An adsorbent for ammonia nitrogen recovery from landfill leachate, its preparation method and its application

By preparing Al-P compounds from sludge ash and combining them with Mg-P compound crystallization technology, the problem of high cost in treating ammonia nitrogen from landfill leachate was solved, achieving efficient ammonia nitrogen recovery and resource utilization, and forming recyclable slow-release fertilizer.

CN122183535BActive Publication Date: 2026-11-17SHANGHAI ENVIRONMENTAL & SANITARY ENG DESIGN INST CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610544900.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-04-23
Publication Date
2026-11-17
Estimated Expiration
2046-04-23

AI Technical Summary

Technical Problem

Existing landfill leachate ammonia nitrogen treatment technologies suffer from high treatment costs, high chemical consumption, high sludge production, and the risk of secondary pollution, making it difficult to achieve efficient recovery and resource utilization of ammonia nitrogen.

Method used

Using sludge ash as raw material, Al-P compounds are prepared through multi-stage acid leaching and pH adjustment with magnesium hydroxide to form an ammonia nitrogen adsorbent. Combined with a Mg-P compound crystallization process, selective adsorption and recovery of ammonia nitrogen are achieved.

Benefits of technology

It reduces treatment costs, improves ammonia nitrogen removal rate, forms recyclable slow-release fertilizer, and realizes the resource utilization of sludge ash, which is both environmentally friendly and economically beneficial.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122183535B_ABST
    Figure CN122183535B_ABST
Patent Text Reader

Abstract

This invention discloses an adsorbent for ammonia nitrogen recovery from landfill leachate, its preparation method, and its application, belonging to the field of landfill leachate treatment technology. The preparation method involves: firstly, extracting phosphorus from sludge ash by acid leaching with hydrochloric acid, while simultaneously dissolving aluminum; adding magnesium hydroxide to adjust the pH of the solution to allow aluminum ions to form flocs and adsorb phosphorus ions, forming an Al-P compound; then adding magnesium hydroxide to the Al-P compound and drying to obtain a highly efficient ammonia nitrogen adsorbent. When this adsorbent is added to the landfill leachate, it promotes a chemical reaction between ammonia nitrogen and magnesium ions, ultimately forming a Mg-P compound precipitate. This invention innovatively achieves the recovery and utilization of phosphorus and aluminum resources from sludge ash, solving the problem of high ammonia nitrogen content in landfill leachate, and has significant environmental benefits and resource recycling value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of landfill leachate treatment technology, and particularly relates to an adsorbent for ammonia nitrogen recovery from landfill leachate, its preparation method, and its application. Background Technology

[0002] Landfill leachate is a high-concentration organic waste liquid formed during landfilling through multiple processes, including anaerobic fermentation, organic matter decomposition, and rainwater leaching. It contains various metabolic products. Studies have shown that it contains numerous toxic and harmful substances and carcinogenic components, posing multi-dimensional and varying degrees of harm to aquatic and soil ecosystems and the health of organisms. Therefore, the efficient treatment of landfill leachate has always been a globally recognized environmental governance challenge, and the development of highly adaptable and stable treatment technologies has become a current research hotspot in the field of environmental engineering.

[0003] Currently, mainstream treatment technologies both domestically and internationally include air stripping, chemical coagulation and sedimentation, anaerobic digestion, adsorption, and biological methods. However, each technology has significant limitations. For example, air stripping requires strong alkaline conditions, resulting in huge reagent consumption and potential secondary air pollution. Chemical coagulation and sedimentation suffers from high reagent dosage and sludge production, and its treatment effect is easily affected by water quality fluctuations. Anaerobic digestion has stringent reaction conditions and long treatment cycles, making it difficult to achieve deep removal of pollutants such as ammonia nitrogen. Biological methods have weak resistance to shock loads, require large land areas, and are easily inhibited by high-salt environments and toxic substances. In contrast, adsorption offers significant advantages. Its operation is simple, reaction conditions are mild, and it boasts high adsorption efficiency and selectivity, adapting to different concentrations of ammonia nitrogen in treatment scenarios. It is also less prone to secondary pollution, and some adsorbents can be regenerated and recycled, demonstrating broad application potential in the treatment of ammonia nitrogen in complex matrix landfill leachate.

[0004] As an efficient technology for the removal and recovery of ammonia nitrogen in landfill leachate, the core principle of adsorption is to selectively enrich ammonia nitrogen through physicochemical interactions on the surface of the adsorbent. Under alkaline conditions, ammonia nitrogen can also combine with magnesium ions and phosphate ions in the adsorbent at a specific molar ratio to form Mg-P compounds. This product can be commercially applied as a slow-release fertilizer, offering both environmental and economic benefits. However, a key bottleneck in practical applications is that the molar concentration of ammonia nitrogen in most landfill leachate is several times that of phosphate, requiring the addition of additional chemical phosphorus sources, resulting in high treatment costs and hindering the large-scale promotion of this technology. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention proposes an adsorbent for ammonia nitrogen recovery from landfill leachate, its preparation method, and its application. Sludge ash (especially sludge incineration ash) has significant resource advantages; its moisture and organic matter content are nearly zero, it is odorless, and its phosphorus content is extremely high (up to approximately 10%). The phosphorus element mainly exists in metal-bound forms such as aluminum phosphorus, iron phosphorus, or calcium phosphorus, making it an ideal novel phosphorus source for Mg-P compound crystallization processes. Therefore, this invention develops a novel treatment method that is both highly efficient and environmentally friendly, and can fully utilize sludge ash to recover ammonia nitrogen from landfill leachate. This not only solves the economic problems of existing technologies but also promotes the resource utilization of sludge ash, possessing significant practical significance and application value.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing an adsorbent for ammonia nitrogen recovery from landfill leachate includes the following steps: S1. The sludge ash is subjected to multi-stage acid leaching with hydrochloric acid. After stirring and reacting, the mixture is centrifuged and filtered step by step to obtain a supernatant containing phosphorus and aluminum. S2. Add magnesium hydroxide to the supernatant obtained in step S1 to adjust the pH to 3.5 and stir. Centrifuge to collect the white precipitate, wash and dry it to obtain the Al-P compound. S3. Add magnesium hydroxide to the Al-P compound obtained in step S2, and then dry it to obtain an ammonia nitrogen adsorbent.

[0007] This invention clarifies the key process for adsorbent preparation (sludge ash acid leaching → Al-P compound preparation → adsorbent molding), achieving efficient recovery of phosphorus and aluminum resources from sludge ash, replacing traditional chemical agents, and reducing adsorbent preparation costs; the process logic is clear and highly operable, providing stable core materials for subsequent ammonia nitrogen recovery, and possessing both resource recycling value and environmental friendliness.

[0008] Furthermore, in step S1, the multi-stage acid extraction is a three-stage acid extraction, and the subsequent extraction uses the supernatant obtained by centrifugation after the previous extraction and new sludge ash.

[0009] This invention employs a three-stage leaching mode that reuses the supernatant from the previous stage in the subsequent stage of leaching. This significantly increases the leaching rate of phosphorus and aluminum in sludge ash, thereby improving resource utilization. It also reduces hydrochloric acid consumption, thereby lowering the environmental pressure and cost of the acid leaching process. Simultaneously, it increases the concentration of phosphorus and aluminum in the subsequent supernatant, providing high-quality raw materials for the preparation of Al-P compounds.

[0010] Furthermore, in step S1, the concentration of the hydrochloric acid is 1M.

[0011] This invention limits the hydrochloric acid concentration to 1M, which ensures effective dissolution of metal-bound phosphorus and aluminum elements in sludge ash, while avoiding excessive concentration that could lead to equipment corrosion and increased consumption of subsequent neutralizing agents (magnesium hydroxide). This balances leaching efficiency with process economy and avoids resource waste.

[0012] Further, in step S1, the liquid-to-solid ratio of hydrochloric acid to sludge ash is 10 mL: 1 g; the stirring reaction time is 2 h; and the centrifugation speed is 300 r / min for 10 min.

[0013] This invention specifies the liquid-to-solid ratio, stirring time, and centrifugation parameters to ensure that the sludge ash and hydrochloric acid fully contact and react, achieving efficient leaching of phosphorus and aluminum. The centrifugation parameters can effectively separate the supernatant from the residue, reduce the introduction of impurities into subsequent processes, ensure product purity, and make the process stable, controllable, and scalable.

[0014] Further, in step S2, the stirring time is 24 hours; the centrifugation speed is 300 r / min and the time is 10 minutes; the washing is performed by washing with deionized water 3 times; and the drying temperature is 45°C.

[0015] This invention precisely controls the reaction conditions for the formation of aluminum ion flocs and the adsorption of phosphorus ions, thereby improving the purity and stability of Al-P compounds. Low-temperature drying avoids damage to the product structure, and the washing step removes soluble impurities, laying the foundation for subsequent optimization of adsorbent performance while reducing energy consumption.

[0016] Furthermore, in step S3, the amount of magnesium hydroxide added satisfies the molar ratio of magnesium to phosphorus in the system being 1.3:1.

[0017] This ratio has been optimized to ensure sufficient magnesium source for subsequent reaction with ammonia nitrogen, enabling efficient generation of Mg-P compounds, while avoiding waste due to excessive magnesium source or impact on ammonia nitrogen recovery efficiency due to insufficient magnesium source, thus balancing treatment efficiency and cost control.

[0018] The present invention also provides an ammonia nitrogen adsorbent prepared by the above preparation method.

[0019] This invention relies on an optimized process for preparation. The adsorbent integrates the core elements of phosphorus, aluminum, and magnesium, exhibiting strong selectivity and high reactivity in the adsorption of ammonia nitrogen in landfill leachate. The raw materials are derived from the resource utilization of sludge ash, with no odor or risk of secondary pollution. The preparation cost is lower than that of traditional chemical adsorbents, and the subsequent products can be recycled, combining environmental benefits with economic efficiency.

[0020] The present invention also provides a method for recovering ammonia nitrogen from landfill leachate, comprising the following steps: adding the ammonia nitrogen adsorbent to the landfill leachate, adjusting the pH to alkaline, stirring and reacting, and then separating the solid and liquid phases to allow the ammonia nitrogen to precipitate and be recovered from the leachate in the form of Mg-P compounds.

[0021] This invention recovers phosphorus from sludge ash, synthesizes an ammonia nitrogen adsorbent by adding a magnesium source, and adds the ammonia nitrogen adsorbent to landfill leachate to recover ammonia nitrogen in the form of Mg-P compounds and convert it into valuable products. At the same time, it realizes the resource utilization of sludge ash, reduces treatment costs, and reduces environmental pollution.

[0022] Furthermore, the dosage of the ammonia nitrogen adsorbent is 0.1-2g of ammonia nitrogen adsorbent per 15mL of leachate.

[0023] This invention specifies a dosage range of 0.1-2 g / 15 mL leachate, which can be flexibly adjusted according to the ammonia nitrogen concentration of the leachate to avoid insufficient ammonia nitrogen removal or excessive adsorbent waste. This range ensures stable ammonia nitrogen removal rate under different operating conditions, improving the applicability and economy of the method.

[0024] Furthermore, the pH is 9.5.

[0025] This value represents the optimal alkaline condition for the reaction of ammonia nitrogen with magnesium and phosphorus elements in the adsorbent to form Mg-P compounds. It promotes the full reaction and enables the ammonia nitrogen removal rate to exceed 80%. At the same time, it avoids excessively high pH, ​​which could lead to increased consumption of magnesium hydroxide and other reagents or cause secondary pollution, thus ensuring process stability and treatment efficiency.

[0026] Compared with the prior art, the present invention has the following advantages and technical effects: This invention utilizes acid leaching of sludge ash to recover and reuse phosphorus and aluminum resources, replacing traditional chemical agents and reducing treatment costs. Simultaneously, the addition of magnesium hydroxide increases the magnesium content in the Al-P compound and raises the pH value of the adsorbent, providing hydroxide ions for the subsequent removal of ammonia nitrogen from landfill leachate. Finally, a Mg-P compound crystallization process achieves highly efficient ammonia nitrogen recovery, with an ammonia nitrogen removal rate exceeding 80%. The resulting magnesium ammonium phosphate crystals can be directly reused as slow-release fertilizer, offering both environmental and economic benefits. Attached Figure Description

[0027] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The process flow diagram for preparing the adsorbent for ammonia nitrogen recovery from landfill leachate is shown in the present invention. Figure 2 The effect of different ammonia nitrogen adsorbent dosages on SCOD removal rate; Figure 3 The effect of different amounts of ammonia nitrogen adsorbent added on ammonia nitrogen removal rate; Figure 4The effect of different ammonia nitrogen adsorbent dosages on total phosphorus removal rate; Figure 5 X-ray diffraction patterns of Mg-P compound products corresponding to different amounts of ammonia nitrogen adsorbent. Detailed Implementation

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0030] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0031] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0032] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0033] This invention provides a method for preparing an adsorbent for ammonia nitrogen recovery from landfill leachate, comprising the following steps: I. Preparation of Ammonia Nitrogen Adsorbent Step 1: Three-stage acid leaching of sludge ash (preparation of phosphorus and aluminum-containing supernatant) Sludge ash was mixed with 1M hydrochloric acid at a liquid-solid ratio of 10 mL:1 g. After stirring for 2 hours, the mixture was centrifuged at 300 rpm for 10 minutes, and the supernatant (primary extraction supernatant) was collected. This primary extraction supernatant was then mixed with fresh sludge ash at the same liquid-solid ratio, and the stirring (2 hours) and centrifugation (300 rpm, 10 minutes) were repeated to collect the secondary extraction supernatant. The secondary extraction supernatant was then mixed with fresh sludge ash at the same liquid-solid ratio, and the stirring and centrifugation processes were repeated. Finally, the mixture was filtered to obtain a tertiary extraction supernatant containing phosphorus and aluminum. This process utilizes hydrochloric acid to leach phosphorus and aluminum from the sludge ash into the supernatant.

[0034] Step 2: Preparation of Al-P compounds Magnesium hydroxide was slowly added to the phosphorus- and aluminum-containing supernatant obtained in step 1 to adjust the pH of the system to 3.5. After stirring continuously for 24 hours, the mixture was centrifuged at 300 r / min for 10 min and the white precipitate was collected. Aluminum ions formed a large number of flocs, which adsorbed phosphorus ions and precipitated together. At the same time, some magnesium ions entered the solid, reducing the amount of magnesium added later. The white precipitate was washed three times with deionized water to remove impurities and then dried at 45°C to obtain the Al-P compound.

[0035] Step 3: Preparation of ammonia nitrogen adsorbent Magnesium hydroxide was added to the Al-P compound obtained in step 2, and the amount added was controlled so that the molar ratio of magnesium to phosphorus in the system was 1.3:1. After mixing evenly, the mixture was dried to obtain the ammonia nitrogen adsorbent. Adding magnesium hydroxide can increase the magnesium content and simultaneously increase the pH value of the solution, providing hydroxide ions for the subsequent removal of ammonia nitrogen from landfill leachate.

[0036] II. Ammonia Nitrogen Recovery from Landfill Leachate Step 4: Adsorption reaction and ammonia nitrogen recovery Take 15 mL of landfill leachate as the treatment target, add 0.1-2 g of the ammonia nitrogen adsorbent prepared in step 3, then adjust the pH of the system to 9.5, stir and react for a period of time, and then perform solid-liquid separation. Collect the precipitate product, and recover the ammonia nitrogen from the leachate in the form of Mg-P compounds.

[0037] Unless otherwise specified, "room temperature" in this invention refers to 25±2℃.

[0038] All raw materials used in this invention were purchased from the market.

[0039] The technical solution of the present invention will be further illustrated by the following embodiments.

[0040] The sludge ash in the following examples is from a wastewater treatment plant in Shanghai.

[0041] Example 1 A method for preparing an adsorbent for ammonia nitrogen recovery from landfill leachate includes the following steps: Step 1: Three-stage acid leaching of sludge ash: Take sludge ash and 1M hydrochloric acid, mix them at a liquid-solid ratio of 10mL:1g (and make up to 1L with 85mL hydrochloric acid), stir and react for 2 hours, then centrifuge at 300r / min for 10 minutes and collect the supernatant (first-stage leaching supernatant); mix the first-stage leaching supernatant with new sludge ash at a liquid-solid ratio of 10mL:1g, and repeat the above stirring reaction (2 hours) and centrifugation (300r / min, 10 minutes) operation to collect the second-stage leaching supernatant; then mix the second-stage leaching supernatant with new sludge ash at the same liquid-solid ratio, and perform stirring and centrifugation operations again, finally filtering to obtain a three-stage leaching supernatant containing phosphorus and aluminum; Step 2: Preparation of Al-P compound: Slowly add magnesium hydroxide to the phosphorus- and aluminum-containing supernatant obtained in Step 1 to adjust the pH of the system to 3.5. After stirring continuously for 24 hours, centrifuge at 300 r / min for 10 min and collect the white precipitate. Wash the white precipitate three times with deionized water to remove impurities, and then dry it at 45℃ to obtain the Al-P compound. Step 3: Preparation of ammonia nitrogen adsorbent: Add magnesium hydroxide to the Al-P compound obtained in step 2, and control the amount added so that the molar ratio of magnesium to phosphorus in the system is 1.3:1. After mixing evenly, dry the mixture to obtain the ammonia nitrogen adsorbent.

[0042] The Al-P compound prepared in step 2 was subjected to XRF testing to determine the content of magnesium and phosphorus. The results are shown in Table 1.

[0043] Table 1. Proportion of each element in Al-P compounds Table 1 shows that the main elements in the Al-P compounds are phosphorus, aluminum, calcium, and silicon, accounting for 20.71%, 16.72%, 15.54%, and 11.03%, respectively. Magnesium content is low, at only 2.35%, therefore an external magnesium source is needed to achieve an n(Mg):n(P) ratio of 1.3:1. Furthermore, it should be noted that the compounds contain a high amount of calcium, which may compete with magnesium ions for adsorption during the process. Additionally, the Al-P compounds contain certain heavy metals, indicating that during the synthesis of the Al-P compounds, a small amount of heavy metals from the acid leaching supernatant precipitated into the solid phase along with the aluminum flocs.

[0044] Application Example 1 The ammonia nitrogen adsorbent prepared in Example 1 was used to treat landfill leachate. Specifically, 15 mL of landfill leachate was diluted with water to 30 mL as the treatment target. Different amounts (0.1, 0.5, 1, 1.5, and 2 g) of the ammonia nitrogen adsorbent prepared in Example 1 were added to the leachate. The pH of the system was then adjusted to 9.5, and after stirring for 2 hours, solid-liquid separation was performed. The precipitate and supernatant were collected, and ammonia nitrogen was recovered from the leachate in the form of Mg-P compounds. The ammonia nitrogen removal rate, COD removal rate, phosphorus and magnesium content, and X-ray diffraction pattern of the Mg-P compound precipitate in the supernatant were measured to evaluate the performance of the adsorbent.

[0045] Analysis of the supernatant after Mg-P compound synthesis: The supernatant after Mg-P compound synthesis was digested, and the magnesium ion content was tested by ICP-OES, while the phosphorus content was determined by spectrophotometry. Simultaneously, the SCOD and ammonia nitrogen contents in the supernatant were determined. The treatment results are shown in [link to treatment]. Figure 2 , Figure 3 and Figure 4 It can be observed that as the adsorbent dosage increases from 0.1g to 2g, its removal efficiency for pollutants in the leachate shows a significant upward trend: when the dosage reaches 2g, the removal rate of soluble chemical oxygen demand (SCOD) is the highest, reaching 80%; the ammonia nitrogen removal rate increases synchronously with the increase of dosage, with a maximum removal rate of 75%; the total phosphorus (TP) removal rate also increases with the increase of dosage, reaching a peak of 84% when the dosage is 2g.

[0046] XRD analysis of the synthesized Mg-P compound precipitate: The synthesized product precipitate was dried and subjected to XRD analysis. The XRD pattern is shown in the figure. Figure 5 .from Figure 5 As can be seen, the product exhibits obvious diffraction peaks at 2θ≈15.7°, 21.0°, 30.6°, and 35.0°, which are consistent with the standard comparison cards (MgHPO4·7H2O_PDF#9-0761, PN-PDF#23-0463), proving that the method can synthesize Mg-P compounds.

[0047] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for preparing an adsorbent for ammonia nitrogen recovery from landfill leachate, characterized in that, Includes the following steps: S1. The sludge ash is subjected to multi-stage acid leaching with hydrochloric acid. After stirring and reacting, the mixture is centrifuged and filtered step by step to obtain a supernatant containing phosphorus and aluminum. The multi-stage acid leaching is a three-stage acid leaching, and the supernatant obtained by centrifugation after the previous stage is used in the subsequent stage of leaching with new sludge ash. S2. Add magnesium hydroxide to the supernatant obtained in step S1 to adjust the pH to 3.5 and stir. Centrifuge to collect the precipitate, wash and dry it to obtain the Al-P compound. S3. Add magnesium hydroxide to the Al-P compound obtained in step S2, and then dry it to obtain an ammonia nitrogen adsorbent.

2. The preparation method according to claim 1, characterized in that, In step S1, the concentration of the hydrochloric acid is 1M.

3. The preparation method according to claim 1, characterized in that, In step S1, The liquid-to-solid ratio of the hydrochloric acid to the sludge ash is 10 mL: 1 g; The stirring reaction time is 2 hours; The centrifugation speed was 300 r / min and the time was 10 min.

4. The preparation method according to claim 1, characterized in that, In step S2, The stirring time is 24 hours; The centrifugation speed was 300 r / min and the time was 10 min; The cleaning process involves washing with deionized water three times. The drying temperature is 45°C.

5. The preparation method according to claim 1, characterized in that, In step S3, the amount of magnesium hydroxide added satisfies the molar ratio of magnesium to phosphorus in the system being 1.3:

1.

6. An ammonia nitrogen adsorbent prepared by the preparation method according to any one of claims 1-5.

7. A method for recovering ammonia nitrogen from landfill leachate, characterized in that, The process includes the following steps: adding the ammonia nitrogen adsorbent as described in claim 6 to the landfill leachate, adjusting the pH to alkaline, stirring and reacting, and then separating the solid and liquid phases to allow ammonia nitrogen to precipitate and be recovered from the leachate in the form of Mg-P compounds.

8. The method for recovering ammonia nitrogen from landfill leachate according to claim 7, characterized in that, The dosage of the ammonia nitrogen adsorbent is 0.1-2g of ammonia nitrogen adsorbent per 15mL of leachate.

9. The method for recovering ammonia nitrogen from landfill leachate according to claim 7, characterized in that, The pH is 9.5.

Citation Information

Patent Citations

  • Method for removing ammonia and nitrogen in garbage percolate

    CN101186408A

  • Urban domestic sludge incineration ash harmless treatment technology and phosphorus compound recycling method