Preparation method and application of high-dispersity multi-walled carbon nanotube powder
By using styrene-maleic anhydride copolymer and monoethanolamine as dispersants, combined with high-pressure homogenization and spray drying processes, the problem of carbon nanotube agglomeration in lithium-ion batteries was solved, achieving excellent dry electrode dispersibility and improved battery performance.
Patent Information
- Application Number
- CN202610276856.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-09
- Publication Date
- 2026-05-15
AI Technical Summary
Carbon nanotubes tend to agglomerate in lithium-ion batteries, resulting in an uneven conductive network that affects battery performance. Furthermore, existing dispersion methods cannot meet the requirements of dry electrode processes.
A dispersant composed of styrene-maleic anhydride copolymer and monoethanolamine is used to form a stable coating layer through high-pressure homogenization and spray drying processes, ensuring that carbon nanotubes have excellent dispersibility in dry electrodes.
Uniform dispersion of carbon nanotubes in dry electrodes was achieved, constructing a complete conductive network and improving the energy density and cycle stability of the battery.
Smart Images

Figure CN122035834A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon nanotube technology, and in particular to a method for preparing highly dispersible multi-walled carbon nanotube powder. Background Technology
[0002] In recent years, carbon nanotubes have made significant progress in the application of conductive agents in lithium-ion batteries. Currently, commercially available carbon nanotubes are mostly multi-walled carbon nanotubes, which are widely used as conductive additives in lithium-ion battery cathodes and polymer composite materials. Compared to traditional carbon black, adding a smaller proportion of highly dispersed carbon nanotubes can meet performance requirements, thereby improving battery energy density. However, due to the strong van der Waals forces between carbon nanotubes, they are prone to agglomeration and entanglement, forming aggregates that are difficult to untangle. This agglomeration severely affects the intrinsic properties of carbon nanotubes, especially when added as a conductive agent to solid-state battery electrodes, leading to uneven distribution of the conductive network and reducing the battery's rate performance and cycle life. Currently, the main method is to disperse powdered carbon nanotubes into a uniform slurry. However, carbon nanotube conductive slurries contain the solvent N-methylpyrrolidone (NMP), which reacts with solid electrolyte oxides, thus failing to meet the requirements of dry electrode technology. Dry electrode technology is a process for directly preparing electrodes through dry powder mixing and calendering, offering advantages such as short process, low cost, and high energy density. However, this process lacks the shear force of liquid media, placing almost stringent requirements on the dispersibility of the conductive agent. If aggregated carbon nanotubes are used directly, it is impossible to construct a uniform three-dimensional conductive network in a dry state, resulting in poor electrode conductivity and a sharp decline in battery performance.
[0003] Currently, methods for improving the dispersibility of carbon nanotube powders mainly include chemical modification and physical dispersion (such as ultrasonication and high-speed shearing). However, neither chemical modification nor physical dispersion modification currently considers compatibility with dry electrode processes. Therefore, developing a method for preparing carbon nanotube powders that can effectively overcome carbon nanotube agglomeration, has excellent dry redispersibility, and is applicable to dry electrode processes has become an urgent technical problem to be solved in this field. Summary of the Invention
[0004] Therefore, based on the above background, the present invention provides a method for preparing highly dispersible multi-walled carbon nanotube powder. Through reasonable dispersant composition and process steps, the agglomeration problem of carbon nanotubes can be effectively solved, and the resulting powder has excellent dry dispersibility and is suitable for dry electrode processes.
[0005] The technical solution provided by this invention is as follows:
[0006] A method for preparing highly dispersible multi-walled carbon nanotube powder includes the following steps:
[0007] S1 Predispersed Slurry Preparation
[0008] Preparation of S1.1 Dispersion Modified Liquid
[0009] A dispersion-modified liquid is prepared by adding a dispersant to water and stirring until homogeneous; the dispersant is composed of a styrene-maleic anhydride copolymer and monoethanolamine.
[0010] S1.2 Multi-walled carbon nanotubes were added to the dispersion modification liquid, and after high-pressure homogenization, a pre-dispersed slurry was prepared.
[0011] S2 spray-drying of the pre-dispersed slurry yields highly dispersible multi-walled carbon nanotube powder.
[0012] Furthermore, the multi-walled carbon nanotubes in step S1.2 undergo pretreatment, which includes the following steps:
[0013] ① High-temperature oxidation treatment of multi-walled carbon nanotubes;
[0014] ② The multi-walled carbon nanotubes after the high-temperature oxidation treatment in step ① are subjected to acid washing and high-temperature oxidation treatment.
[0015] ③ Wash the multi-walled carbon nanotubes that have undergone acid washing and high-temperature oxidation treatment in step ② with water until neutral, dry them, and pulverize them to obtain pretreated multi-walled carbon nanotubes.
[0016] Further, the dispersant in step S1.1 is composed of styrene-maleic anhydride copolymer and monoethanolamine in a mass ratio of (1-3):(2-3), wherein the number average molecular weight (Mn) of the styrene-maleic anhydride copolymer is 1,500 to 10,000 g / mol.
[0017] In further step S1.2, the mass ratio of the amount of multi-walled carbon nanotubes added to the dispersant is (2-9):1.
[0018] The conditions for spray drying in further step S2 are as follows:
[0019] Inlet temperature 120-200℃, outlet temperature 80-110℃, feed rate <150ml / h, atomization pressure <0.2MPa.
[0020] Based on the same inventive concept, the present invention also provides a highly dispersed multi-walled carbon nanotube powder prepared by the aforementioned method for preparing highly dispersed multi-walled carbon nanotube powder.
[0021] Based on the same inventive concept, this invention also provides the application of the highly dispersed multi-walled carbon nanotube powder prepared by the aforementioned method in the preparation of solid-state batteries.
[0022] Furthermore, the electrodes of the solid-state battery are prepared using a dry electrode method.
[0023] The beneficial effects achieved by this invention are as follows:
[0024] (1) The present invention uses a reasonable ratio of styrene-maleic anhydride copolymer (SMA) and monoethanolamine (MEA) to form a stable coating layer on the surface of carbon nanotubes, providing a lasting steric hindrance and electrostatic stabilization effect, and improving the dispersibility of carbon nanotube powder. The SMA molecular chain is strongly adsorbed on the surface of carbon nanotubes through the π-π conjugation effect. On the one hand, MEA acts as an organic base, reacting with the anhydride groups in SMA to generate carboxylate, enhancing its water solubility and steric hindrance effect. On the other hand, its hydroxyl groups (forming hydrogen bonds) can also assist in adsorption. The two work together to form a stable polymer coating layer on the surface of carbon nanotubes. After drying, the coating layer can prevent the carbon nanotubes from hard agglomerating, and its structure has dynamic responsiveness under the shear force of dry mixing, which can realize the rapid redispersibility of carbon nanotubes and achieve excellent dry dispersibility.
[0025] (2) The carbon nanotube powder of the present invention can be rapidly deagglomerated and uniformly distributed in dry mixing, which is particularly suitable for solid-state battery systems with extremely high requirements for electrode uniformity. It can effectively construct a perfect conductive network and improve the battery capacity and cycle stability.
[0026] (3) The present invention uses a reasonably formulated dispersant combined with process steps. It utilizes high pressure homogenization to provide strong shear force to break agglomerates and forces the dispersant molecules to fully wrap the newly exposed carbon nanotube surface. Then, combined with spray drying, the dispersion state is fixed instantly, ensuring that the obtained powder has the characteristics of easy redispersibility in dry state, so that it can also meet the requirements of solvent-free mixing of dry electrodes.
[0027] (4) The multi-walled carbon nanotubes of the present invention can be applied to dry electrode solid-state batteries, which can significantly reduce the electrode interface resistance and improve the utilization rate of active materials, thereby improving the energy density and cycle life of the battery.
[0028] Instruction manual illustrations
[0029] Figure 1 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 1.
[0030] Figure 2 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 2.
[0031] Figure 3 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 2.
[0032] Figure 4 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 2.
[0033] Figure 5 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 2.
[0034] Figure 6 The image shows an electron microscope image of the multi-walled carbon nanotube powder prepared in Example 2. Detailed Implementation
[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] The technical solution of this invention: A method for preparing highly dispersible multi-walled carbon nanotube powder, comprising the following steps:
[0037] 1) Pretreatment of multi-walled carbon nanotubes
[0038] To prevent the presence of a large number of metallic impurities in multi-walled carbon nanotubes, which could affect the electron diffusion rate of the battery and increase internal resistance, carbon nanotubes need to undergo purification pretreatment through high-temperature oxidation and acid washing.
[0039] The purpose of high-temperature oxidation is to expose the catalyst metal particles at the ports or nodes of carbon nanotubes.
[0040] The specific preprocessing includes the following steps:
[0041] ① High-temperature oxidation
[0042] The raw powder of multi-walled carbon nanotubes is put into an oxidation furnace, and then nitrogen and air are introduced (the volume ratio of nitrogen and oxygen is controlled within the range of (2-5):1, and the total flow rate of the mixed gas of 30-100g carbon nanotubes is controlled within 3-6L / min), so that the carbon nanotubes react at 480-520℃ for 15-45min, and the general burn-off rate is 1%-5%.
[0043] After the high-temperature oxidation is completed, the air and heating power are turned off, and only nitrogen is passed through to allow the material to cool to room temperature before collecting the carbon nanotubes after high-temperature oxidation.
[0044] ② Pickling treatment
[0045] After high-temperature oxidation, carbon nanotubes are added to an acid solution and stirred at 60-90℃ for 8-12 hours. After filtration, they are washed with pure water until neutral, dried, and crushed to a particle size of <50μm.
[0046] The acid solution can be a hydrochloric acid solution with a mass fraction of 10%-20%.
[0047] After high-temperature oxidation and acid washing, the Fe content of multi-walled carbon nanotubes is ≤250ppm and the Co content is ≤50ppm.
[0048] 2) Mix pure water, monoethanolamine (MEA), and polyethylene-maleic anhydride copolymer (SMA) in a certain amount and proportion, stir evenly (the mass concentration of monoethanolamine is controlled at 3-8%), and then add the pretreated multi-walled carbon nanotubes obtained in step 1) in a certain proportion and stir evenly.
[0049] 3) The homogenized material is fed into a high-pressure homogenizer and homogenized at a pressure of approximately 900-1100 bar for a total processing time of 10-30 minutes to obtain a pre-dispersed slurry. This step effectively breaks up the carbon nanotube aggregates through the ultra-high shear force on the slurry and forces the dispersant molecules to fully coat the newly exposed carbon nanotube surface.
[0050] 4) Spray dry the obtained carbon nanotube conductive slurry. The equipment process conditions are: inlet temperature 120-200℃, outlet temperature 80-110℃, feed rate <300ml / h, and atomization pressure <0.2MPa.
[0051] The outlet temperature is a key control parameter. Maintaining it within a lower range of 80-110℃ ensures gentle moisture removal, preventing the carbon nanotubes from re-aggregating instantly due to excessively rapid drying. Lower feed rates and atomization pressures help form smaller droplets, reducing the number of carbon nanotubes per droplet. This results in loosely structured microspheres after drying, rather than dense lumps, which greatly facilitates subsequent redispersion.
[0052] Equipment Operation Procedure: After connecting the power supply, first turn on the fan, then the heater, to envelop the inside of the equipment in hot air. Next, insert the feed tube into the carbon nanotube conductive slurry, then turn on the compressor and peristaltic pump to atomize the slurry into small spray droplets for rapid drying. After the slurry has dried, replace the feed with clean pure water to clean the feed tube and injection needle. After cleaning, turn off the impact needle, peristaltic pump, and compressor in sequence. Wait until the outlet air temperature is below 60℃ before finally turning off the fan. This is to use the fan to drive air to cool the equipment and prevent high temperatures from burning out equipment components. After the equipment has completely stopped operating, collect the carbon nanotube powder in the finished product tank, then disassemble the equipment parts and rinse them with water, such as the spray gun, drying tower, and cyclone separator.
[0053] The number average molecular weight of the polyethylene-maleic anhydride copolymer used in the following examples was controlled at 8000-10000 g / mol, and it was purchased from Hubei Jusheng Technology Co., Ltd.
[0054] Monoethanolamine, also known as 2-aminoethanol, CAS number 141-43-5, was purchased from Shandong Zhengxing New Materials Co., Ltd.
[0055] Multi-walled carbon nanotubes were purchased from Beijing Deco Island Gold Technology Co., Ltd.
[0056] Example 1: A method for preparing highly dispersible multi-walled carbon nanotube powder, comprising the following steps:
[0057] 1) Take materials according to the following proportions:
[0058] The mass ratio of polyethylene-maleic anhydride copolymer to monoethanolamine is 1:1;
[0059] The mass ratio of multi-walled carbon nanotube powder to (polyethylene-maleic anhydride copolymer + monoethanolamine) is 9:1.
[0060] 2) Pretreatment of multi-walled carbon nanotubes
[0061] ① High-temperature oxidation
[0062] The raw powder of multi-walled carbon nanotubes is put into an oxidation furnace, and then nitrogen and air are introduced (the volume ratio of nitrogen and oxygen is controlled within the range of 5:1, and the total flow rate of the mixed gas for 80g of carbon nanotubes is controlled within 5L / min). The carbon nanotubes are reacted at 480-520℃ for 15-45min, and the general burn-off rate of 1%-5% is achieved.
[0063] After the high-temperature oxidation is completed, the air and heating power are turned off, and only nitrogen is passed through to allow the material to cool to room temperature before collecting the carbon nanotubes after high-temperature oxidation.
[0064] ② Pickling treatment
[0065] The carbon nanotubes, after high-temperature oxidation treatment, are placed in a 10% hydrochloric acid solution and stirred at 85±3℃ for 8-12 hours. After filtration, they are washed with pure water until neutral, dried, and crushed to a particle size of <50μm.
[0066] 3) Mix pure water, monoethanolamine (MEA), and polyethylene-maleic anhydride copolymer (SMA) in a certain amount and proportion, stir evenly (the mass concentration of monoethanolamine is controlled at 6%), and then add the pretreated multi-walled carbon nanotubes obtained in step 1) in a certain proportion and stir evenly.
[0067] 4) The homogenized material is fed into a high-pressure homogenizer and homogenized at a pressure of about 800-900 bar. The total processing time is controlled within 15 minutes to obtain a pre-dispersed slurry.
[0068] 5) The obtained carbon nanotube conductive slurry was spray-dried. The equipment process conditions were: inlet temperature 120℃, outlet temperature 85℃, feed rate 85ml / h, and atomization pressure 0.15MPa.
[0069] Example 2: A method for preparing highly dispersible multi-walled carbon nanotube powder, comprising the following steps:
[0070] 1) Take materials according to the following proportions:
[0071] The mass ratio of polyethylene-maleic anhydride copolymer to monoethanolamine is 1:1;
[0072] The mass ratio of multi-walled carbon nanotube powder to (polyethylene-maleic anhydride copolymer + monoethanolamine) is 3:1.
[0073] The other preparation steps are the same as in Example 1.
[0074] Example 3: A method for preparing highly dispersed multi-walled carbon nanotube powder, comprising the following steps:
[0075] 1) Take materials according to the following proportions:
[0076] The mass ratio of polyethylene-maleic anhydride copolymer to monoethanolamine is 3:2;
[0077] The mass ratio of multi-walled carbon nanotube powder to (polyethylene-maleic anhydride copolymer + monoethanolamine) is 3:1.
[0078] The other preparation steps are the same as in Example 1.
[0079] Example 4: A method for preparing highly dispersible multi-walled carbon nanotube powder, comprising the following steps:
[0080] 1) Take materials according to the following proportions:
[0081] The mass ratio of multi-walled carbon nanotube powder to polyethylene-maleic anhydride copolymer is 3:1.
[0082] Compared to Example 2, this embodiment removes monoethanolamine, and in step 3), pure water and polyethylene-maleic anhydride copolymer (SMA) are mixed and stirred evenly according to a certain amount and ratio (the mass concentration of polyethylene-maleic anhydride copolymer is the same as in Example 2), and other preparation steps are the same as in Example 1.
[0083] Example 5: A method for preparing highly dispersed multi-walled carbon nanotube powder, comprising the following steps:
[0084] 1) Pretreatment of multi-walled carbon nanotubes
[0085] Same as Example 1.
[0086] 2) Add the pretreated multi-walled carbon nanotubes obtained in step 1) to pure water (the volume added is the same as the amount of pure water added in step 3 of Example 1) and stir until homogeneous;
[0087] 3) The homogenized material is fed into a high-pressure homogenizer and homogenized at a pressure of about 800-900 bar. The total processing time is controlled within 15 minutes to obtain a pre-dispersed slurry.
[0088] 4) The obtained carbon nanotube conductive slurry was spray-dried. The equipment process conditions were: inlet temperature 210℃, outlet temperature 105℃, feed rate 85ml / h, and atomization pressure 0.15MPa.
[0089] 5) The obtained carbon nanotube conductive slurry was spray-dried under the following equipment conditions: inlet temperature 120℃, outlet temperature 85℃, feed rate 85ml / h, and atomization pressure 0.15MPa.
[0090] Example 6: A method for preparing highly dispersible multi-walled carbon nanotube powder, comprising the following steps:
[0091] 1) Take materials according to the following proportions:
[0092] The mass ratio of polyethylene-maleic anhydride copolymer to monoethanolamine is 2:3;
[0093] The mass ratio of multi-walled carbon nanotube powder to (polyethylene-maleic anhydride copolymer + monoethanolamine) is 3:1.
[0094] The other preparation steps are the same as in Example 1.
[0095] Example 7: A method for preparing highly dispersed multi-walled carbon nanotube powder, comprising the following steps:
[0096] 1) Take materials according to the following proportions:
[0097] The mass ratio of polyethylene-maleic anhydride copolymer to monoethanolamine is 3:1;
[0098] The mass ratio of multi-walled carbon nanotube powder to (polyethylene-maleic anhydride copolymer + monoethanolamine) is 3:1.
[0099] The other preparation steps are the same as in Example 1.
[0100] Electron microscopy was performed on the highly dispersed multi-walled carbon nanotube powders prepared in Examples 1 to 6. The results are shown in the appendix. Figure 1 To be continued Figure 6 , by appendix Figure 1As can be seen, the carbon nanotubes in Examples 1 to 3 and Example 6 were not entangled, and the carbon nanotube powders in Examples 1, 2, and 6 had a loose microspherical structure. The particles were well dispersed spherical or near-spherical, relatively uniform in size, with clear gaps between the particles, and a loose and porous structure. This morphology indicates that during the spray drying process, the carbon nanotubes, well coated and isolated by the dispersant (SMA+MEA), formed independent and uniform droplets, which became independent microspheres after drying. This structure is very beneficial for re-deagglomeration in dry mixing and uniform dispersion in the electrode material, thereby constructing a highly efficient conductive network. The carbon nanotube powder in Example 3 had increased structural density, and the particle boundaries were not as clear as in Examples 1 and 2, but the particle outlines were still visible. In contrast, the carbon nanotube powder in Example 4 showed obvious adhesion and fusion between particles, indicating that a certain degree of agglomeration occurred between the powders in Example 4. Analysis showed that the lack of MEA for the synergistic effect of polyethylene-maleic anhydride copolymer weakened the stabilizing effect of the dispersant on the carbon nanotubes, making local agglomeration more likely to occur during the drying process. In Example 5, the carbon nanotubes formed large-area, dense entanglements and agglomerates, with almost no independent particle structures, exhibiting a severe agglomeration state.
[0101] Dry mixing and dispersibility test
[0102] The dispersion of carbon nanotubes (CNTs) after dry mixing significantly affects resistivity and electrode performance. Poor dispersion leads to discontinuous conductive networks, increases resistivity, and reduces the electrochemical performance of the electrode. In other words, the dispersion of carbon nanotubes can be reflected to some extent by the electrochemical performance of the electrode.
[0103] Specifically, the multi-walled carbon nanotube powder product prepared in the above embodiment was used as a conductive agent and dry-mixed with lithium iron phosphate active material, sulfide solid electrolyte powder, and PTFE binder powder at a mass ratio of 90:5:3:2. The mixed powder was then rolled into a self-supporting electrode film using a calender, and finally hot-pressed onto an aluminum foil current collector to obtain the positive electrode sheet. A solid-state battery was assembled using this electrode sheet for testing (the battery was assembled in an argon-filled glove box; before assembly, the water content was ensured to be <0.1 ppm and the oxygen content <0.1 ppm).
[0104] Electrode resistivity: The resistivity of dry electrode sheets was measured using the four-probe method.
[0105] Battery rate performance test: Assembled into a solid-state battery, the stability and discharge specific capacity were tested at 0.5C rate for 150 cycles at room temperature.
[0106] The battery test results are shown in Table 1.
[0107] Table 1: Battery Test Results
[0108]
[0109] As shown in the table above, compared to Example 5 which only used SMA to modify multi-walled carbon nanotubes, the addition of MEA significantly synergistically improves the dispersibility of multi-walled carbon nanotubes with SMA. Furthermore, the resistivity, stability, and discharge specific capacity of the electrode indicate that Example 2 exhibits the best performance. This demonstrates that the carbon nanotube powder prepared using the process and proportions of Example 2 exhibits the best dispersibility during dry mixing, enabling the construction of the most complete and uniform conductive network in the electrode, thereby achieving the lowest interfacial resistance and optimal electrochemical performance. Examples 1 to 3 and 6 all used a composite dispersant composed of styrene-maleic anhydride copolymer (SMA) and monoethanolamine (MEA). Their overall performance was superior to Example 4 (which did not use MEA) and Example 5 (which did not use any dispersant). Example 2 was the best, while Example 6's performance was slightly lower than Example 2 but significantly better than the other comparative examples. This indicates that good dispersion can be achieved within a specific ratio range of SMA and MEA, and the higher the amount of MEA, the better the dispersion effect of multi-walled carbon nanotubes. In Example 1, compared to Example 2, the ratio of carbon nanotubes to dispersant was higher (i.e., the amount of dispersant was relatively lower), resulting in a slight decrease in performance. This shows that insufficient dispersant affects the complete coating and dispersion stability of carbon nanotubes. In Example 4, compared to Example 2, using only SMA without adding MEA resulted in a significant decline in all performance indicators. This shows that the absence of MEA greatly reduces the dispersion effect of SMA, making the powder more prone to agglomeration during drying and subsequent dry mixing. Example 5 showed the worst performance; analysis revealed severe agglomeration of the undispersed carbon nanotubes, preventing the formation of an effective conductive network in the dry electrode.
[0110] It is evident that the high-dispersibility multi-walled carbon nanotube powder prepared by using SMA and MEA composite dispersant provided by this invention can effectively improve the dispersibility of the powder in the dry electrode process, thereby significantly reducing the electrode resistivity and improving the cycle stability and discharge capacity of solid-state batteries.
[0111] The composition of the dispersant (synergistic effect of SMA and MEA) and its mass ratio to carbon nanotubes are key factors affecting the dispersibility and battery performance of the final product. Within the reasonable proportion range of this invention, the formulation in Example 2 achieves optimal performance.
[0112] The absence of MEA components or the complete omission of dispersants will lead to increased carbon nanotube aggregation and deterioration of battery performance.
[0113] The embodiments shown are merely one implementation of the present invention, and the actual structure is not limited to this. In conclusion, if those skilled in the art are inspired by this and design similar structures and embodiments without departing from the spirit of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing highly dispersible multi-walled carbon nanotube powder, characterized in that, Includes the following steps: S1 Predispersed Slurry Preparation Preparation of S1.1 Dispersion Modified Liquid A dispersion-modified liquid is prepared by adding a dispersant to water and stirring until homogeneous; the dispersant is composed of a styrene-maleic anhydride copolymer and monoethanolamine. S1.2 Multi-walled carbon nanotubes were added to the dispersion modification liquid, and after high-pressure homogenization, a pre-dispersed slurry was prepared. S2 spray-drying of the pre-dispersed slurry yields highly dispersible multi-walled carbon nanotube powder.
2. The method for preparing highly dispersible multi-walled carbon nanotube powder according to claim 1, characterized in that, Step S1.2 involves the pretreatment of multi-walled carbon nanotubes. The pretreatment of multi-walled carbon nanotubes includes the following steps: ① Perform high-temperature oxidation treatment on multi-walled carbon nanotubes at 450-600℃ for 30-60 minutes; ②The multi-walled carbon nanotubes after the high-temperature oxidation treatment in step ① are subjected to acid washing. ③ Wash the multi-walled carbon nanotubes treated by acid washing in step ② until neutral, dry them, and pulverize them to obtain pretreated multi-walled carbon nanotubes.
3. The method for preparing highly dispersible multi-walled carbon nanotube powder according to claim 1, characterized in that, The dispersant in step S1.1 is composed of styrene-maleic anhydride copolymer and monoethanolamine in a mass ratio of (1-3):(2-3), wherein the number average molecular weight (Mn) of the styrene-maleic anhydride copolymer is 1,500 to 10,000 g / mol.
4. The method for preparing highly dispersible multi-walled carbon nanotube powder according to claim 1, characterized in that, In step S1.2, the mass ratio of the amount of multi-walled carbon nanotubes added to the dispersant is (2-9):
1.
5. The method for preparing highly dispersible multi-walled carbon nanotube powder according to claim 1, characterized in that, The conditions for spray drying in step S2 are as follows: Inlet temperature 120℃-200℃, outlet temperature 80-110℃, feed rate <150ml / h, atomization pressure <0.2MPa.
6. The highly dispersed multi-walled carbon nanotube powder prepared by the method for preparing highly dispersed multi-walled carbon nanotube powder according to any one of claims 1 to 5.
7. The application of the highly dispersed multi-walled carbon nanotube powder prepared by the method for preparing highly dispersed multi-walled carbon nanotube powder according to any one of claims 1 to 5 in the preparation of solid-state batteries.
8. The application according to claim 7, characterized in that, The electrodes of the solid-state battery are prepared using a dry electrode method.