Method for improving yellowing of PHA
By combining PHA with organic peroxide crosslinking agents, anti-hydrolysis agents, and antioxidants, the problems of yellowing and poor transparency of PHA materials were solved, and the stability and transparency of the materials were improved.
Patent Information
- Application Number
- CN202610112918.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-27
- Publication Date
- 2026-04-24
AI Technical Summary
Existing PHA materials suffer from yellowing and poor transparency, which limits their widespread application.
PHA was compounded with organic peroxide crosslinking agents, anti-hydrolysis agents and antioxidants and then thermally processed to improve yellowing and increase transparency.
It effectively inhibits the yellowing of PHA, improves the transparency and thermal stability of the material, and expands its application range.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of downstream processing in biochemical engineering. More specifically, this invention relates to a method for improving yellowing of PHA. Background Technology
[0002] Due to the problem of white pollution, traditional blown film materials such as PE are being banned and replaced by biodegradable materials such as PBAT, PLA, and PBS. Biodegradation requires specific composting conditions and is therefore subject to limitations.
[0003] Polyhydroxyalkanoates (PHA) are a novel bio-based and renewable biodegradable material. Compared to traditional non-recyclable plastics such as petroleum, PHA's biggest advantage is that its production substrates are all recyclable carbon sources (e.g., starch sugars, food waste, and hydrolyzed straw sugars). Furthermore, the entire polymerization process of PHA is biopolymerization rather than chemical polymerization, significantly reducing carbon emissions during production, which is of great significance in responding to the goals of "carbon neutrality" and "carbon peaking." In addition, PHA has excellent biodegradability. While most biodegradable materials require composting conditions to degrade, PHA is spontaneously biodegradable, degrading naturally in a controlled manner without composting. It ultimately produces carbon dioxide and water, without polluting the environment, making it a recognized environmentally friendly material.
[0004] Poly-β-hydroxybutyrate (PHB) and poly-(3-hydroxybutyrate-co-4-hydroxybutyrate), P3HB4HB, are both biomaterials with good biocompatibility, biodegradability, and mechanical properties. However, while possessing many advantages, they also have their own drawbacks, such as PHB's yellowing and poor transparency, which significantly limit their applications. Therefore, it is necessary to modify PHB materials to improve yellowing inhibition and transparency, resulting in ideal specialized materials. Summary of the Invention
[0005] In order to solve the above-mentioned problems of PHA, the inventors have invented a method to improve the yellowing of PHA, wherein PHA such as PHB can improve and inhibit yellowing and increase transparency by compounding with organic peroxide crosslinking agents, anti-hydrolysis agents and antioxidants.
[0006] Therefore, the present invention provides a method for preparing yellowing-improving PHA, which includes the following steps: (1) mixing PHA material with a compound additive containing a crosslinking agent, an antioxidant and an anti-hydrolysis agent; and (2) subjecting the mixture obtained in step (1) to thermal processing.
[0007] In one embodiment, the PHA comprises one or a combination of two or more of the following: poly-3-hydroxybutyrate (PHB), poly-3-hydroxyvalerate (PHV), poly-3-hydroxypropionate (P3HP), a copolymer of 3-hydroxybutyric acid and 4-hydroxybutyric acid (P34HB), a copolymer of 3-hydroxybutyric acid and 3-hydroxyvalerate (PHBV), poly-3-hydroxyoctanoate (PHO), poly-3-hydroxynonanoate (PHN), a copolymer of 3-hydroxybutyric acid and 3-hydroxyhexanoate (PHBHHx), a copolymer of 3-hydroxybutyric acid, 4-hydroxybutyric acid and 3-hydroxyvalerate (P3HB4HB3HV), or a copolymer of 3-hydroxybutyric acid, 4-hydroxybutyric acid and 5-hydroxyvalerate (P3HB4HB5HV).
[0008] In another preferred embodiment, the PHA is PHA powder. Preferably, the PHA powder is prepared by microbial fermentation. Preferably, the PHA powder can be obtained by the following steps: a) fermenting recombinant bacteria, such as Escherichia coli or halophilic bacteria, in a culture medium to obtain PHA fermentation broth; b) centrifuging the PHA fermentation broth to remove the supernatant and washing it with water; c) breaking down the PHA emulsion after washing to precipitate intracellular PHA products in the broken-down solution; d) separating and concentrating the PHA products in the solution using a centrifuge to obtain a suspension concentrate with a dry matter content of 25% to 30%; e) drying the concentrate to obtain powdered PHA product.
[0009] In another embodiment, the PHA is a PHB that satisfies one or more of the following conditions: 1) a molecular weight of 30 to 1,000,000 (Da) (e.g., 20, 30, 40, 50, 60, 70, 80, 90, and 1,000,000 Da); 2) a molecular weight distribution (PDI, Mw / Mn) of 1 to 2.3 (e.g., 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, and 2.3); 3) a particle size of 3 to 20 micrometers (e.g., 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20 micrometers); and 4) a raw material content of 60 wt% to 99 wt% (based on the total weight of the biodegradable coating composite material) (e.g., 60 wt%, 65 wt%). wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%).
[0010] In one embodiment, the crosslinking agent is selected from organic peroxide crosslinking agents, preferably from bis-tert-butylperoxyisopropylbenzene (BIPB), dicumyl peroxide (DCP), di-tert-butyl peroxide (DTBP), and benzoyl peroxide (BPO).
[0011] In one embodiment, the antioxidant is selected from hindered phenolic antioxidants, phosphite-based auxiliary antioxidants, thioester antioxidants (preferably antioxidants DLTDP and DSTDP), natural antioxidants, and combinations thereof. The hindered phenolic antioxidants include antioxidants 1010, 1076, 2246, 626, 245, 168, and BHT (butylated hydroxyanisole). The natural antioxidants are preferably selected from vitamin C, vitamin E, β-carotene, polyphenolic compounds, selenium, coenzyme Q10, plant extracts, and combinations thereof.
[0012] In one embodiment, the anti-hydrolysis agent is selected from polycarbodiimide, monocarbodiimide, dicarbodiimide, oxazoline compounds, epoxy compounds, and isocyanate compounds. Anti-hydrolysis agents with similar chemical structures or mechanisms of action to polycarbodiimide mainly include monocarbodiimide, oxazoline compounds, epoxy compounds, and isocyanate compounds, all of which inhibit the autocatalytic hydrolysis process by capturing the terminal carboxyl groups or active hydrogen generated during hydrolysis. Monocarbodiimide is a monofunctional analog of polycarbodiimide, containing only one -N=C=N- functional group in its molecule. It is a liquid or crystalline solid at room temperature, exhibiting high reactivity and solubility. It can rapidly react with the terminal carboxyl groups to generate stable acylurea, making it suitable for scenarios requiring efficient and rapid stabilization. Oxazoline compounds (such as 2-oxazoline) react with carboxylic acids through a five-membered nitrogen-containing heterocyclic structure to generate stable products. Their mechanism is similar to that of carbodiimides, but with a greater emphasis on end-capping, while also improving polymer compatibility. Epoxides (such as glycidyl ethers) utilize the high reactivity of epoxy groups to react with terminal carboxyl or hydroxyl groups, not only inhibiting catalysis but also repairing chain scissions, especially in polyurethanes where they are more effective than carbodiimides. Isocyanates achieve chain end-capping through the reaction of -NCO groups with active hydrogen (such as terminal carboxyl or amine groups), thereby blocking the hydrolysis catalytic cycle. Their mechanism is similar to that of carbodiimides, but they are more suitable for biodegradable polyester systems.
[0013] In one embodiment, the weight ratio of the PHA material to the compounding agent is approximately 100:0.1~5 (e.g., 0.1, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5 or 5.0).
[0014] In one embodiment, the weight ratio of the crosslinking agent, antioxidant, and anti-hydrolysis agent in the compound is approximately 0.1~0.5 (0.1, 0.2, 0.3, 0.4, 0.5): 0.3~1.0 (e.g., 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0): 0.3~1.0 (e.g., 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0).
[0015] In one embodiment, the compounding agent further comprises one or more of a penetration enhancer, a nucleating agent, a filler, a chain extender, a compatibilizer, and a lubricant, preferably comprising a penetration enhancer and a nucleating agent, as well as optional fillers, chain extenders, compatibilizers, and / or lubricants.
[0016] In one embodiment, the antireflective agent is an organosilicon antireflective agent (e.g., product number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.).
[0017] In one embodiment, the weight percentage of the penetration enhancer in the compound is about 0.1-2%.
[0018] In one embodiment, the nucleating agent is selected from: inorganic nucleating agents, organic nucleating agents, and polymeric nucleating agents, preferably from fatty acid amides including ethylene bis-stearamide (EBS), erucamide, oleamide, linoleamide, and palmitamide; fatty alcohol derivatives including xylitol, neopentyl glycol, trimethylolethane, pentaerythritol, isosorbide, sorbitol, mannitol, maltitol, and erythritol; hexagonal crystal compounds including boron nitride, silicon nitride, titanium nitride, boron carbide, silicon carbide, titanium carbide, magnesium oxide, and aluminum oxide; AD-506; LD-6; and combinations thereof.
[0019] In a preferred embodiment, the nucleating agent is P252, a nucleating agent for BRUGGOLEN P250 thermoplastic from Germany.
[0020] In one embodiment, the filler material is selected from inorganic fillers including talc, calcium carbonate, silica, montmorillonite, and Le zeolite.
[0021] In one embodiment, the chain extender is selected from: Chengju New Materials series CE-100, CE-208, CE301, BASF series ADR4468, ADR4370S, ADR4400, ADR4300, 7200N and combinations thereof.
[0022] In one embodiment, the compatibilizer is selected from Chengju New Materials series CA-200, CA-100, EsunBio5004K, BASF series compatibilizer 8110, compatibilizer 8210, compatibilizer AX8900 and combinations thereof.
[0023] In one embodiment, the lubricant is selected from ethylene bis-stearamide (EBS), talc, mica powder, potassium carbonate, hexagonal boron nitride, and combinations thereof.
[0024] In a preferred embodiment, the PHA is PHB, or a mixture of PHB and P34HB, and the compounding additives include: crosslinking agent BIPB (di-tert-butyl peroxide diisopropylbenzene) or DCP (diisopropylbenzene peroxide); antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]); hydrolysis resistant agent: polycarbodiimide; clearing agent (organosilicon clearing agent (e.g., product number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.)); nucleating agent: P252.
[0025] In a preferred embodiment, the PHA is PHB, and the compounding additives include: crosslinking agent BIPB (bis-tert-butyl peroxide diisopropylbenzene), 0.1 parts by weight; antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), 0.2 parts by weight; anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight; clearing agent (organosilicon clearing agent (e.g., product number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.)), 0.8 parts by weight; nucleating agent: P252, 0.1 parts by weight.
[0026] In a preferred embodiment, the PHA is a mixture of PHB and P34HB, and the compounding additives include: crosslinking agent BIPB (bis-tert-butyl peroxide diisopropylbenzene), 0.1 parts by weight; antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), 0.2 parts by weight; anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight; clearing agent (organosilicon clearing agent (e.g., product number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.)), 0.8 parts by weight; nucleating agent: P252, 0.1 parts by weight.
[0027] In a preferred embodiment, the PHA is PHB, and the compounding additives include: crosslinking agent DCP (dicumyl peroxide), 0.1 parts by weight; antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), 0.2 parts by weight; anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight; brightening agent (organosilicon brightening agent (e.g., product number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.)), 0.8 parts by weight; nucleating agent: P252, 0.1 parts by weight.
[0028] In one embodiment, the thermal processing includes melting, extruding, cooling, drying and granulating the mixture obtained in step (1) in a twin-screw extruder, and optionally also includes hot pressing.
[0029] In one embodiment, the twin-screw extruder is configured as follows: feed rate: 5 to 160 kg / h; zone temperature: 110 to 180°C; screw speed: 80 to 220 r / min (e.g., 200 r / min); cooling (air-cooled or water-cooled) temperature controlled at 40 to 60°C.
[0030] In a preferred embodiment, a high-speed mixer is used for mixing in step (1), for example, mixing at 1500 rpm for 10 minutes.
[0031] In a preferred embodiment, the twin-screw extruder has a heating temperature of 110-180°C, a screw length-to-diameter ratio of 44:1, a screw speed of 200 rpm, and is used for extrusion granulation.
[0032] Another aspect of the present invention provides the application of PHA prepared according to the method of the present invention in the preparation of packaging materials, biomedical materials, drug carriers, biodegradable agricultural films, slow-release fertilizers, ecological building materials, conductive materials, food or cosmetics.
[0033] Materials primarily composed of PHB and P34HB exhibit yellowing during heat processing. This yellowing is mitigated and transparency improved by using compounded additives, including organic peroxidizers, anti-hydrolysis agents, and antioxidants. Crosslinking agents, through their active groups at both ends, covalently bond with the hydroxyl and sulfide groups on the PHA molecule, forming a bridging structure that transforms the linear polymer material into a three-dimensional network structure. The synergistic effect of stabilizers and antioxidants enhances thermal stability, simultaneously suppresses PHA yellowing during heat processing, and improves transparency.
[0034] In a particularly preferred embodiment PHB: Molecular weight 300,000-1,200,000 Daltons, 60-98 parts by weight; or P34HB: Molecular weight 300,000-600,000 Daltons, 40-10 parts by weight.
[0035] Additives: Crosslinking agent: 0.1-0.5 parts by weight, anti-hydrolysis agent: 0.3-1.0 parts by weight, antioxidant: 0.3-1.0 parts by weight.
[0036] Crosslinking agent: organic peroxide BIPB (di-tert-butyl peroxide diisopropylbenzene) is a chemical raw material mainly used as a crosslinking agent for rubber and plastics. It is characterized by being odorless and having low irritation. The following is its core information: chemical properties Chemical name: Di-tert-butylperoxide diisopropylbenzene CAS No.: 2212-81-9 (or 25155-25-3) Anti-hydrolysis agent: polycarbodiimide Antioxidants: one or more of the following: 1010 (chemical name: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 168 (chemical name: tris[2,4-di-tert-butylphenyl]phosphite, CAS No.: 31570-04-4).
[0037] Special material preparation: Weigh each component according to the weight ratio, mix for 10 min using a high-speed mixer at 1500 rpm, and then extrude and granulate using a parallel twin-screw extruder at a heating temperature of 110-180℃, a screw length-to-diameter ratio of 44:1-56:1, and a screw speed of 100-400 rpm.
[0038] The beneficial effects of this invention are: A) Use biologically derived, biosynthesized, and biodegradable PHA as the main raw material to improve the thermal processing performance of PHB.
[0039] B) By improving the crosslinking modification of PHB and PHB blends, thermal decomposition can be effectively reduced and yellowing can be prevented during secondary thermal processing.
[0040] C) The production process is simple and the cost is low, and it has broad application prospects. Attached Figure Description
[0041] The above features and advantages of the present invention will become more apparent from the following detailed description taken in conjunction with the accompanying drawings, wherein: Figure 1 The color of the PHA obtained in Comparative Example 1; Figure 2 The color of the PHA obtained in Example 1; Figure 3 The color of the PHA obtained in Example 2; and Figure 4 The color of PHA obtained in Example 3. Detailed Implementation
[0042] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0043] Unless otherwise indicated, the terms used herein have their general technical meanings as understood by those skilled in the art.
[0044] In this invention, the singular articles “a” and “the” cover a plurality of indicators unless the context clearly indicates otherwise. All references cited herein are incorporated herein by reference in their entirety.
[0045] The use of "comprising" or "including" in this invention is an open-ended description that includes all specified components or steps described, as well as other specified components or steps that do not materially affect the description.
[0046] The term "and / or" as used in this invention encompasses all combinations of items connected by the term, and should be considered as if each combination had been individually listed herein. For example, "A and / or B" includes "A", "A and B", and "B". As another example, "A, B and / or C" includes "A", "B", "C", "A and B", "A and C", "B and C", and "A and B and C".
[0047] The present invention is further illustrated in the following examples. These examples are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified, the reagents, materials, etc., used in the examples are commercially available. All quantitative experiments were performed in triplicate, and the results were averaged. Unless otherwise indicated, parts refer to parts by weight. Example 1
[0048] Example 1 PHB: Molecular weight 800,000, 98 parts by weight (Beijing Microstructure Workshop Biotechnology Co., Ltd.); Crosslinking agent: BIPB peroxide (di-tert-butyl peroxide diisopropylbenzene, purchased from AkzoNormion), 0.1 parts by weight; Antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], purchased from Rianon), 0.2 parts by weight; Anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight (purchased from Shanghai Langyi); Brightening agent 0.8 parts by weight (organosilicon, item number XY-6118, purchased from Dongguan Yunfeiyang Plastic Technology Co., Ltd.); Nucleating agent: 0.1 parts by weight (P252 purchased from Brügmann).
[0049] Special material preparation: Weigh each component according to the weight ratio, mix at 1500 rpm for 10 min using a high-speed mixer (Suzhou Haoda Machinery Co., Ltd., SHR-50A high-speed mixer), and then extrude and granulate using a parallel twin-screw extruder (China Nanjing Juli Chemical Machinery Co., Ltd., model SHJ-35B) with a heating temperature of 110-180℃, a screw length-to-diameter ratio of 44:1, and a screw speed of 200 rpm.
[0050] Example 2 PHB: 800,000 molecular weight, 80 parts by weight (Beijing Microstructure Workshop Biotechnology Co., Ltd.); P34HB, 4HB ratio of 15 mol%, molecular weight 710,000, 20 parts by weight (Beijing Microstructure Workshop Biotechnology Co., Ltd.); Crosslinking agent: BIPB (bis-tert-butyl peroxide diisopropylbenzene), 0.1 parts by weight; Antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, Rianon), 0.2 parts by weight; Anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight (Shanghai Langyi); Brightening agent: 0.8 parts by weight (Dongguan Yunfeiyang Plastic Technology Co., Ltd.); Nucleating agent: 0.1 parts by weight (Brügmann P252).
[0051] Special material preparation: Weigh each component according to the weight ratio, mix at 1500 rpm for 10 min using a high-speed mixer (Suzhou Haoda Machinery Co., Ltd., SHR-50A high-speed mixer), and then extrude and granulate using a parallel twin-screw extruder (China Nanjing Juli Chemical Machinery Co., Ltd., model SHJ-35B) with a heating temperature of 110-180℃, a screw length-to-diameter ratio of 44:1, and a screw speed of 200 rpm.
[0052] Example 3 PHB: Molecular weight 800,000, 98 parts (Beijing Microstructure Factory Biotechnology Co., Ltd.); Crosslinking agent: DCP (dicumyl peroxide) (Nouryon, Akzo), 0.1 parts by weight; Antioxidant: 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, Rianlon), 0.2 parts by weight; Anti-hydrolysis agent: polycarbodiimide, 0.1 parts by weight (Shanghai Langyi); Brightening agent 0.8 parts by weight (Dongguan Yunfeiyang Plastic Technology Co., Ltd.); Nucleating agent: 0.1 parts by weight (Brügmann P252).
[0053] Special material preparation: Weigh each component according to the weight ratio, mix at 1500 rpm for 10 min using a high-speed mixer (Suzhou Haoda Machinery Co., Ltd., SHR-50A high-speed mixer), and then extrude and granulate using a parallel twin-screw extruder (China Nanjing Juli Chemical Machinery Co., Ltd., model SHJ-35B) with a heating temperature of 110-180℃, a screw length-to-diameter ratio of 44:1, and a screw speed of 200 rpm.
[0054] Comparative Example 1 100% PHB (molecular weight 800,000, 98 parts (Beijing Microstructure Workshop Biotechnology Co., Ltd.)) was mixed at 1500 rpm for 10 min using a high-speed mixer (Suzhou Haoda Machinery Co., Ltd., SHR-50A high-speed mixer) and extruded into granules using a parallel twin-screw extruder (China Nanjing Juli Chemical Machinery Co., Ltd., model SHJ-35B) with a heating temperature of 110-180℃, a screw length-to-diameter ratio of 44:1, and a screw speed of 200 rpm.
[0055] The PHA particles prepared in Examples 1 to 3 and Comparative Example 1 were tested for brightness (L value), A value, and B value. The L value represents lightness (0-100, 0 is black, 100 is white); the A value represents red-green hue (positive value is red, negative value is green); and the B value represents yellow-blue hue (positive value is yellow, negative value is blue).
[0056] The measuring instrument used is a benchtop spectrophotometer - YS6080 (Guangdong Sanenshi Technology Co., Ltd.). Operating instructions: 1. Black and White Calibration: On the measurement interface, click "□"; return to the main menu interface, click "Black and White Calibration," and perform black calibration first. Position the black tube as prompted and press the measurement button to perform calibration. After completion, press 1 to continue and perform white calibration. Position the white board as prompted and press the measurement button to perform calibration. After correct calibration, the instrument system will count down according to the user-set black and white calibration validity period. 2. Conduct the test: Prepare the sample, measure each sample three times, changing the position each time, and record the values.
[0057] The final data is the average of the three measurements.
[0058] The results are shown in Table 1 below.
[0059]
[0060] 1. Brightness (L value) comparison Highest value: Example 1 (80.45) is the sample with the highest brightness.
[0061] Lowest value: Comparative Example 1 (73.23) is the sample with the lowest brightness.
[0062] 2. Comparison of A-values (red and green axes) Reddish sample: Comparative Example 1 (4.36) is the only sample that is clearly reddish.
[0063] Greenish sample: Example 3 (-0.58) is a greenish sample, while the A values of other samples are close to neutral.
[0064] 3. Comparison of B-values (yellow-blue axis) The highest value: Comparative Example 1 (32.12) is the sample with the highest degree of yellowing.
[0065] Minimum value: Example 1 (18.56) is the sample with the lowest yellowness. Examples 2 and 3 also have low yellowness, indicating that the yellowness has been improved.
[0066] In the compound additives of the present invention, the crosslinking agent, antioxidant, and anti-hydrolysis agent have a synergistic effect on the anti-yellowing effect of PHA.
[0067] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0068] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately. Furthermore, various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the spirit of the present invention, and should also be regarded as the content disclosed by the present invention.
Claims
1. A method for preparing yellowing-improving PHA, comprising the following steps: (1) Mix the PHA material with a compound additive containing a crosslinking agent, an antioxidant and an anti-hydrolysis agent; and (2) The mixture obtained in step (1) is subjected to thermal processing.
2. The method according to claim 1, wherein the PHA comprises one or a combination of two or more of the following: poly-3-hydroxybutyrate (PHB), poly-3-hydroxyvalerate (PHV), poly-3-hydroxypropionate (P3HP), a copolymer of 3-hydroxybutyric acid and 4-hydroxybutyric acid (P34HB), a copolymer of 3-hydroxybutyric acid and 3-hydroxyvalerate (PHBV), poly-3-hydroxyoctanoate (PHO), poly-3-hydroxynonanoate (PHN), a copolymer of 3-hydroxybutyric acid and 3-hydroxyhexanoate (PHBHHx), a copolymer of 3-hydroxybutyric acid, 4-hydroxybutyric acid and 3-hydroxyvalerate (P3HB4HB3HV), or a copolymer of 3-hydroxybutyric acid, 4-hydroxybutyric acid and 5-hydroxyvalerate (P3HB4HB5HV).
3. The method according to claim 1 or 2, wherein the crosslinking agent is selected from organic peroxide crosslinking agents, preferably selected from bis-tert-butylperoxyisopropylbenzene (BIPB), dicumyl peroxide (DCP), di-tert-butyl peroxide (DTBP) and benzoyl peroxide (BPO).
4. The method according to any one of claims 1 to 3, wherein the antioxidant is selected from hindered phenolic antioxidants, phosphite-based auxiliary antioxidants, thioester antioxidants, natural antioxidants, and combinations thereof, wherein the hindered phenolic antioxidants include antioxidant 1010, antioxidant 1076, antioxidant 2246, antioxidant 626, antioxidant 245, antioxidant 168, and antioxidant BHT (butylated hydroxyanisole), and the natural antioxidant is preferably selected from vitamin C, vitamin E, β-carotene, polyphenolic compounds, selenium, coenzyme Q10, plant extracts, and combinations thereof.
5. The method according to any one of claims 1 to 4, wherein the anti-hydrolysis agent is selected from polycarbodiimide, monocarbodiimide, dicarbodiimide, oxazoline compounds, epoxy compounds and isocyanate compounds.
6. The method according to any one of claims 1 to 5, wherein: 1) The weight ratio of the PHA material to the compounding agent is approximately 100:0.1~5; and / or 2) The weight ratio of the crosslinking agent, antioxidant and anti-hydrolysis agent in the compound is approximately 0.1~0.5 : 0.3~1.0 : 0.3~1.
0.
7. The method according to any one of claims 1 to 6, wherein the compounding agent further comprises one or more of a penetration enhancer, a nucleating agent, a filler, a chain extender, a compatibilizer, and a lubricant, preferably comprising a penetration enhancer and a nucleating agent, as well as optional fillers, chain extenders, compatibilizers, and / or lubricants.
8. The method according to any one of claims 1 to 7, wherein the thermal processing comprises melting, extruding, cooling, drying and granulating the mixture obtained in step (1) in a twin-screw extruder, optionally further comprising hot pressing.
9. The method according to claim 8, wherein the twin-screw extruder is configured as follows: feeding speed: 5 to 160 kg / h; zone temperature: 110 to 180°C; screw speed: 80 to 220 r / min; cooling (air cooling or water cooling) temperature controlled at 40 to 60°C.