A thin film and a method for manufacturing the same, a chip

By stacking SiCOH and SiON nanoporous thin film structures, the incompatibility between dielectric constant and mechanical strength of porous thin film dielectric layers is solved, achieving a balance between low dielectric constant and high mechanical strength, thereby improving chip performance and reliability.

CN122294930APending Publication Date: 2026-06-26WUHAN CHUXING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411885338.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-19
Publication Date
2026-06-26

AI Technical Summary

Technical Problem

When existing porous films are used as dielectric layers, it is difficult to achieve both low dielectric constant and high mechanical strength, which makes the chips prone to cracking during assembly and use, affecting reliability.

Method used

The first and second films are stacked together. The first film includes SiCOH and SiCNOH, and the second film includes SiON. Both contain nanopores. The cross-linked structure is formed by treating with nitrogen-hydrogen compound plasma to improve mechanical strength and reduce dielectric constant.

Benefits of technology

The dielectric constant of the thin film was 2.5-2.7, and the mechanical strength was greater than 1.1 GPa, which effectively reduced RC delay and improved chip reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122294930A_ABST
    Figure CN122294930A_ABST
Patent Text Reader

Abstract

This application relates to the field of porous thin film technology, and particularly to a thin film, its preparation method, and a chip. The thin film includes a first film layer and a second film layer stacked together. The first film layer includes SiCOH and SiCNOH, and the second film layer includes SiON. Both the first and second film layers contain nanopores. Because both the first and second film layers contain nanopores, the thin film exhibits a low dielectric constant. Furthermore, due to the Si-N-Si and Si-C-N crosslinking structures in SiCNOH and SiON, the thin film also possesses high mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of porous thin film technology, and in particular to a thin film and its preparation method, and a chip. Background Technology

[0002] A chip comprises multiple layers of metal interconnects, with dielectric layers separating adjacent interconnect layers. Each interconnect layer contains multiple metal wires that connect different electronic components to form complex circuits. The electronic components reside on the semiconductor layers of the chip, while the interconnect and dielectric layers are built upon them to ensure circuit integrity and functionality.

[0003] With the development of semiconductor technology, electronic components have become smaller, and more electronic components can be integrated on a single chip. This leads to an increase in the number and length of metal interconnects between electronic components. The resistance and capacitance of these metal interconnects cause signal transmission delays, which in turn makes the resistor-capacitor delay (RC delay) phenomenon in the chip more pronounced. RC delay has become an important factor affecting chip performance.

[0004] To reduce RC delay in chips, engineers typically use low-dielectric-constant (Low-k) thin films as dielectric layers to reduce the capacitance of metal interconnects. Currently, the industry commonly reduces the dielectric constant of thin films by increasing the number of holes in the film. However, increasing the number of holes in the film leads to a decrease in the film's mechanical strength, making it prone to cracking during chip assembly or use when used as a dielectric layer. This can cause short circuits or open circuits, thereby reducing chip reliability. Summary of the Invention

[0005] This application discloses a thin film, its preparation method, and a chip, to solve the problem that it is difficult to have both low dielectric constant and high mechanical strength when porous thin films are used as dielectric layers in related chips.

[0006] To achieve the above objectives, this application provides the following technical solution:

[0007] In a first aspect, this application provides a thin film comprising a first film layer and a second film layer stacked together, the first film layer comprising SiCOH and SiCNOH, and the second film layer comprising SiON, wherein both the first film layer and the second film layer comprise nanopores.

[0008] In the thin film of this application, since both the first and second film layers contain nanopores, the thin film has a low dielectric constant. At the same time, because SiCNOH and SiON contain SI-N-SI and SI-CN crosslinking structures, the thin film also has high mechanical strength.

[0009] In some embodiments, the mechanical strength of the film is greater than 1.1 GPa.

[0010] In some embodiments, the dielectric constant of the thin film is 2.5-2.7.

[0011] In some embodiments, the porosity of the second membrane layer is less than that of the first membrane layer.

[0012] In some embodiments, the thin film is composed of silicon, carbon, nitrogen, oxygen and hydrogen atoms in the form of a covalently linked network, and / or the pore size of the nanopores is less than or equal to 3 nm.

[0013] Secondly, this application provides a method for preparing a thin film, the method comprising the following steps:

[0014] Provide SiCOH membranes;

[0015] A thin film is obtained by plasma treatment of a SiCOH film using nitrogen-hydrogen compounds. The thin film includes a first film layer and a second film layer stacked together. The first film layer includes SiCOH and SiCNOH, and the second film layer includes SiON. Both the first film layer and the second film layer include nanopores.

[0016] In some embodiments, the nitrogen-hydrogen compound includes ammonia.

[0017] In some embodiments, the reaction temperature is 200-300 degrees Celsius, the reaction pressure is 5-15 Torr, the nitrogen-hydrogen compound plasma flow rate is 2000-3000 cubic centimeters per minute, the radio frequency power is 250-750 watts, and the processing time is 90-180 seconds.

[0018] In some embodiments, the pore size of the nanopore is less than or equal to 3 nm, and / or the dielectric constant of the thin film is 2.5-2.7.

[0019] Thirdly, this application provides a chip that includes the thin film of the first aspect or includes a thin film prepared using the preparation method of the second aspect. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the structure of a thin film provided in an embodiment of this application;

[0021] Figure 2 A schematic flowchart illustrating a method for preparing a thin film according to an embodiment of this application;

[0022] Figure 3 This is a schematic diagram of a method for preparing a thin film according to an embodiment of this application.

[0023] Icons: 100 - First film layer; 200 - Second film layer; 300 - Substrate layer; 400 - SiCOH film;

[0024] 01-Nanopores. Detailed Implementation

[0025] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application. In the description of the embodiments of this application, unless otherwise stated, " / " means "or", for example, A / B can mean A or B; "and / or" in the text is merely a description of the relationship between related objects, indicating that there can be three relationships, for example, A and / or B can represent: A alone, A and B at the same time, and B alone. In addition, in the description of the embodiments of this application, "multiple" means two or more.

[0026] Hereinafter, the terms "first" and "second" are used for descriptive purposes only and should not be construed as implying or suggesting relative importance or implicitly indicating the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature, and in the description of the embodiments of this application, unless otherwise stated, "multiple" means two or more.

[0027] With the advancement of semiconductor technology and the increasing miniaturization and integration of components, the resistive-capacitive delay (RC delay) caused by metal interconnects has gradually become more significant. Researchers have sought to reduce RC delay by using ultra-low dielectric constant materials (Low-k materials) as spacers. The methods employed in the Low-k thin film industry to reduce the K-value mainly fall into two categories: doping with atoms to reduce polarizability and increasing porosity to reduce the molecular density of the material.

[0028] To reduce RC delay in chips, engineers typically use low-dielectric-constant (Low-k) thin films as dielectric layers to reduce the capacitance of metal interconnects. Currently, the industry mainly reduces the dielectric constant of the film by increasing the number of holes in it. However, increasing the number of holes in the film leads to a decrease in its mechanical strength, making it impossible to balance the mechanical strength and dielectric constant.

[0029] In view of this, the present application provides a thin film, Figure 1 This is a schematic diagram of the structure of a thin film provided in an embodiment of this application, with reference to... Figure 1 The thin film includes a first film layer 100 and a second film layer 200 stacked together. The first film layer 100 includes SiCOH and SiCNOH, and the second film layer 200 includes SiON. Both the first film layer 100 and the second film layer 200 include nanopores O1.

[0030] Nanopores refer to pores of the nanometer size. The presence of nanopores in a thin film can result in a lower dielectric constant.

[0031] In one possible implementation, the pore size of the nanopore is less than or equal to 3 nm. For example, the pore size of the nanopore can be 3 nm, 2 nm, 1 nm, 0.5 nm, 0.1 nm, etc.

[0032] It should be noted that "the first film layer includes SiCOH" means that the first film layer includes Si, C, O, and H atoms. "The first film layer includes SiCNOH" means that the first film layer includes Si, C, O, N, and H atoms. "The second film layer includes SiON" means that the second film layer includes Si, O, and N atoms.

[0033] Understandably, the first film layer is composed of silicon, carbon, nitrogen, oxygen, and hydrogen atoms in a covalently linked network. Specifically, the first film layer includes Si-H bonds, Si-N-Si bonds, Si-CN bonds, Si-ON bonds, Si-O-Si bonds, and cross-linked structures formed by the aforementioned covalent bonds, giving the first film layer high mechanical strength.

[0034] Understandably, the second film layer is composed of silicon, oxygen, and nitrogen atoms in a covalently linked network. Specifically, the second film layer includes Si-O bonds, Si-N-Si bonds, Si-ON bonds, Si-O-Si bonds, and cross-linked structures formed by the aforementioned covalent bonds, resulting in high mechanical strength.

[0035] In one possible implementation, the surface of the second film layer is slightly porous, with low porosity, high mechanical strength, and low dielectric constant.

[0036] In one possible implementation, the mechanical strength of the film is greater than 1.1 GPa. For example, the mechanical strength of the film may be 1.2 GPa, 1.3 GPa, 1.4 GPa, 1.5 GPa, 1.6 GPa, 1.7 GPa, 1.8 GPa, 1.9 GPa, 2.0 GPa, 2.5 GPa, 3.0 GPa, etc.

[0037] In one possible implementation, the dielectric constant of the thin film is 2.5-2.7. For example, the dielectric constant of the thin film can be 2.5, 2.52, 2.54, 2.55, 2.57, 2.59, 2.6, 2.62, 2.65, 2.68, 2.7, and any other value between 2.5 and 2.7.

[0038] In one possible implementation, the porosity of the second membrane layer is less than that of the first membrane layer, making the second membrane layer more compact and possessing higher mechanical strength.

[0039] Based on the same technical concept, embodiments of this application also provide a method for preparing a thin film. Figure 2 This is a schematic flowchart of a method for preparing a thin film provided in an embodiment of this application, referring to... Figure 2 The preparation method includes the following steps:

[0040] S1: Provides a SiCOH membrane;

[0041] S2: The SiCOH film is subjected to plasma treatment using nitrogen-hydrogen compounds to obtain a thin film, wherein the thin film includes a first film layer and a second film layer stacked together, the first film layer includes SiCOH and SiCNOH, and the second film layer includes SiON, wherein both the first film layer and the second film layer include nanopores.

[0042] In one possible implementation, the nitrogen-hydrogen compound includes, but is not limited to, ammonia. It is understood that the amount of nitrogen atoms incorporated into the film is controlled by controlling the mass of the nitrogen-hydrogen compound, so that the film in this application has high mechanical strength while having a low dielectric constant.

[0043] In one possible implementation, the reaction temperature is 200-300 degrees Celsius, the reaction pressure is 5-15 Torr, the nitrogen-hydrogen compound plasma flow rate is 2000-3000 cubic centimeters per minute, the radio frequency power is 250-750 watts, and the processing time is 90-180 seconds.

[0044] The reaction temperature can be 200 degrees, 210 degrees, 220 degrees, 230 degrees, 240 degrees, 250 degrees, 260 degrees, 270 degrees, 280 degrees, 290 degrees, 300 degrees, or any other value between 200 and 300 degrees.

[0045] The reaction pressure can be 5 Torr, 6 Torr, 7 Torr, 8 Torr, 9 Torr, 10 Torr, 11 Torr, 12 Torr, 13 Torr, 14 Torr, 15 Torr, or any other value between 5 and 15 Torr.

[0046] The nitrogen-hydrogen compound plasma flux can be any other value between 2000 sccm, 2100 sccm, 2200 sccm, 2300 sccm, 2400 sccm, 2500 sccm, 2600 sccm, 2700 sccm, 2800 sccm, 2900 sccm, 3000 sccm, and 2000-3000 sccm.

[0047] The radio frequency power can be 250 watts, 300 watts, 350 watts, 400 watts, 450 watts, 500 watts, 550 watts, 600 watts, 650 watts, 700 watts, 750 watts, or any other value between 250 and 750 watts.

[0048] The processing time can be 90 seconds, 100 seconds, 110 seconds, 120 seconds, 130 seconds, 150 seconds, 160 seconds, 170 seconds, 180 seconds, or any other value between 90 and 180 seconds.

[0049] In one possible implementation, the preparation method in this application further includes the preparation of a SiCOH film. Figure 3 This is a schematic diagram of a method for preparing a thin film according to an embodiment of this application, with reference to... Figure 3 The preparation of SiCOH membranes includes:

[0050] Diethoxy(methyl)silane (DEMS) and atom transfer radical polymerization (ATRP) were reacted under oxygen conditions to obtain SiCOH film 400.

[0051] In one possible implementation, a SiCOH film 400 is formed on the surface of the substrate 300. The substrate 300 may be a silicon (Si) substrate 300.

[0052] Continue to refer to Figure 3 The SiCOH film 400 was treated with NH3 plasma to obtain the film in this application.

[0053] Among them, NH3 is decomposed into H under the action of plasma. + NH + N + free radicals, H + During plasma treatment, free radicals react with methyl groups (Si-CH3 from ATRP) to generate methane gas (CH4). This methane gas condenses and escapes, forming large-pore structures within the film, thereby reducing its dielectric constant. Simultaneously, H... +Free radicals can transform Si-CH3 into Si-H. The free volume of the Si-H bond is smaller than that of the Si-CH3 bond, resulting in a shrinkage phenomenon. The polymer chain becomes more compact, and the concentration of Si-O-Si bonds per unit volume increases, thereby improving the mechanical strength of the film.

[0054] In addition, NH + and N + Free radicals can combine with some SI-C and SI+ in the film to form a small amount of cross-linked structures of SI-N-SI and SI-CN, which can significantly increase the mechanical strength of the film.

[0055] In the preparation method of this application, because the cost of nitrogen-hydrogen compounds is relatively low, the preparation method of this application is simple and the raw material cost is low. Compared with the existing methods for preparing thin films with low dielectric constants, the production cost and reaction time of the method in this application are significantly reduced.

[0056] In one possible implementation, the pore size of the nanopore is less than or equal to 3 nm, and / or the dielectric constant of the thin film is 2.5-2.7.

[0057] Based on the same technical concept, embodiments of this application also provide a chip, which includes the thin film in various possible embodiments of this application or includes a thin film prepared using the preparation methods in various possible embodiments. This thin film can serve as a dielectric layer in the chip because it has a low dielectric constant and high mechanical properties, thereby effectively reducing the RC delay of the chip. Furthermore, the dielectric layer using the aforementioned thin film exhibits high reliability.

[0058] It is understood that the thin film in this application can also be used to prepare other electronic devices, and is not limited to chips.

[0059] Obviously, those skilled in the art can make various modifications and variations to the embodiments of this application without departing from the spirit and scope of this application. Therefore, if these modifications and variations of this application fall within the scope of the claims of this application and their equivalents, this application also intends to include these modifications and variations.

Claims

1. A film, characterized by, The thin film comprises a first film layer and a second film layer stacked, the first film layer comprises SiCOH and SiCNOH, the second film layer comprises SiON, and the first film layer and the second film layer both comprise nanopores.

2. The film according to claim 1, characterized in that, The mechanical strength of the thin film is greater than 1.1 GPa.

3. The film of claim 1, wherein The dielectric constant of the thin film is 2.5-2.

7.

4. The film according to any one of claims 1 to 3, characterized in that, The porosity of the second film layer is less than that of the first film layer.

5. The film according to any one of claims 1 to 3, characterized in that, The thin film is composed of silicon, carbon, nitrogen, oxygen and hydrogen atoms in the form of covalent connection network, and / or the pore size of the nanopores is less than or equal to 3 nm.

6. A method of producing a film, characterized by, The method comprises the following steps: providing a SiCOH film; plasma treating the SiCOH film with a nitrogen-hydrogen compound to obtain the thin film, wherein the thin film comprises a first film layer and a second film layer stacked, the first film layer comprises SiCOH and SiCNOH, the second film layer comprises SiON, and the first film layer and the second film layer both comprise nanopores.

7. The production method according to claim 6, wherein The nitrogen-hydrogen compound comprises ammonia.

8. The preparation method according to claim 6, characterized in that, The plasma treatment comprises: the reaction temperature is 200-300 degrees, the reaction pressure is 5-15 torr, the nitrogen-hydrogen compound plasma flow is 2000-3000 cubic centimeters per minute, the radio frequency power is 250-750 watts, and the processing time is 90-180 seconds.

9. The production method according to claim 8, characterized by, The pore size of the nanopores is less than or equal to 3 nm, and / or the dielectric constant of the thin film is 2.5-2.

7.

10. A chip, characterized by The method comprises the thin film as claimed in any one of claims 1-5 or the thin film prepared by the preparation method as claimed in any one of claims 6-9.