Optical element and preparation method thereof

By using the combination of microstructure film layer and dielectric film layer in optical components, the problem of high reflectivity in traditional anti-reflection films in a specific wavelength range is solved, and ultra-low reflectivity in the range of 300nm~950nm is achieved, which significantly improves the Light transmittance.

CN118915201AInactive Publication Date: 2024-11-08NINGBO SUNNY AUTOMOTIVE OPTECH

Patent Information

Application Number
CN202411411825.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The maximum reflectivity of light in the range of 420nm to 680nm cannot be lower than 1%, and the high-performance anti-reflection effect cannot be achieved.

Method used

Using an optical element with a microstructure film layer, the microstructure film layer is arranged on one side of the substrate layer, and a microstructure film layer with a low refractive index is formed by physical etching, oxidation treatment or water bath reaction, and combined with the dielectric film layer to achieve Ultra-low reflectivity in the range of 300nm~950nm.

Benefits of technology

Average ultra-low reflectivity in the range of 300nm~950nm, with the highest reflectivity not exceeding 0.2%, and the reflectivity in the range of 400nm~850nm does not exceeding 0.1%, which significantly reduces the reflection loss of incident light and increases the transmission of light. Rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915201A_ABST
    Figure CN118915201A_ABST
Patent Text Reader

Abstract

The invention discloses an optical element and a preparation method thereof, the optical element comprises a base material layer and a microstructure film layer, and the microstructure film layer is arranged on at least one side surface of the base material layer, so that the reflectivity R of the formed optical element to light with the wavelength in the range of 300-950 nm meets the following condition: 0% < R < = 0.2%. According to the optical element, by arranging the microstructure film layer with the low refractive index, the anti-reflection effect of the large-range optical wave band of 300 nm to 950 nm can be achieved, meanwhile, the surface contact area is increased through the microstructure, the ultra-low reflection effect can be effectively achieved, the highest reflectivity does not exceed 0.2%, the reflection loss of incident light can be effectively reduced, and the light transmittance is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optical technology, and in particular to an optical element with a microstructured film layer and a preparation method thereof. Background Art

[0002] In the field of optical technology, anti-reflection film is an indispensable optical element in the optical system and is currently the most widely used optical film. Anti-reflection film can reduce the reflection loss of incident light, increase the transmittance of light, make the image display clearer, and improve the utilization rate of light energy.

[0003] However, traditional anti-reflection films achieve anti-reflection effects by alternating high and low refractive index layers through thin film interference. The maximum reflectivity Rmax of the anti-reflection films currently produced on the market for light in the wavelength range of 420nm~680nm is less than or equal to 1%. It can be seen that due to the limitations of traditional coating principles, it is impossible to achieve high-performance anti-reflection films, and there is still high reflection. Summary of the invention

[0004] The embodiments of the present application provide an optical element and a method for preparing the same that can at least partially solve at least one of the above-mentioned disadvantages or other disadvantages in the prior art.

[0005] The first aspect of the present application provides an optical element, which includes a substrate layer and a microstructure film layer, wherein the microstructure film layer is arranged on at least one side surface of the substrate layer so that the reflectivity R of the formed optical element for light in the wavelength range of 300mm~950nm satisfies: 0%<R≤0.2%.

[0006] According to an exemplary embodiment of the present application, the reflectivity R of the optical element for light in the wavelength range of 400 nm to 850 nm satisfies: 0%<R≤0.1%.

[0007] According to an exemplary embodiment of the present application, the optical element satisfies: 0.61≤n / ns≤0.93, wherein n is the refractive index of the microstructure film layer, and ns is the refractive index of the substrate layer.

[0008] According to an exemplary embodiment of the present application, the refractive index n of the microstructure film layer and the refractive index ns of the substrate layer respectively satisfy: 1.1≤n≤1.4, 1.5≤ns≤1.8.

[0009] According to an exemplary embodiment of the present application, the microstructure film layer includes at least one microstructure, and the microstructure satisfies: 0.13≤h / p≤40, wherein h is the height of the microstructure in a direction perpendicular to the surface of the substrate layer, and p is the maximum diameter of the microstructure in a direction parallel to the surface of the substrate layer.

[0010] According to an exemplary embodiment of the present application, a height h of the microstructure in a direction perpendicular to the surface of the substrate layer and a maximum diameter p of the microstructure in a direction parallel to the surface of the substrate layer respectively satisfy: 80nm≤h≤800nm, 20nm≤p≤600nm.

[0011] According to an exemplary embodiment of the present application, the refractive index of the microstructure film layer at the first preset height satisfies the following conditional formula: ;as well as ; Wherein, r is the radius of the microstructure film layer, z is the number of microstructures in the microstructure film layer, ai is the cross-sectional area of ​​the microstructure at the first preset height, and the height direction of the microstructure film layer is perpendicular to the surface of the substrate layer on which the microstructure film layer is disposed.

[0012] According to an exemplary embodiment of the present application, at the second preset height, the microstructure film layer satisfies: ; Among them, M0 is the length of the microstructure film layer in the direction parallel to the surface of the substrate layer, z1 is the number of microstructures on the M0 length of the microstructure film layer, mi is the length of the cross-section of the microstructure at the second preset height, and the second preset height is within 1 / 3 of the height of the microstructure film layer from one end away from the substrate layer to one end close to the substrate layer.

[0013] According to an exemplary embodiment of the present application, the refractive index of the microstructure film layer gradually decreases from one end close to the substrate layer to one end away from the substrate layer; and the refractive index of the microstructure film layer at a third preset height is 1.3~1.65, and the third preset height is in the range of 1 / 5 of the height of the microstructure film layer from one end close to the substrate layer to one end away from the substrate layer; the refractive index of the microstructure film layer at a fourth preset height is 1~1.05, and the fourth preset height is in the range of 1 / 5 of the height of the microstructure film layer from one end away from the substrate layer to one end close to the substrate layer.

[0014] According to an exemplary embodiment of the present application, the material of the microstructure film layer includes at least aluminum oxide.

[0015] According to an exemplary embodiment of the present application, the surface contact angle WAC of the optical element satisfies: WAC≤5°.

[0016] According to an exemplary embodiment of the present application, the optical element further includes a dielectric film layer, and the dielectric film layer is disposed between the substrate layer and the microstructure film layer.

[0017] According to an exemplary embodiment of the present application, the dielectric film layer includes a first dielectric film layer and a second dielectric film layer, the first dielectric film layer and the second dielectric film layer are alternately stacked, and the total number of layers of the first dielectric film layer and the second dielectric film layer is less than or equal to 10 layers.

[0018] According to an exemplary embodiment of the present application, the total number of layers of the first dielectric film layer and the second dielectric film layer is 2 layers or 4 layers.

[0019] According to an exemplary embodiment of the present application, the thickness of the first dielectric film layer is 5 nm to 120 nm, and the thickness of the second dielectric film layer is 10 nm to 200 nm.

[0020] According to an exemplary embodiment of the present application, the dielectric film layer satisfies: 1.1≤n1 / n2≤1.2, wherein n1 is the refractive index of the first dielectric film layer, and n2 is the refractive index of the second dielectric film layer.

[0021] According to an exemplary embodiment of the present application, the material of the dielectric film layer includes at least one of Ta, Si, Al, Ti, Ti oxide, Ta oxide, Si oxide, and Al oxide.

[0022] According to an exemplary embodiment of the present application, the material of the substrate layer includes at least one of plastic, glass, metal and composite materials thereof, and the material of the substrate layer is plastic, and the dielectric film layer includes at least one of Si, Al, Si oxide and Al oxide.

[0023] The second aspect of the present application provides a method for preparing an optical element, which includes: providing a substrate layer; and forming a microstructured film layer on at least one side surface of the substrate layer, so that the reflectivity R of the formed optical element for light in the wavelength range of 300nm~950nm satisfies: 0%<R≤0.2%.

[0024] According to an exemplary embodiment of the present application, forming a microstructured film layer on at least one surface of a substrate layer includes: forming a uniform film layer on at least one surface of the substrate layer; and forming the microstructured film layer based on the uniform film layer.

[0025] According to an exemplary embodiment of the present application, forming a uniform film layer on at least one side surface of the substrate layer includes: forming a uniform film layer on at least one side surface of the substrate layer by at least one of physical vapor deposition and chemical vapor deposition.

[0026] According to an exemplary embodiment of the present application, forming a microstructured film layer based on a uniform film layer includes: forming the microstructured film layer by treating the uniform film layer through at least one of physical etching, oxidation treatment, and water bath reaction.

[0027] According to an exemplary embodiment of the present application, a microstructured film layer is formed by physically etching a uniform film layer, comprising: at a preset reaction temperature, using an etching gas as a carrier, controlling the etching power and the amount of etching gas introduced, bombarding the uniform film layer with beam energy to form a microstructured film layer having a cylindrical microstructure; wherein the refractive index of the formed microstructured film layer satisfies the following conditional formula: ; Wherein, T is the preset reaction temperature, k is the etching power, and l is the amount of etching gas introduced.

[0028] According to an exemplary embodiment of the present application, the preset reaction temperature is 25° C. to 400° C.; the etching power is 0.1 KW to 5 KW; and the amount of etching gas introduced is 1 sccm to 1000 sccm.

[0029] According to an exemplary embodiment of the present application, the preset reaction temperature is 70° C. to 120° C.; the etching power is 1 KW to 3 KW; and the amount of etching gas introduced is 30 sccm to 70 sccm.

[0030] According to an exemplary embodiment of the present application, a microstructured film layer is formed by oxidation treatment of a uniform film layer, comprising: treating the uniform film layer with a strong oxidizing substance to react and dissolve a portion of the uniform film layer to form a microstructured film layer having a banded microstructure; wherein the strong oxidizing substance comprises at least hydrogen peroxide.

[0031] According to an exemplary embodiment of the present application, a microstructured membrane layer is formed by treating a uniform membrane layer through a water bath reaction, comprising: forming a microstructured membrane layer having a grass-like or cone-like microstructure by reacting deionized water with the uniform membrane layer.

[0032] According to an exemplary embodiment of the present application, forming a microstructure film layer on at least one side surface of a substrate layer includes: forming a dielectric film layer on at least one side surface of the substrate layer; and forming the microstructure film layer on the dielectric film layer.

[0033] The optical element provided in the present application can achieve an anti-reflection effect in a wide range of optical bands from 300nm to 950nm by providing a microstructure film layer with a low refractive index. At the same time, the microstructure increases the surface contact area, which can effectively achieve an ultra-low reflection effect, with a maximum reflectivity of no more than 0.2%. In some exemplary embodiments, the maximum reflectivity of the optical element in the optical band of 400nm to 850nm does not exceed 0.1%. In other exemplary embodiments, the maximum reflectivity of the optical element in the optical band of 400mm to 750nm does not exceed 0.1%, which can effectively reduce the reflection loss of incident light and increase the transmittance of light. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Other features, purposes and advantages of the embodiments of the present application will become more apparent by reading the detailed description of the non-limiting embodiments made with reference to the following drawings, in which: Figure 1 A cross-sectional view of the structure of an optical element according to an exemplary embodiment of the present application is shown; Figure 2 A structural cross-sectional view showing another optical element according to an exemplary embodiment of the present application; Figure 3 A structural cross-sectional view showing another optical element according to an exemplary embodiment of the present application; Figure 4 A side view of a single cone-shaped microstructure according to an exemplary embodiment of the present application is shown; Figure 5 A curve diagram showing a change in the refractive index of a single cone-shaped microstructure according to an exemplary embodiment of the present application is shown; Figure 6 A structural cross-sectional view of an optical element in Example 1 of the present application is shown; Figure 7 shows a reflectivity curve diagram of the optical element in Example 1 of the present application; Figure 8 A structural cross-sectional view of an optical element in Example 2 of the present application is shown; Fig. 9 A microscopic topography of the surface of the optical element in Example 2 of the present application is shown; Fig.10 Another microscopic topography of the surface of the optical element in Example 2 of the present application is shown; Fig.11 shows a reflectivity curve diagram of the optical element in Example 2 of the present application; Fig.12 A surface contact angle test diagram of an optical element in Example 2 of the present application is shown; Fig.13 A schematic flow chart showing a method for preparing an optical element according to an exemplary embodiment of the present application is shown; Fig.14 A schematic flow chart showing another method for preparing an optical element according to an exemplary embodiment of the present application is shown; Fig.15 A schematic diagram of a manufacturing process flow of an optical element according to an exemplary embodiment of the present application is shown; Fig.16 Another schematic diagram of a manufacturing process flow of an optical element according to an exemplary embodiment of the present application is shown.

[0035] Reference numerals: 100, substrate layer; 200, dielectric film layer; 210, first dielectric film layer; 220, second dielectric film layer; 300, uniform film layer; 400, microstructure film layer; 410, microstructure. DETAILED DESCRIPTION

[0036] In order to better understand the present application, a more detailed description will be made of various aspects of the present application with reference to the accompanying drawings. It should be understood that these detailed descriptions are only descriptions of exemplary embodiments of the present application, and are not intended to limit the scope of the present application in any way. Throughout the specification, the same reference numerals refer to the same elements. The expression "and / or" includes any and all combinations of one or more of the associated listed items.

[0037] It should be noted that, in the present specification, the expressions first, second, etc. are only used to distinguish one feature from another feature, but do not mean any limitation to the features.

[0038] In the drawings, the thickness, size and shape of each component may be slightly exaggerated for convenience of explanation. The drawings are only examples and are not drawn strictly to scale.

[0039] It should also be understood that the terms "comprising", "including", "having" and / or "provided with", when used in this specification, indicate the presence of stated features, elements and / or components, but do not exclude the presence of one or more other features, elements, components and / or combinations thereof. In addition, the term "exemplarily" is intended to refer to an example or illustration.

[0040] Unless otherwise defined, all terms (including technical and scientific terms) used in this application have the same meaning as commonly understood by those skilled in the art to which this application belongs. It should also be understood that terms (such as those defined in commonly used dictionaries) should be understood to have the same meaning as they have in the context of the relevant technology, and should not be interpreted in an idealized or overly formal sense, unless explicitly defined in this application.

[0041] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0042] A first aspect of the present application provides an optical element.

[0043] In an exemplary embodiment, the optical element includes a substrate layer 100 and a microstructure film layer 400. The material of the substrate layer 100 includes at least one of plastic, glass, metal and composite materials thereof. The substrate layer 100 serves as a base and has a bearing function for other film layers. The material of the substrate layer 100 can be selected according to actual needs. The microstructure film layer 400 is disposed on at least one side surface of the substrate layer 100, and includes at least one microstructure 410. The shape of a single microstructure 410 includes at least one of a cylindrical, conical, sheet-like, ribbon-like and a bush-like shape. Each shape of the microstructure 410 can be prepared by the same or different methods, so that the microstructure film layer 400 can achieve a low refractive index or a variable refractive index effect, which is beneficial to achieve an anti-reflection effect. The material of the microstructure film layer 400 includes at least aluminum oxide. Exemplarily, the microstructure 410 in the microstructure film layer 400 is cylindrical ( Figure 1 ), or the microstructure 410 in the microstructure film layer 400 is in the shape of a strip ( Figure 2 ), or the microstructure 410 in the microstructure film layer 400 is conical ( Figure 3 ).

[0044] In an exemplary embodiment, the reflectivity R of the optical element for light in the wavelength range of 300 nm to 950 nm satisfies: 0%<R≤0.2%.

[0045] The optical element of the exemplary embodiment of the present application can achieve an anti-reflection effect in a wide range of optical bands from 300mm to 950nm by setting a microstructure film layer 400 with a low refractive index. At the same time, the microstructure 410 increases the surface contact area, which can effectively achieve an ultra-low reflection effect. The maximum reflectivity does not exceed 0.2%, which can effectively reduce the reflection loss of incident light and increase the transmittance of light.

[0046] In an exemplary embodiment, the reflectivity R of the optical element for light in the wavelength range of 400nm~850nm satisfies: 0%<R≤0.1%, which can effectively reduce the reflection loss of the incident light and increase the transmittance of the light. The microstructure film layer 400 of the present application can also achieve ultra-low reflection of light in the wavelength range of 400nm~850nm under the condition of large-angle light incidence. Exemplarily, when the incident angle is 30°, the reflectivity R of the optical element for light in the wavelength range of 400nm~850nm can also satisfy: 0%<R≤0.1%.

[0047] In an exemplary embodiment, the reflectivity R of the optical element for light in the wavelength range of 400nm to 750nm satisfies: 0%<R≤0.1%, which can effectively reduce the reflection loss of the incident light and increase the transmittance of the light.

[0048] In an exemplary embodiment, the optical element satisfies: 0.61≤n / ns≤0.93, wherein n is the refractive index of the microstructure film layer 400 , and ns is the refractive index of the substrate layer 100 .

[0049] In an exemplary embodiment, the refractive index n of the microstructure film layer 400 and the refractive index ns of the substrate layer 100 respectively satisfy: 1≤n≤1.65, 1.5≤ns≤1.8. Further, 1.1≤n≤1.4.

[0050] In the present application, by controlling the refractive index of the substrate layer 100 to be always greater than the refractive index of the microstructure film layer 400 and controlling the refractive indexes of the substrate layer 100 and the microstructure film layer 400 to be within the above-defined range, it is beneficial to achieve the effect of ultra-low reflection.

[0051] In an exemplary embodiment, the microstructure film layer 400 includes at least one microstructure 410, and the microstructure 410 satisfies: 0.13≤h / p≤40, wherein h is the height of the microstructure 410 in a direction perpendicular to the surface of the substrate layer 100, and p is the maximum diameter of the microstructure 410 in a direction parallel to the surface of the substrate layer 100.

[0052] In an exemplary embodiment, a height h of the microstructure 410 in a direction perpendicular to the surface of the substrate layer 100 and a maximum diameter p of the microstructure 410 in a direction parallel to the surface of the substrate layer 100 respectively satisfy: 80 nm≤h≤800 nm, 20 nm≤p≤600 nm.

[0053] The reflectivity R of the microstructure film layer 400 is related to the height h of the microstructure 410 and the diameter p of the microstructure 410. The maximum length of the microstructure 410 in the x direction is the diameter p, and the maximum thickness in the y direction is the height h. For example, Figure 4 An exemplary embodiment of the present application is shown ( Figure 3 ) is a side view of a single conical microstructure 410, from Figure 4It can be seen that the maximum length of the end of a single microstructure 410 close to the substrate layer 100 in the x direction is the diameter p, and the maximum thickness of a single microstructure 410 in the y direction is the height h. It should be noted that the height h of the microstructure 410 is measured at the significant boundary of the compactness of the contact between the microstructure film layer 400 and the substrate layer 100, which is the bottom of the microstructure 410, and the distance between the bottom of the microstructure 410 and the top of the microstructure 410 is the height h of the microstructure 410, wherein the bottom of the microstructure 410 is the end of the microstructure 410 close to the substrate layer 100, and the top of the microstructure 410 is the end of the microstructure 410 away from the substrate layer 100. When the microstructure satisfies the range of 0.13≤h / p≤40, the reflectivity R of the microstructure film layer 400 satisfies the range of 0%<R≤0.2%. Among them, when p is larger, the refractive index at any height of the microstructure film layer 400 changes faster, and the reflectivity R is closer to 0.2%; when p is smaller, the refractive index at any height of the microstructure film layer 400 changes more uniformly, and the reflectivity R is closer to 0%.

[0054] It should be noted that the average value of the maximum height h of the plurality of microstructures 410 in the y direction is the height H of the microstructure film layer 400. In an ideal state, h may be the same as H. The height H of the microstructure film layer 400 is measured in the same manner as the height h of the microstructure 410. When the microstructure film layer 400 is directly disposed on the substrate layer 100, the significant boundary of the compactness of the contact between the microstructure film layer 400 and the substrate layer 100 is the bottom end of the microstructure film layer 400, and the distance between the bottom end of the microstructure film layer 400 and the top end of the microstructure film layer 400 is the height H of the microstructure film layer 400, wherein the bottom end of the microstructure film layer 400 is the end of the microstructure film layer 400 close to the substrate layer 100, and the top end of the microstructure film layer 400 is the end of the microstructure film layer 400 away from the substrate layer 100.

[0055] For example, when the height H of the microstructure film layer 400 is in the range of 80 nm to 800 nm, it is beneficial to improve the anti-reflection effect of the microstructure film layer 400. If H is lower than 80 nm, the refractive index of the microstructure film layer 400 changes little, and the anti-reflection effect will be worse; if H exceeds 800 nm, the stress of the microstructure film layer 400 is too great, and the film layer may crack.

[0056] It should be noted that the reflectivity band can be adjusted by adjusting the height H of the microstructure film layer 400. The larger H is, for example, when H is H1, the anti-reflection effect in the infrared band can be achieved; the smaller H is, for example, when H is H2, the anti-reflection effect in the ultraviolet band can be achieved; when H is H3, the anti-reflection effect in the visible light band can be achieved. H1 can be greater than H3, and H3 can be greater than H2, wherein H1, H2 and H3 can be a range or a specific value.

[0057] In an exemplary embodiment, the refractive index of the microstructure film layer 400 at the first preset height satisfies the following conditional formula: ;as well as ; Among them, r is the radius of the microstructure film layer 400, z is the number of microstructures 410 in the microstructure film layer 400, ai is the cross-sectional area of ​​the microstructure 410 at the first preset height, and the height direction of the microstructure film layer 400 is perpendicular to the surface of the substrate layer 100 on which the microstructure film layer 400 is disposed.

[0058] It should be noted that the refractive index of the microstructure film layer 400 at the first preset height is:

[0059] In an exemplary embodiment, r and ai satisfy: 50 nm ≤ r ≤ 800 nm; 1 nm 2 ≤ai≤106nm 2 . For example, ai satisfies: 103nm 2 ≤ai≤105nm 2 .

[0060] It should be noted that the refractive index at different positions in the microstructure film layer 400 is related to the volume size it occupies in a specific space. Using differential thinking, the refractive index of the microstructure film layer 400 at the first preset height can be characterized and calculated by the ratio of the cross-sectional area to the area of ​​the microstructure film layer 400. The first preset height here can be any height in the direction perpendicular to the surface of the substrate layer 100 on which the microstructure film layer 400 is provided. By accurately calculating the refractive index at any height of the microstructure film layer 400, after knowing the refractive index at any height of the microstructure film layer 400, in conjunction with the material of the substrate layer 100 and the selection of the dielectric film layer 200, an ultra-low reflection film design with an ultra-long bandwidth can be realized, the design accuracy of the optical element with anti-reflection effect can be improved, and further guidance can be provided for obtaining the number and thickness of the dielectric layer, thereby guiding the development of production work.

[0061] In an exemplary embodiment, at the second preset height, the microstructure film layer 400 satisfies: ; Among them, M0 is the length of the microstructure film layer 400 in the direction parallel to the surface of the substrate layer 100, z1 is the number of microstructures 410 on the length M0 of the microstructure film layer 400, mi is the length of the cross section of the microstructure 410 at the second preset height, and the second preset height is within 1 / 3 of the height of the microstructure film layer 400 from one end away from the substrate layer 100 to one end close to the substrate layer 100, that is, the second preset height is within 1 / 3H from the top of the microstructure film layer 400. By controlling the above conditions, it is beneficial to achieve the effect of ultra-low reflection.

[0062] In an exemplary embodiment, the refractive index of the microstructure film layer 400 gradually decreases from the end close to the substrate layer 100 to the end away from the substrate layer 100; and the refractive index of the microstructure film layer 400 at a third preset height is 1.3~1.65, and the third preset height is within 1 / 5 of the height of the microstructure film layer 400 from the end close to the substrate layer 100 to the end away from the substrate layer 100, that is, the third preset height is within 1 / 5H from the bottom of the microstructure film layer 400 upward; the refractive index of the microstructure film layer 400 at a fourth preset height is 1~1.05, and the fourth preset height is within 1 / 5 of the height of the microstructure film layer 400 from the end away from the substrate layer 100 to the end close to the substrate layer 100, that is, the fourth preset height is within 1 / 5H from the top of the microstructure film layer 400.

[0063] The present application uses an ellipsometer, a reflectivity tester and other equipment to simulate and calculate the refractive index at different positions of the microstructure film layer 400. For example, Figure 5 An exemplary embodiment of the present application is shown ( Figure 3 ), wherein the height h of the microstructure 410 on the abscissa refers to the height from any point on the microstructure 410 to the substrate layer 100, and the ordinate is the refractive index of the microstructure 410. The refractive index has a gradual change, that is, the refractive index of the microstructure film layer 400 gradually decreases from the end close to the substrate layer 100 to the end far away from the substrate layer 100, as shown in FIG. Figure 5 As shown, the variation rule is nonlinear, and the refractive index of the end of the microstructure film layer 400 away from the substrate layer 100 is infinitely close to the refractive index of air 1. Therefore, there will be no obvious refractive index difference when light is incident from air to the surface of the optical element, achieving ultra-low reflection.

[0064] In an exemplary embodiment, the surface contact angle WAC of the optical element satisfies: WAC≤5°. The present application provides a microstructured film layer 400 to perform a structured treatment on the film layer surface, which not only increases the surface contact area, but also effectively reduces the water contact angle on the film layer surface, so that the surface contact angle does not exceed 5° at most, thereby achieving ultra-low reflection and ultra-hydrophilic effects.

[0065] In an exemplary embodiment, a waterproof film is provided on the microstructure film layer 400 to achieve a super-hydrophobic effect.

[0066] In an exemplary embodiment, the optical element further includes a dielectric film layer 200 ( Figure 6 ), the dielectric film layer 200 is disposed between the substrate layer 100 and the microstructure film layer 400.

[0067] It should be noted that, when the dielectric film layer 200 is set between the substrate layer 100 and the microstructure film layer 400, the height h of the microstructure 410 is measured at the significant boundary of the density of the contact between the microstructure film layer 400 and the dielectric film layer 200, which is the bottom end of the microstructure 410, and the distance between the bottom end of the microstructure 410 and the top end of the microstructure 410 is the height h of the microstructure 410, wherein the bottom end of the microstructure 410 is the end of the microstructure 410 close to the dielectric film layer 200, and the top end of the microstructure 410 is the end of the microstructure 410 away from the dielectric film layer 200. At this time, the height H of the microstructure film layer 400 is calculated as follows: the significant boundary of the density of the contact between the microstructure film layer 400 and the dielectric film layer 200 is the bottom end of the microstructure film layer 400, and the distance between the bottom end of the microstructure film layer 400 and the top end of the microstructure film layer 400 is the height H of the microstructure film layer 400, wherein the bottom end of the microstructure film layer 400 is the end of the microstructure film layer 400 close to the dielectric film layer 200, and the top end of the microstructure film layer 400 is the end of the microstructure film layer 400 away from the dielectric film layer 200.

[0068] In an exemplary embodiment, the dielectric film layer 200 includes a first dielectric film layer 210 and a second dielectric film layer 220 , which are alternately stacked, and the total number of the first dielectric film layer 210 and the second dielectric film layer 220 is less than or equal to 10 layers.

[0069] When only the microstructure film layer 400 is provided on the substrate layer 100, super-hydrophilic anti-reflection can be achieved. On this basis, by adding a dielectric film layer 200, the spectral bandwidth of anti-reflection can be increased on the basis of achieving effective anti-reflection. For example, the bandwidth can be controlled by changing the number of dielectric film layers 200, the thickness of the film layer, etc.

[0070] In an exemplary embodiment, the total number of layers of the first dielectric film layer 210 and the second dielectric film layer 220 is 2 or 4. In the present application, when the total number of layers of the first dielectric film layer 210 and the second dielectric film layer 220 is 2 or 4, the anti-reflection bandwidth of the optical element is wider, the film layer is thinner, the stability is better, and the processing cost is lower.

[0071] In an exemplary embodiment, the thickness of the first dielectric film layer 210 is 5 nm to 120 nm, and the thickness of the second dielectric film layer 220 is 10 nm to 200 nm. By controlling the above conditions, it is beneficial to achieve the effect of ultra-low reflection.

[0072] In an exemplary embodiment, the dielectric film layer 200 satisfies: 1.1≤n1 / n2≤1.2, where n1 is the refractive index of the first dielectric film layer 210 and n2 is the refractive index of the second dielectric film layer 220. n1 / n2 is close to 1, and the microstructure film layer 400 can better achieve the ultra-low reflection effect.

[0073] In an exemplary embodiment, the material of the dielectric film layer 200 includes at least one of Ta, Si, Al, Ti, Ti oxide, Ta oxide, Si oxide, and Al oxide. Ti oxide may include, but is not limited to, TiO2 and Ti3O5. Ta oxide may include, but is not limited to, Ta2O5. Si oxide may include, but is not limited to, SiO2 and SiO. Al oxide may include, but is not limited to, Al2O3.

[0074] In an exemplary embodiment, the material of the substrate layer 100 is plastic, and the dielectric film layer 200 includes at least one of Si, Al, Si oxide, and Al oxide. In this embodiment, when the material of the substrate layer 100 is plastic, at least one of Si, Al, Si oxide, and Al oxide is used as the dielectric film layer 200 on the plastic substrate. In post-processing, such as under the action of an ion source, the stress of the dielectric film layer 200 can be adjusted and optimized to match the thermal deformation characteristics of the plastic and improve the bonding strength. The excellent bonding strength can effectively improve the firmness and anti-pulling performance between the film layers.

[0075] Specific examples of optical elements applicable to the above-mentioned embodiments are further described below. Example 1

[0076] Figure 6 FIG. 2 shows a cross-sectional view of the structure of the optical element in Example 1 of the present application. Figure 6As shown, the optical element of this embodiment includes a substrate layer 100, a dielectric film layer 200 and a microstructure film layer 400. The dielectric film layer 200 is disposed on one side surface of the substrate layer 100, and the microstructure film layer 400 is disposed on the dielectric film layer 200. The substrate layer 100 is made of glass material. The dielectric film layer 200 includes two layers (for example, a first dielectric film layer 210 and a second dielectric film layer 220). The first dielectric film layer 210 is disposed on the substrate layer 100 and is made of Al2O3 material with a thickness of 30nm; the second dielectric film layer 220 is disposed on the first dielectric film layer 210 and is made of SiO2 material with a thickness of 50nm. The microstructure film layer 400 includes at least one microstructure 410, which is made of Al2O3 material with a thickness of 150nm. The shape of a single microstructure 410 in the microstructure film layer 400 is cylindrical, and the refractive index of the microstructure film layer 400 is 1.283.

[0077] Figure 7 shows the reflectivity curve of the optical element, from Figure 7 It can be seen that in the 463nm~900nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.2%. In the 485nm~850nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.1%.

[0078] It should be noted that the above specific embodiments are exemplary embodiments that can illustrate the solution of the present application and do not constitute a limitation on the solution of the present application. By adjusting the height of the microstructure film layer 400 and matching the material of the substrate layer 100 and the selection of the dielectric film layer 200, the design of an ultra-low reflection optical element with an ultra-long bandwidth (300mm~950nm) can be achieved. Example 2

[0079] Figure 8 FIG. 2 shows a cross-sectional view of the structure of the optical element in Example 2 of the present application. Figure 8As shown, the optical element of this embodiment includes a substrate layer 100, a dielectric film layer 200 and a microstructure film layer 400, wherein the dielectric film layer 200 is disposed on one side surface of the substrate layer 100, and the microstructure film layer 400 is disposed on the dielectric film layer 200. The substrate layer 100 is made of plastic, and the refractive index is 1.55. The dielectric film layer 200 includes four layers (for example, two first dielectric film layers 210 and two second dielectric film layers 220), and the two first dielectric film layers 210 and the two second dielectric film layers 220 are alternately stacked, and for the stack formed by the first dielectric film layer 210 and the second dielectric film layer 220, the first dielectric film layer 210 is closer to the substrate layer 100 than the second dielectric film layer 220. The first dielectric film layer 210 is made of Al2O3 material, and the second dielectric film layer 220 is made of SiO2 material. From the substrate layer 100 to the microstructure film layer 400, the thicknesses of the four layers of the dielectric film layer 200 are 3 nm, 63 nm, 5 nm and 103 nm respectively. The microstructure film layer 400 includes at least one microstructure 410 made of Al2O3 material.

[0080] Fig. 9 and Fig.10 FIG. 4 shows a microscopic morphology of the surface of the optical element, namely, a microstructure film layer 400 (transmission electron microscope image), wherein: Fig. 9 and Fig.10 The 100 nm in the figure is the scale. Fig. 9 It can be seen that the microstructure film layer 400 includes a plurality of microstructures 410, and the shape of a single microstructure 410 is approximately conical, wherein the height of one microstructure 410 is 356nm, and the height of another microstructure 410 is 362nm. After measurement, the height of the microstructure film layer 400 is 360nm. Fig.10 As can be seen in the figure, the multiple microstructures 410 are evenly arranged. The conical microstructures 410 are sharp outside and thick inside, and the refractive index is lower the farther away from the substrate layer 100, and the refractive index is higher the closer to the substrate layer 100, so as to form an optical element with a gradual refractive index, so that the optical element has a better anti-reflection effect.

[0081] Fig.11 shows the reflectivity curve of the optical element, from Fig.11 It can be seen that when the incident angle is 0°, in the 450nm~850nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.2%; in the 470nm~850nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.1%. When the incident angle is 30°, in the 450nm~850nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.2%; in the 460nm~825nm band, the maximum reflectivity Rmax of the optical component is less than or equal to 0.1%.

[0082] Fig.12A surface contact angle test diagram of the optical element is shown. After testing, the surface contact angle WCA of the optical element is 3.5°, achieving the super-hydrophilic property of the surface of the optical element.

[0083] It should be noted that the above specific embodiments are exemplary embodiments that can illustrate the solution of the present application and do not constitute a limitation on the solution of the present application. By adjusting the height of the microstructure film layer 400 and matching the material of the substrate layer 100 and the selection of the dielectric film layer 200, the design of an ultra-low reflection optical element with an ultra-long bandwidth (300mm~950nm) can be achieved.

[0084] The second aspect of the present application provides a method for preparing an optical element, and the optical element according to the first aspect of the present application can be formed by using the preparation method.

[0085] In an exemplary embodiment, Fig.13 As shown, the method for preparing the optical element includes: S1: providing a substrate layer; S2: forming a microstructure film layer on at least one surface of the substrate layer, so that the reflectivity R of the formed optical element for light within a wavelength range of 300 nm to 950 nm satisfies: 0%<R≤0.2%.

[0086] In an exemplary embodiment, Fig.14 As shown, the method for preparing the optical element further includes: S1: providing a substrate layer; S2: forming a dielectric film layer on at least one side surface of the substrate layer; S3: forming a microstructure film layer on the dielectric film layer, so that the reflectivity R of the formed optical element for light within a wavelength range of 300 nm to 950 nm satisfies: 0%<R≤0.2%.

[0087] In an exemplary embodiment, the reflectivity R of the optical element for light in the wavelength range of 400 nm to 850 nm satisfies: 0%<R≤0.1%.

[0088] In an exemplary embodiment, the reflectivity R of the optical element for light within a wavelength range of 400 nm to 750 nm satisfies: 0%<R≤0.1%.

[0089] When only a microstructured film layer is provided on the substrate layer, super-hydrophilic anti-reflection can be achieved. On this basis, by adding a dielectric film layer, the spectral bandwidth of the anti-reflection can be increased while achieving effective anti-reflection. For example, the bandwidth can be controlled by changing the number of dielectric film layers, the thickness of the film layers, etc.

[0090] It should be noted that the substrate layer can be directly made of existing materials as a substrate, and other film layers can be directly prepared on the substrate; it can also be prepared by using a processing technology, which is not limited. The material of the substrate layer includes at least one of plastic, glass, metal and a composite material thereof.

[0091] In an exemplary embodiment, forming a microstructured film layer on at least one side of the substrate layer includes: forming a uniform film layer on at least one side of the substrate layer, and forming the microstructured film layer by post-processing the uniform film layer. The material of the uniform film layer includes at least aluminum oxide.

[0092] In an exemplary embodiment, the method of forming the uniform film layer includes at least one of physical vapor deposition and chemical vapor deposition, and the post-treatment includes at least one of physical etching, oxidation treatment, and water bath reaction.

[0093] It should be noted that the method for forming a uniform film layer and the post-processing method can be selected as needed. Different post-processing methods can realize microstructures of different shapes, thereby realizing the preparation of different microstructure film layers, and different refractive indices can be achieved through different microstructure film layers, thereby adjusting the anti-reflection effect.

[0094] In an exemplary embodiment, the microstructured film layer is formed by physically etching a uniform film layer, including: at a preset reaction temperature, using an etching gas as a carrier, controlling the etching power and the amount of etching gas introduced, bombarding the uniform film layer with beam energy to form the microstructured film layer. The refractive index of the formed microstructured film layer satisfies the following conditional formula: ; Wherein, T is the preset reaction temperature, k is the etching power, and l is the amount of etching gas introduced.

[0095] It should be noted that the refractive index of the microstructured film layer formed by physical etching of the uniform film layer is: .

[0096] Exemplarily, the preset reaction temperature is 25°C to 400°C; the etching power is 0.1KW to 5KW; and the amount of etching gas introduced is 1sccm to 1000sccm. Exemplarily, the preset reaction temperature is 70°C to 120°C; the etching power is 1KW to 3KW; and the amount of etching gas introduced is 30sccm to 70sccm.

[0097] Exemplarily, the etching gas includes at least one of oxygen and argon.

[0098] Exemplarily, the uniform film layer is formed into a microstructured film layer having a cylindrical microstructure by physical etching.

[0099] This application can achieve control of cylindrical microstructures by adjusting the physical etching process parameters. By controlling the process parameters within a reasonable range, the refractive index and other parameters can be accurately controlled, thereby improving the accuracy of the control of the anti-reflection effect of the film layer. When the refractive index of the film layer is reduced, the refractive index deviation between the air and the film layer is reduced, which can effectively reduce light reflection.

[0100] In an exemplary embodiment, a microstructured film layer is formed by oxidation treatment of a uniform film layer, including: treating the uniform film layer with a strong oxidizing substance to react and dissolve a portion of the uniform film layer to form a microstructured film layer; wherein the strong oxidizing substance includes at least hydrogen peroxide, and may also be other substances with strong oxidizing properties, which are not limited.

[0101] Exemplarily, the uniform film layer is subjected to an oxidation treatment to form a microstructured film layer having a band-shaped microstructure.

[0102] In an exemplary embodiment, forming the microstructured membrane layer by treating the uniform membrane layer with a water bath reaction includes: forming the microstructured membrane layer by reacting deionized water with the uniform membrane layer.

[0103] Exemplarily, the uniform film layer is subjected to a water bath reaction to form a microstructured film layer having a grass-like or cone-like microstructure.

[0104] In an exemplary embodiment, the method of forming the dielectric film layer includes at least one of physical vapor deposition, chemical vapor deposition, electron gun evaporation coating, and vacuum coating. The material of the dielectric film layer includes at least one of Ta, Si, Al, Ti, Ti oxide, Ta oxide, Si oxide, and Al oxide. Ti oxide may include but is not limited to TiO2 and Ti3O5. Ta oxide may include but is not limited to Ta2O5. Si oxide may include but is not limited to SiO2 and SiO. Al oxide may include but is not limited to Al2O3.

[0105] For example, Fig.15A schematic diagram of a preparation process flow of an optical element of the present application is shown. In an embodiment in which a microstructure film layer 400 is formed by post-processing of physical etching, the preparation method of the optical element includes: vapor-depositing a first dielectric film layer 210 of Al2O3 with a thickness of 30nm on a glass substrate layer 100 by electron gun evaporation coating, and then vapor-depositing a second dielectric film layer 220 of SiO2 with a thickness of 50nm on the first dielectric film layer 210, and then vapor-depositing a uniform film layer 300 of Al2O3 with a thickness of 150nm on the second dielectric film layer 220; at a temperature of 120°C, using oxygen as a carrier, controlling the ion beam power to 10KW, and the oxygen intake to 100sccm, performing physical etching on the uniform film layer 300 to form cylindrical holes and microstructures 410, and forming a microstructure film layer 400 with a low refractive index after filling the through holes with air to achieve an anti-reflection effect. The electron beam power during the coating process of the dielectric film layer 200 is 1KW, and the oxygen flow rate is 50sccm. Using this method, the optical element in Example 1 provided in the first aspect of the present application can be prepared.

[0106] For example, Fig.16 Another schematic diagram of the preparation process flow of the optical element of the present application is shown. In an embodiment in which a microstructure film layer 400 is formed by a post-treatment method of a water bath reaction, the preparation method of the optical element includes: evaporating a first dielectric film layer 210 of Al2O3 on a plastic substrate layer 100 by electron gun evaporation coating, then evaporating a second dielectric film layer 220 of SiO2 on the first dielectric film layer 210, then evaporating a first dielectric film layer 210 of Al2O3 on the second dielectric film layer 220, then evaporating a second dielectric film layer 220 of SiO2 on the first dielectric film layer 210, and then evaporating a uniform film layer 300 of Al2O3 with a thickness of 50nm on the second dielectric film layer 220; placing the above structure in hot water to hydrolyze part of the uniform film layer 300 of Al2O3 to form a conical or grass-shaped microstructure 410 and holes, and after filling the through holes with air, a loose microstructure film layer 400 with a low refractive index and a thickness of 360nm is formed to achieve an anti-reflection effect. Wherein, Al2O3 and SiO2 are used as the dielectric film layer 200, and the thermal expansion performance of the plastic substrate is matched to improve the firmness between the film layers under the premise of satisfying the optical film layer design. Using this method, the optical element in Example 2 provided in the first aspect of the present application can be prepared.

[0107] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are formed by replacing each other with the technical features with similar functions disclosed in this application (but not limited to).

Claims

1. An optical element, characterized in that: include: substrate layer; as well as The microstructure film layer is disposed on at least one side of the substrate layer so that the reflectivity R of the formed optical element for light within the wavelength range of 300nm to 950nm satisfies: 0%<R≤0.2%.

2. The optical element according to claim 1, characterized in that The reflectivity R of the optical element for light within a wavelength range of 400 nm to 850 nm satisfies: 0%<R≤0.1%.

3. The optical element according to claim 1, characterized in that The optical element satisfies: 0.61≤n / ns≤0.93, wherein n is the refractive index of the microstructure film layer, and ns is the refractive index of the substrate layer.

4. The optical element according to claim 3, characterized in that The refractive index n of the microstructure film layer and the refractive index ns of the substrate layer respectively satisfy: 1.1≤n≤1.4; 1.5≤ns≤1.

8.

5. The optical element according to claim 1, characterized in that The microstructure film layer includes at least one microstructure, and the microstructure satisfies: 0.13≤h / p≤40, wherein h is the height of the microstructure in a direction perpendicular to the surface of the substrate layer, and p is the maximum diameter of the microstructure in a direction parallel to the surface of the substrate layer.

6. The optical element according to claim 5, characterized in that The height h of the microstructure in a direction perpendicular to the surface of the substrate layer and the maximum diameter p of the microstructure in a direction parallel to the surface of the substrate layer respectively satisfy: 80nm≤h≤800nm; 20nm≤p≤600nm.

7. The optical element according to claim 1, characterized in that The refractive index of the microstructure film layer at the first preset height satisfies the following conditional formula: ; as well as ; Among them, r is the radius of the microstructure film layer, z is the number of microstructures in the microstructure film layer, ai is the cross-sectional area of ​​the microstructure at the first preset height, and the height direction of the microstructure film layer is perpendicular to the surface of the substrate layer on which the microstructure film layer is disposed.

8. The optical element according to claim 1, characterized in that At the second preset height, the microstructure film layer satisfies: ; Among them, M0 is the length of the microstructure film layer in the direction parallel to the surface of the substrate layer, z1 is the number of microstructures on the length M0 of the microstructure film layer, mi is the length of the cross-section of the microstructure at the second preset height, and the second preset height is within 1 / 3 of the height of the microstructure film layer from one end away from the substrate layer to one end close to the substrate layer.

9. The optical element according to claim 1, characterized in that The refractive index of the microstructure film layer gradually decreases from an end close to the substrate layer to an end far away from the substrate layer; and The refractive index of the microstructure film layer at a third preset height is 1.3-1.65, and the third preset height is within a range of 1 / 5 of the height of the microstructure film layer from one end close to the substrate layer to one end away from the substrate layer; The refractive index of the microstructure film layer at a fourth preset height is 1-1.05, and the fourth preset height is within a range of 1 / 5 of the height of the microstructure film layer from one end away from the substrate layer to one end close to the substrate layer.

10. The optical element according to claim 1, characterized in that The material of the microstructure film layer at least includes aluminum oxide.

11. The optical element according to claim 1, characterized in that The surface contact angle WAC of the optical element satisfies: WAC≤5°.

12. The optical element according to any one of claims 1 to 11, characterized in that: The optical element further comprises a dielectric film layer, and the dielectric film layer is arranged between the substrate layer and the microstructure film layer.

13. The optical element according to claim 12, characterized in that The dielectric film layer comprises a first dielectric film layer and a second dielectric film layer, the first dielectric film layer and the second dielectric film layer are alternately stacked, and the total number of layers of the first dielectric film layer and the second dielectric film layer is less than or equal to 10 layers.

14. The optical element according to claim 13, characterized in that The total number of layers of the first dielectric film layer and the second dielectric film layer is 2 layers or 4 layers.

15. The optical element according to claim 13, characterized in that The thickness of the first dielectric film layer is 5 nm to 120 nm, and the thickness of the second dielectric film layer is 10 nm to 200 nm.

16. The optical element according to claim 13, characterized in that The dielectric film layer satisfies: 1.1≤n1 / n2≤1.2, wherein n1 is the refractive index of the first dielectric film layer, and n2 is the refractive index of the second dielectric film layer.

17. The optical element according to claim 12, characterized in that The material of the dielectric film layer includes at least one of Ta, Si, Al, Ti, Ti oxide, Ta oxide, Si oxide and Al oxide.

18. The optical element according to claim 17, characterized in that The material of the substrate layer includes at least one of plastic, glass, metal and composite materials thereof; and The material of the substrate layer is plastic, and the dielectric film layer includes at least one of Si, Al, Si oxide and Al oxide.

19. A method for preparing an optical element, characterized in that: The preparation method comprises: providing a substrate layer; and A microstructure film layer is formed on at least one side surface of the substrate layer, so that the reflectivity R of the formed optical element for light within a wavelength range of 300 nm to 950 nm satisfies: 0%<R≤0.2%.

20. The preparation method according to claim 19, characterized in that: Forming a microstructure film layer on at least one side surface of the substrate layer comprises: forming a uniform film layer on at least one side surface of the substrate layer; The microstructured film layer is formed based on the uniform film layer.

21. The preparation method according to claim 20, characterized in that: Forming a uniform film layer on at least one side surface of the substrate layer comprises: The uniform film layer is formed on at least one side surface of the substrate layer by at least one of physical vapor deposition and chemical vapor deposition.

22. The preparation method according to claim 20, characterized in that: Forming the microstructured film layer based on the uniform film layer comprises: The uniform film layer is processed by at least one of physical etching, oxidation treatment, and water bath reaction to form the microstructure film layer.

23. The preparation method according to claim 22, characterized in that: The uniform film layer is processed by physical etching to form a microstructure film layer, comprising: At a preset reaction temperature, using etching gas as a carrier, by controlling etching power and an amount of etching gas introduced, the uniform film layer is bombarded with beam energy to form a microstructure film layer having a cylindrical microstructure; The refractive index of the formed microstructure film layer satisfies the following conditional formula: ; Wherein, T is the preset reaction temperature, k is the etching power, and l is the amount of etching gas introduced.

24. The preparation method according to claim 23, characterized in that: The preset reaction temperature is 25° C. to 400° C.; the etching power is 0.1 KW to 5 KW; and the amount of etching gas introduced is 1 sccm to 1000 sccm.

25. The preparation method according to claim 24, characterized in that: The preset reaction temperature is 70° C. to 120° C.; the etching power is 1 KW to 3 KW; and the amount of etching gas introduced is 30 sccm to 70 sccm.

26. The preparation method according to claim 22, characterized in that: The uniform film layer is oxidized to form a microstructured film layer, comprising: Through the treatment of the strong oxidizing substance, a portion of the uniform film layer is reacted and dissolved to form a microstructured film layer having a banded microstructure; Wherein, the strong oxidizing substance at least includes hydrogen peroxide.

27. The preparation method according to claim 22, characterized in that: The uniform film layer is treated by a water bath reaction to form a microstructured film layer, comprising: A microstructured membrane layer having a grass-like or cone-like microstructure is formed by reacting deionized water with the uniform membrane layer.

28. The preparation method according to any one of claims 19 to 27, characterized in that: Forming a microstructure film layer on at least one side surface of the substrate layer comprises: forming a dielectric film layer on at least one side surface of the substrate layer; and The microstructure film layer is formed on the dielectric film layer.

Citation Information

Patent Citations

  • Microstructure film system, optical imaging lens and method for preparing film system

    CN113031124A

  • Anti-reflection microstructure and manufacturing method thereof

    CN115016048A

  • Optical imaging lens

    CN214669795U

  • Anti-reflection film and optical element having the same, optical system, and optical device

    JP2018185394A

  • Optical element, optical system and optical apparatus having antireflection coating

    US20140177059A1

Cited By

  • Metamaterial anti-reflection film for radioisotope thermophotovoltaic cell and preparation method and application thereof

    CN119937068A