A soft magnetic nanomaterial made of iron, cobalt, and nickel and its electrodeposition preparation method

Fe35-42Co27-34Ni30-31 nanocrystalline alloys were prepared by electrodeposition. By combining multi-scale control of electrodeposition parameters, the problem of balancing strong plasticity and soft magnetic properties in soft magnetic materials was solved. This resulted in nanocrystalline alloys with high strength, toughness and excellent soft magnetic properties, expanding their application in new energy vehicles and downstream industries of new energy.

CN121709401BActive Publication Date: 2026-11-17XI AN JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511899124.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-16
Publication Date
2026-11-17
Estimated Expiration
2045-12-16

AI Technical Summary

Technical Problem

Existing soft magnetic materials face challenges in balancing strong plasticity and soft magnetic properties, making them difficult to apply in high-performance and extreme environments.

Method used

Fe35-42Co27-34Ni30-31 nanocrystalline alloys were prepared by electrodeposition. By combining multi-scale control of the plating solution composition, AC power duty cycle and additive composition during the electrodeposition process, nanocrystalline alloys with FCC structure were formed. Hard 9R phase was introduced to improve the strength, toughness and soft magnetism of the material.

Benefits of technology

It achieves a combination of high strength and toughness with excellent soft magnetic properties, significantly improving the ultimate tensile strength and saturation magnetization of the material, reducing coercivity, and expanding its application scope in new energy vehicles and downstream industries of new energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121709401B_ABST
    Figure CN121709401B_ABST
Patent Text Reader

Abstract

This invention discloses an iron-cobalt-nickel nanomaterial and its electrodeposition preparation method, belonging to the field of structure-functional integrated materials technology. The preparation method utilizes multi-scale control of the plating bath composition, AC power duty cycle, and additive composition during the electrodeposition process to prepare Fe with a face-centered cubic (FCC) structure. 35‑ 42 Co 27‑34 Ni 30‑31 This nanocrystalline alloy combines ultra-high strength and toughness with excellent soft magnetic properties. Additives can be used to reduce grain size, thereby lowering coercivity; adjusting the plating bath composition can increase saturation magnetization; and controlling the duty cycle can introduce a nine-layer atomic stacking sequence (9R) phase for strengthening. Multi-dimensional control achieves ultra-high strength, high plasticity, and excellent soft magnetic properties, making it suitable for key fields such as new energy vehicles and electrical and electronic engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of integrated structural and functional materials technology, specifically relating to an iron-cobalt-nickel nano-soft magnetic material and its electrodeposition preparation method. Background Technology

[0002] Driven by new energy vehicles and downstream industries, the market size of soft magnetic materials with excellent mechanical properties is growing rapidly. Soft magnetic materials with superior mechanical properties play a role in energy coupling, transfer, and conversion in various devices, and can be widely used in high-performance motors and other power conversion equipment. In today's world of increasingly scarce energy and serious environmental problems, improving the deformation resistance, reducing wear and tear, lowering coercivity, and increasing core efficiency of soft magnetic materials is of great significance for energy conservation and environmental pollution control.

[0003] The core research challenge of soft magnetic materials with excellent mechanical properties lies in the mutual constraints of performance parameters: high magnetization and low coercivity are key electromagnetic parameters to ensure energy conversion efficiency, but these often require the material to have a single, homogeneous soft magnetic phase structure; while to obtain excellent mechanical properties, especially high ultimate tensile strength and high elongation, it is necessary to form a multiphase toughening structure or introduce nanoprecipitates. This constraint means that most soft magnetic materials currently available, while prioritizing basic electromagnetic properties, generally have low ultimate tensile strength and elongation, which has become a key bottleneck restricting their application in high-performance, extreme environments. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide an iron-cobalt-nickel nano-soft magnetic material and its electrodeposition preparation method, so as to solve the problem that the strong plasticity and soft magnetic properties of ferromagnetic materials in the prior art cannot be achieved at the same time.

[0005] To achieve the above objectives, the present invention employs the following technical solution: A method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials includes the following steps: S1, a coating is prepared on the surface of a cathode plate by electrodeposition; during the electrodeposition process, the plating solution is a mixed solution of ferric sulfate, nickel sulfate, nickel chloride, cobalt sulfate and boric acid, and the duty cycle of the AC power supply is 0.5-0.8; anionic surface brightener and wetting agent are added to the plating solution; S2, peel off the coating to obtain Fe. 35-42 Co 27-34 Ni 30-31 The nanocrystalline alloy has a grain size at the nanometer level and contains a nanoscale hard 9R phase inside the grain.

[0006] A further improvement of the present invention is that: Preferably, in S1, the plating solution contains Fe2+ Co 2+ and Ni 2+ The molar ratio is (12.3-18.7):(21.4-28.7):(59.0-59.9).

[0007] Preferably, in S1, the anionic surface brightener includes sodium saccharin and 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.

[0008] Preferably, in S1, the concentration of sodium saccharin in the plating solution is 2-5 g / L, the concentration of 1,4-butynediol is 0.1-0.5 g / L, and the concentration of sodium dodecyl sulfate is 0.03-0.06 g / L.

[0009] Preferably, in S1, the current density during the electrodeposition process is 2-2.5 A / dm³. 2 The plating bath temperature is 55-70 ℃, and the pulse current plating time is 90-120 h.

[0010] Preferably, in S1, during the electrodeposition process, the anode plate is a soluble anode, including a nickel plate, an iron plate, or a cobalt plate, and the cathode plate is a stainless steel plate.

[0011] Preferably, in S1, the electroplating solution is purified by adsorbing impurities with activated carbon, and the pH value of the plating solution is adjusted to 1.5-2.5 after impurity removal.

[0012] A soft magnetic nanomaterial of iron, cobalt, and nickel prepared by any of the above methods, comprising Fe 35~42 Co 27- 34 Ni 30-31 Nanocrystalline alloys and hard 9R phase, wherein the Fe 35-42 Co 27-34 Ni 30-31 The nanocrystalline alloy has an FCC single-phase structure.

[0013] Preferably, the Fe 35-42 Co 27-34 Ni 30-31 The average grain size of the nanocrystalline alloy is 20-23 nm, and the grain size of the hard 9R phase is 3-20 nm.

[0014] Preferably, the iron-cobalt-nickel nano-soft magnetic material has an ultimate tensile strength of 2.7-2.9 GPa, an elongation at break of 12.4-13.9%, a room temperature coercivity of 0.40-0.60 Oe, and a saturation magnetization of 146-150 emu / g.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for electrodepositing iron-cobalt-nickel nanofiber soft magnetic materials. This method involves multi-scale control of the plating bath composition, AC power duty cycle, and additive composition during the electrodeposition process to prepare Fe nanofibers with a face-centered cubic (FCC) structure. 35-42 Co 27-34 Ni 30-31 For the first time, a nanocrystalline alloy possessing both high strength and toughness, as well as soft magnetic properties, has been successfully synthesized. This is achieved by controlling the grain size through additives, resulting in nanocrystals significantly smaller than the ferromagnetic phase exchange length. This strongly averages the magnetic anisotropy, reducing coercivity. Simultaneously, the composition of the plating bath is adjusted to introduce a higher density of ferromagnetic material, increasing saturation magnetization. Localized chemical composition fluctuations are introduced through duty cycle control, inducing the transformation of low stacking fault energies into a hard 9R phase. This invention utilizes grain refinement and 9R phase strengthening to excite multiple phase transformation mechanisms during plastic deformation, increasing the dislocation density of the nanomaterial and thus improving its work hardening ability, strength, and toughness. The plating composition is controlled through the plating bath composition during electrodeposition, and nanocrystalline materials are prepared through the synergistic effect of additives. A strengthening phase is introduced by adjusting the AC power supply duty cycle. Ultimately, high strength and toughness, along with excellent soft magnetic properties, are achieved through composition, nanocrystal size, and the nano-strengthening phase, solving the challenge of achieving a balance between these two properties.

[0016] This invention also discloses an iron-cobalt-nickel nanocrystalline soft magnetic material prepared by the above-described method. Its high-density ferromagnetic phase within the grains enhances saturation magnetization, and the grain size is significantly smaller than the ferromagnetic exchange length, resulting in strong averaging of magnetic anisotropy. Simultaneously, grain boundaries promote magnetic moment exchange coupling, effectively reducing domain wall pinning and significantly lowering coercivity. Furthermore, multi-scale control of electrodeposition parameters introduces 9R phase strengthening, overcoming the technical defects of insufficient dislocation accommodation and lack of work hardening ability due to ultrafine grains. While maintaining ductility, it significantly improves room-temperature tensile strength, expanding its application range in key areas such as new energy vehicles and downstream industries of new energy. By introducing nanostructures during electrodeposition, the work hardening ability of the material is improved during plastic deformation, ultimately resulting in good ductility and a significantly increased maximum tensile strength. Simultaneously, the size effect of the nanograins gives the alloy extremely low coercivity and extremely high saturation magnetization, exhibiting excellent soft magnetic properties. This ultra-high strength iron-cobalt-nickel nanocrystalline soft magnetic material can expand the application range of soft magnetic alloys in key structural areas such as electrical and electronic equipment. Attached Figure Description

[0017] Figure 1 The image shows a surface photograph analysis of Example 1; Figure 2 The XRD pattern is shown in Example 1. Figure 3 The room temperature stress-strain curves for Examples 1, 2, and 3 are shown. Figure 4 Magnetization curves for Examples 1, 2, and 3; Figure 5 The transmission Kikuchi diffraction (TKD) diagram and phase diagram of Example 1 are shown below; Figure 6 This is a statistical chart of TKD grain size in Example 1; Figure 7 This is a spherical aberration electron microscope image of Example 1. Detailed Implementation

[0018] The present invention will now be described in further detail with reference to the accompanying drawings: To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0019] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0020] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0021] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0022] For any alloy, the control of microstructure is particularly crucial—nanograin size enhances material strength and plasticity, precise control of magnetic domain structure directly affects coercivity and saturation magnetization, and introducing defects (reinforcing phases) can further improve mechanical properties and soft magnetic properties. This invention balances conflicting properties through multi-scale structural control, meeting the requirements for high mechanical properties and high soft magnetic properties. It solves the problems of poor room-temperature ductility and brittle fracture in existing soft magnetic materials.

[0023] The first aspect of this invention discloses a method for preparing an iron-cobalt-nickel nanocrystalline soft magnetic alloy with excellent mechanical properties, comprising the following steps: S1, a coating is prepared on the surface of a cathode plate by electrodeposition. During the electrodeposition process, the composition of the plating solution, the duty cycle of the AC power supply and the composition of the additives are controlled to achieve multi-scale control of electrodeposition. S2, after peeling off the coating, FeCoNi nanocrystalline alloy is obtained. The grain size of the alloy is at the nanoscale, and there is a nanoscale hard 9R phase inside the nanocrystals, thereby forming a multi-scale nanostructure.

[0024] A further improvement of the present invention is that: In S1, the duty cycle of the AC power supply is set to 0.5-0.8.

[0025] In S1, the electroplating solution used for electrodeposition is a mixed solution of ferric sulfate, nickel sulfate, nickel chloride, cobalt sulfate, and boric acid, wherein Fe in the plating solution... 2+ Co 2+ Ni 2+ The molar ratio of cations is (12.3-18.7):(21.4-28.7):(59.0-59.9).

[0026] In S1, the additives include anionic surface brighteners and wetting agents, wherein the anionic surface brighteners include sodium saccharin and 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.

[0027] Among them, sodium saccharin is 2-5 g / L, 1,4-butynediol is 0.1-0.5 g / L, and sodium dodecyl sulfate is 0.03-0.06 g / L.

[0028] In S1, the current density during the electrodeposition process is 2-2.5 A / dm³. 2 The stirring speed is 500-1200 r / min, the plating bath temperature is 55-70 ℃, and the pulse current electroplating time is 90-120 h.

[0029] In S2, the nanocrystalline alloy prepared has the composition of Fe. 35-42 Co 27-34 Ni 30-31 It has an FCC single-phase structure with an average grain size of 20-23 nm.

[0030] The second aspect of this invention discloses an iron-cobalt-nickel nanocrystalline soft magnetic alloy Fe with excellent mechanical properties, prepared by the above-described method. 35-42 Co 27-34 Ni 30-31It exhibits an FCC single-phase structure with an average grain size of 20-23 nm. The grains of this iron-cobalt-nickel nanocrystalline alloy contain a large number of hard 9R phases with a size of 3-20 nm, forming a multi-scale nanostructure.

[0031] This alloy is a nanocrystalline soft magnetic alloy with excellent mechanical properties, exhibiting superior room temperature tensile properties, with an ultimate tensile strength of 2.7-2.9 GPa and an elongation at break of 12.4-13.9%. The room temperature coercivity of the iron-cobalt-nickel nanoalloy is 0.40-0.60 Oe, and the saturation magnetization is 146-150 emu / g.

[0032] This invention utilizes multi-scale controlled pulse electrodeposition parameters to prepare nanocrystalline FeCoNi medium-entropy soft magnetic alloys, and systematically studies their mechanical properties, electromagnetic properties, and microstructure. Results show that nanocrystalline Fe... 35-42 Co 27-34 Ni 30-31 The medium-entropy alloy exhibits exceptionally high performance in room temperature tensile tests, with yield strengths ranging from 1.95 to 2.05 GPa, ultimate tensile strengths from 2.75 to 2.91 GPa, and elongation at break of 12.5% ​​to 13.9%. Alongside these superior tensile strengths, it demonstrates excellent soft magnetic properties with a room temperature coercivity of 0.40 to 0.60 Oe and a saturation magnetization of 146 to 150 emu / g. Microstructural analysis reveals an average grain size of 20 to 23 nm. The high-density ferromagnetic phase enhances the saturation magnetization, while the significantly smaller nanograin size compared to the ferromagnetic phase exchange length strongly averages the magnetic anisotropy, reducing coercivity and thus improving soft magnetic properties. This addresses the challenge of balancing strength and toughness with soft magnetic properties. Microstructural characterization further demonstrates that the nanograin boundaries and 9R phase structure in the nanocrystalline FeCoNi alloy hinder dislocation slip, enhancing work hardening capabilities. The nanostructured FeCoNi medium-entropy alloy prepared by the method in this invention achieves a new breakthrough in the combination of strong toughness and soft magnetic properties.

[0033] This invention uses electrodeposition to prepare a coating on the surface of a cathode plate. After peeling off the coating, a nanocrystalline iron-cobalt-nickel alloy is obtained. By controlling the composition of the plating solution, the duty cycle of the AC power supply, and the composition of additives during the electrodeposition process at multiple scales, a Fe alloy with a face-centered cubic (FCC) structure is prepared. 35-42 Co 27-34 Ni 30-31This invention presents, for the first time, a nanocrystalline alloy possessing both high toughness and soft magnetic properties. By controlling grain size through additive regulation, fine-grained strengthening and reduced coercivity are achieved. Higher density ferromagnetic materials are introduced through the regulation of the plating solution composition to increase saturation magnetization. Duty cycle regulation introduces local chemical composition fluctuations to induce the formation of a hard 9R phase in low stacking fault energy regions. This invention utilizes fine-grained strengthening and 9R phase strengthening to enable the material to undergo multiple phase transformation mechanisms during plastic deformation, forming additional geometrically necessary dislocations, increasing the dislocation density of the nanomaterial, thereby improving the material's work hardening ability, and ultimately significantly enhancing its strength and toughness.

[0034] In some embodiments of the present invention, the specific process of S1 is as follows: according to the preset Fe 2+ Co 2+ Ni 2+ First, a base electroplating solution was prepared based on the ion molar ratio. This solution was then subjected to adsorption purification and electrolytic purification treatments to obtain a plating solution that met the requirements. The purified plating solution was transferred to an electroplating tank, and appropriate amounts of anionic surfactants and wetting agents were added to improve the quality of the plating layer. Subsequently, the pretreated soluble anode and cathode substrates were placed in the tank, and electrodeposition was performed under optimized pulse parameters to deposit Fe on the surface of the cathode material. 35-42 Co 27-34 Ni 30-31 alloy.

[0035] In some specific examples, the substance containing Fe 2+ Co 2+ Ni 2+The preparation method for an electroplating solution with a cation ratio of (12.3-18.7):(21.4-28.7):(59.0-59.9) is as follows: Using deionized water, prepare solutions with the following concentrations: ferrous sulfate (FeSO4) 36-54 g / L, nickel sulfate (NiSO4·6H2O) 250 g / L, nickel chloride (NiCl2·6H2O) 50 g / L, cobalt sulfate (CoSO4·7H2O) 110-160 g / L, and boric acid (H3BO3) 40 g / L. After preparing the basic plating solution, add an appropriate amount of activated carbon and continuously adsorb it for 20-30 min under magnetic stirring. Then, use a vacuum filtration device to remove the activated carbon and the various impurities it has adsorbed. Subsequently, perform electrolytic purification on the plating solution for 12 h to further remove residual impurity ions. After completing the above impurity removal steps, the pH of the plating solution is adjusted to the range of 1.5-2.5 using 15% (v / v) dilute sulfuric acid to obtain the final purified plating solution. This impurity removal treatment effectively removes insoluble particles, organic contaminants, and other metallic cation impurities from the plating solution, thereby significantly improving the purity of the plating solution and laying the foundation for obtaining a dense and high-performance coating. Activated carbon, as a porous carbonaceous material, with its well-developed pore structure and huge specific surface area, can efficiently adsorb insoluble particles such as dust and fine sand introduced into the plating solution, as well as organic contaminants mixed in during the preparation process, making it a key material for achieving initial purification of the plating solution.

[0036] In some specific examples, the wetting agent is prepared as follows: first, sodium dodecyl sulfate is mixed with a small amount of deionized water to form a paste, then deionized water is poured into it, and it is heated on an electric furnace and kept at a slight boiling state for 10 minutes to fully dissolve it and remove harmful impurities. Finally, it is added to the plating solution and stirred and mixed evenly to obtain the wetting agent, wherein the concentration of sodium dodecyl sulfate used is 1 g / L.

[0037] In some specific examples, weighed sodium saccharin and 1,4-butynediol are first added to the plating solution and allowed to dissolve completely. Sodium saccharin acts as a grain refiner, and 1,4-butynediol acts as an anionic surface brightener. The concentrations of sodium saccharin and 1,4-butynediol are 2-5 g / L and 0.1-0.5 g / L, respectively. The main function of sodium saccharin is to inhibit grain growth and brighten the coating surface, while 1,4-butynediol not only improves the brightness of the coating but also significantly reduces the internal stress of the coating, preventing the formation of coating cracks. Adding sodium dodecyl sulfate as a wetting agent to the electroplating solution is characterized by: the sodium dodecyl sulfate effectively reducing the surface tension between the plating solution and the cathode interface, allowing hydrogen gas generated during electrodeposition to escape rapidly, preventing the formation of residual bubbles in the coating, thereby fundamentally preventing the generation of pinholes and pitting defects, and achieving a significant improvement in the surface smoothness and internal density of the coating.

[0038] In some embodiments of the present invention, in S1, both the anode and cathode substrates undergo mechanical and chemical pretreatment. First, the soluble anode, including nickel, iron, or cobalt plates, is cut to a predetermined size and mechanically polished to remove the surface oxide layer. Subsequently, the anode and cathode are ultrasonically cleaned sequentially: the anode undergoes alkali washing and acid washing to remove oil and surface impurities; the cathode undergoes alkali washing to remove oil, acid washing to remove the oxide layer, and surface activation. This process provides a clean and activated electrode surface for the electroplating experiment.

[0039] The cathode plate treatment process includes alkaline washing, water washing, acid washing, and final rinsing. The specific steps are as follows: First, ultrasonically clean the cathode plate for 3 minutes in an alkaline washing solution (formula: NaOH 40 g / L, Na2CO3 25 g / L, Na2Si3O3 10 g / L, Na3PO4 5 g / L) at 70-80°C to remove oil stains; then ultrasonically clean it for 3 minutes in deionized water; next, briefly ultrasonically clean it for 5 seconds in a 15% (v / v) H2SO4 solution to remove the oxide layer and achieve surface activation; finally, rinse quickly with deionized water to complete the treatment. The purified plating solution is then added to the electroplating container, along with anionic brighteners and wetting agents. The surface-treated anode and cathode plates are then placed into the electroplating container. In some embodiments of the present invention, during the pulse electroplating process, a pre-plating test is first conducted to control the concentration of metal ions in the plating solution; then, at a current density of 1.8-2.2 A / dm³, the plating is further refined. 2 Nanocrystalline alloy coatings were obtained by electroplating with pulsed current for 96 h under the following conditions: stirring speed 500-1200 r / min, duty cycle 0.5-0.8, plating bath temperature 55-70 ℃, and plating bath pH value 2.

[0040] Given the long formal electroplating cycle, continuous dynamic maintenance of the plating solution is necessary to ensure process stability. This includes: regularly monitoring and replenishing the consumed main salt metal ions; and monitoring the continuous consumption of H+ by the cathode hydrogen evolution reaction. + The increased pH of the plating solution necessitates the use of a 15% sulfuric acid solution as an adjuster to maintain the pH within the set range. Simultaneously, to compensate for the consumption of organic additives during the electrodeposition process, sodium saccharin and 1,4-butynediol need to be added to the plating solution at rates of 0.2 g / h and 0.02 g / h, respectively, to stabilize the coating quality.

[0041] It should be noted that the electroplating process uses a three-anode deposition method, in which three anodes are suspended and fixed side by side on any side of the surface inside the electroplating container, and the cathode material is suspended and fixed 2 cm below the opposite plating tank surface. The distance between the cathode material and the two sides of the electroplating container is adjusted so that the distance between the cathode material and the two sides of the electroplating container is the same. The stirring motor is then turned on to carry out electroplating.

[0042] This invention discloses an iron-cobalt-nickel nanoalloy with an FCC phase structure prepared by any one of the above preparation methods. The iron-cobalt-nickel nanoalloy has an average grain size of 20-23 nm, a tensile strength of 2.75-2.91 GPa, a plasticity of 12.4-13.9%, a coercivity of 0.40 Oe, and a saturation magnetization of 150 emu / g.

[0043] The iron-cobalt-nickel nanoalloy with FCC phase structure finally prepared by this invention has a large number of 9R phases inside the nanocrystals. This structure is a long-period stacking fault structure, which can emit dislocations and provide resistance to dislocation slip, thereby improving its work hardening ability. The high-density ferromagnetic phase inside the alloy increases the saturation magnetization intensity, and the ultrafine grain size is significantly smaller than the ferromagnetic phase exchange length, which strongly averages the magnetic anisotropy and reduces the coercivity.

[0044] The following is a further explanation with reference to specific embodiments: Example 1 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+ The molar proportions were 13.5%, 27.0%, and 59.5%, respectively: 240 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 900 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed at room temperature for more than 15 min. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the impurity ions were removed by electrolysis with a DC current of 0.1 A for 12 h. S2, sodium saccharin (C7H5O3NS) 3 g / L, 1,4-butynediol (C4H6O2) 0.2 g / L, and sodium dodecyl sulfate (C) were added to the above 6 L plating solution respectively. 12 H 25 Add 0.05 g / L of SO4Na to a final volume of 6 L, and then add 15% (v / v) dilute sulfuric acid to adjust the pH of the plating solution to 1.5.

[0045] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and the titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0046] For 100 mm The 100 mm stainless steel cathode plate is chamfered at all four corners and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85 ℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0047] S4. After 1 hour of pre-plating to adjust the plating solution composition, the electroplating test officially began. The pulse electroplating time was 96 hours, and the average pulse current density was 2.0 A / dm³. 2 The duty cycle was 0.8, the stirring speed was 800 r / min, the temperature of the electroplating solution after impurity removal was 65℃, and the pH value of the plating solution was controlled at around 2.0. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 37 Co 31 Ni 32 .

[0048] By photographing and analyzing the surface quality of the coating alloy in the above embodiments, it was found that the alloy surface is smooth and flat, with a dense structure and no cracks. The test results are shown in the figure below.

[0049] The surface quality of the coating alloy in the above embodiments was analyzed by taking photographs, such as... Figure 1 As shown, the alloy surface is smooth and flat, with a dense structure and no cracks.

[0050] See Figure 2 As can be seen by X-ray diffraction (XRD), the coating alloy prepared in the above example has a face-centered cubic (FCC) single-phase structure.

[0051] See Figure 3 The blue line sample was stretched at room temperature using an Instron 5966 stretching machine at 5... 10 -3The coating prepared in the above example was subjected to tensile tests at a strain rate of / S to test its strength and plasticity. The results showed that the tensile strength was 2.91 GPa and the plasticity was 12.4%.

[0052] See Figure 4 The blue line sample was measured using a Vibrating Sample Magnetometer (VSM) manufactured by LakeShore. The hysteresis loop was measured to obtain a room temperature coercivity of 0.40 Oe and a saturation magnetization of 146 emu / g.

[0053] See Figure 5 and Figure 6 As can be seen by using transmission Kikuchi diffraction (TKD) technique, the average size of the sample prepared by electrodeposition in the above example is 21.6 nm, which is a single-phase FCC structure.

[0054] See Figure 7 Aberration-corrected electron microscopy characterization revealed a large number of 9R stacking fault structures inside the material. These structures can emit dislocations and impede dislocation movement, thereby improving the strength and toughness of the alloy.

[0055] Example 2 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+ The molar proportions were 14.6%, 25.9%, and 59.5%, respectively: 260 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 850 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed for more than 15 min at room temperature. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the solution was electrolyzed with a DC current of 0.1 A for 12 h to remove the impurity ions. S2, add sodium saccharin (C7H5O3NS) 3 g / L, 1,4-butynediol (C4H6O2) 0.2 g / L, and sodium dodecyl sulfate (C4H6O2) to the above plating solution respectively. 12 H 25 Add 0.05 g / L of SO4Na to a final volume of 6 L, and then add 15% (v / v) dilute sulfuric acid to adjust the pH of the plating solution to 1.5.

[0056] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and the titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0057] For 100 mm The four corners of the 100 mm stainless steel cathode plate are chamfered, and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0058] S4. After 1 hour of pre-plating and adjustment of the plating solution composition, the formal electroplating test began. The pulse electroplating time was 96 hours, and the average pulse current density was 2.0 A / dm³. 2 The duty cycle was 0.8, the stirring speed was 800 r / min, the temperature of the electroplating solution after impurity removal was 65 ℃, and the pH value of the plating solution was controlled at around 2.0. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 38 Co 30 Ni 32 .

[0059] By photographing and analyzing the surface quality of the coating alloy in the above embodiments, it was found that the alloy surface is smooth and flat, has a dense structure, and is free of cracks.

[0060] See Figure 3 The green line sample was stretched at room temperature using an Instron 5966 tensile testing machine at 5... 10 -3 The tensile test was conducted on the coating prepared in the above example at a strain rate of / S to test its strength and plasticity. The results showed that the tensile strength was 2.85 GPa and the plasticity was 13.9%.

[0061] See Figure 4 The green line sample was measured using a Vibrating Sample Magnetometer (VSM) manufactured by LakeShore. The hysteresis loop was measured to obtain a room temperature coercivity of 0.55 Oe and a saturation magnetization of 148 emu / g.

[0062] Example 3 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+ The molar proportions were 12.3%, 28.7%, and 59%, respectively: 220 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 950 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed for more than 15 min at room temperature. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the solution was electrolyzed with a DC current of 0.1 A for 12 h to remove the impurity ions. S2, add sodium saccharin (C7H5O3NS) 3 g / L, 1,4-butynediol (C4H6O2) 0.2 g / L, and sodium dodecyl sulfate (C4H6O2) to the above plating solution respectively. 12 H 25 Add 0.05 g / L of SO4Na to a final volume of 6 L, and then add 15% (v / v) dilute sulfuric acid to adjust the pH of the plating solution to 1.5.

[0063] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and a pure titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0064] For 100 mm The four corners of the 100 mm stainless steel cathode plate are chamfered, and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85 ℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0065] S4. After 1 hour of pre-plating and adjustment of the plating solution composition, the formal electroplating test began. The pulse electroplating time was 96 hours, and the average pulse current density was 2.0 A / dm³. 2 The duty cycle was 0.8, the stirring speed was 800 r / min, the temperature of the electroplating solution after impurity removal was 65℃, and the pH value of the plating solution was controlled at around 2.0. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 35 Co 30 Ni 31 .

[0066] By photographing and analyzing the surface quality of the coating alloy in the above embodiments, it was found that the alloy surface is smooth and flat, has a dense structure, and is free of cracks.

[0067] See Figure 3 The red line sample was stretched at room temperature using an Instron 5966 stretching machine at 5... 10 -3 The tensile test was conducted on the coating prepared in the above example at a strain rate of / S to test its strength and plasticity. The results showed that the tensile strength was 2.75 GPa and the plasticity was 13.4%.

[0068] See Figure 4 The red line sample was measured using a Vibrating Sample Magnetometer (VSM) manufactured by LakeShore. The hysteresis loop was measured to obtain a room temperature coercivity of 0.60 Oe and a saturation magnetization of 150 emu / g.

[0069] Example 4 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+ The molar proportions were 18.7%, 21.4%, and 59.9%, respectively: 280 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 800 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed for more than 15 min at room temperature. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the solution was electrolyzed with a DC current of 0.1 A for 12 h to remove the impurity ions. S2, add sodium saccharin (C7H5O3NS) 2 g / L, 1,4-butynediol (C4H6O2) 0.1 g / L, and sodium dodecyl sulfate (C4H6O2) to the above plating solution respectively. 12 H25 Add 0.03 g / L of SO4Na to a final volume of 6 L, and then add 15% (v / v) dilute sulfuric acid to adjust the pH of the plating solution to 1.5.

[0070] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and the titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0071] For 100 mm The four corners of the 100 mm stainless steel cathode plate are chamfered, and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85 ℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0072] S4. After 1 hour of pre-plating and adjustment of the plating solution composition, the formal electroplating test began. The pulse electroplating time was 90 hours, and the average pulse current density was 2.2 A / dm³. 2 The duty cycle was 0.5, the stirring speed was 800 r / min, the temperature of the electroplating solution after impurity removal was 55 ℃, and the pH value of the plating solution was controlled at around 1.5. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 39 Co 31 Ni 30 .

[0073] Example 5 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+The molar proportions were 12.3%, 28.7%, and 59%, respectively: 300 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 750 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed for more than 15 min at room temperature. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the solution was electrolyzed with a DC current of 0.1 A for 12 h to remove the impurity ions. S2, add sodium saccharin (C7H5O3NS) 5 g / L, 1,4-butynediol (C4H6O2) 0.5 g / L, and sodium dodecyl sulfate (C4H6O2) to the above plating solution respectively. 12 H 25 Add 0.06 g / L of SO4Na to a final volume of 6 L, and then add 15% (v / v) dilute sulfuric acid to adjust the pH of the plating solution to 2.5.

[0074] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and the titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0075] For 100 mm The four corners of the 100 mm stainless steel cathode plate are chamfered, and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85 ℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0076] S4. After 1 hour of pre-plating to adjust the plating solution composition, the electroplating test officially began. The pulse electroplating time was 120 hours, and the average pulse current density was 2.5 A / dm³. 2The duty cycle was 0.6, the stirring speed was 800 r / min, the temperature of the purified electroplating solution was 70 ℃, and the pH value of the solution was controlled at around 2.5. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 41 Co 28 Ni 31 .

[0077] Example 6 S1, prepare a plating solution containing iron, cobalt, and nickel ions, Fe 2+ Co 2+ and Ni 2+ The molar proportions were 18.7%, 21.4%, and 59.9%, respectively: 320 g of ferrous sulfate (FeSO4), 1500 g of nickel sulfate (NiSO4·6H2O), 300 g of nickel chloride (NiCl2·6H2O), 700 g of cobalt sulfate (CoSO4·7H2O), and 240 g of boric acid (H3BO3) were prepared using deionized water. 30 g of activated carbon was added to the prepared plating solution, and the solution was magnetically stirred and adsorbed at room temperature for more than 15 min. After standing for 3 h, the residual activated carbon and impurities were removed by vacuum filtration. Then, the solution was electrolyzed with a DC current of 0.1 A for 12 h to remove the impurity ions. S2, add sodium saccharin (C7H5O3NS) 4 g / L, 1,4-butynediol (C4H6O2) 0.5 g / L, and sodium dodecyl sulfate (C4H6O2) to the above plating solution respectively. 12 H 25 Add 0.05 g / L of SO4Na to a final volume of 6 L, and adjust the pH of the plating solution to 1 by adding 15% (v / v) dilute sulfuric acid.

[0078] S3, for dimensions of 100 mm 100 mm soluble nickel anode plate, 50 mm 100 mm soluble iron anode plate and 50 mm A 100 mm soluble cobalt anode plate was polished to remove the surface oxide layer. The prepared alkaline cleaning solution was heated to 80-85 °C, stirred, and fully dissolved. The anode plate was then immersed in the alkaline cleaning solution for ultrasonic cleaning for 3 min, followed by ultrasonic cleaning in deionized water for 3 min, and finally ultrasonically cleaned in an acid cleaning solution for 15 s. Afterward, it was quickly rinsed with deionized water to complete the anode plate treatment. Using the aforementioned nickel plate as the anode and the titanium plate as the cathode, electrolysis was performed at 0.1 A DC for 12 h.

[0079] For 100 mm The four corners of the 100 mm stainless steel cathode plate are chamfered, and the burrs on the edges are ground off. The prepared alkaline cleaning solution is heated to 80-85 ℃, stirred, and fully dissolved. The cathode plate is then immersed in the alkaline cleaning solution for ultrasonic cleaning for 5 minutes, followed by ultrasonic cleaning in deionized water for 3 minutes. Finally, it is immersed in the acid cleaning solution for ultrasonic cleaning for 15 seconds, and then quickly rinsed with deionized water to complete the treatment of the cathode plate. It is then quickly immersed in the plating solution to begin electroplating.

[0080] S4. After 1 hour of pre-plating and adjustment of the plating solution composition, the electroplating experiment officially began. The pulse electroplating time was 100 hours, and the average pulse current density was 2.5 A / dm³. 2 The duty cycle was 0.7, the stirring speed was 800 r / min, the temperature of the purified electroplating solution was 60 ℃, and the pH value of the solution was controlled at around 1.5. During the electroplating process, the metal ion concentration and solution pH value were continuously monitored, and additives were added as needed to obtain the desired coating alloy. The measured coating thickness was 1.2 mm, and the coating composition was Fe. 42 Co 27 Ni 31 .

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials, characterized in that, Includes the following steps: S1, a coating is prepared on the surface of a cathode plate by electrodeposition; during the electrodeposition process, the plating solution is a mixed solution of ferric sulfate, nickel sulfate, nickel chloride, cobalt sulfate and boric acid, and the duty cycle of the AC power supply is 0.5-0.8; anionic surface brightener and wetting agent are added to the plating solution; in S1, the anionic surface brightener includes sodium saccharin and 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate; S2, the plated layer is stripped to obtain Fe 35-42 Co 27-34 Ni 30-31 A nanocrystalline alloy has a grain size of nanometer level and a nanometer-level hard 9R phase in the grain interior.

2. The method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials according to claim 1, characterized in that, In S1, the molar ratio of Fe 2+ , Co 2+ , and Ni 2+ in the plating solution is (12.3-18.7) : (21.4-28.7) : (59.0-59.9).

3. The method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials according to claim 1, characterized in that, In S1, the concentration of sodium saccharin in the plating solution is 2-5 g / L, the concentration of 1,4-butynediol is 0.1-0.5 g / L, and the concentration of sodium dodecyl sulfate is 0.03-0.06 g / L.

4. The method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials according to claim 1, characterized in that, In S1, the current density in the electrodeposition process is 2-2.5 A / dm 2 , the plating solution temperature is 55-70 ℃, and the pulse current electroplating time is 90-120 h.

5. The method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials according to claim 1, characterized in that, In S1, during the electrodeposition process, the anode plate is a soluble anode, including nickel, iron, and cobalt plates, while the cathode plate is a stainless steel plate.

6. The method for electrodepositing iron-cobalt-nickel nano-soft magnetic materials according to claim 1, characterized in that, In S1, the plating solution is purified by adsorbing impurities with activated carbon, and the pH value of the plating solution is adjusted to 1.5-2.5 after impurity removal.

7. A soft magnetic nanomaterial of iron, cobalt, and nickel prepared by any one of claims 1-6, characterized in that, including Fe 35-42 Co 27-34 Ni 30-31 nanocrystalline alloys and hard 9R phase, the Fe 35-42 Co 27-34 Ni 30-31 nanocrystalline alloys are FCC single phase structure.

8. The iron-cobalt-nickel nano-soft magnetic material according to claim 7, characterized in that, The Fe 35-42 Co 27-34 Ni 30-31 The average grain size of the nanocrystalline alloy is 20-23 nm, and the grain size of the hard 9R phase is 3-20 nm.

9. The iron-cobalt-nickel nano-soft magnetic material according to claim 7, characterized in that, The iron-cobalt-nickel nano-soft magnetic material has an ultimate tensile strength of 2.7-2.9 GPa, an elongation at break of 12.4-13.9%, a room temperature coercivity of 0.40-0.60 Oe, and a saturation magnetization of 146-150 emu / g.

Citation Information

Patent Citations

  • Process for preparing bright diphase and double-peak nanocrystalline nickel-cobalt alloy coating by adopting single pulse electrodepositing

    CN106987863A

  • Preparation process of electrodeposition single-phase component gradient nanocrystalline iron-cobalt-nickel alloy

    CN115449867A