A method for preparing high-entropy ceramic matrix composites using a reactive infiltration process.
By generating high-entropy carbide ceramic matrices in situ through reactive melting infiltration, the problems of long preparation cycles, high porosity, and high raw material costs of high-entropy ceramic matrix composites in existing technologies are solved. This enables rapid densification and performance improvement of high-entropy ceramic matrix composites, which are suitable for thermal protection materials for hypersonic vehicles.
Patent Information
- Application Number
- CN202610533789.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-04-22
AI Technical Summary
Existing high-entropy ceramic matrix composite material preparation processes suffer from problems such as long preparation cycles, low ceramic yield, high composite material porosity, high raw material costs, and insufficient introduction of high-entropy ceramic phases, which limit their application in hypersonic vehicle thermal protection materials.
A reactive melting process is employed, in which at least four single-component carbides are mixed with a carbon source, and a multi-component ceramic slurry is introduced through vacuum or pressure impregnation. Reactive melting is then carried out under the embedding of a transition metal or alloy to generate a high-entropy carbide ceramic matrix in situ, thereby achieving rapid densification of the composite material.
The high-entropy ceramic matrix content was significantly increased, enhancing the material's high-temperature stability, oxidation resistance, and ablation resistance, thus meeting the stringent requirements of hypersonic vehicles for ultra-high temperature materials and reducing the preparation cycle and cost.
Smart Images

Figure CN122079650B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic matrix composites technology, and more specifically, to a method for preparing high-entropy ceramic matrix composites using a reactive infiltration process. Background Technology
[0002] As the Mach number of hypersonic vehicles increases, their nose cones, wing leading edges, and other components face more severe aerodynamic heating, placing stringent demands on thermal protection materials. Fiber-reinforced ceramic matrix composites, due to their superior properties such as high specific strength, oxidation resistance, and high-temperature resistance, have enormous application potential in the field of hypersonic vehicle thermal protection materials. Currently widely used single-component or multi-component ultra-high-temperature ceramic matrix composites suffer from insufficient temperature resistance due to the limited melting points of their matrix components. This makes it difficult to meet the requirements of next-generation aircraft for higher-performance thermal protection materials, thus hindering the development of thermal protection materials.
[0003] Against this backdrop, high-entropy ceramics have attracted widespread attention as an emerging material system. High-entropy ceramics are single-phase compounds composed of cations or anions of at least four elements in equimolar or near-equimolar ratios. The different lattice structures of the cations and anions induce significant lattice distortions within the material, thereby increasing the activation energy for atomic diffusion and significantly delaying grain boundary migration and elemental segregation at high temperatures, resulting in excellent high-temperature stability. Among various high-entropy ceramic systems, high-entropy carbide ceramics possess relatively high melting points and superior high-temperature mechanical properties. Furthermore, the "relay oxidation" behavior of high-entropy carbide ceramics during oxidation and ablation processes gives them superior oxidation and ablation resistance, demonstrating great application potential in the field of thermal protection materials for hypersonic vehicles. Using high-entropy carbide ceramics as a matrix to prepare fiber-reinforced high-entropy ceramic matrix composites can further extend the service temperature limits of existing thermal protection materials.
[0004] Patent 1 (CN115784746A) discloses a high-entropy ceramic matrix composite material and its preparation method. This method involves multiple cycles of impregnation, curing, and pyrolysis of a carbon fiber preform in a high-entropy carbide precursor solution containing Ti, Zr, Nb, Mo, Hf, and Ta metal elements to ultimately obtain a C / (TiZrNbMoHfTa)C composite material. While this process can achieve the preparation of high-entropy ceramic matrix composite materials, the low yield of the precursor ceramic leads to an excessively long preparation cycle, and the final composite material has a high porosity, limiting its production and application.
[0005] Document 1 "Fabrication and properties of C f / (Ti 0.2 Zr 0.2 Hf 0.2 Nb0.2 Ta 0.2 )C-SiC high-entropy ceramic matrix composites via precursor infiltration and pyrolysis[J]. 2021, 41(12): 5863-5871. "Using high-entropy carbide precursor (PHEC) and polycarbosilane (PCS) as raw materials, a two-step precursor impregnation and pyrolysis (PIP) process was used to synthesize (Ti) high-entropy ceramic matrix composites via precursor infiltration and pyrolysis[J]. 2021, 41(12): 5863-5871." 0.2 Zr 0.2 Hf 0.2 Nb 0.2 Ta 0.2 C and SiC were introduced into a three-dimensional needled carbon fiber preform to prepare C f / (Ti 0.2 Zr 0.2 Hf 0.2 Nb 0.2 Ta 0.2 C-SiC high-entropy ceramic matrix composites. This process improved the ceramic yield by optimizing the precursor composition and PIP process, and the prepared composite material had a density of 2.40 g / cm³. 3 The porosity was 13.32 vol%, but there are still problems such as excessively high porosity of composite materials and long preparation cycle.
[0006] Document 2 "Fabrication and properties of 3-dimensional 5-directional C f / (Zr 0.2 Hf 0.2 Ta 0.2 Nb 0.2 Ti 0.2 Zr2C-SiC high-entropy ceramic matrix composites by precursor infiltration and pyrolysis process[J]. 2025, 51: 15055-15066. The PIP process was used to introduce Zr2C into fiber preforms deposited at the PyC / SiC composite interface. 0.2 Hf 0.2 Ta 0.2 Nb 0.2 Ti 0.2 The composite material, prepared using C and SiC ceramic matrices, exhibits an open porosity >18 vol% and a density of approximately 1.85 g / cm³. 3Because the composite material prepared by this process has a high open porosity and a low content of high-entropy ceramic matrix, the prepared C... f / (Zr 0.2 Hf 0.2 Ta 0.2 Nb 0.2 Ti 0.2 After ablation at approximately 2000 °C for 60 s, the linear ablation rate of the C-SiC composite material is >4.8 μm / s, and the mass ablation rate is >1.958 mg / s.
[0007] Patent 2 (CN113321510A) discloses a method for preparing high-entropy ceramic matrix composites. This method involves impregnating a porous C / C preform with high-entropy carbide ceramic powder and phenolic resin slurry, followed by multiple rounds of high-temperature curing and pyrolysis to obtain a high-entropy ceramic matrix composite intermediate. Subsequently, RMI densification is performed using Si powder to finally obtain a dense C / C-(Zr) composite. 0.2 Hf 0.2 Ta 0.2 Nb 0.2 Ti 0.2 High-entropy ceramic matrix composites can be produced using this method. However, the high-entropy carbide ceramic powder required for this process necessitates ball milling, high-temperature sintering, and sieving, resulting in high raw material costs. Furthermore, the preparation of intermediates for high-entropy ceramic matrix composites using this method requires multiple rounds of curing and pyrolysis processes, leading to a lengthy preparation cycle. Although the porosity of the composite material prepared by this method is significantly lower than that prepared by the PIP process, its density is only 2.81 g / cm³. 3 This demonstrates that the high-entropy carbide ceramic phase introduced through this process has a limited content, which is not conducive to improving the ablation resistance of the composite material.
[0008] In summary, existing PIP (Polymerization Injection) processes for preparing high-entropy ceramic matrix composites suffer from drawbacks such as long preparation cycles, complex processes, and low precursor ceramic yields. Furthermore, the resulting composites exhibit low high-entropy ceramic content and high matrix porosity. While RMI (Refined Motion Injection) processes can yield high-entropy ceramic matrix composites with lower open porosity, they still face challenges such as high raw material costs and low high-entropy ceramic incorporation amounts, limiting further improvements in the ablation resistance of high-entropy ceramic matrix composites. Therefore, there is an urgent need to optimize and innovate the preparation process of high-entropy ceramic matrix composites, exploring low-temperature, rapid, and easily scalable preparation methods to achieve rapid densification of high-entropy ceramic matrix composites. Summary of the Invention
[0009] To overcome the shortcomings of the prior art, the present invention provides a method for preparing high-entropy ceramic matrix composites using a reactive melting process, the method specifically comprising the following steps: Step S1: At least four single-component carbides selected from TiC, ZrC, HfC, VC, NbC, TaC, MoC, and WC are ball-milled and then mixed with a carbon source to obtain a carbon-containing mixed powder. The carbon-containing mixed powder is dispersed in a dispersion liquid to obtain a multi-component ceramic slurry. Step S2: A continuous fiber preform is woven from continuous fibers as raw materials. An interface layer is deposited on the surface of the continuous fiber preform, and then a matrix layer is introduced to obtain a semi-dense composite material. Step S3: Using a vacuum impregnation method or a pressure impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded with transition metal, transition metal alloy or transition metal silicide alloy, and then subjected to reactive infiltration to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material.
[0010] Compared with existing technologies, this invention uses at least four types of single-component carbides as raw materials and combines them with a reactive melting process to generate a high-entropy carbide ceramic matrix in situ. This effectively solves the problems of long preparation cycle, low ceramic yield, and high porosity of composite materials in existing precursor impregnation and pyrolysis processes. At the same time, it improves the shortcomings of traditional reactive melting processes, such as high raw material cost and insufficient introduction of high-entropy ceramic phase. While achieving rapid densification of composite materials, it significantly increases the content of high-entropy ceramic matrix, enhances the high-temperature stability, oxidation resistance, and ablation resistance of the material, and better meets the stringent requirements of hypersonic vehicle thermal protection structures for ultra-high temperature materials.
[0011] In one possible implementation, in step S1, the particle size of the monocomponent carbide is 0.1-30 μm.
[0012] Compared with the prior art, the present invention controls the particle size of the monocomponent carbides within a suitable range, which enables more uniform mixing of multiple monocomponent carbides after ball milling, reduces powder agglomeration and component segregation, improves the dispersion quality and in-situ reaction efficiency of subsequent slurry, promotes the stable formation and uniform distribution of high-entropy carbide ceramics, thereby improving the density and matrix uniformity of composite materials, and improving the problems of low high-entropy ceramic content, uneven structure and unstable performance in the prior art.
[0013] In one possible implementation, in step S1, the carbon source is selected from at least one of graphite, carbon black, graphene and organic carbon sources, and the volume content of the carbon source in the carbon-containing mixed powder is 5 vol%-30 vol.
[0014] Compared with the prior art, the present invention selects a suitable carbon source and controls its volume content in the carbon-containing mixed powder, which can provide a sufficient and stable carbon supply for the in-situ reaction to generate high-entropy carbides, ensure that the melt-infiltrated alloy and the carbon source react fully to form a high-entropy ceramic phase, improve the filling effect of the internal pores of the composite material and the overall density, and solve the technical problems of insufficient introduction of high-entropy ceramic, low density and limited ablation resistance in the prior art.
[0015] In one possible implementation, in step S1, the dispersion includes a dispersant and a solvent, wherein the solvent is selected from at least one of water, ethanol, toluene, and xylene, and the mass ratio of the carbon-containing mixed powder to the solvent is (0.5-3):1.
[0016] Compared with the prior art, the present invention selects a suitable solvent and controls the mass ratio of carbon-containing mixed powder to solvent, which enables the multi-component ceramic slurry to have good fluidity and wettability, ensuring that the slurry fully enters the internal pores of the semi-dense composite material and is evenly distributed, reducing pore residue and uneven filling, providing good structural conditions for the in-situ generation of high-entropy carbide ceramics, and effectively reducing the porosity of the composite material and increasing its density.
[0017] In one possible implementation, in step S1, the dispersant is selected from one of polyethyleneimine, polyacrylate, polymethacrylate, polyvinylpyrrolidone, and ammonium citrate, and the dispersant accounts for 1wt%-2wt% of the mass of the multi-component ceramic slurry.
[0018] Compared with the prior art, the present invention uses a specific type of dispersant and controls its mass content in the slurry, which can significantly reduce the agglomeration of single-component carbides and carbon sources, improve the stability and dispersion uniformity of the slurry, and enable each component to be fully dispersed in the system and maintain high reactivity. This promotes the full synthesis and uniform molding of high-entropy carbide ceramics and improves problems such as matrix composition fluctuations and poor performance consistency caused by poor powder dispersion.
[0019] In one possible implementation, in step S1, the carbon-containing mixed powder is dispersed in a dispersion liquid by first stirring and then ultrasonically dispersing. The stirring time is 3-24 hours, and the specific parameters of the ultrasonic dispersion are as follows: time is 10-60 minutes, and ultrasonic vibration frequency is 28-200 kHz.
[0020] Compared with existing technologies, the present invention adopts a process of stirring followed by ultrasonic dispersion, which can fully refine and uniformly disperse carbon-containing mixed powders, further enhance the reactivity and solid solution capacity of single-component carbides, reduce the synthesis temperature of high-entropy ceramics, accelerate the in-situ reaction rate, avoid the defects of existing technologies such as long preparation cycle, high energy consumption and complex process caused by multiple high-temperature cycle treatments, and improve the densification efficiency and microstructure uniformity of composite materials.
[0021] In one possible implementation, in step S2, the continuous fiber is selected from at least one of carbon fiber and silicon carbide fiber; the structure of the continuous fiber preform is selected from one of two-dimensional plain weave, two-dimensional braid, three-dimensional needle punch, and three-dimensional braid.
[0022] Compared with existing technologies, this invention uses carbon fiber and silicon carbide fiber and adopts a specific structure to prepare continuous fiber preforms, which can give full play to the load-bearing and toughening effect of continuous fibers, so that the composite material has high specific strength, high modulus and good structural toughness, meets the high load-bearing requirements of thermal protection structures, and improves the problems of high-temperature failure and insufficient mechanical properties of traditional single-component ceramic matrix composite materials.
[0023] In one possible implementation, in step S2, the material of the interface layer is selected from one of PyC, BN, SiC and Si3N4, and the thickness is 100–400 nm. The substrate layer is made of PyC or SiC and has a thickness of 0.5-5 μm.
[0024] Compared with the prior art, the present invention sets an interface layer and a matrix layer with appropriate composition and thickness on the fiber surface, which can effectively protect the fiber from damage during high-temperature melting and infiltration, optimize the interface bonding state between the fiber and the matrix, adjust the load transfer and crack propagation mode, give full play to the toughening effect of the fiber, improve the overall mechanical properties and high-temperature structural stability of the composite material, and solve problems such as fiber damage and insufficient toughness caused by unreasonable interface design.
[0025] In one possible implementation, the parameters of the vacuum impregnation method in step S3 are as follows: impregnation pressure ≤ -0.85MPa, impregnation time 20-50min, drying after completion, and 5-10 cycles. The parameters for the pressure impregnation method are as follows: impregnation pressure ≥ 0.8 MPa, impregnation time 15-30 min, followed by drying.
[0026] Compared with existing technologies, this invention uses a parameter-optimized vacuum impregnation or pressure impregnation process to introduce multi-component ceramic slurry, which enables the slurry to fully penetrate into the interior of the semi-dense composite material, improves the filling rate and distribution uniformity of single-component carbides and carbon sources, and overcomes the defects of insufficient slurry impregnation and low introduction of high-entropy raw materials in existing technologies. This provides sufficient raw materials for the large-scale generation of high-entropy ceramic matrix, further enhancing the density and ablation resistance of the composite material.
[0027] In one possible implementation, the parameters for reaction infiltration in step S4 are as follows: the atmosphere is vacuum, the heating rate is 1-50℃ / min, the holding temperature is 20-500℃ higher than the melting point of the transition metal, transition metal alloy or transition metal silicide alloy, the holding time is 10-300 min, and the cooling rate is 5-10℃ / min.
[0028] Compared with existing technologies, this invention performs reactive melting and infiltration under suitable atmosphere and process parameters, which can ensure that the infiltrated alloy is fully melted, rapidly infiltrates, and reacts stably with the carbon source. It achieves in-situ synthesis of high-entropy carbide ceramics and efficient densification of composite materials at lower temperatures, avoiding problems such as fiber damage, coarse grains, long cycles, and high costs caused by multiple high-temperature heat treatments. It improves the stability of material performance and is more suitable for large-scale production. Attached Figure Description
[0029] Figure 1 The image shows the XRD pattern of the high-entropy ceramic matrix composite material prepared in Example 3 of this invention.
[0030] Figure 2 Cross-sectional SEM image of high-entropy ceramic matrix composites prepared by reactive melt infiltration.
[0031] Figure 3 The ablation properties of C / SiC-(ZrHfNbTa)C high-entropy ceramic matrix composites prepared by reactive melt infiltration were investigated. Detailed Implementation
[0032] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation methods and typical parameters of the present invention, and are not intended to limit the parameter range described in the present invention. Reasonable variations derived therefrom are still within the protection scope of the claims of the present invention.
[0033] It should be noted that the endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0034] Unless otherwise defined, all terms, symbols, and other scientific terms used herein are intended to have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In some instances, terms having a conventional meaning are defined herein for clarification or ease of reference, and such definitions should not be construed as indicating a significant difference from conventional understanding in the art. The technical methods described or referenced herein are generally well understood by those skilled in the art and employed by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents, and instruments shall be performed according to the manufacturer's instructions and parameters.
[0035] Example 1 This embodiment provides a high-entropy ceramic matrix composite material, which is prepared by the following method: Step S1: Select equimolar amounts of TiC, HfC, NbC, and TaC with an average particle size of 10 μm, mix them, and place them in a WC ball mill jar for ball milling. The ball milling speed is 300 r / min, and the ball milling time is 20 h. After ball milling, mix with carbon black to obtain a carbon-containing mixed powder, wherein the volume content of carbon black in the carbon-containing mixed powder is 5 vol%. The carbon-containing mixed powder was first stirred in a dispersion liquid for 4 hours, and then ultrasonically dispersed to obtain a multi-component ceramic slurry. The dispersion liquid included polyvinylpyrrolidone and water, and the mass ratio of carbon-containing mixed powder to water was 1.5:1. The mass content of polyvinylpyrrolidone in the multi-component ceramic slurry was 1.5wt%. The specific parameters of the ultrasonic dispersion treatment were as follows: time was 20 min, and ultrasonic vibration frequency was 120 kHz. Step S2: Using T300 carbon fiber as raw material, a three-dimensional woven continuous fiber preform is woven. A BN interface layer with a thickness of 200 nm is deposited on the surface of the continuous fiber preform using the CVI process, and then a SiC matrix layer with a thickness of 0.5 μm is deposited. Step S3: Using a pressure impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2; a vacuum + pressure cyclic impregnation method is used, with the following specific parameters: vacuum impregnation pressure ≤ -0.85 MPa, impregnation time 30 min, followed by pressure impregnation, impregnation pressure ≥ 0.8 MPa, impregnation time 20 min, and drying after completion. The above steps are repeated 5 times. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded in a Ti-Zr alloy block and placed in a vacuum induction sintering furnace. The reaction melting and infiltration are carried out at 1650℃ to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material. The heating rate is 5℃ / min, the holding time is 30 min, and the cooling rate is 5℃ / min.
[0036] The density of the high-entropy ceramic matrix composite material prepared in this embodiment is 3.99 g / cm³. 3 The porosity is 14.13 vol.
[0037] Example 2
[0038] This embodiment provides a high-entropy ceramic matrix composite material, which is prepared by the following method: Step S1: Select equimolar amounts of TiC, ZrC, HfC, NbC, TaC, and WC with an average particle size of 1 μm, mix them, and place them in a WC ball mill jar for ball milling. The ball milling speed is 300 r / min, and the ball milling time is 20 h. After ball milling, mix with graphene to obtain a carbon-containing mixed powder, wherein the volume content of graphene in the carbon-containing mixed powder is 15 vol%. The carbon-containing mixed powder was first stirred in a dispersion liquid for 3 hours, and then ultrasonically dispersed to obtain a multi-component ceramic slurry. The dispersion liquid included polyacrylate and ethanol, and the mass ratio of carbon-containing mixed powder to ethanol was 0.5:1. The mass content of polyacrylate in the multi-component ceramic slurry was 1 wt%. The specific parameters of the ultrasonic dispersion treatment were as follows: time was 10 min, and ultrasonic vibration frequency was 28 kHz. Step S2: A three-dimensional needle-punched continuous fiber preform is woven using T300 carbon fiber as raw material. A Si3N4 interface layer with a thickness of 300 nm is deposited on the surface of the continuous fiber preform using the CVI process, followed by the deposition of a SiC matrix layer with a thickness of 5 μm. Step S3: Using a vacuum impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. The parameters of the vacuum impregnation method are as follows: impregnation pressure ≤ -0.85MPa, impregnation time is 30min, after completion, it is dried and the process is repeated 7 times. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded in a Ti-Zr alloy block and placed in a vacuum induction sintering furnace. The reaction melting and infiltration are carried out at 1700℃ to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material. The heating rate is 15℃ / min, the holding time is 30min, and the cooling rate is 10℃ / min.
[0039] The density of the high-entropy ceramic matrix composite material prepared in this embodiment is 3.94 g / cm³. 3 The porosity is 16.68 vol.
[0040] Example 3
[0041] This embodiment provides a high-entropy ceramic matrix composite material, which is prepared by the following method: Step S1: Select equimolar amounts of ZrC, HfC, NbC, and TaC with an average particle size of 5 μm, mix them, and place them in a WC ball mill jar for ball milling. The ball milling speed is 300 r / min, and the ball milling time is 20 h. After ball milling, mix with graphite to obtain a carbon-containing mixed powder, wherein the volume content of graphite in the carbon-containing mixed powder is 10 vol%. The carbon-containing mixed powder was first stirred in a dispersion liquid for 24 hours, and then ultrasonically dispersed to obtain a multi-component ceramic slurry. The dispersion liquid included ammonium citrate and toluene, and the mass ratio of carbon-containing mixed powder to toluene was 3:1. The mass content of ammonium citrate in the multi-component ceramic slurry was 2wt%. The specific parameters of the ultrasonic dispersion treatment were as follows: time was 60 min, and ultrasonic vibration frequency was 200 kHz. Step S2: Using T300 carbon fiber as raw material, a three-dimensional needle-punched continuous fiber preform is woven. A 200nm thick PyC interface layer is deposited on the surface of the continuous fiber preform using the CVI process, followed by a 3μm thick SiC matrix layer. Step S3: Using a vacuum impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. The parameters of the vacuum impregnation method are as follows: impregnation pressure ≤ -0.90MPa, impregnation time is 30min, after completion, it is dried and the process is repeated 5 times. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded in a Zr-Hf alloy block and placed in a vacuum induction sintering furnace. The reaction melting and infiltration are carried out at 2000℃ to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material. The heating rate is 10℃ / min, the holding time is 10min, and the cooling rate is 5℃ / min.
[0042] The density of the high-entropy ceramic matrix composite material prepared in this embodiment is 6.51 g / cm³. 3 The porosity is 13.93 vol.
[0043] Example 4
[0044] This embodiment provides a high-entropy ceramic matrix composite material, which is prepared by the following method: Step S1: Select equimolar amounts of TiC, ZrC, HfC, VC, NbC, and TaC with an average particle size of 8 μm, mix them, and place them in a WC ball mill jar for ball milling. The ball milling speed is 300 r / min, and the ball milling time is 20 h. After ball milling, mix with graphite to obtain a carbon-containing mixed powder, wherein the volume content of graphite in the carbon-containing mixed powder is 20 vol%. The carbon-containing mixed powder was first stirred in a dispersion liquid for 12 hours, and then ultrasonically dispersed to obtain a multi-component ceramic slurry. The dispersion liquid included polymethyl methacrylate and xylene, and the mass ratio of carbon-containing mixed powder to xylene was 2:1. The mass content of polymethyl methacrylate in the multi-component ceramic slurry was 1.5 wt%. The specific parameters of the ultrasonic dispersion treatment were as follows: time was 30 min, and ultrasonic vibration frequency was 40 kHz. Step S2: Using T700 carbon fiber as raw material, a three-dimensional needle-punched continuous fiber preform is woven. A PyC interface layer with a thickness of 400 nm is deposited on the surface of the continuous fiber preform using the CVI process, and then a SiC matrix layer with a thickness of 4 μm is deposited. Step S3: Using a pressure impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. The parameters of the pressure impregnation method are as follows: impregnation pressure ≥ 0.8 MPa, impregnation time 30 min, drying after completion, and 10 cycles. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded in a Si-Hf alloy block and placed in a vacuum induction sintering furnace. The reaction melting and infiltration are carried out at 1650℃ to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material. The heating rate is 3℃ / min, the holding time is 30min, and the cooling rate is 5℃ / min.
[0045] The density of the high-entropy ceramic matrix composite material prepared in this embodiment is 5.33 g / cm³. 3 The porosity is 7.27 vol%.
[0046] Example 5
[0047] This embodiment provides a high-entropy ceramic matrix composite material, which is prepared by the following method: Step S1: Select equimolar amounts of ZrC, HfC, NbC, and TaC with an average particle size of 10 μm, mix them, and place them in a WC ball mill jar for ball milling. The ball milling speed is 300 r / min, and the ball milling time is 20 h. After ball milling, mix with graphite to obtain a carbon-containing mixed powder, wherein the volume content of graphite in the carbon-containing mixed powder is 30 vol%. The carbon-containing mixed powder was first stirred in a dispersion for 8 hours, and then ultrasonically dispersed to obtain a multi-component ceramic slurry. The dispersion included polyethyleneimine and a water-ethanol mixed solvent, and the mass ratio of the carbon-containing mixed powder to the mixed solvent was 1:1. The mass content of polyethyleneimine in the multi-component ceramic slurry was 1.2 wt%. The specific parameters of the ultrasonic dispersion were as follows: time was 40 min, and the ultrasonic vibration frequency was 80 kHz. Step S2: Using T700 carbon fiber as raw material, a three-dimensional needle-punched continuous fiber preform is woven. A 200nm thick PyC interface layer is deposited on the surface of the continuous fiber preform using the CVI process, followed by a 3μm thick SiC matrix layer. Step S3: Using a vacuum impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. The parameters of the vacuum impregnation method are as follows: impregnation pressure ≤ -0.85MPa, impregnation time is 30min, after completion, it is dried and 10 times. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded in a Si-Hf alloy block and placed in a vacuum induction sintering furnace. The reaction melting and infiltration are carried out at 1650℃ to generate a high-entropy carbide ceramic matrix in situ and achieve densification, thus obtaining a high-entropy ceramic matrix composite material. The heating rate is 10℃ / min, the holding time is 30min, and the cooling rate is 5℃ / min.
[0048] The density of the high-entropy ceramic matrix composite material prepared in this embodiment is 5.78 g / cm³. 3 The porosity was 3.83 vol%; after 120 s of oxyacetylene flame ablation at 2329 °C, the linear ablation rate was 1.575 μm / s and the mass ablation rate was 0.387 mg / s.
[0049] Figure 1 The image shows the XRD pattern of the high-entropy ceramic matrix composite material prepared in Example 3 of this invention. Significant diffraction peaks of the (ZrHfNbTa)C high-entropy carbide are present, and C and SiC diffraction peaks corresponding to the carbon fibers and SiC matrix are also detected, confirming the successful preparation of the continuous fiber-reinforced high-entropy ceramic matrix composite material by the method described in this invention.
[0050] Figure 2 Cross-sectional SEM image of high-entropy ceramic matrix composites prepared by reactive melt infiltration. Figure 2 (a) Figure 2 Image (d) shows a cross-sectional SEM image of the C / SiC-(TiZrHfNbTa)C composite material prepared in Example 1. Figure 2 (b) Figure 2 Image (e) shows a cross-sectional SEM image of the C / SiC-(ZrHfNbTa)C composite material prepared in Example 3. Figure 2 (c) Figure 2 Image (f) shows a cross-sectional SEM image of the C / SiC-(TiZrHfNbTa)C composite material prepared in Example 5. In the image, the white phase is high-entropy carbide, the gray phase is SiC, and the black phase is carbon fiber, which proves that this process can synthesize a dense high-entropy carbide ceramic matrix in situ inside the semi-dense C / SiC composite material.
[0051] Figure 3 The ablation properties of C / SiC-(ZrHfNbTa)C high-entropy ceramic matrix composites prepared by reactive melt infiltration were investigated. Figure 3 (a) shows the ablation temperature-time curve of the composite material prepared in Example 5. During the ablation process, the temperature of the sample surface stabilized at around 2300 °C, with a maximum of 2329 °C. Figure 3 (b) Figure 3 (c) shows the surface morphology of the composite material before and after ablation. After ablation, the surface of the composite material is protected by dense oxides and no fiber exposure occurs, which confirms that the high-entropy ceramic matrix composite material prepared by this process has good ablation performance.
[0052] While the disclosure is as stated above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of this disclosure, and all such changes and modifications will fall within the protection scope of this invention.
Claims
1. A method for preparing high-entropy ceramic matrix composites using a reactive infiltration process, characterized in that, The method specifically includes the following steps: Step S1: At least four single-component carbides selected from TiC, ZrC, HfC, VC, NbC, TaC, MoC, and WC are ball-milled and then mixed with a carbon source to obtain a carbon-containing mixed powder. The carbon-containing mixed powder is dispersed in a dispersion liquid to obtain a multi-component ceramic slurry. Step S2: A continuous fiber preform is woven from continuous fibers as raw materials. An interface layer is deposited on the surface of the continuous fiber preform, and then a matrix layer is introduced to obtain a semi-dense composite material. Step S3: Using a vacuum impregnation method or a pressure impregnation method, the multi-component ceramic slurry obtained in step S1 is introduced into the interior of the semi-dense composite material obtained in step S2. Step S4: After the semi-dense composite material with multi-component ceramic slurry is introduced, it is embedded with transition metal, transition metal alloy or transition metal silicide alloy, and then subjected to reactive infiltration to generate a high-entropy carbide ceramic matrix in situ and achieve densification, so as to obtain a high-entropy ceramic matrix composite material. The material of the interface layer is selected from PyC, BN, SiC and Si3N4, and the thickness is 100–400 nm; the material of the substrate layer is PyC or SiC, and the thickness is 0.5–5 μm. In step S4, the parameters for reaction infiltration are as follows: the atmosphere is vacuum, the heating rate is 1-50℃ / min, the holding temperature is 20-500℃ higher than the melting point of the transition metal, transition metal alloy or transition metal silicide alloy, the holding time is 10-300 min, and the cooling rate is 5-10℃ / min.
2. The method as described in claim 1, characterized in that, In step S1, the particle size of the monocomponent carbide is 0.1-30 μm.
3. The method as described in claim 1, characterized in that, In step S1, the carbon source is selected from at least one of graphite, carbon black, graphene and organic carbon source, and the volume content of the carbon source in the carbon-containing mixed powder is 5 vol%-30 vol.
4. The method as described in claim 1, characterized in that, In step S1, the dispersion includes a dispersant and a solvent. The solvent is selected from at least one of water, ethanol, toluene, and xylene, and the mass ratio of the carbon-containing mixed powder to the solvent is (0.5-3):
1.
5. The method as described in claim 4, characterized in that, In step S1, the dispersant is selected from one of polyethyleneimine, polyacrylate, polymethacrylate, polyvinylpyrrolidone, and ammonium citrate, and the mass content of the dispersant in the multi-component ceramic slurry is 1wt%-2wt%.
6. The method as described in claim 1, characterized in that, In step S1, the carbon-containing mixed powder is dispersed in the dispersion liquid by first stirring and then ultrasonically dispersing. The stirring time is 3-24 hours, and the specific parameters of the ultrasonic dispersion are as follows: time is 10-60 minutes, and ultrasonic vibration frequency is 28-200 kHz.
7. The method as described in claim 1, characterized in that, In step S2, the continuous fiber is selected from at least one of carbon fiber and silicon carbide fiber; the structure of the continuous fiber preform is selected from one of two-dimensional plain weave, two-dimensional braiding, three-dimensional needle punching and three-dimensional braiding.
8. The method as described in claim 1, characterized in that, In step S3, the parameters of the vacuum impregnation method are as follows: impregnation pressure ≤ -0.85MPa, impregnation time 20-50min, drying after completion, and repeating 5-10 times; the parameters of the pressure impregnation method are as follows: impregnation pressure ≥ 0.8MPa, impregnation time 15-30min, drying after completion.
Citation Information
Patent Citations
High-entropy ceramic-based composite material and preparation method thereof
CN113321510A
High-entropy ceramic-based composite material and preparation method thereof
CN115784746A
High-entropy ceramic-based composite material and preparation method thereof
CN117567158A
High-entropy ceramic block and preparation method thereof
CN118184353A