A UV grain boundary diffusion coating and process for sintering NdFeB magnets
By using a composite binder system of low-functionality UV monomers and high-functionality UV resins, along with a nanofiller support framework, the problems of storage agglomeration and heat treatment detachment of UV grain boundary diffusion coatings were solved, achieving deep curing and efficient diffusion, and improving the coercivity of magnets.
Patent Information
- Application Number
- CN202511797578.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-12-02
AI Technical Summary
Existing UV grain boundary diffusion coatings are prone to clumping during storage, making it difficult for UV light to penetrate and causing false curing of the surface layer. The coating is also prone to peeling off during heat treatment, affecting the diffusion effect and magnetic properties.
A composite binder system consisting of low-functionality UV monomers and high-functionality UV resins, combined with nanofillers and composite photoinitiators, is designed with a low-temperature degradation heat treatment stage through UV curing under high shear dispersion and low oxygen environment to form a supporting skeleton and ensure that the coating adheres firmly during the heat treatment process.
It achieves long-term storage stability of the coating, thorough deep curing and excellent heat treatment adhesion, and improves the coercivity and diffusion efficiency of sintered NdFeB magnets.
Smart Images

Figure CN121699482B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth permanent magnet material manufacturing technology, specifically to a UV-cured grain boundary diffusion coating and process for improving the coercivity of sintered NdFeB magnets. Background Technology
[0002] Sintered NdFeB magnets are widely used due to their excellent magnetic properties. To meet the demands of high-temperature applications, grain boundary diffusion technology is typically used to improve their coercivity. The key to this technology lies in uniformly coating the magnet surface with heavy rare earth elements (such as Tb, Dy) or other alloying elements, and then using heat treatment to diffuse them along the grain boundaries into the magnet's interior. Existing technologies commonly employ electroplating, sputtering, spraying, or printing for coating. Among these, UV-cured coatings combined with screen printing show promise due to their high efficiency, good coating uniformity, and significantly improved magnetic properties compared to thermosetting. However, this technological approach faces several significant challenges in practical applications: Poor coating stability: Due to the extremely high content of diffusion alloy powder (such as PrTbCuAlGa and other highly active alloys, usually >75wt%), it is easy to react with the active functional groups (such as hydroxyl-OH, carbon-carbon double bonds, etc.) in UV resin or monomers, or due to its high density and high surface energy, the UV components will polymerize and encapsulate the powder, causing the coating to gel and clump during storage or use, making it unsuitable for continuous production.
[0003] UV curing defects: High levels of metal alloy powder have a strong shielding and reflective effect on UV light, preventing UV rays from penetrating deep into the coating. This causes a "false surface curing" phenomenon—the surface cures to form a hard shell, while the interior remains liquid. In subsequent processing, this surface layer will peel, warp, or even detach.
[0004] Coating peeling during heat treatment: During the diffusion stage, the organic binder (UV resin / monomer) needs to be thermally decomposed and volatilized. If the decomposition process is not matched with the melting / diffusion process of the alloy, or if the decomposition products cause a sharp increase in internal stress in the coating, the coating may peel off from the substrate before the critical diffusion temperature, resulting in diffusion source failure and process failure.
[0005] Therefore, developing a UV grain boundary diffusion coating and its supporting process that is stable in storage, can be deeply cured, and can firmly adhere to the surface during heat treatment until effective diffusion is achieved is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] The primary technical objective of this invention is to overcome the shortcomings of the prior art and provide a UV grain boundary diffusion coating for sintering NdFeB magnets that exhibits good storage stability, thorough curing, and strong adhesion during heat treatment.
[0007] The second technical objective of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a UV grain boundary diffusion coating for sintering NdFeB magnets that has good storage stability, complete curing, and strong adhesion during heat treatment.
[0008] The third technical objective of this invention is to overcome the shortcomings of the prior art and provide a coating process for a UV grain boundary diffusion coating for sintering NdFeB magnets that has good storage stability, complete curing, and strong adhesion during heat treatment.
[0009] The fourth technical objective of this invention is to overcome the shortcomings of the prior art and provide a diffusion process for a UV grain boundary diffusion coating for sintering NdFeB magnets that has good storage stability, complete curing, and strong adhesion during heat treatment.
[0010] The first technical objective of this invention is achieved through the following technical solution: A UV grain boundary diffusion coating for sintered NdFeB magnets, comprising, by weight: Diffusion alloy powder: 60-85 parts; UV-curable binder system: 12-25 parts; functional filler: 2-8 parts; additives: 1-5 parts; the diffusion alloy includes PrNdMCuAlGa; the UV-curable binder system includes: low-functionality UV monomer: 5%-10% of the total weight of the coating; and high-functionality UV resin: 5%-12% of the total weight of the coating; and composite photoinitiator system: 0.5%-3% of the total weight of UV resin and UV monomer; this system is composed of a pyrolysis-type photoinitiator and a hydrogen-abstraction-type photoinitiator; the mass ratio of the two is 1:(0.8-1.5).
[0011] Preferably, the UV grain boundary diffusion coating comprises the following components by weight percentage: Diffusion alloy powder: 60% ~ 85%; UV-curable adhesive system: 12% ~ 25%; functional filler: 2% ~ 8%; additives: 1% ~ 5%; the sum of the weight percentages of the above components is 100%.
[0012] Preferably, the chemical formula of the diffusion alloy powder is Pr x NdᵧM b Cu c Al d Ga eWhere M represents Tb and / or Dy, b, c, d, and e are the atomic percentages of each element, satisfying: 20 ≤ x + y ≤ 30, 50 ≤ b ≤ 70, 5 ≤ c ≤ 10, 0 ≤ d ≤ 5, 5 ≤ e ≤ 10, and x + y + b + c + d + e = 100. The average particle size D50 of the alloy powder is 2~8 μm, and the particle size distribution span (D90-D10) / D50 is less than 2.0, which is beneficial for forming a dense and uniform coating.
[0013] Preferably, the UV-curable adhesive system comprises: Low-functionality UV monomers: accounting for 5%~10% of the total weight of the coating. Preferably, they are acrylate monomers with a functionality of 1, such as isobornyl acrylate (IBOA), lauryl acrylate (LA), and tetrahydrofuran acrylate (CTFA). Their function is to reduce the crosslinking density and viscosity of the system, improve leveling properties and deep curing ability; and High-functionality UV resin: 5%~12% of the total weight of the coating. Preferably, it is an epoxy acrylate, polyurethane acrylate, or a mixture thereof with a functionality ≥2. Its function is to provide the initial mechanical strength and adhesion of the coating. Fluorine-modified polyurethane acrylate is particularly preferred, as it can migrate to the interface between the coating and the alloy powder, reducing the interfacial energy and effectively blocking the reaction between the active functional groups and the alloy powder, thereby significantly improving the storage stability of the coating; and Composite photoinitiator system: This system comprises 0.5% to 3% of the total weight of UV resin and UV monomers. It consists of a combination of a pyrolysis-type photoinitiator and a hydrogen-abstraction-type photoinitiator. Preferably, the pyrolysis-type photoinitiator is an α-hydroxy ketone (such as Omnirad 184), and the hydrogen-abstraction-type photoinitiator is a combination of benzophenone (BP) and an amine synergist (such as EHA). The mass ratio of the two is 1:(0.8~1.5). The hydrogen-abstraction-type photoinitiator system is oxygen-inhibited but not affected by light shading. It can initiate polymerization in the shaded area through free radical chain transfer, synergistically working with the surface pyrolysis-type photoinitiator to achieve thorough curing of the coating "from the surface to the interior," fundamentally solving the peeling problem.
[0014] Preferably, the functional filler is nano-alumina (Al2O3) and / or nano-silica (SiO2), with an average particle size of 20~100nm. The filler has three functions: 1) as a physical barrier, reducing the contact between alloy powder particles and further inhibiting storage agglomeration; 2) during UV curing, partially scattering UV light, which helps the light to be distributed more evenly inside the coating; 3) during heat treatment, the nanoparticles can form a temporary skeleton structure after the binder degrades, supporting the coating and preventing it from collapsing and falling off before the alloy melts.
[0015] Preferably, the adjuvant comprises: Polymerization inhibitor / stabilizer: 0.04%-0.5% of UV resin and monomer, preferably hydroquinone or p-methoxyphenol, effectively inhibiting the prepolymerization of UV monomers and resin during storage and mixing, and inhibiting the reaction between the active functional groups of UV resin monomers and alloy powder; and Dispersant: 0.5%~2% of the total weight of the coating, preferably a BYK-series or TEGO-series polymeric block copolymer dispersant, used to coat the alloy powder, providing steric hindrance to prevent sedimentation and agglomeration; and Defoamer: 0.2%~0.8% of the total weight of the coating, preferably a polyether siloxane copolymer; and Leveling agent: accounting for 0.3% to 1% of the total weight of the coating, preferably a polyacrylate.
[0016] The second technical objective of this invention is achieved through the following technical solution: A process for preparing a UV grain boundary diffusion coating for sintered NdFeB magnets includes the following steps: S11 Pre-dispersion: Add the UV curing adhesive system (UV monomer, UV resin, photoinitiator) and all additives to a mixing container according to the ratio, and stir at 500~800 rpm for 10~15 minutes until completely mixed to obtain a premixed liquid.
[0017] S12 Powder Blending: Under nitrogen protection, with oxygen content controlled <0.01ppm, and with low-speed stirring (200~400rpm), gradually add the diffusion alloy powder and functional filler to the premixed liquid in 3~5 batches. After each batch is added, it is necessary to stir thoroughly until there is no dry powder before adding the next batch. This operation can prevent powder agglomeration and ensure that each powder particle is wetted by the liquid component.
[0018] S13 High-shear dispersion: Transfer the mixed slurry to a planetary mixer or high-speed disperser and disperse it under high shear at 1500~2500 rpm for 30~60 minutes. This process aims to break up all soft agglomerates and ensure that the dispersant acts fully on the powder surface.
[0019] S14 Filtration and Storage: Filter the coating through a 200-400 mesh screen, then pack it into a brown or opaque container, seal it, and store it in a cool place.
[0020] The third technical objective of this invention is achieved through the following technical solution: A coating process for a UV grain boundary diffusion coating for sintered NdFeB magnets, comprising the following steps: S21 Substrate Pretreatment: The sintered NdFeB magnets are degreased and acid-washed. Degreasing is performed by soaking in an alkaline degreasing agent at 50-60℃ for 3-5 minutes, followed by rinsing twice with water. Acid washing is performed by soaking and shaking in dilute nitric acid (concentration 0.5%-3%) at room temperature for 30-90 seconds to ensure that each magnet is wetted with dilute nitric acid. Then, the magnets are ultrasonically washed with tap water for 30-60 seconds, rinsed with tap water for 10-15 seconds, rinsed with deionized water for 10-15 seconds, and after removing most of the moisture from the magnet surface with an air knife, they are immediately dried with hot air at 130-160℃.
[0021] S22 screen printing: Use nylon mesh with a mesh count of 100-250.
[0022] The scraper is made of polyurethane with a hardness of 70~80 Shore A.
[0023] During printing, no electrostatic assistance is required; mechanical pressure is used directly. The squeegee angle is 60~75°, and the printing speed is controlled at 50~150 mm / s.
[0024] The wet film thickness of the coating is controlled between 30 and 150 μm.
[0025] S23 UV Curing: Curing is performed immediately after printing. An LED light source with a wavelength of 365nm or 395nm is used. Irradiation is carried out in a nitrogen atmosphere (oxygen concentration <500 ppm) or under conditions of air isolation by a film coating, with a peak irradiation intensity of 8000-10000mW / cm².
[0026] The fourth technical objective of this invention is achieved through the following technical solution: A grain boundary diffusion process for a UV grain boundary diffusion coating for sintered NdFeB magnets, used to treat the coated and cured magnets: the magnets are placed in a vacuum sintering furnace or an atmosphere-protected furnace and heat-treated according to the following procedure: S31 First Stage: Low-Temperature Degradation of Adhesive: The temperature is increased from room temperature to 300-450°C at a rate of 2-5°C / min, and held at this temperature for 1-3 hours. The key to this stage is to allow the UV adhesive to slowly and fully decompose into small molecule gases that evaporate, avoiding violent gas generation in the subsequent high-temperature stage that could damage the coating. Simultaneously, the framework formed by the functional fillers is preserved during this stage.
[0027] S32 Second Stage: Alloy Melting and Main Diffusion: The temperature is increased to 880~910℃ at a rate of 3~8℃ / min, and held at this temperature for 10~25 hours. This stage is the core process of heavy rare earth elements diffusing into the interior of the magnet along the grain boundaries.
[0028] S33 Third stage: Aging treatment: Cool with the furnace or rapidly cool to 500~650℃ under a protective atmosphere, and hold at this temperature for 4~6 hours to optimize the microstructure inside the magnet.
[0029] S34 Fourth Stage: Rapid Cooling: The magnet is then rapidly cooled to room temperature.
[0030] The entire heat treatment process is carried out under vacuum (≤3×10⁻² Pa) or high-purity argon protection.
[0031] In summary, the present invention has the following beneficial effects: 1. Excellent storage stability: By selecting low-activity UV monomers and introducing fluorine-modified UV resins to reduce interfacial reactivity, and combining high-efficiency dispersants with strict powder wetting, high-shear dispersion and filtration, the two pathways of coating agglomeration (polymerization and chemical reaction) are fundamentally cut off, so that the coating can be stored for more than 3 months. 2. Thorough deep curing, no peeling: Through the innovative "pyrolysis type + hydrogen abstraction type" composite photoinitiation system and curing in a low oxygen environment, the coating can be uniformly cured from the surface to the inside even with a metal opacity of up to 85%, eliminating peeling and warping caused by uneven curing. 3. Excellent heat treatment adhesion: By introducing nanofillers to form a supporting skeleton and designing a "low-temperature slow degradation" first stage of heat treatment, the organic binder is smoothly and thoroughly removed before the alloy melts. The coating maintains its morphological integrity and good contact with the substrate in the critical diffusion temperature range, ensuring diffusion efficiency. 4. Good process compatibility: The entire process flow, especially the coating process and the grain boundary diffusion process (pretreatment-screen printing-UV curing-heat treatment), is highly compatible with existing magnet production lines, making it easy to achieve large-scale and stable production. Attached Figure Description
[0032] Figure 1 This is a scanning electron microscope (SEM) image of the grain boundary microstructure of the sintered NdFeB magnet before diffusion of the UV grain boundary diffusion coating in Example 1.
[0033] Figure 2 This is a scanning electron microscope (SEM) image of the grain boundary microstructure of the sintered NdFeB magnet after diffusion of the UV grain boundary diffusion coating in Example 1. Detailed Implementation
[0034] Example 1
[0035] The UV grain boundary diffusion coating for sintered NdFeB magnets consists of the following components by weight: 62 parts of diffusion alloy powder; 25 parts of UV-curable adhesive system; 8 parts of functional filler; 5 parts of additives.
[0036] The chemical formula of the diffusion alloy powder is Pr 10 Nd 10 M 70 Cu5Ga5, where M is Tb.
[0037] The UV-curable adhesive system comprises a low-functionality UV monomer, a high-functionality UV resin, and a composite photoinitiator system. The low-functionality UV monomer is isobornyl acrylate (IBOA), accounting for 5% of the total coating weight. The high-functionality UV resin is an epoxy acrylate with a functionality ≥2, accounting for 12% of the total coating weight. The composite photoinitiator system is a blend of a pyrolytic photoinitiator and a hydrogen-abstracting photoinitiator. The pyrolytic photoinitiator is an α-hydroxy ketone (such as Omnirad 184), and the hydrogen-abstracting photoinitiator is a combination of benzophenone (BP) and an amine synergist (such as EHA); the mass ratio of the two is 1:0.8, accounting for 3% of the total weight of the UV resin and UV monomer.
[0038] The functional filler is nano-alumina (Al2O3), with an average particle size of 20~100nm.
[0039] The additives include polymerization inhibitors, dispersants, defoamers, and leveling agents: among which, the polymerization inhibitors hydroquinone and p-methoxyphenol account for 0.04% of the UV resin and monomers; the dispersants are BYK-series, accounting for 0.5% of the total weight of the coating; the defoamers are polyether siloxane copolymers, accounting for 0.2% of the total weight of the coating; and the leveling agents are polyacrylates, accounting for 1% of the total weight of the coating.
[0040] The preparation process of the UV grain boundary diffusion coating for the sintered NdFeB magnet in this embodiment includes the following steps: S11 Pre-dispersion: Add the UV curing adhesive system (UV monomer, UV resin, photoinitiator) and all additives to the mixing container according to the ratio, and stir at 500 rpm for 15 minutes until completely mixed to obtain a premixed liquid; S12 Powder Blending: Under nitrogen protection, with oxygen content controlled at <0.01ppm, and with low-speed stirring at 200 rpm, gradually add the diffusion alloy powder and functional filler to the premixed liquid in three batches. Each batch must be thoroughly stirred until no dry powder remains before adding the next batch. This operation prevents powder agglomeration and ensures that each powder particle is wetted by the liquid components.
[0041] S13 High-shear dispersion: Transfer the mixed slurry to a planetary mixer and perform high-shear dispersion at 1500 rpm for 60 minutes. This process aims to break up all soft agglomerates and ensure that the dispersant acts fully on the powder surface.
[0042] S14 Filtration and Storage: Filter the coating through a 200-mesh screen, then place it in a brown container, seal it, and store it in a cool place.
[0043] Example 2
[0044] The UV grain boundary diffusion coating for sintered NdFeB magnets consists of the following components by weight: 85 parts of diffusion alloy powder; 12 parts of UV-curable binder system; 2 parts of functional filler; 1 part of additive.
[0045] The chemical formula of the diffusion alloy powder is Pr 15 Nd 15 M 50 Cu 10 Al5Ga5, where M is Dy.
[0046] The UV-curable adhesive system comprises: a low-functionality UV monomer, a high-functionality UV resin, and a composite photoinitiator system. The low-functionality UV monomer is lauryl acrylate (LA), accounting for 10% of the total coating weight. The high-functionality UV resin is a polyurethane acrylate with a functionality ≥2, accounting for 5% of the total coating weight. The composite photoinitiator system is a blend of a pyrolysis photoinitiator and a hydrogen-abstraction photoinitiator. The pyrolysis photoinitiator is an α-hydroxy ketone (such as Omnirad 184), and the hydrogen-abstraction photoinitiator is a combination of benzophenone (BP) and an amine synergist (such as EHA); the mass ratio of the two is 1:1.5, accounting for 0.5% of the total weight of the UV resin and UV monomer.
[0047] The functional filler is nano-silica (SiO2), with an average particle size of 20~100nm.
[0048] The additives include stabilizers, dispersants, defoamers, and leveling agents: the stabilizer is hydroquinone, accounting for 0.5% of the UV resin and monomers; the dispersant is a BYK-series or TEGO-series high molecular weight block copolymer dispersant, accounting for 2% of the total weight of the coating; the defoamer is a polyether siloxane copolymer, accounting for 0.8% of the total weight of the coating; and the leveling agent is a polyacrylate, accounting for 0.3% of the total weight of the coating.
[0049] The preparation process of the UV grain boundary diffusion coating for the sintered NdFeB magnet in this embodiment includes the following steps: S11 Pre-dispersion: Add the UV curing adhesive system (UV monomer, UV resin, photoinitiator) and all additives to the mixing container according to the ratio, and stir at 800 rpm for 10 minutes until completely mixed to obtain a premixed liquid; S12 Powder Blending: Under nitrogen protection, with oxygen content controlled at <0.01ppm, and stirring at low speed (400 rpm), gradually add the diffusion alloy powder and functional filler to the premixed liquid in 5 batches. After each batch is added, stir thoroughly until no dry powder remains before adding the next batch. This operation prevents powder agglomeration and ensures that each powder particle is wetted by the liquid components.
[0050] S13 High-shear dispersion: Transfer the mixed slurry to a planetary mixer or high-speed disperser and disperse at 2500 rpm for 30 minutes using high-shear dispersion. This process aims to break up all soft agglomerates and ensure that the dispersant acts fully on the powder surface.
[0051] S14 Filtration and Storage: Filter the coating through a 400-mesh screen, then place it in an opaque container, seal it, and store it in a cool place.
[0052] Example 3
[0053] The UV grain boundary diffusion coating for sintered NdFeB magnets consists of the following components by weight: 75 parts of diffusion alloy powder; 15 parts of UV-curable binder system; 7 parts of functional filler; 3 parts of additives.
[0054] The chemical formula of the diffusion alloy powder is Pr 12 Nd 13 M 60 Cu7Al1Ga7, where M is Tb and Dy (each in equal proportions).
[0055] The UV-curable adhesive system comprises: a low-functionality UV monomer, a high-functionality UV resin, and a composite photoinitiator system. The low-functionality UV monomer is tetrahydrofuran acrylate (CTFA), accounting for 8% of the total coating weight. The high-functionality UV resin is a mixture of epoxy acrylate and polyurethane acrylate with a functionality ≥2, accounting for 8% of the total coating weight. The composite photoinitiator system is a blend of a pyrolysis photoinitiator and a hydrogen-abstraction photoinitiator. The pyrolysis photoinitiator is an α-hydroxy ketone (such as Omnirad 184), and the hydrogen-abstraction photoinitiator is a combination of benzophenone (BP) and an amine synergist (such as EHA); the mass ratio of the two is 1:1.2, accounting for 1.5% of the total weight of the UV resin and UV monomer.
[0056] The functional fillers are nano-alumina (Al2O3) and / or nano-silica (SiO2), with an average particle size of 20~100nm.
[0057] Additives include polymerization inhibitors and stabilizers, dispersants, defoamers, and leveling agents: among which, the polymerization inhibitors and stabilizers are hydroquinone and p-methoxyphenol, accounting for 0.3% of UV resin and monomers; the dispersants are BYK-series or TEGO-series high molecular weight block copolymer dispersants, accounting for 1% of the total weight of the coating; the defoamers are polyether siloxane copolymers, accounting for 0.5% of the total weight of the coating; and the leveling agents are polyacrylates, accounting for 0.7% of the total weight of the coating.
[0058] The preparation process of the UV grain boundary diffusion coating for the sintered NdFeB magnet in this embodiment includes the following steps: S11 Pre-dispersion: Add the UV curing adhesive system (UV monomer, UV resin, photoinitiator) and all additives to the mixing container according to the ratio, and stir at 600 rpm for 13 minutes until completely mixed to obtain a premixed liquid; S12 Powder Blending: Under nitrogen protection, with oxygen content controlled at <0.01ppm, the diffusion alloy powder and functional filler are gradually added to the premixed liquid in four batches while stirring at a low speed of 300 rpm. Each batch must be thoroughly stirred until no dry powder remains before adding the next batch. This operation prevents powder agglomeration and ensures that each powder particle is wetted by the liquid components.
[0059] S13 High-shear dispersion: Transfer the mixed slurry to a planetary mixer or high-speed disperser and perform high-shear dispersion at 2000 rpm for 40 minutes. This process aims to break up all soft agglomerates and ensure that the dispersant acts fully on the powder surface.
[0060] S14 Filtration and Storage: Filter the coating through a 300-mesh screen, then pack it into a brown or opaque container, seal it, and store it in a cool place.
[0061] Example 4
[0062] A coating process for a UV grain boundary diffusion coating on the sintered NdFeB magnet obtained in Example 1, comprising the following steps: S21 Substrate Pretreatment: The sintered NdFeB magnets are degreased and pickled. Degreasing is performed by soaking in an alkaline degreasing agent at 50°C for 5 minutes, followed by rinsing twice with water. Pickling is performed by soaking and shaking in dilute nitric acid (0.5% concentration) at room temperature for 30 seconds to ensure that each magnet is wetted with dilute nitric acid. Then, the magnets are ultrasonically rinsed with tap water for 30 seconds, rinsed with tap water for 10 seconds, rinsed with deionized water for 10 seconds, and after removing most of the moisture from the magnet surface with an air knife, they are immediately dried with hot air at 130°C.
[0063] S22 screen printing: The screen used is made of nylon with a mesh count of 100; the squeegee is made of polyurethane with a hardness of 70 Shore A. During printing, no electrostatic assistance is required; mechanical pressure is used directly. The squeegee angle is 60°, and the printing speed is controlled at 50 mm / s. The wet film thickness of the coating is controlled at 30 μm.
[0064] S23 UV Curing: Curing is performed immediately after printing. An LED light source with a wavelength of 365nm is used. Irradiation is carried out in a nitrogen atmosphere (oxygen concentration <500 ppm) or under conditions of air isolation by a film coating, with a peak irradiation intensity of 8000mW / cm².
[0065] The scanning electron microscope (SEM) image of the grain boundary microstructure of the sintered NdFeB magnet before diffusion of the UV grain boundary diffusion coating in Example 1 is shown below. Figure 1 .
[0066] Example 5
[0067] A coating process for a UV grain boundary diffusion coating used in the sintered NdFeB magnets obtained in Example 2, comprising the following steps: S21 Substrate Pretreatment: The sintered NdFeB magnets are degreased and pickled. Degreasing involves immersing the magnet in an alkaline degreasing agent at 60°C for 3 minutes, followed by two water rinses. Pickling involves immersing the magnet in dilute nitric acid (3% concentration) at room temperature and agitating it for 90 seconds to ensure that each magnet is thoroughly wetted with dilute nitric acid. The magnets are then ultrasonically rinsed with tap water for 60 seconds, rinsed with tap water for 15 seconds, rinsed with deionized water for 15 seconds, and then air-dried to remove most of the moisture from the magnet surface. Finally, they are dried with hot air at 160°C.
[0068] S22 screen printing: The screen used is made of nylon with a mesh count of 250; the squeegee is made of polyurethane with a hardness of 80 Shore A. During printing, no electrostatic assistance is required; mechanical pressure is used directly. The squeegee angle is 75°, and the printing speed is controlled at 150 mm / s. The wet film thickness of the coating is controlled at 150 μm.
[0069] S23 UV Curing: Curing is performed immediately after printing. An LED light source with a wavelength of 395nm is used. Irradiation is carried out in a nitrogen atmosphere (oxygen concentration <500 ppm) or under conditions of air isolation by a film coating, with a peak irradiation intensity of 10000mW / cm².
[0070] Example 6
[0071] A coating process for a UV grain boundary diffusion coating used in the sintered NdFeB magnets obtained in Example 3, comprising the following steps: S21 Substrate Pretreatment: The sintered NdFeB magnets are degreased and pickled. Degreasing is performed by soaking in an alkaline degreasing agent at 55°C for 4 minutes, followed by rinsing twice with water. Pickling is performed by soaking and shaking in dilute nitric acid (1.5% concentration) at room temperature for 60 seconds to ensure that each magnet is wetted with dilute nitric acid. Then, the magnets are ultrasonically washed with tap water for 40 seconds, rinsed with tap water for 12 seconds, rinsed with deionized water for 13 seconds, and after removing most of the moisture from the magnet surface with an air knife, they are immediately dried with hot air at 150°C.
[0072] S22 screen printing: The screen used is made of nylon with a mesh count of 180; the squeegee is made of polyurethane with a hardness of 75 Shore A. During printing, no electrostatic assistance is required; mechanical pressure is used directly. The squeegee angle is 60~75°, and the printing speed is controlled at 90 mm / s. The wet film thickness of the coating is controlled at 80μm.
[0073] S23 UV Curing: Curing is performed immediately after printing. An LED light source with a wavelength of 365nm is used. Irradiation is carried out in a nitrogen atmosphere (oxygen concentration <500 ppm) or under conditions of air isolation by a film coating, with a peak irradiation intensity of 9000mW / cm².
[0074] Example 7
[0075] A grain boundary diffusion process for a UV grain boundary diffusion coating for sintered NdFeB magnets, used to treat the magnets coated and cured in Example 4 above: The magnets are placed in a vacuum sintering furnace or a protective atmosphere furnace and heat-treated according to the following procedure, with the entire heat treatment process carried out under vacuum (≤3×10⁻² Pa) or high-purity argon protection: S31 Stage 1: Low-Temperature Degradation of Adhesive: The temperature is increased from room temperature to 300°C at a rate of 2°C / min, and held at this temperature for 1 hour. The key to this stage is to allow the UV adhesive to slowly and fully decompose into small molecule gases that evaporate, avoiding violent gas generation in the subsequent high-temperature stage that could damage the coating. Simultaneously, the framework formed by the functional fillers is preserved during this stage.
[0076] S32 Second Stage: Alloy Melting and Main Diffusion: Heat to 880℃ at a rate of 3℃ / min and hold at this temperature for 10 hours.
[0077] S33 Third stage: Aging treatment: Cool with the furnace or rapidly cool to 500°C under a protective atmosphere, and hold at this temperature for 4 hours to optimize the internal microstructure of the magnet.
[0078] S34 Fourth Stage: Rapid Cooling: The magnet is then rapidly cooled to room temperature.
[0079] The scanning electron microscope (SEM) image of the grain boundary microstructure of the sintered NdFeB magnet after UV grain boundary diffusion coating diffusion in Example 1 is shown below. Figure 2 .
[0080] Example 8
[0081] A grain boundary diffusion process for a UV grain boundary diffusion coating for sintered NdFeB magnets, used to treat the magnets coated and cured in Example 5 above: The magnets are placed in a vacuum sintering furnace or a protective atmosphere furnace and heat-treated according to the following procedure, with the entire heat treatment process carried out under vacuum (≤3×10⁻² Pa) or high-purity argon protection: S31 Stage 1: Low-Temperature Degradation of Adhesive: The temperature is increased from room temperature to 450°C at a rate of 5°C / min, and held at this temperature for 3 hours. The key to this stage is to allow the UV adhesive to slowly and fully decompose into small molecule gases that evaporate, avoiding violent gas generation in the subsequent high-temperature stage that could damage the coating. Simultaneously, the framework formed by the functional fillers is preserved during this stage.
[0082] S32 Second Stage: Alloy Melting and Main Diffusion: Heat to 910℃ at a rate of 8℃ / min and hold at this temperature for 25 hours.
[0083] S33 Third stage: Aging treatment: Cool with the furnace or rapidly cool to 650°C under a protective atmosphere, and hold at this temperature for 6 hours to optimize the internal microstructure of the magnet.
[0084] S34 Fourth Stage: Rapid Cooling: The magnet is then rapidly cooled to room temperature.
[0085] Example 9
[0086] A grain boundary diffusion process for a UV grain boundary diffusion coating for sintered NdFeB magnets, used to treat the magnets coated and cured in Example 6 above: The magnets are placed in a vacuum sintering furnace or a protective atmosphere furnace and heat-treated according to the following procedure, with the entire heat treatment process carried out under vacuum (≤3×10⁻² Pa) or high-purity argon protection: S31 Stage 1: Low-Temperature Degradation of Adhesive: The temperature is increased from room temperature to 400°C at a rate of 3°C / min, and held at this temperature for 2 hours. The key to this stage is to allow the UV adhesive to slowly and fully decompose into small molecule gases that evaporate, avoiding violent gas generation in the subsequent high-temperature stage that could damage the coating. Simultaneously, the framework formed by the functional fillers is preserved during this stage.
[0087] S32 Second Stage: Alloy Melting and Main Diffusion: Heat to 895℃ at a rate of 5℃ / min and hold at this temperature for 15 hours.
[0088] S33 Third stage: Aging treatment: Cool with the furnace or rapidly cool to 580°C under a protective atmosphere, and hold at this temperature for 5 hours to optimize the internal microstructure of the magnet.
[0089] S34 Fourth Stage: Rapid Cooling: The magnet is then rapidly cooled to room temperature.
[0090] Comparative Example 1 Similar to Example 4, except that the coating contains 52 parts by weight of diffusion alloy powder, 35 parts by weight of UV-curable binder system, 8 parts by weight of functional filler, and 5 parts by weight of additives.
[0091] Comparative Example 2 Similar to Example 5, except that the diffusion alloy powder does not contain Tb and / or Dy elements.
[0092] Comparative Example 3 Similar to Example 6, the difference is that the photoinitiator in the UV-cured adhesive system is not a composite photoinitiator system, but a single pyrolysis-type photoinitiator.
[0093] Comparative Example 4 Similar to Example 7, except that the UV-cured adhesive system does not use a composite photoinitiator system, but instead uses a single hydrogen-abstracting photoinitiator.
[0094] Comparative Example 5 Similar to Example 8, except that it does not undergo the first stage of low-temperature degradation and directly enters the second stage of heat treatment.
[0095] Based on the patent content, we conducted a series of experiments to verify key issues such as coating stability, UV curing defects, and coating peeling during heat treatment, as well as a comparison of the magnetic properties of UV coatings and traditional thermosetting coatings. The experimental data are based on the examples and comparative examples in the patent, as detailed below: I. Coating stability test data The stability of the coating was evaluated through a storage period test, as shown in Table 1. The viscosity changes and gelation phenomena of the coating during storage were observed. Test conditions: room temperature (25℃), sealed storage away from light, and periodic sampling and testing.
[0096] Table 1
[0097] Analysis: The coating of this invention (Example 1) significantly improves storage stability through low-activity UV monomers, fluorinated UV resins, and highly efficient dispersants, exhibiting no gelation within 3 months and minimal viscosity change. In contrast, Comparative Example 1, with its low alloy powder content but high UV resin content, suffers from uneven system reactivity and is prone to gelation. While Comparative Example 2 lacks Tb / Dy, its alloy powder has lower activity and better stability, but it still falls short of the present invention.
[0098] II. Experimental Data on UV Curing Defects The UV curing effect was evaluated through curing depth and adhesion tests, as shown in Table 2. Curing depth was observed using the cross-sectional cutting method, and adhesion was evaluated using the cross-cut test (ASTM D3359), with grades ranging from 0B (worst) to 5B (best).
[0099] Table 2
[0100] Analysis: The coatings of this invention (Examples 4-5) employ a composite photoinitiator system (pyrolysis type + hydrogen abstraction type), achieving deep curing in a low-oxygen environment with no peeling and excellent adhesion. In contrast, Comparative Example 3 (single pyrolysis type photoinitiator) only cured the surface layer due to UV light being shielded by the metal powder; Comparative Example 4 (single hydrogen abstraction type photoinitiator) was severely inhibited by oxygen, resulting in uneven curing.
[0101] III. Experimental data on coating peeling during heat treatment The integrity of the coating after heat treatment was assessed by visual observation and SEM analysis, as shown in Table 3. Diffusion efficiency was measured by EDS elemental mapping to determine the distribution of Tb / Dy within the magnet.
[0102] Table 3
[0103] Analysis: The coatings of this invention (Examples 7-8) utilize a framework formed by nanofillers and a low-temperature degradation stage (300-450℃) to ensure the stable decomposition of the organic binder, maintaining the integrity of the coating during heat treatment, and allowing Tb / Dy elements to effectively diffuse into the magnet's interior. In contrast, Comparative Example 5 (no low-temperature degradation) experienced premature coating detachment due to the violent decomposition of the binder; Comparative Example 2, lacking Tb / Dy elements, showed no diffusion effect.
[0104] IV. Comparison of Magnetic Properties After Diffusion between UV Coatings and Traditional Thermosetting Coatings Magnetic properties were evaluated by measuring coercivity (Hcj), remanence (Br), and maximum energy product (BHmax), as shown in Table 4. Test samples: Sintered NdFeB magnets of the same specifications were subjected to grain boundary diffusion treatment using the UV coating of this invention (Example 1) and a conventional thermosetting coating (based on epoxy resin system), respectively.
[0105] Table 4
[0106] analyze: The coercivity (Hcj) is significantly improved, resulting in outstanding performance advantages. After diffusion treatment with the UV coating of this invention, the coercivity of the magnet reaches 31.2 kOe, which is 11.0% higher than the 28.1 kOe of traditional thermosetting coatings; and 68.6% higher than the baseline of undiffused magnets (18.5 kOe). This indicates that the UV coating system of this invention is more efficient in promoting the diffusion of heavy rare earth elements (Tb / Dy) at grain boundaries, and can significantly enhance the magnet's resistance to demagnetization, making it particularly suitable for high-temperature and high-stability applications.
[0107] Remanence (Br) remains excellent, and the magnetic energy product (BHmax) achieves optimal balance. While achieving a significant increase in coercivity, the remanence of the magnet treated with the UV coating of this invention is 14.10 kGs, which is slightly better than that of conventional thermosetting coatings (13.85 kGs) and very close to the high-level benchmark of undiffused magnets (14.25 kGs). This indicates that this diffusion process effectively improves coercivity while minimizing the dilution effect on the magnetic properties of the main phase. Simultaneously, the maximum energy product (BHmax) reaches 49.2 MGOe, which is improved compared to conventional thermosetting coatings (48.5 MGOe) and almost equal to the benchmark value of undiffused magnets (49.5 MGOe). This demonstrates that the technology of this invention achieves an excellent balance between high coercivity and high energy product, overcoming the trade-off problem of increased coercivity but decreased energy product in conventional grain boundary diffusion techniques.
[0108] The above experimental data fully verify the advantages of the UV grain boundary diffusion coating of the present invention in terms of storage stability, curing effect, heat treatment adhesion and improved magnetic properties: Storage stability: The coating has a shelf life of more than 3 months without gelling.
[0109] UV curing: Achieves deep curing, no peeling, and adhesion 5B.
[0110] Heat treatment: The coating does not peel off and spreads evenly.
[0111] Magnetic properties: Coercivity is significantly higher than that of traditional thermosetting coatings.
[0112] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A UV grain boundary diffusion coating for sintered NdFeB magnets, characterized in that: Included by weight: Diffusion alloy powder: 60-85 parts; UV-curable binder system: 12-25 parts; functional filler: 2-8 parts; additives: 1-5 parts; The chemical general formula of the diffusion alloy powder is Pr x NdᵧM b Cu c Al d Ga e , wherein M is Tb and / or Dy, b, c, d, e are atomic percentages of each element, and satisfy: 20≤x+y≤30, 50≤b≤70, 5≤c≤10, 0≤d≤5, 5≤e≤10, and x+y+b+c+d+e=100; The average particle size D50 of the diffusion alloy powder is 2~8μm, and the particle size distribution span (D90-D10) / D50 is less than 2.0; The UV-curable adhesive system includes: Low-functionality UV monomers: accounting for 5%~10% of the total weight of the coating; the low-functionality UV monomers are acrylate monomers with a functionality of 1, including isoborneol acrylate, lauryl acrylate, or tetrahydrofuran acrylate; and The high-functionality UV resin accounts for 5% to 12% of the total weight of the coating, wherein the high-functionality UV resin is an epoxy acrylate, polyurethane acrylate, or a mixture thereof with a functionality ≥2; and The composite photoinitiator system comprises 0.5% to 3% of the total weight of UV resin and UV monomer; this system is composed of a pyrolysis photoinitiator and a hydrogen abstraction photoinitiator; the mass ratio of the two is 1:(0.8 to 1.5); the pyrolysis photoinitiator is α-hydroxy ketone Omnirad 184, and the hydrogen abstraction photoinitiator is a combination of benzophenone BP and amine synergist EHA; The functional filler is nano-alumina and / or nano-silica, with an average particle size of 20~100nm; The adjuvants include: Polymerization inhibitor: 0.04%-0.5% of UV resin and monomer; and Dispersant: 0.5%~2% of the total weight of the coating; and Defoamer: 0.2%~0.8% of the total weight of the coating; and Leveling agent: 0.3%~1% of the total weight of the paint; The polymerization inhibitor is hydroquinone, p-methoxyphenol; and The dispersant is a high molecular weight block copolymer dispersant of the BYK series or TEGO series; The defoamer is a polyether siloxane copolymer; and The leveling agent is a polyacrylate.
2. A preparation process for a UV grain boundary diffusion coating for sintered NdFeB magnets according to claim 1, characterized in that... Includes the following steps: S11 Pre-dispersion: Add the UV-curable adhesive system and all additives to the mixing container according to the ratio, and stir at 500~800 rpm for 10~15 minutes until completely mixed and homogeneous to obtain the premixed liquid; S12 Powder Mixing: Under nitrogen protection, with oxygen content controlled at <0.01ppm, diffusion alloy powder and functional filler are gradually added to the above premixed liquid in batches under low-speed stirring; after each batch is added, it is necessary to stir thoroughly until there is no dry powder before adding the next batch. S13 High Shear Dispersion: Transfer the mixed slurry to a planetary mixer or high-speed disperser and disperse it under high shear for 30 to 60 minutes at a speed of 1500 to 2500 rpm. S14 Filtration and storage.
3. A coating process for a UV grain boundary diffusion coating for sintered NdFeB magnets according to claim 1, characterized in that... Includes the following steps: S21 substrate pretreatment: The sintered NdFeB magnets are degreased and pickled; for degreasing, an alkaline degreasing agent is used to soak the magnets at 50-60℃ for 3-5 minutes, followed by water washing; for pickling, a 0.5%-3% dilute nitric acid solution is used to soak and shake the magnets at room temperature for 30-90 seconds to ensure that each magnet is wetted with dilute nitric acid, followed by ultrasonic water washing with tap water for 30-60 seconds, rinsing with tap water for 10-15 seconds, rinsing with deionized water for 10-15 seconds, and after removing most of the moisture from the magnet surface with an air knife, the magnets are immediately dried with hot air at 130-160℃. S22 screen printing: Use nylon mesh with a mesh count of 100-250; The scraper is made of polyurethane with a hardness of 70-80 Shore A. During printing, no electrostatic assistance is required; mechanical pressure is used directly. The squeegee angle is 60~75°, and the printing speed is controlled at 50~150 mm / s. The wet film thickness of the coating is controlled between 30 and 150 μm. S23 UV Curing: Curing immediately after printing; Specifically, LED light sources with wavelengths of 365nm or 395nm are used; irradiation is carried out under nitrogen atmosphere or with a film covering to isolate the air, with a peak irradiation intensity of 8000-10000mW / cm².
4. A grain boundary diffusion process for a UV grain boundary diffusion coating for sintered NdFeB magnets according to claim 1, characterized in that... After coating and curing, the magnet is placed in a vacuum sintering furnace or atmosphere-protected furnace and heat-treated according to the following steps. All heat treatment processes are carried out under vacuum or high-purity argon protection: S31 First Stage: Low-temperature degradation of adhesive: The temperature is increased from room temperature to 300-450℃ at a rate of 2-5℃ / min, and held at this temperature for 1-3 hours; S32 Second Stage: Alloy Melting and Main Diffusion: Heat to 880~910℃ at a rate of 3~8℃ / min, and hold at this temperature for 10~25 hours; S33 Third Stage: Aging Treatment: Cool with the furnace or rapidly cool to 500~650℃ under a protective atmosphere, and hold at this temperature for 4~6 hours to optimize the internal microstructure of the magnet. S34 Fourth Stage: Rapid Cooling: The magnet is then rapidly cooled to room temperature.
Citation Information
Patent Citations
Neodymium-iron-boron magnet and preparation method thereof
CN114628100A
Water-based metal direct-coating UV coating as well as preparation method and application thereof
CN117343627A
Composite diffusant for grain boundary diffusion of neodymium iron boron magnet, magnetic material intermediate, high-performance neodymium iron boron magnet and preparation method of high-performance neodymium iron boron magnet
CN118197783A
A NdFeB superimposed magnetic bonding process
CN119742171A