Hollow SiO2 nanosphere-based antireflection film based on inorganic template and preparation method thereof

Through the combination of the inorganic template ZnS-SiO2 core-shell structure and acid SiO2 sol, the problems of adsorption pollution and high-temperature annealing of traditional anti-reflection films are solved, high transmittance and wear resistance are achieved, and the stability and optical performance of the film layer are improved. .

CN118930069APending Publication Date: 2024-11-12SHANGHAI XIYUAN NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411234830.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The porous structure of traditional anti-reflective films is prone to adsorbing pollutants and absorbing moisture, resulting in a decrease in light transmittance and scratch resistance. There may be template residues and exhaust gas problems during high-temperature annealing.

Method used

The inorganic template ZnS-SiO2 core-shell structure nanospheres were prepared by coating and acid etching. The self-supported hollow SiO2 nanosphere anti-reflective film was prepared, and the acid SiO2 sol was used as a binder for short-term annealing at high temperature to avoid high temperature long Time calcination and the production of harmful gases.

Benefits of technology

High transmittance, wear resistance and durability are achieved, template residues and exhaust gas problems are avoided, and the mechanical strength and optical properties of the film layer are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930069A_ABST
    Figure CN118930069A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of nano materials, and particularly relates to a hollow SiO2 nanosphere-based antireflection film based on an inorganic template and a preparation method. The preparation method comprises the following steps: preparing a ZnS-SiO2 core-shell structure nanosphere by adopting a ZnS nanosphere with a pore structure as a template, coating a film on a glass substrate, and removing a ZnS core by an acid etching method to obtain a hollow SiO2 nanosphere coating with a self-supporting structure inside; and permeating a layer of acidic SiO2 sol on the hollow SiO2 nanosphere coating, and annealing at high temperature to obtain the hollow SiO2 nanosphere and acidic SiO2 composite antireflection film with a self-supporting structure inside. The antireflection film provided by the invention has high transmittance and high adhesion with a substrate, has higher hardness compared with a coating prepared from other hollow SiO2, and has excellent wear resistance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano materials, and in particular relates to a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template and a preparation method thereof. Background Art

[0002] Solar photovoltaic devices are generally used outdoors, and their anti-reflection films must have high transmittance and meet the requirements of scratch resistance and weather resistance. Therefore, anti-reflection films for solar photovoltaics with high comprehensive performance have always been a hot topic in the industry. Traditional anti-reflection films reduce the refractive index by preparing a porous structure, thereby improving its light transmittance. However, the tiny gaps in these traditional anti-reflection films are connected to the atmosphere outside the film. This open-pore structure makes the film layer easy to adsorb pollutants and absorb moisture, which in turn leads to a decrease in light transmittance and scratch resistance. As one of the most promising anti-reflection coating materials, hollow SiO2 nanoparticles have excellent chemical stability, corrosion resistance, heat resistance and significant hardness, and have become the focus of attention in recent years. The anti-reflection film based on hollow SiO2 nanospheres not only exhibits high transmittance due to its low refractive index, but also has a closed-pore structure inside and a continuous and smooth surface. Compared with the traditional anti-reflection film with an open-pore structure, it has better wear resistance, anti-fouling and moisture resistance.

[0003] The most commonly used method for preparing closed-cell anti-reflection films based on hollow SiO2 nanospheres is the template method, among which polyacrylic acid (PAA) is one of the widely used templates. People use the sol-gel method to prepare PAA-SiO2 core-shell structure on the substrate, and then use high-temperature annealing to remove PAA to obtain a hollow SiO2 nanosphere anti-reflection film (Ceramics International 49 (2023) 6805–6810). During the preparation process, high-temperature annealing at about 450°C for more than 60 minutes is usually required. This process may cause problems such as PAA residue or collapse of hollow SiO2 nanospheres. In addition, when high-temperature calcination is used to remove organic templates such as PAA, a large amount of waste gas will be generated, which will cause irreversible damage to the equipment. Summary of the invention

[0004] One of the purposes of the present invention is to provide a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The preparation method first coats the film and then etches it in combination with a suitable adhesive to achieve the preparation of a self-supporting hollow SiO2 anti-reflection film. Then, a suitable annealing temperature is designed to achieve an anti-reflection film with high transmittance and high adhesion to the substrate. The coating has a higher hardness than other hollow SiO2 coatings and has excellent wear resistance and durability.

[0005] To achieve the above object, the present invention adopts the following technical solution: a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template, comprising the following steps:

[0006] S1, taking ZnS-SiO2 core-shell structure nanospheres with an outer diameter of 80-120nm, wherein the ZnS nanospheres are the core and SiO2 is the shell; the ZnS-SiO2 core-shell structure nanospheres are uniformly dispersed in anhydrous ethanol at a dispersion concentration of 0.015-0.05g / ml, and used as a coating solution 1;

[0007] S2, using tetraethyl orthosilicate TEOS as a silicon source, nitric acid HNO3 as a catalyst, and anhydrous ethanol EtOH as a solvent, hydrolysis polymerization reaction is used to prepare acidic SiO2 sol, and the acidic SiO2 sol is diluted 2-10 times and used as coating solution 2;

[0008] S3, pre-treating the glass substrate to obtain a clean and dry surface, using a coating solution 1 to coat the surface of the glass substrate to form a coating 1, wherein the thickness of the coating 1 is 100 to 500 nm, drying the glass substrate with the coating 1 and placing it in a 0.5 to 1 mol / L dilute hydrochloric acid solution, soaking it for 1 to 3 hours and then taking it out, rinsing it with deionized water for multiple times and then drying it, thereby obtaining a hollow SiO2 nanosphere anti-reflection film with a self-supporting structure on the glass substrate;

[0009] S4, using the coating solution 2, coating the surface of the hollow SiO2 nanosphere anti-reflection film prepared in step S3 to form a coating 2, the thickness of the coating 2 is 20-100 nm, and a composite film is obtained; after annealing the composite film at 680-720° C. for 2-3 min, cooling it to room temperature to obtain a hollow SiO2 nanosphere-based anti-reflection film with a thickness of 120-600 nm based on an inorganic template;

[0010] There is no particular order for steps S1 and S2.

[0011] As a further improvement of the preparation method of hollow SiO2 nanosphere-based anti-reflection film based on inorganic template:

[0012] Preferably, the preparation method of ZnS-SiO2 core-shell structure nanospheres with an outer diameter of 80 to 120 nm in step S1 is as follows:

[0013] S11, taking ZnS nanospheres with an outer diameter of 60 to 100 nm, a porous structure inside, and monodispersity, adding them to anhydrous ethanol for ultrasonic dispersion, adding PVP, ammonia water, and deionized water at a temperature of 20 to 30° C. while stirring, and obtaining solution A after sufficient stirring;

[0014] S12, tetraethyl orthosilicate TEOS and anhydrous ethanol EtOH were mixed, and stirred at room temperature, which was recorded as solution B; wherein the mass ratio of ZnS nanospheres in solution A to TEOS in solution B was 1:(2-3);

[0015] S13. Slowly add solution B to solution A twice, with a time interval of 2 to 3 hours between the two additions, and react for 7 to 9 hours. The reaction product is washed by centrifugation with deionized water and anhydrous ethanol and then dried to obtain ZnS-SiO2 core-shell structured nanospheres with an outer diameter of 80 to 120 nm.

[0016] Preferably, the concentration of ammonia water in step S11 is 1.3-3.2 mol / L, and the mass ratio of ZnS nanospheres, anhydrous ethanol, PVP, ammonia water and deionized water is 0.5:(25-40):0.2:(2-3):2.

[0017] Preferably, in step S12, tetraethyl orthosilicate TEOS and anhydrous ethanol EtOH are mixed in a volume ratio of (1-1.5):5.

[0018] Preferably, the preparation method of the ZnS nanospheres with a diameter of 60 to 100 nm, an internal porous structure, and monodispersity described in step S11 is as follows: thiourea, zinc acetate and deionized water are mixed, stirred at room temperature until completely dissolved, and then polyvinyl pyrrolidone PVP is added and stirred sufficiently to obtain a mixed solution, wherein the mass ratio of thiourea, zinc acetate, deionized water and PVP is (2.85 to 3.80):0.22:25:(0.5 to 0.75); the mixed solution is transferred to a polytetrafluoroethylene liner, and then the reactor is encapsulated, and the reaction is carried out at 120 to 150° C. for 4 to 6 hours and then naturally cooled to room temperature. The reaction product is centrifuged and washed with deionized water and anhydrous ethanol respectively and then dried to obtain ZnS nanospheres with a diameter of 60 to 100 nm, an internal porous structure, and monodispersity.

[0019] Preferably, the steps of pretreating the glass substrate in step S3 are as follows: placing the glass substrate cut into a suitable size into a NaOH solution for ultrasonication for 10 to 15 minutes, rinsing it with tap water, then soaking it in deionized water and wiping it with a dust-free cloth, then soaking it in anhydrous ethanol, and then taking it out and drying it to obtain a clean and dry surface.

[0020] Preferably, the specific preparation steps of the acidic SiO2 sol in step S2 are as follows:

[0021] Tetraethyl orthosilicate (TEOS) and anhydrous ethanol are mixed, and magnetically stirred for 15 to 20 minutes at room temperature to prepare solution C; HNO3 and H2O are mixed and stirred for 10 to 15 minutes to prepare solution D; solution D is slowly added dropwise to solution C to prepare a reaction precursor solution, and the prepared reaction precursor solution is placed in a constant temperature water bath at 60°C, and magnetically stirred at a speed of 600 to 800 r / min. After reacting for 3 to 5 hours, it is aged at room temperature for 1 to 5 days to prepare an acidic SiO2 sol.

[0022] Preferably, the molar ratio of TEOS, anhydrous ethanol, HNO3, and H2O in solution C and solution D is 1:7:(0.03-0.035):4.

[0023] Preferably, the coating method in step S3 and step S4 is pull-up coating, and the specific parameters are as follows: the descending speed is 50-100 mm / min, the immersion time is 10-30 s, and the ascending speed is 50-100 mm / min.

[0024] The second object of the present invention is to provide a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template obtained by the preparation method of the hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template as described in any one of the above.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1) This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The preparation method uses ZnS nanospheres with a porous structure as a template to prepare ZnS-SiO2 core-shell structure nanospheres and coat them on a glass substrate. The ZnS core is removed by acid etching to obtain a hollow SiO2 nanosphere coating with a self-supporting structure inside. Then, a layer of acidic SiO2 sol is infiltrated on the hollow SiO2 nanosphere coating, and annealed at high temperature to obtain a hollow SiO2 nanosphere with a self-supporting structure inside and an acidic SiO2 composite anti-reflection film. The thickness of the film layer can be adjusted according to the number of coatings, the concentration of the coating solution and the pulling speed.

[0027] In the preparation method, ZnS nanospheres are inorganic templates, which can be completely removed by HCl etching, avoiding the harmful gases generated during high-temperature and long-term annealing when using organic templates to damage the equipment. Acid-catalyzed SiO2 sol is used as a binder, which can penetrate into the gaps between the hollow spheres through capillary action to achieve "bridging" of the hollow spheres. This "bridging" effect significantly enhances the mechanical strength of the film, and can further regulate the refractive index of the film, so that its light transmittance is further improved, providing more freedom for regulating the optical properties of the anti-reflection film. The present invention uses an inorganic template ZnS, which has pores inside. The template can be removed by acid etching, and the hollow SiO2 nanosphere structure with a self-supporting structure inside is very stable, and avoids the generation of a large amount of waste gas during high-temperature annealing.

[0028] 2) It is easy to prepare self-supporting hollow SiO2 nanospheres, but it is not easy to prepare them into anti-reflection films. This is because acid etching is involved in the process of preparing hollow SiO2 spheres using ZnS as a template. This pickling process will change the surface charge state of SiO2 and cause agglomeration, resulting in the obtained SiO2 hollow spheres cannot be directly used for coating. In the present invention, ZnS-SiO2 core-shell structure coating is first used, and then etching is performed. Finally, acidic silicon oxide is used as a binder, and high-temperature short-time annealing is performed to obtain an anti-reflection film with good transmittance and high hardness. On the one hand, based on reasonable process technology (including coating first and then etching, appropriate coating solution concentration adjustment, etc.), the preparation of self-supporting hollow SiO2 anti-reflection film is realized; on the other hand, the acidic SiO2 film is used as a binder and annealed at 680-720°C for 2-3 minutes, which is consistent with the glass tempering conditions, avoiding additional high-temperature annealing and saving costs. Conventional acidic SiO2 used as a binder generally adopts low-temperature annealing, which results in poor film adhesion, or adopts 500°C annealing for 2h, which requires an additional high-temperature annealing process.

[0029] 3) The present invention uses a low-cost process to prepare a self-supporting hollow SiO2 nanosphere anti-reflection film with high transmittance and durability bonded by acidic SiO2. The main structure of the coating is a hollow SiO2 nanosphere with a self-supporting structure inside. Its structure is more stable than that of ordinary hollow SiO2, and the pores of the coating are not easy to collapse, and the high transmittance can be maintained for a long time. The anti-reflection film of the present invention has high transmittance and high adhesion to the substrate. Compared with other hollow SiO2 coatings, the hardness is higher and it has excellent wear resistance and durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 (a) is a SEM picture of the hollow SiO2 nanosphere anti-reflection film prepared in Example 1 (the inset is a transmission image of the hollow spheres), (b) is a SEM picture (b) of the hollow SiO2 nanosphere-based anti-reflection film 1 based on an inorganic template prepared in Example 1.

[0031] Figure 2 The transmittance tests were conducted on pure glass, the hollow SiO2 nanosphere anti-reflection film prepared in Example 1, and the hollow SiO2 nanosphere-based anti-reflection film 1 based on an inorganic template prepared in Example 1. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0033] Preparation Example 1

[0034] This preparation example provides a method for preparing ZnS nanospheres, and the specific steps are as follows:

[0035] Thiourea, zinc acetate and deionized water are mixed, stirred at room temperature until completely dissolved, and then polyvinyl pyrrolidone (PVP) is added and stirred thoroughly to obtain a mixed solution, wherein the mass ratio of thiourea, zinc acetate, deionized water and PVP is 3.80:0.22:25:0.75; the mixed solution is transferred to a polytetrafluoroethylene liner, and then the reactor is encapsulated, and the mixture is reacted at 140°C for 5 hours and then naturally cooled to room temperature. The reaction product is centrifugally washed with deionized water and anhydrous ethanol and then dried to obtain ZnS nanospheres with an outer diameter of 60 nm, an internal pore structure and monodispersity.

[0036] Preparation Example 2

[0037] This preparation example provides a method for preparing ZnS-SiO2 core-shell structure nanospheres using the ZnS nanospheres of Example 1, and the specific steps are as follows:

[0038] The monodisperse ZnS nanospheres with a diameter of 60 nm and a porous structure inside obtained in Preparation Example 1 were added to anhydrous ethanol for ultrasonic dispersion, and PVP, ammonia water and deionized water were added at 30° C. while stirring, and solution A was obtained after sufficient stirring; wherein the concentration of ammonia water was 1.7 mol / L, and the mass ratio of ZnS nanospheres, anhydrous ethanol, PVP, ammonia water and deionized water was 0.5:25:0.2:2.5:2;

[0039] S12, tetraethyl orthosilicate TEOS and anhydrous ethanol EtOH were mixed in a volume ratio of 1:5, and stirred evenly at room temperature, which was recorded as solution B;

[0040] S13, slowly adding solution B to solution A twice, wherein the mass ratio of ZnS nanospheres in solution A to TEOS in solution B is 1:2. The time interval between the two additions is 2 hours, and the reaction is 8 hours. The reaction product is washed by centrifugation with deionized water and anhydrous ethanol and then dried to obtain ZnS-SiO2 core-shell structure nanospheres, and the outer diameter of the nanospheres is 80 nm.

[0041] Preparation Example 3

[0042] This preparation example provides a method for preparing an acidic SiO2 sol, which specifically comprises the following steps:

[0043] Tetraethyl orthosilicate (TEOS) and anhydrous ethanol were mixed, and magnetically stirred for 20 minutes at room temperature to prepare solution C; HNO3 and H2O were mixed and stirred for 20 minutes to prepare solution D; solution D was slowly added dropwise to solution C to prepare a reaction precursor solution, wherein the molar ratio of TEOS, anhydrous ethanol, HNO3, and H2O in solution C and solution D was 1:7:0.035:4, the prepared reaction precursor solution was placed in a constant temperature water bath at 60°C, and magnetically stirred at a speed of 750r / min. After reacting for 3 hours, it was aged at room temperature for 5 days to prepare an acidic SiO2 sol.

[0044] Preparation Example 4

[0045] This preparation example provides a method for pretreating a glass substrate, and the specific steps are as follows:

[0046] Place the glass substrate cut into appropriate size into a NaOH solution for ultrasonic treatment for 10 minutes, rinse with tap water, soak it in deionized water and wipe it carefully with a dust-free cloth, then soak it in anhydrous ethanol, take it out and dry it to obtain a clean glass substrate for use.

[0047] Example 1

[0048] This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template, and the specific steps are as follows:

[0049] S1. Take the ZnS-SiO2 core-shell structure nanospheres with an outer diameter of 80 nm obtained in Preparation Example 2, and evenly disperse them in anhydrous ethanol at a dispersion concentration of 0.02 g / ml, and use them as coating solution 1.

[0050] S2, take the acidic SiO2 sol prepared in Preparation Example 3, dilute the acidic SiO2 sol 3 times, and use it as the coating solution 2;

[0051] S3, take the glass substrate pretreated in Preparation Example 4, use the above-mentioned coating solution 1 to coat the surface of the glass substrate, the thickness of the coating 1 is 100nm, and after drying the coating, place it in a 1mol / L dilute hydrochloric acid solution and soak it for 3h, then take it out, rinse it with deionized water for several times and dry it, and obtain a hollow SiO2 nanosphere anti-reflection film with a self-supporting structure on the glass substrate;

[0052] S4. Use coating liquid 2 to coat the surface of the hollow SiO2 nanosphere anti-reflection film prepared in step S3. The thickness of the coating 2 is 50nm to obtain a composite film. After annealing the composite film at 700°C for 2.5min, cool it to room temperature to obtain a hollow SiO2 nanosphere-based anti-reflection film 1 with a thickness of 150nm based on an inorganic template.

[0053] Figure 1(a) is a SEM image of the hollow SiO2 nanosphere anti-reflection film prepared in Example 1 (the inset is a transmission image of the hollow sphere), (b) is a SEM image of the hollow SiO2 nanosphere-based anti-reflection film 1 based on an inorganic template prepared in Example 1. Figure 1 It can be seen that the surface of the hollow SiO2 nanosphere anti-reflection film is relatively smooth, but the gaps between the particles are large, while the surface of the hollow SiO2 nanosphere-based anti-reflection film based on the inorganic template is smoother, and the pores between the particles are completely filled.

[0054] Figure 2 The transmittance test was conducted on pure glass, the hollow SiO2 nanosphere anti-reflection film with a self-supporting structure prepared in Example 1, and the hollow SiO2 nanosphere-based anti-reflection film 1 based on an inorganic template prepared in Example 1. Figure 2 It can be seen that the maximum transmittance of the hollow SiO2 nanosphere anti-reflection film in the range of 300-1100nm is 95.87%, which is significantly improved compared with 91.51% of the blank glass substrate; and the maximum transmittance of the hollow SiO2 nanosphere-based anti-reflection film based on the inorganic template in the range of 300-1100nm is 97.15%, with better performance.

[0055] Example 2

[0056] This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The specific steps are referred to in Example 1, except that the acidic SiO2 sol is diluted 2 times and used as the coating solution 2. The hollow SiO2 nanosphere-based anti-reflection film 2 based on an inorganic template is prepared, and the film thickness is 176nm. After testing, the maximum transmittance is 96.37%.

[0057] Example 3

[0058] This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The specific steps are as described in Example 1, except that the acidic SiO2 sol is diluted 10 times and used as a coating solution 2 to prepare a hollow SiO2 nanosphere-based anti-reflection film 3 based on an inorganic template, with a film thickness of 141 nm. After testing, the maximum transmittance is 96.31%.

[0059] Example 4

[0060] This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The specific steps are as described in Example 1, except that the dispersion concentration of the ZnS-SiO2 core-shell structure nanospheres in anhydrous ethanol is adjusted to 0.033 g / ml and used as a coating solution 1. A hollow SiO2 nanosphere-based anti-reflection film 4 based on an inorganic template is obtained, and the film thickness is 202 nm. After testing, the maximum transmittance is 95.38%.

[0061] Example 5

[0062] This embodiment provides a method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template. The specific steps are referred to in Example 1, except that the dispersion concentration of ZnS-SiO2 core-shell structure nanospheres in anhydrous ethanol is adjusted to 0.05 g / ml and used as a coating solution 1. A hollow SiO2 nanosphere-based anti-reflection film 5 based on an inorganic template is obtained, and the film thickness is 249 nm. After testing, the maximum transmittance is 94.32%.

[0063] Those skilled in the art should understand that the above are only some specific embodiments of the present invention, rather than all embodiments. It should be noted that for those of ordinary skill in the art, many modifications and improvements can be made, and all modifications or improvements that do not exceed the scope of protection of the present invention should be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template, characterized in that: The steps include: S1, taking ZnS-SiO2 core-shell structure nanospheres with an outer diameter of 80-120nm, wherein the ZnS nanospheres are the core and SiO2 is the shell; the ZnS-SiO2 core-shell structure nanospheres are uniformly dispersed in anhydrous ethanol at a dispersion concentration of 0.015-0.05g / ml, and used as a coating solution 1; S2, using tetraethyl orthosilicate TEOS as a silicon source, nitric acid HNO3 as a catalyst, and anhydrous ethanol EtOH as a solvent, hydrolysis polymerization reaction is used to prepare acidic SiO2 sol, and the acidic SiO2 sol is diluted 2-10 times and used as coating solution 2; S3, pre-treating the glass substrate to obtain a clean and dry surface, using a coating solution 1 to coat the surface of the glass substrate to form a coating 1, wherein the thickness of the coating 1 is 100 to 500 nm, drying the glass substrate with the coating 1 and placing it in a 0.5 to 1 mol / L dilute hydrochloric acid solution, soaking it for 1 to 3 hours and then taking it out, rinsing it with deionized water for multiple times and then drying it, thereby obtaining a hollow SiO2 nanosphere anti-reflection film with a self-supporting structure on the glass substrate; S4, using the coating solution 2, coating the surface of the hollow SiO2 nanosphere anti-reflection film prepared in step S3 to form a coating 2, the thickness of the coating 2 is 20-100 nm, and a composite film is obtained; after annealing the composite film at 680-720° C. for 2-3 min, cooling it to room temperature to obtain a hollow SiO2 nanosphere-based anti-reflection film with a thickness of 120-600 nm based on an inorganic template; There is no particular order for steps S1 and S2.

2. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 1, characterized in that: The preparation method of ZnS-SiO2 core-shell structure nanospheres with an outer diameter of 80 to 120 nm in step S1 is as follows: S11, taking ZnS nanospheres with an outer diameter of 60 to 100 nm, a porous structure inside, and monodispersity, adding them to anhydrous ethanol for ultrasonic dispersion, adding PVP, ammonia water, and deionized water at a temperature of 20 to 30° C. while stirring, and obtaining solution A after sufficient stirring; S12, tetraethyl orthosilicate TEOS and anhydrous ethanol EtOH were mixed, and stirred at room temperature, which was recorded as solution B; wherein the mass ratio of ZnS nanospheres in solution A to TEOS in solution B was 1:(2-3); S13. Slowly add solution B to solution A twice, with a time interval of 2 to 3 hours between the two additions, and react for 7 to 9 hours. The reaction product is washed by centrifugation with deionized water and anhydrous ethanol and then dried to obtain ZnS-SiO2 core-shell structured nanospheres with an outer diameter of 80 to 120 nm.

3. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 2, characterized in that: In step S11, the concentration of ammonia water is 1.3-3.2 mol / L, and the mass ratio of ZnS nanospheres, anhydrous ethanol, PVP, ammonia water and deionized water is 0.5:(25-40):0.2:(2-3):

2.

4. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 2, characterized in that: In step S12, tetraethyl orthosilicate TEOS and anhydrous ethanol EtOH are mixed in a volume ratio of (1-1.5):

5.

5. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 2, characterized in that: The preparation method of the ZnS nanospheres with a diameter of 60 to 100 nm, an internal porous structure, and monodispersity described in step S11 is as follows: thiourea, zinc acetate and deionized water are mixed, stirred at room temperature until completely dissolved, and then polyvinyl pyrrolidone PVP is added and stirred sufficiently to obtain a mixed solution, wherein the mass ratio of thiourea, zinc acetate, deionized water and PVP is (2.85 to 3.80):0.22:25:(0.5 to 0.75); the mixed solution is transferred to a polytetrafluoroethylene liner, and then the reactor is encapsulated, and the reaction is carried out at 120 to 150° C. for 4 to 6 hours and then naturally cooled to room temperature. The reaction product is centrifuged and washed with deionized water and anhydrous ethanol and then dried to obtain ZnS nanospheres with a diameter of 60 to 100 nm, an internal porous structure, and monodispersity.

6. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 1, characterized in that: The steps of pretreatment of the glass substrate in step S3 are as follows: put the glass substrate cut into a suitable size into a NaOH solution for ultrasonication for 10 to 15 minutes, rinse it with tap water, soak it in deionized water and wipe it with a dust-free cloth, then soak it in anhydrous ethanol, take it out and dry it to obtain a clean and dry surface.

7. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 1, characterized in that: The specific preparation steps of the acidic SiO2 sol in step S2 are as follows: Tetraethyl orthosilicate (TEOS) and anhydrous ethanol are mixed, and magnetically stirred for 15 to 20 minutes at room temperature to prepare solution C; HNO3 and H2O are mixed and stirred for 10 to 15 minutes to prepare solution D; solution D is slowly added dropwise to solution C to prepare a reaction precursor solution, and the prepared reaction precursor solution is placed in a constant temperature water bath at 60°C, and magnetically stirred at a speed of 600 to 800 r / min. After reacting for 3 to 5 hours, it is aged at room temperature for 1 to 5 days to prepare an acidic SiO2 sol.

8. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 7, characterized in that: The molar ratio of TEOS, anhydrous ethanol, HNO3, and H2O in solution C and solution D is 1:7:(0.03-0.035):

4.

9. The method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template according to claim 1, characterized in that: The coating method in step S3 and step S4 is pull-up coating, and the specific parameters are as follows: the descending speed is 50-100 mm / min, the immersion time is 10-30 s, and the ascending speed is 50-100 mm / min.

10. A hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template obtained by the method for preparing a hollow SiO2 nanosphere-based anti-reflection film based on an inorganic template as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Anti-reflection glass substrate as well as preparation method and application thereof

    CN103771727A

  • Self-supporting hollow SiO2 nanosphere and preparation method thereof

    CN118289767A

  • Photovoltaic module surface self-cleaning antireflection coating and preparation method thereof

    CN118545914A

Cited By

  • Glass self-cleaning coating liquid as well as preparation method and application thereof

    CN122011812A

  • Self-cleaning functional repairing method for photovoltaic cover plate glass

    CN122254770A