicone rubber. Example 7

[0046] The difference between this example and Example 1 is that in step (1), 0.5 mol / L Fe(N03)2-9H20 solution (50 mL) is used instead of Co(N03)2-6H20 solution, mixed with 0.5 mol / L Ce(N03)3-6H20 aqueous solution (100 mL) to establish a theoretical Fe / Ce molar ratio of 0.5:1. The amount of 1.5 mol / L NaOH solution added is maintained at 134 mL.

[0047] Step (2) is exactly the same as Example 1, using vinyltrimethoxysilane for grafting, and finally obtaining Vinyl-Fe / Ce02 material.

[0048] Step (3) is exactly the same as Example 1, using 1 phr of Vinyl-Fe / Ce02 material to prepare silicone rubber. Example 8

[0049] The difference between this example and Example 1 is that in step (1), 0.5 mol / L Ni(N03)2-6H20 solution (50 mL) is used instead of Co(N03)2-6H20 solution, mixed with 0.5 mol / L Ce(N03)3-6H20 aqueous solution (100 mL) to establish a theoretical Ni / Ce molar ratio of 0.5:1. The amount of 1.5 mol / L NaOH solution added is maintained at 134 mL.

[0050] Step (2) is exactly the same as Example 1, using vinyltrimethoxysilane for grafting, and finally obtaining Vinyl-Ni / Ce02 material.

[0051] Step (3) is exactly the same as Example 1, using 1 phr of Vinyl-Ni / Ce02 material to prepare silicone rubber. Example 9

[0052] The difference between this example and Example 1 is that in step (1), 0.5 mol / L ZrOCl2-8H20 solution (50 mL) is used instead of Co(N03)2-6H20 solution, mixed with 0.5 mol / L Ce(N03)3-6H20 aqueous solution (100 mL) to establish a theoretical Zr / Ce molar ratio of 0.5:1. The amount of 1.5 mol / L NaOH solution added is maintained at 134 mL. The standing time of 2 h is extended to 4 h.

[0053] Step (2) is identical to Example 1, using vinyltrimethoxysilane for grafting, resulting in a Vinyl-Zr / CeO2 material.

[0054] Step (3) is identical to Example 1, using 1 phr of the Vinyl-Zr / CeO2 material for the preparation of the silicone rubber.

[0055] Example 10: The difference between this example and Example 1 is that in Step (1), a 0.5 mol / L solution of HfOCl2·8H2O (50 mL) is used instead of the Co(NO3)2·6H2O solution, mixed with a 0.5 mol / L aqueous solution of Ce(NO3)3·6H2O (100 mL), establishing a theoretical Hf / Ce molar ratio of 0.5 : 1. The amount of 1.5 mol / L NaOH solution added is maintained at 134 mL. The 2 h standing time is extended to 4 h.

[0056] Step (2) is identical to Example 1, using vinyltrimethoxysilane for grafting, resulting in a Vinyl-Hf / CeO2 material.

[0057] Step (3) is identical to Example 1, using 1 phr of the Vinyl-Hf / CeO2 material for the preparation of the silicone rubber.

[0058] Example 11: The difference between this example and Example 1 is that in Step (1), a 0.5 mol / L solution of Cu(NO3)2·3H2O (50 mL) is used instead of the Co(NO3)2·6H2O solution, mixed with a 0.5 mol / L aqueous solution of Ce(NO3)3·6H2O (100 mL), establishing a theoretical Cu / Ce molar ratio of 0.5 : 1. The amount of 1.5 mol / L NaOH solution added is maintained at 134 mL.

[0059] Step (2) is identical to Example 1, using vinyltrimethoxysilane for grafting, resulting in a Vinyl-Cu / CeO2 material.

[0060] Step (3) is identical to Example 1, using 1 phr of the Vinyl-Cu / CeO2 material for the preparation of the silicone rubber.

[0061] Example 12: The difference between this embodiment and Example 1 is that in step (1), a 0.5 mol / L La(NO3)3·6H2O solution (25 mL) is used instead of the Co(NO3)2·6H2O solution, and mixed with a 0.5 mol / L Ce(NO3)3·6H2O aqueous solution (100 mL) to establish a theoretical La / Ce molar ratio of 0.25:1. The amount of 1.5 mol / L NaOH solution added is changed to 125 mL.

[0062] Step (2) is exactly the same as in Example 1, using vinyltrimethoxysilane for grafting, and finally obtaining Vinyl-La / CeO2 material.

[0063] Step (3) is exactly the same as in Example 1, using 1 phr of Vinyl-La / CeO2 material to prepare silicone rubber.

[0064] Comparative Example 1: This comparative example provides a pure silicone rubber without any added functional fillers as a benchmark for performance comparison.

[0065] By weight (phr), vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1.4 phr), 1-ethynyl-1-cyclohexanol (0.5 phr), silica (40 phr), and the Vinyl-Co / CeO2 material (1 phr) obtained in step (2) were first premixed on a three-roll mill for 10 min, and then divinyltetramethyldisiloxane platinum complex (0.5 phr) was added and mixed for 0.5 h. The mixed rubber was placed in a flat vulcanizing machine and vulcanized at 140 ℃ and 8 MPa for 20 min. Then the sample was transferred to a forced-air oven and baked at 180 ℃ for 1 h to obtain the pure silicone rubber.

[0066] Comparative Example 2: This comparative example is used to illustrate the performance differences between a single CeO2 filler and the M / CeO2 composite filler of the present invention.

[0067] (1) Preparation of CeO2 nanoparticles: 150 mL of 0.5 mol / L Ce(NO3)3·6H2O aqueous solution was stirred at room temperature, and 201 mL of 1.5 mol / L NaOH solution was gradually added. The subsequent stirring, standing, filtering, washing, drying and calcination steps were the same as step (1) in Example 1 to obtain pure CeO2 nanoparticles.

[0068] (2) Preparation of Vinyl-CeO2 material: Using 3g of the above CeO2 nanoparticles, the surface modification steps are exactly the same as step (2) in Example 1 to obtain Vinyl-CeO2 material.

[0069] (3) Silicone rubber composite: The steps are exactly the same as step (3) in Example 1, and silicone rubber is prepared using 1 phr Vinyl-CeO2 material.

[0070] Comparative Example 3: This comparative example is used to illustrate the effect of fillers without surface modification on the properties of silicone rubber.

[0071] Preparation of Co / CeO2 nanoparticles: The steps are exactly the same as step (1) in Example 1.

[0072] (2) Step (2) of Example 1 is omitted, and the surface of Co / CeO2 nanoparticles is not modified.

[0073] (3) Silicone rubber compound: By weight (phr), vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1.4 phr), 1-ethynyl-1-cyclohexanol (0.5 phr), silica (40 phr) and Co / CeO2 nanoparticles (1 phr) obtained in step (1) were placed on a three-roll mill and premixed for 10 min. Then, divinyltetramethyldisiloxane platinum complex (0.5 phr) was added and mixed for 0.5 h. The compound was placed in a flat vulcanizing machine and vulcanized at 140 ℃ and 8 MPa for 20 min. Then, the sample was transferred to a forced-air oven and baked at 180 ℃ for 1 h to obtain the silicone rubber containing unmodified Co / CeO2 filler.

[0074] Table 1 compares the high-temperature resistance, heat aging resistance, and flame retardant properties of silicone rubber in Examples 1, 3-11, and Comparative Examples 1-3.

[0075] XRD and FTIR characterization were used to verify the consistency between the synthesized product and the expected structure. XRD patterns showed that the diffraction peaks of CeO2 matched the standard card (PDF: 34-0394), confirming the successful construction of the fluorite structure. In the Co / CeO2 sample, although diffraction peaks of Co3O4 (PDF: 74-1656) appeared, the main CeO2 phase was still maintained. Further analysis of the (111) crystal plane revealed that the diffraction peak intensity of Co / CeO2 was significantly lower than that of pure CeO2, indicating that Co had been incorporated into the CeO2 lattice, forming a Co–O–Ce solid solution structure with oxygen vacancies. In the FTIR spectrum, the modified Vinyl-Co / CeO2 showed a distinct CH=CH2 characteristic absorption peak at 1413 cm⁻¹, proving that the vinyl group had been successfully grafted. When introduced into the silicone rubber system, a significant improvement in the dispersion of Vinyl-Co / CeO2 in the matrix was observed, and the agglomeration phenomenon was significantly reduced (see [link]). Figure 3 ).

[0076] High-temperature resistance, thermo-oxidative aging resistance, and flame retardancy tests show that the cerium-based filler with oxygen vacancies can efficiently promote free radical capture, adsorption of gas-phase decomposition products, and catalyze the formation of a dense protective char layer. Even at low addition levels, it can significantly improve the heat resistance, thermo-oxidative aging resistance, and flame retardancy rating of silicone rubber (see [reference]). Figure 4 (and Table 1).

[0077] Table 1 compares the high-temperature resistance, heat aging resistance, and flame retardant properties of silicone rubber in Examples 1, 3-11, and Comparative Examples 1-3.

[0078] .

Claims

1. A high temperature heat-oxygen aged and flame retardant oxygen containing voided cerium based filler silicone rubber, characterized in that, The material comprises a silicone rubber matrix and a cerium-based composite filler dispersed in the silicone rubber matrix, the cerium-based composite filler being M / CeO2 nanoparticles with oxygen vacancies, wherein M is at least one metal selected from Mn, Fe, Co, Ni, Zr, Hf, Cu and La; the theoretical molar ratio of M to Ce in the M / CeO2 nanoparticles is 0.05:1 to 2:1; and the surface of the M / CeO2 nanoparticles is modified by a silane coupling agent containing an unsaturated bond.

2. A high temperature heat aged and flame retardant oxygen containing vacancy ceria based filler silicone rubber according to claim 1, characterized in that, The silane coupling agent containing an unsaturated bond is at least one selected from vinyltrimethoxysilane, vinyltriethoxysilane and vinyltris(2-methoxyethoxy)silane.

3. A high temperature heat and oxidative aging resistant and flame retardant oxygen containing vacant ceria based filler silicone rubber according to claim 1, characterized in that, The silicone rubber matrix is any one of an addition type silicone rubber, a condensation type silicone rubber or a peroxide vulcanization type silicone rubber.

4. A high temperature heat aged and flame retardant oxygen containing vacancy ceria based filler silicone rubber as claimed in claim 1, wherein, When the silicone rubber matrix is an addition type silicone rubber, the components of the composite material are as follows in parts by mass: 100 parts by mass of a vinyl-terminated polysiloxane; 20 to 40 parts by mass of a reinforcing filler; 0.5 to 10 parts by mass of a hydrogen-containing silicone oil; 0.1 to 5 parts by mass of a platinum-based catalyst; and 0.5 to 2 parts by mass of the cerium-based composite filler.

5. A high temperature heat and oxygen aging resistant and flame retardant oxygen containing vacant cerium based filler silicone rubber according to claim 1, characterized in that, The content of the cerium-based composite filler in the composite material is 0.1 to 10 parts by mass, based on 100 parts by mass of raw silicone rubber.

6. A process for the preparation of a high temperature heat and oxygen aged and flame retardant oxygen containing voided ceria based filler silicone rubber, characterized in that, The method comprises the following preparation steps: (1) The molar ratio of a transition metal M to cerium (Ce) is fixed at 0.1 to 1:1, wherein M is one of Mn, Fe, Co, Ni, Zr, Hf, Cu and La; a transition metal salt solution is mixed with a cerium nitrate solution, and stirring is continued at room temperature for 1 h; during the stirring, a certain concentration of an alkali solution is slowly added dropwise, and after the dropwise addition is completed, the reaction is continued for 3 h, and then the mixture is left to stand for 2-5 h; after the reaction is completed, the mixture is suction filtered, washed until the filtrate is neutral (pH=7), the obtained solid is dried in a blast drying oven at 80 ℃ for 12 h, and then calcined at 400-700 ℃ for 2-3 h to obtain M / CeO2 nanoparticles; (2) The M / CeO2 nanoparticles obtained in step (1) are dispersed in an alcohol solvent, and ultrasonic treatment is performed for 0.5-1 h to make them uniformly dispersed; at the same time, a vinyl-containing siloxane, an alcohol solvent, deionized water and a catalyst are placed in a three-necked flask, and hydrolysis is performed at 40 ℃ for 1-1.5 h; then, the dispersed M / CeO2 nanoparticle alcohol solution is added to the three-necked flask, and under the protection of an inert gas, the temperature is raised to 90 ℃ and the reaction is performed for 2-4 h, and after the reaction is completed, the mixture is left to stand for 30 min; the product is suction filtered, washed until neutral, and then washed with an alcohol solvent for 3-5 times, and finally dried in a blast drying oven at 70 ℃ for 12 h to obtain a vinyl-grafted Vinyl-M / CeO2 material. (3) mixing vinyl silicone oil (100 phr), hydrogen-containing silicone oil (1-3 phr), inhibitor (0.1-1 phr), organic platinum catalyst (0.1-1 phr), white carbon black (20-40 phr) and the Vinyl-M / CeO2 material obtained in step (2) (0.5-2 phr) by weight parts (phr) on a three-roll mill at room temperature for 0.5-1.5 h; the mixing rubber is placed in a flat vulcanizing machine for one-stage vulcanization, and then the sample is transferred into a blast oven for two-stage vulcanization to obtain the silicone rubber containing the oxygen vacancy cerium-based filler.

7. The method for preparing a high-temperature hot-oxygen aging and flame-retardant oxygen-containing ceria-based filler silicone rubber according to claim 6, characterized in that, In step (1), the suitable transition metal salt includes but is not limited to the following water-soluble salts: manganese (such as manganese chloride, manganese sulfate, manganese acetate), iron (such as ferrous sulfate, ferrous chloride, iron nitrate), cobalt (such as cobalt chloride, cobalt nitrate, cobalt acetate), nickel (such as nickel sulfate, nickel nitrate, nickel chloride), zirconium (such as zirconium oxychloride, zirconyl nitrate), hafnium (such as hafnium sulfate, hafnium nitrate), copper (such as copper sulfate, copper nitrate, copper chloride) and lanthanum (such as lanthanum chloride, lanthanum nitrate, lanthanum acetate); The alkali solution is one of sodium hydroxide, sodium carbonate and sodium bicarbonate; The concentration of the transition metal salt solution and the cerium nitrate solution is independently 0.1-1.0 mol / L; The concentration of the sodium hydroxide solution is 1-3 mol / L; The concentration of the sodium hydroxide solution is 1.2-2 mol / L.

8. The method for preparing a high-temperature hot-oxygen aging and flame-retardant oxygen-containing ceria-based filler silicone rubber according to claim 6, characterized in that, In step (1), the calcination process is carried out in an air atmosphere or a nitrogen atmosphere; the heating rate of calcination is 1-5 ℃ / min.

9. The method of claim 6, wherein the method is characterized by, In step (2), the alcohol solvent is at least one of methanol, ethanol and isopropanol; the mass ratio of the M / CeO2 nanoparticles to the alcohol solvent is 1:(8-15); The vinyl-containing siloxane is at least one of vinyltrimethoxysilane, vinyltriethoxysilane and vinyltris(2-methoxyethoxy)silane; The catalyst is an acidic catalyst; the acidic catalyst is at least one of hydrochloric acid, nitric acid, sulfuric acid, acetic acid (glacial acetic acid) and formic acid; the acidic catalyst is acetic acid (glacial acetic acid); The mass ratio of the M / CeO2 nanoparticles, the vinyl-containing siloxane, the alcohol solvent, the deionized water and the catalyst is 1:(0.01-0.05):(8-12):(0.2-0.5):(0.0005-0.002); the mass ratio of the M / CeO2 nanoparticles, the vinyl-containing siloxane, the alcohol solvent, the deionized water and the catalyst is 1:(0.013-0.02):(9-11):(0.3-0.4):(0.0007-0.001); the pH value of the hydrolysis process is controlled between 4 and 5; the inert gas is nitrogen or argon.

10. The method of claim 6, wherein the method is characterized by, In step (3), the inhibitor is one of 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol and 3,5-dimethyl-1-hexyn-3-ol. The organic platinum catalyst is defined as a commercial dilute solution with a platinum content of about 3000 ppm, including divinyltetramethyldisiloxane platinum complex or 3-methyl-1-butyne-3-ol platinum complex; The mixing process is carried out in two steps: first, the vinyl silicone oil, hydrogen-containing silicone oil, inhibitor, white carbon black and Vinyl-M / CeO2 material are premixed for 5-10 min, and then the organic platinum catalyst is added for mixing for 0.5-1.5 h; The vulcanization process adopts two-stage vulcanization: the first stage is hot pressing at 120-150 ℃ and 8 MPa for 10-30 min (one-stage vulcanization); then the sample is baked in a blast drying oven at 150-200 ℃ for 1-2 h (two-stage vulcanization).

Citation Information

Patent Citations

  • Flame-retardant tracking-resistant silicone rubber as well as preparation method and application thereof

    CN120944363A