A method for manufacturing Luneburg lenses
By employing bead foaming and high-temperature gradient foaming processes, combined with skin removal, the problems of dielectric discontinuity and low efficiency in Luneburg lenses have been solved, enabling the fabrication of Luneburg lenses with high efficiency and low cost, suitable for aerospace and automotive equipment.
Patent Information
- Application Number
- CN202610757804.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-05-29
AI Technical Summary
The existing Luneburg lens fabrication process suffers from dielectric discontinuity and low efficiency. Furthermore, the high-temperature and high-pressure physical foaming process is difficult to control. 3D printing and ceramic firing processes are costly and have low industrialization efficiency. Layered fabrication leads to step changes in dielectric constant and interlayer electromagnetic wave loss.
The process employs bead foaming, room temperature low-pressure pre-compression, instantaneous high-temperature gradient foaming, and skin removal. Through the mixing of polymer, nano-calcium carbonate, and dielectric constant modifier, followed by melt blending, extrusion granulation, molding, pre-compression, instantaneous high-temperature gas injection, and skin removal, a continuously gradient dielectric structure is formed.
It has enabled the efficient and low-cost mass production of Luneburg lenses, with good dielectric continuity, reduced electromagnetic wave reflection loss, and met the lightweight and mechanical requirements of aerospace and automotive equipment, thus improving industrial adaptability.
Smart Images

Figure REF-OBJ-1780018227633-000001
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electromagnetic wave dielectric device fabrication technology, and relates to a method for fabricating a Luneburg lens. Background Technology
[0002] A Luneburg lens is a spherical dielectric antenna with a spherically symmetric gradient dielectric constant distribution. Its dielectric constant changes continuously from the center to the outer layer, allowing it to efficiently focus incident plane waves to a single point on the sphere or convert spherical waves into plane waves. It has irreplaceable application value in satellite communications, radar detection, electronic countermeasures, and vehicle-mounted millimeter-wave communications. Because electromagnetic waves can be blocked and their propagation direction altered within this lens, it can also serve as an electromagnetic interference device. When radar waves pass through this device, they are refracted and amplified in a spherically symmetric manner, causing a small aircraft to appear as a large image on the radar screen, misleading observers into believing it is a large aircraft. Stealth aircraft often temporarily install Luneburg lenses during non-combat transit flights to facilitate detection by civil aviation air traffic control radar.
[0003] Chinese invention patent application CN118005986A discloses a foamed material with a gradient dielectric constant distribution and its preparation method. The material undergoes two physical foaming processes using the same method, and the gradient change in cell size is controlled by controlling the second gas saturation time. However, both physical foaming processes involve high-temperature and high-pressure gases, making the saturation process difficult to control.
[0004] Chinese invention patent application CN114874027A discloses a low dielectric loss ceramic material Luneburg lens and its preparation process. Each dielectric layer is made of porous ceramic material. The porous ceramic material is obtained by foaming and sintering Al2O3·SiO2 as the skeleton raw material and alkali metal and / or mineral raw materials containing alkaline earth metals as auxiliary materials.
[0005] Chinese invention patent application CN112736485A discloses a foamed Luneburg lens and its manufacturing process. The first step is to 3D print spheres with different numbers of layers, each layer containing a different dielectric constant modifier; the second step is to foam the lens with supercritical fluid to obtain foam spheres.
[0006] In the above technical solutions, the gas saturation process of the two high-temperature and high-pressure physical foaming processes is difficult to control and takes a long time. The industrialization efficiency of 3D printing and ceramic firing processes is low and the cost is high. In addition, the layered preparation will cause problems such as step change of dielectric constant and electromagnetic wave loss between layers, making it difficult to balance the preparation efficiency and dielectric continuity of Luneburg lenses. Summary of the Invention
[0007] The purpose of this invention is to provide a method for manufacturing Luneburg lenses, which solves the problems of dielectric discontinuity and low efficiency in existing technologies by using bead foaming, room temperature low pressure pre-pressing, instantaneous high temperature gradient foaming and skin removal processes, thereby achieving efficient and low-cost mass production and excellent performance of Luneburg lenses.
[0008] The objective of this invention can be achieved through the following technical solutions: A method for manufacturing a Luneburg lens includes the following steps: Step 1: Mix the polymer, nano-calcium carbonate as a cell nucleating agent, and dielectric constant regulator evenly, melt blend, extrude and granulate to obtain plastic microparticles; then add the plastic microparticles to a sealed foaming kettle for bead foaming to obtain foamed beads; fill the foamed beads into the cavity of a spherical mold and mold them to obtain foam spheres.
[0009] Step 2: Add the foam spheres to the pre-compression tank, introduce pre-compression gas until the pressure inside the tank reaches 0.3-1.0 MPa, and maintain the pressure at 20-30℃ for 4-18 hours to obtain pre-compressed foam spheres.
[0010] Step 3: Place the pre-compressed foam spheres into a heating chamber at 20-30℃, and instantly inject high-temperature gas into the heating chamber. After the injection is completed, immediately shut off the chamber, depressurize and cool to obtain gradient pore foam spheres.
[0011] Step 4: Remove the dense skin from the surface of the gradient pore foam ball to obtain the Luneburg lens.
[0012] The mass ratio of polymer, nano-calcium carbonate and dielectric constant modifier is 100:0.5-1.2:8-25.
[0013] Furthermore, the dielectric constant modifier is any one of barium titanate, zirconium oxide, zinc oxide, and silicon nitride, or a mixture thereof in any proportion.
[0014] Furthermore, the polymer is any one of polypropylene, polyethylene, and thermoplastic elastomer.
[0015] Furthermore, the process parameters for melt blending are as follows: Zone 1 temperature 175±5℃, Zone 2 temperature 185±5℃, Zone 3 temperature 195±5℃, Zone 4 temperature 205±5℃, main machine speed 250-350r / min, and feeding speed 80-120r / min.
[0016] Furthermore, in the bead foaming process, supercritical carbon dioxide is introduced, and the pressure is increased to 3.0-5.0 MPa at a rate of 0.2-0.5 MPa / min, while the temperature is increased to 140-155℃ at a rate of 1-2℃ / min, and the pressure holding time is 40-70 min.
[0017] Furthermore, saturated steam is introduced during the molding process, with a steam pressure of 0.15-0.35 MPa and a heating time of 15-50 seconds.
[0018] Furthermore, the pressurization rate of the pre-pressurized gas is 0.1-0.2 MPa / min.
[0019] Furthermore, the pre-compressed gas can be any one of compressed air, nitrogen, and carbon dioxide.
[0020] Furthermore, the high-temperature gas can be either high-pressure steam or high-temperature hot air.
[0021] Furthermore, the temperature of the high-pressure steam is 155-175℃, the injection pressure is 0.25-0.45MPa, and the injection time is 1-6s.
[0022] Furthermore, the temperature of the hot air is 170-195℃, the wind speed is 8-15m / s, and the jetting time is 2-8s.
[0023] Furthermore, the skin removal process uses a CNC spherical turning machine, employing polycrystalline diamond tools to uniformly machine along the spherical surface at a speed of 200-500 r / min and a cutting depth of 0.2-0.5 mm.
[0024] The beneficial effects of this invention are: This invention employs polymer bead foaming and molding processes to prepare foam spheres with uniform cell structure. Subsequently, gradient cell formation is achieved by pre-pressurizing the foam spheres with gas at room temperature (20-30℃) and low pressure (0.3-1.0MPa) combined with instantaneous high-temperature gas injection for 1-8 seconds. Then, by removing the dense outer skin of the gradient cell foam spheres, the internal gradient cell structure is exposed, making the dielectric constant of the lens surface layer close to that of air. This minimizes reflection loss during the electromagnetic wave incident phase. The one-piece molding method completely solves the problems of abrupt change in dielectric constant and interlayer electromagnetic wave loss caused by layered preparation. It successfully achieves a balance between preparation efficiency, production cost, and dielectric continuity, significantly improving industrial applicability.
[0025] This invention utilizes a gas pre-pressurization process within a sealed pre-pressurization tank to allow pre-pressurized gas to slowly permeate from the surface of the foam spheres towards the core, naturally forming a radial concentration gradient with a high gas concentration on the surface and a low gas concentration in the core. Triggered by the instantaneous injection of high-temperature gas, the gas within the pores expands due to the concentration difference, ultimately resulting in a continuous, gradually changing structure where the core pores are small and the surface pores are large. Since the dielectric constant of the polymer foam is negatively correlated with the pore size ratio, the lens dielectric constant also achieves a continuous radial gradient with a high core dielectric constant and a low surface dielectric constant, without any abrupt changes or interlayer interfaces. This structurally ensures stable refraction and efficient transmission of electromagnetic waves within the lens, significantly reducing transmission loss.
[0026] This invention offers an intuitive and simple logic for controlling the dielectric gradient of lenses. It precisely regulates the gas permeation gradient and cell expansion using only three core process parameters: pre-pressurization gas pressure, pre-pressurization holding time, and high-temperature gas injection time. The pre-pressurization gas pressure determines the driving force for gas permeation, with high pressure creating a steep gradient and low pressure creating a gentler gradient. The pre-pressurization holding time controls the gas permeation depth, adapting to small-sized, high-gradient foam spheres in a short time and large-sized, continuous-gradient foam spheres in a longer time. The high-temperature gas injection time regulates the energy supply for cell expansion, creating a distinct size difference in a short time and a smooth transition in a long time. Compared to existing layered fabrication processes that require precise design of the dielectric modifier ratio for multiple substrates, and high-temperature, high-pressure foaming processes that require strict temperature and pressure matching, this solution offers fewer control dimensions and lower precision requirements for production equipment and operations. It effectively ensures consistency in key performance aspects such as dielectric gradient and dimensional accuracy across multiple batches of products, reducing the difficulty of quality control in large-scale production.
[0027] This invention uses polymers such as polypropylene as the base material, and forms a closed-cell foam structure through bead foaming and secondary gradient foaming. The lens density is much lower than that of ceramic-based Luneburg lenses, achieving extreme lightweighting of the product. It is perfectly suited for weight-sensitive applications such as aircraft and automotive equipment. At the same time, the integral foam spheres obtained through steam molding are free of layering and splicing gaps. The gradient cell structure after secondary foaming completely retains the good mechanical toughness and thermal stability of polymer foam, giving the lens excellent vibration resistance and temperature resistance. It can adapt to the mechanical and environmental requirements of different application scenarios such as aerospace, radar detection, and automotive millimeter-wave communication, and has a wider range of applications. Detailed Implementation
[0028] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.
[0029] Example 1: This example provides a method for manufacturing a Luneburg lens, including the following steps: S1: By mass, add 100 parts polypropylene, 0.5 parts cell nucleating agent (nano calcium carbonate, particle size 50-200nm) and 8 parts dielectric constant modifier (barium titanate powder, particle size 100-500nm) to a high-speed mixer and mix at high speed for 5 minutes. Then add the mixture to a twin-screw extruder and extrude at the following zone temperatures: Zone 1 170℃, Zone 2 180℃, Zone 3 190℃, Zone 4 200℃, main machine speed 250r / min, feed speed 80r / min. The extruded melt is water-cooled, stretched, and pelletized to obtain plastic microparticles with a single particle weight of 0.8mg.
[0030] S2: By mass, add 300 parts of deionized water and 0.6 parts of kaolin to the foaming kettle and stir at 100 r / min until completely dispersed. Add 100 parts of plastic microparticles, close and seal the foaming kettle, and purge the air in the kettle with nitrogen (replace 3 times, each time holding the pressure at 0.5 MPa and then releasing the pressure to atmospheric pressure). Purge supercritical carbon dioxide into the foaming kettle and pressurize it to 3.0 MPa at a rate of 0.2 MPa / min, while simultaneously heating it to 140℃ at a rate of 1℃ / min. Hold the pressure for 40 min to allow the carbon dioxide to fully penetrate into the plastic microparticles. Release the pressure to obtain foamed beads with a foaming ratio of 3 times.
[0031] Under high temperature and pressure, supercritical carbon dioxide, as a small molecule physical foaming agent, slowly penetrates into the molecular gaps of plastic microparticles to form a thermodynamically stable homogeneous system. When the pressure is rapidly released, the system pressure drops sharply, the solubility of carbon dioxide decreases drastically, and it precipitates out from the homogeneous system. Under the induction of the cell nucleating agent, a large number of uniform cell nuclei are formed. The cell nuclei grow rapidly under the action of pressure difference. The viscoelasticity of the polypropylene melt limits the excessive expansion of the cells, and finally forms uniform closed-cell foamed beads.
[0032] S3: Freely fill the foamed beads into the cavity of the spherical mold, close and lock the mold, introduce saturated steam from the bottom of the mold at a pressure of 0.15MPa, heat for 15s until the surface of the beads melts, close the steam inlet, maintain the mold closing force, introduce cooling water into the water cooling channel of the mold, maintain pressure and cool for 8min, open the mold and discharge the material to obtain foam spheres.
[0033] The heat of saturated steam softens and melts the polypropylene melt on the surface of the foamed beads, causing the beads to bond and fuse together to form a continuous integral structure. Cooling water quickly removes the heat, causing the molten polypropylene surface to crystallize and solidify rapidly, while retaining the uniform cell structure inside the beads, ultimately resulting in a seamless, layer-free integral foam sphere.
[0034] S4: Add the foam spheres to the pre-compression tank, ensuring that the spheres are not compressed and do not contact the tank wall. Close and seal the pre-compression tank, open the air inlet valve, and introduce compressed air into the tank at a rate of 0.1 MPa / min until the pressure inside the tank reaches 0.3 MPa. Maintain the pressure at 20℃ for 4 hours (adjust the time according to the size of the spheres). After the pre-compression is completed, maintain the pressure inside the tank to obtain pre-compressed foam spheres.
[0035] Compressed air, as the permeation medium, needs to slowly permeate from the skin to the core through the closed pores and cell walls of the foam spheres. The skin area comes into contact with the compressed air first, and the gas molecules are quickly adsorbed and dissolved in the polymer matrix of the skin cell walls. However, because the core is far from the skin, the gas needs to permeate layer by layer to reach it. There is a natural permeation time difference. Within the set pre-compression time, the air cannot completely permeate to the core, ultimately forming a radial concentration gradient with a high gas concentration on the skin and a low gas concentration in the core (the amount of gas adsorbed / dissolved on the skin cell walls is much greater than that in the core), providing the core conditions for subsequent gradient expansion.
[0036] S5: Place the pre-compressed foam spheres into a 20°C heating chamber (the pre-compressor tank also functions as a heating chamber; after rapid depressurization of the pre-compressor tank, it functions as a heating chamber through its internal mechanism). Instantly open the high-temperature gas injection port to inject high-pressure steam into the heating chamber, achieving rapid heating and expansion. The temperature of the high-pressure steam is 155°C, the injection pressure is 0.25 MPa, and the injection time is 1 second. Immediately close the high-temperature gas injection port, open the heating chamber exhaust port, and allow it to naturally depressurize to atmospheric pressure and cool to room temperature to obtain gradient-cell foam spheres.
[0037] The high-temperature gas (high-pressure steam) injected instantaneously, with its high thermal conductivity, preferentially transfers heat to the surface of the foam spheres in a very short time. Due to the heat transfer delay caused by the closed-cell structure, a temperature gradient is formed where the surface heats up rapidly and the core heats up slowly. The foam spheres, after being pre-compressed, have a distribution of high gas concentration on the surface and low gas concentration in the core. When the high-concentration gas on the surface is heated, the pressure rises sharply, and the expansion driving force is much greater than that of the low-concentration gas in the core. This causes the surface pores to expand significantly, while the core pores basically maintain their original size. At the same time, the viscoelasticity of polypropylene decreases at high temperatures, which can accommodate the expansion of the pores. After heating is stopped, natural cooling allows the viscoelasticity of polypropylene to recover rapidly, fixing the pore gradient morphology of dense inside and sparse outside. Since the dielectric constant of the polymer foam is negatively correlated with its porosity, a continuous dielectric gradient distribution is ultimately formed, with small pores in the core (low porosity, high dielectric) and large pores on the surface (high porosity, low dielectric), perfectly matching the core requirements of Luneburg lenses.
[0038] S6: Fix the gradient-cell foam ball on a CNC spherical turning machine, use a polycrystalline diamond tool at a speed of 200 r / min and a cutting depth of 0.2 mm to uniformly process along the spherical surface, uniformly remove the dense skin, and blow away the debris with 0.2 MPa compressed air to obtain the Luneburg lens.
[0039] Example 2: This example provides a method for manufacturing a Luneburg lens, including the following steps: S1: By mass, add 100 parts polypropylene, 1.2 parts cell nucleating agent (nano calcium carbonate, particle size 50-200nm) and 25 parts dielectric constant modifier (barium titanate powder, particle size 100-500nm) to a high-speed mixer and mix at high speed for 10 minutes. Then add it to a twin-screw extruder and extrude at the following zone temperatures: Zone 1 180℃, Zone 2 190℃, Zone 3 200℃, Zone 4 210℃, main machine speed 350r / min, feed speed 120r / min. The extruded melt is water-cooled, stretched, and pelletized to obtain plastic microparticles with a single particle weight of 1.2mg.
[0040] S2: By mass, add 500 parts of deionized iron and 1.5 parts of kaolin to the foaming kettle and stir at 200 r / min until completely dispersed. Add 100 parts of plastic microparticles, close and seal the foaming kettle, and purge the air in the kettle with nitrogen (replace 3 times, each time holding the pressure at 0.5 MPa and then releasing the pressure to atmospheric pressure). Purge supercritical carbon dioxide into the foaming kettle and pressurize it to 5.0 MPa at a rate of 0.5 MPa / min, while simultaneously heating it to 155℃ at a rate of 2℃ / min. Hold the pressure for 70 min to allow the carbon dioxide to fully penetrate into the plastic microparticles. Release the pressure to obtain foamed beads with a foaming ratio of 20.
[0041] S3: Freely fill the foamed beads into the cavity of the spherical mold, close and lock the mold, introduce saturated steam from the bottom of the mold at a pressure of 0.35 MPa, heat for 15-50 seconds until the surface of the beads melts, close the steam inlet, maintain the mold closing force, introduce cooling water into the water cooling channel of the mold, maintain pressure and cool for 25 minutes, open the mold and discharge the material to obtain foam spheres.
[0042] S4: Add the foam spheres to the pre-compression tank, ensuring that the spheres are not compressed and do not contact the tank wall. Close and seal the pre-compression tank, open the air inlet valve, and introduce compressed air into the tank at a rate of 0.2 MPa / min until the pressure inside the tank reaches 1.0 MPa. Maintain the pressure at 30℃ for 18 hours (adjust the time according to the size of the spheres). After the pre-compression is completed, maintain the pressure inside the tank to obtain pre-compressed foam spheres.
[0043] S5: Place the pre-compressed foam spheres into a heating chamber at 30°C (the pre-compressor tank also serves as the heating chamber; after rapid depressurization of the pre-compressor tank, it functions as a heating chamber through its internal mechanism). Instantly open the high-temperature gas injection port to inject high-pressure steam into the heating chamber, achieving rapid heating and expansion. The temperature of the high-pressure steam is 175°C, the injection pressure is 0.45 MPa, and the injection time is 6 seconds. Immediately close the high-temperature gas injection port, open the heating chamber exhaust port, and allow it to naturally depressurize to atmospheric pressure and cool to room temperature to obtain gradient-cell foam spheres.
[0044] S6: Fix the gradient-cell foam ball on a CNC spherical turning machine, use a polycrystalline diamond tool at a speed of 500 r / min and a cutting depth of 0.5 mm to uniformly process along the spherical surface, uniformly remove the dense skin, and blow away the debris with 0.3 MPa compressed air to obtain the Luneburg lens.
[0045] Example 3: This example provides a method for manufacturing a Luneburg lens, including the following steps: S1: By mass, add 100 parts polypropylene, 0.8 parts cell nucleating agent (nano calcium carbonate, particle size 50-200nm) and 16 parts dielectric constant modifier (barium titanate powder, particle size 100-500nm) to a high-speed mixer and mix at high speed for 7 minutes. Then add the mixture to a twin-screw extruder and extrude at the following zone temperatures: Zone 1 175℃, Zone 2 185℃, Zone 3 195℃, Zone 4 205℃, main machine speed 300r / min, feed speed 100r / min. The extruded melt is water-cooled, stretched, and pelletized to obtain plastic microparticles with a single particle weight of 1.0mg.
[0046] S2: By mass, add 400 parts of deionized oil and 1 part of kaolin to the foaming kettle and stir at 150 r / min until completely dispersed. Add 100 parts of plastic microparticles, close and seal the foaming kettle, and purge the air in the kettle with nitrogen (replace 3 times, each time holding the pressure at 0.5 MPa and then releasing the pressure to atmospheric pressure). Purge supercritical carbon dioxide into the foaming kettle and pressurize it to 4.0 MPa at a rate of 0.3 MPa / min, while simultaneously heating it to 147°C at a rate of 1°C / min. Hold the pressure for 55 min to allow the carbon dioxide to fully penetrate into the plastic microparticles. Release the pressure to obtain foamed beads with a foaming ratio of 11 times.
[0047] S3: Freely fill the foamed beads into the cavity of the spherical mold, close and lock the mold, introduce saturated steam from the bottom of the mold at a pressure of 0.25 MPa (corresponding to a temperature of 132℃), heat for 30 seconds until the surface of the beads melts, close the steam inlet, maintain the mold closing force, introduce cooling water into the water cooling channel of the mold, maintain pressure and cool for 12 minutes, open the mold and discharge the material to obtain foam spheres.
[0048] S4: Add the foam spheres to the pre-compression tank, ensuring that the spheres are not compressed and do not contact the tank wall. Close and seal the pre-compression tank, open the air inlet valve, and introduce compressed air into the tank at a rate of 0.15 MPa / min until the pressure inside the tank reaches 0.6 MPa. Maintain the pressure at 25℃ for 11 hours (adjust the time according to the size of the spheres). After the pre-compression is completed, maintain the pressure inside the tank to obtain pre-compressed foam spheres.
[0049] S5: Place the pre-compressed foam spheres into a 25°C heating chamber (the pre-compressor tank also functions as a heating chamber; after rapid depressurization of the pre-compressor tank, it functions as a heating chamber through its internal mechanism). Instantly open the high-temperature gas injection port and inject high-pressure steam into the heating chamber to achieve rapid heating and expansion. The temperature of the high-pressure steam is 165°C, the injection pressure is 0.35MPa, and the injection time is 3s. Immediately close the high-temperature gas injection port, open the heating chamber exhaust port, and allow it to naturally depressurize to atmospheric pressure and cool to room temperature to obtain gradient-cell foam spheres.
[0050] S6: Fix the gradient-cell foam ball on a CNC spherical turning machine, use a polycrystalline diamond tool at a speed of 350 r / min and a cutting depth of 0.3 mm to uniformly process along the spherical surface, uniformly remove the dense skin, and blow away the debris with 0.25 MPa compressed air to obtain the Luneburg lens.
[0051] Example 4: This example provides a method for preparing a Luneburg lens. The difference from Example 3 is that zirconium oxide powder is used instead of barium titanate powder in step S1.
[0052] Example 5: This example provides a method for preparing a Luneburg lens. The difference from Example 3 is that silicon nitride powder is used instead of barium titanate powder in step S1.
[0053] Example 6: This example provides a method for preparing a Luneburg lens. The difference from Example 3 is that polyethylene is used instead of polypropylene in step S1.
[0054] Example 7: This example provides a method for preparing a Luneburg lens. The difference from Example 3 is that nitrogen is used instead of compressed air in step S4.
[0055] Example 8: This example provides a method for preparing a Luneburg lens. The difference from Example 3 is that in step S5, high-temperature hot air is used instead of high-pressure water vapor. The temperature of the high-temperature hot air is 170°C, the wind speed is 8 m / s, and the spraying time is 2 s.
[0056] Example 9: This example provides a method for preparing a Luneburg lens. The difference from Example 8 is that the temperature of the high-temperature hot air in step S5 is 195°C, the wind speed is 15 m / s, and the spraying time is 8 s.
[0057] Comparative Example 1: This comparative example provides a method for preparing a Luneburg lens. The difference from Example 3 is that step S4 is removed, and the foam spheres prepared in step S3 are used instead of the pre-compressed foam spheres in step S5.
[0058] Comparative Example 2: This comparative example provides a method for manufacturing a Luneburg lens, referring to the existing technology of "two-stage high-temperature and high-pressure physical foaming" (refer to CN118005986A), as follows: Step 1: First, put the plastic microparticles prepared in Example 3 into the cavity of a spherical mold, set the temperature inside the mold cavity to 138°C, and inject the foaming agent gas carbon dioxide into the mold cavity until the pressure inside the mold cavity reaches 14MPa. Keep it at the same temperature and pressure for 51.56 hours. Step 2: Depressurize the pressure inside the mold cavity to ambient pressure at a depressurization rate of 300 MPa / s, and let it stand for 24 hours under normal temperature and pressure (25℃, 0.101325 MPa) to obtain primary foamed spheres.
[0059] Step 3: Place the primary foamed sphere into the cavity of the spherical mold, set the temperature inside the mold cavity to 148℃, and inject the foaming agent gas carbon dioxide into the mold cavity until the pressure inside the mold cavity reaches 13.5MPa. Keep it at the same temperature and pressure for 1.1 hours, and then release the pressure inside the mold cavity to the ambient pressure at a depressurization rate of 300MPa / s to obtain the Luneburg lens.
[0060] The Luneburg lenses prepared in Examples 1-9 and Comparative Examples 1-2 were subjected to performance tests: Dielectric constant gradient continuity: Referring to the resonant cavity method (GB / T 1409-2006), one test point was taken every 5 mm along the lens radius direction (0-75 mm), and the dielectric constant deviation rate (standard deviation / mean value × 100%) was calculated. The instrument used was a vector network analyzer (Agilent N5230A), with a test frequency of 10 GHz, an ambient temperature of 25℃, and a humidity of 50%.
[0061] Electromagnetic wave transmittance: The transmittance of electromagnetic waves in the 10 GHz band was tested using the free space method when the waves were incident perpendicularly. A microwave anechoic chamber and a signal generator (Rohde & Schwarz SMW200A) were used. The electromagnetic wave incident angle was 0° and the power was 10 dBm.
[0062] Product density: The mass and volume of the lens were measured by the water displacement method, and the density (ρ=m / V) was calculated at room temperature of 25℃.
[0063] The test results are shown in the table below: Table 1 Performance Test Overview As shown in Table 1, the dielectric constant gradient deviation rate of Examples 1-9 is less than that of Comparative Examples 1-2. This may be because Examples 1-9 constructed a radial gas concentration gradient from the skin to the core through gas pre-compression, and the gradient expansion was triggered by instantaneous heating to form a continuous non-step bubble gradient, thereby achieving a continuous gradual change in dielectric constant. However, Comparative Example 1 lacked the pre-compression step and could not form an effective gradient structure, resulting in a disordered dielectric distribution. Comparative Example 2 adopted a two-stage high-temperature and high-pressure foaming process, which is prone to dielectric constant jumps due to uneven gas saturation, resulting in a significantly increased deviation rate.
[0064] As shown in Table 1, the electromagnetic wave transmittance of Examples 1-9 is higher than that of Comparative Examples 1-2. This may be because the examples removed the high dielectric dense skin, making the surface dielectric constant close to that of air, which greatly optimized the impedance matching and reduced the electromagnetic wave incident and reflected loss.
[0065] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus.
[0066] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A method for manufacturing a Luneburg lens, characterized in that, Includes the following steps: Step 1: Mix the polymer, nano-calcium carbonate as a cell nucleating agent, and dielectric constant regulator evenly, melt blend, extrude and granulate to obtain plastic microparticles; then add the plastic microparticles to a sealed foaming kettle for bead foaming to obtain foamed beads; fill the foamed beads into the cavity of a spherical mold, and mold them to obtain foam spheres; Step 2: Add the foam spheres to the pre-compression tank, introduce pre-compression gas until the pressure inside the tank reaches 0.3-1.0 MPa, and maintain the pressure at 20-30℃ for 4-18 hours to obtain pre-compressed foam spheres; Step 3: Place the pre-compressed foam spheres into a heating chamber at 20-30℃, and instantly inject high-temperature gas into the heating chamber. After the injection is completed, immediately close the chamber, depressurize and cool to obtain gradient pore foam spheres. Step 4: Remove the dense skin from the surface of the gradient-porous foam ball to obtain the Luneburg lens; The mass ratio of the polymer, nano-calcium carbonate, and dielectric constant modifier is 100:0.5-1.2:8-25; The pressurization rate of the pre-compressed gas is 0.1-0.2 MPa / min; The high-temperature gas mentioned in step three is either high-pressure steam or high-temperature hot air; The high-pressure steam has a temperature of 155-175℃, an injection pressure of 0.25-0.45MPa, and an injection duration of 1-6s. The temperature of the high-temperature hot air is 170-195℃, the wind speed is 8-15m / s, and the jetting time is 2-8s; The skin removal process described in step four uses a CNC spherical turning machine, employing polycrystalline diamond tools to uniformly machine along the spherical surface at a speed of 200-500 r / min and a cutting depth of 0.2-0.5 mm.
2. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, The dielectric constant modifier mentioned in step one is any one of barium titanate, zirconium oxide, zinc oxide and silicon nitride or a mixture thereof in any ratio.
3. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, The polymer mentioned in step one is any one of polypropylene, polyethylene, and thermoplastic elastomer.
4. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, The process parameters for melt blending in step one are: zone 1 temperature 175±5℃, zone 2 temperature 185±5℃, zone 3 temperature 195±5℃, zone 4 temperature 205±5℃, main machine speed 250-350r / min, and feeding speed 80-120r / min.
5. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, In the bead foaming process described in step one, supercritical carbon dioxide is introduced, and the pressure is increased to 3.0-5.0 MPa at a rate of 0.2-0.5 MPa / min, while the temperature is increased to 140-155℃ at a rate of 1-2℃ / min, and the pressure holding time is 40-70 min.
6. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, In the molding process described in step one, saturated steam is introduced at a pressure of 0.15-0.35 MPa and a heating time of 15-50 seconds.
7. The method for manufacturing a Luneburg lens according to claim 1, characterized in that, The pre-compressed gas mentioned in step two is any one of compressed air, nitrogen, and carbon dioxide.
Citation Information
Patent Citations
Foaming Luneberg lens and production process thereof
CN112736485A
Low-dielectric-loss ceramic material Longbour lens and preparation process thereof
CN114874027A
Foaming material with gradient dielectric constant distribution and preparation method thereof
CN118005986A
Preparation method of polymer foaming material with gradient hole structure
CN110204778A
Method for preparing foamed Longbou lens
CN116001176A