A method for preparing a recombinant collagen hydrogel with self-assembly ability of layered fibers by photo-crosslinking
The preparation of recombinant collagen hydrogels by photocrosslinking method solves the problem of insufficient mechanical properties and realizes recombinant collagen hydrogels with layered fiber self-assembly ability and mechanical properties, which are suitable for applications such as 3D printing.
Patent Information
- Application Number
- CN202610595614.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-30
- Publication Date
- 2026-08-04
AI Technical Summary
Existing recombinant collagen hydrogels, while possessing a biomimetic structure, lack sufficient mechanical properties, making it difficult to meet the application requirements of 3D printing and other applications.
Recombinant collagen hydrogels were prepared using a photocrosslinking method. By adding methacrylic anhydride to a recombinant collagen solution and performing photocrosslinking, a hydrogel with the ability to self-assemble layered fibers was formed.
The prepared recombinant collagen hydrogel has a triple helix structure and layered fiber self-assembly capability, and also possesses certain mechanical properties, making it suitable for fields such as 3D printing.
Smart Images

Figure CN122502471A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing recombinant collagen hydrogels with layered fiber self-assembly capabilities through photocrosslinking, belonging to the field of genetic engineering technology. Background Technology
[0002] Collagen is the most abundant protein in mammals, found in skin, cartilage, tendons, and other tissues, accounting for 30% of all proteins in the body. Its three-dimensional helical structure provides structural support and regulates local biological responses, playing a crucial role in tissue and organ formation. Collagen functions in mammals as collagen fibers, which exhibit various morphologies, including fibrils and networks. Due to its excellent biocompatibility, biodegradability, and safety, collagen is widely used in biomedicine and tissue engineering, such as in drug delivery systems, cell culture, artificial blood vessels, tendon, bone, and skin scaffolds, and hemostatic materials. As a highly efficient biomaterial, collagen's superior biocompatibility and biodegradability have led to the widespread application of collagen-based hydrogels. Hydrogels consist of a three-dimensional network structure, are semi-solids that are insoluble in water but have extremely high water absorption capacity and rapidly expand upon contact with water. The fibrous structure formed by collagen-based hydrogels is similar to that of the natural extracellular matrix, thus exhibiting excellent biochemical properties and rapidly activating cellular responses.
[0003] However, collagen extracted from animal tissues presents challenges such as complex composition, difficulty in monomer separation, batch-to-batch inhomogeneity, and the safety risks associated with viral contamination. Compared to other preparation methods, microbial expression systems offer significant advantages, including low cost, short cycle time, and high expression levels. *Escherichia coli* (E. coli) Escherichia coli Microbial expression systems, due to their simple operation and short fermentation cycle, are currently an ideal model host for studying collagen expression and properties. Microbially expressed recombinant collagen exhibits advantages such as no viral risks, low immunogenicity, good water solubility, processability, and stable quality. Therefore, high-quality recombinant collagen can be obtained using microbial expression systems.
[0004] Currently, recombinant collagen has received widespread attention in the fields of regenerative medicine and tissue engineering. Patent CN119529061 A discloses a recombinant type I human collagen, hydrogel, and its application in the field of cosmetic fillers. It prepares a composite hydrogel by combining this recombinant type I human recombinant collagen with nanocellulose, exhibiting high stability, low swelling, high weight retention, and strong adhesion and hemostatic abilities. CN 110790950 A discloses a method for preparing recombinant collagen hydrogels through photocrosslinking with the addition of methacrylic anhydride and its application in 3D printing. The prepared hydrogel has good physicochemical properties and biocompatibility. However, while research on the application of recombinant collagen in hydrogel preparation is widespread, research on how to prepare recombinant collagen hydrogels with biomimetic structures is relatively limited.
[0005] The inventors' team initially used protein computational analysis and thermal stability prediction to... The α1 chain of type II collagen was analyzed, and sequences with a high predicted tendency for triple helix formation were selected. (GPP)10 sequences were then added to the N- and C-termini of these sequences. Expression using these sequences yielded recombinant collagen with a triple helix structure and the ability to assemble into periodic light and dark stripes. However, this recombinant collagen hydrogel exhibited poor mechanical properties and insufficient self-support.
[0006] Therefore, there is an urgent need for a method to prepare recombinant collagen hydrogels that possess both a biomimetic structure and certain mechanical properties. Summary of the Invention
[0007] To address the aforementioned issues, this application addresses the problem of preparing hydrogels with certain mechanical properties from recombinant collagen expressed in a microbial system while possessing a biomimetic structure. It introduces a method of preparing hydrogels using photocrosslinking within chemical crosslinking of recombinant collagen. This preparation method enables the recombinant collagen hydrogels to possess a triple helix structure and the ability to self-assemble layered fibers, while also exhibiting certain mechanical properties. This successfully applies the recombinant collagen hydrogels to the field of 3D printing.
[0008] The first objective of this invention is to provide a method for preparing recombinant collagen with the ability to self-assemble layered fibers, comprising the steps of: Methacrylic anhydride was added to the recombinant collagen solution at a rate of 1.4~2 μL / min, and the reaction and displacement were carried out to obtain recombinant collagen with the ability to self assemble layered fibers. The molar ratio of methacrylic anhydride to recombinant collagen is 8-12:1.
[0009] In one embodiment, the recombinant collagen has the following structure: From the N-terminus to the C-terminus, the sequence consists of the first repeat sequence, the collagen domain, and the second repeat sequence. Optionally, the amino acid sequences of the first repeat sequence and the second repeat sequence are as shown in SEQ ID NO.3; Optionally, the amino acid sequence of the collagen domain is shown in SEQ ID NO.2.
[0010] In one embodiment, the N-terminus of the recombinant collagen is further connected to a folding domain; the amino acid sequence of the folding domain is shown in SEQ ID NO.1; Optionally, there is an enzyme cleavage site between the folded domain and the first repeat sequence, and the amino acid sequence of the enzyme cleavage site is LVPRGSP.
[0011] In one embodiment, the reaction temperature is 35~40 ℃, the rotation speed is 200~220 rpm, and the pH is 7.0~7.4.
[0012] In one embodiment, the recombinant collagen is presented as layered fibers by using TEM scanning to obtain light and dark stripes.
[0013] A second object of the present invention is to provide recombinant collagen with the ability to self-assemble layered fibers, prepared by any of the above methods.
[0014] The third objective of this invention is to provide a recombinant collagen hydrogel prepared from the aforementioned recombinant collagen with layered fiber self-assembly capability; Optionally, the recombinant collagen hydrogel is prepared by: dissolving recombinant collagen in a buffer solution, adding methacrylic anhydride, and reacting to obtain methacrylic anhydride-modified recombinant collagen; replacing and self-assembling to obtain methacrylamide-self-assembled recombinant collagen; adding a photocrosslinking agent to form a recombinant collagen hydrogel through photocrosslinking.
[0015] A fourth objective of this invention is to provide the application of the recombinant collagen with the ability to self-assemble layered fibers or the aforementioned recombinant collagen hydrogel in the fields of biology, food, chemical industry, medicine, biomaterials, tissue engineering, or cosmetics.
[0016] In one embodiment, the application includes: using recombinant collagen with layered fiber self-assembly capability to prepare drug delivery materials, three-dimensional scaffold materials, hemostatic materials, tissue filler materials, and biosensors.
[0017] A fifth object of the present invention is to provide a recombinant collagen product containing the above-mentioned recombinant collagen with the ability to self-assemble layered fibers or the above-mentioned recombinant collagen hydrogel.
[0018] In one embodiment, the recombinant collagen hydrogel is prepared by: dissolving recombinant collagen in a buffer solution, adding methacrylic anhydride, and reacting to obtain methacrylic anhydride-modified recombinant collagen; using a phosphate buffer to replace the reaction system to remove unreacted methacrylic anhydride and impurities, and self-assembling at 4°C to obtain methacrylamide-self-assembled recombinant collagen; adding a photocrosslinking agent, and photocrosslinking to form a recombinant collagen hydrogel.
[0019] In one embodiment, the concentration of the recombinant collagen solution is 2 mmol·L⁻¹. -1 The molar ratio of amino groups to methacrylic anhydride in the recombinant collagen is 1:8~12, and the reaction temperature is 32~36℃.
[0020] In one embodiment, NaOH is used to adjust the pH to be stable at 7.4 during the reaction.
[0021] The sixth objective of this invention is to provide a method for improving the mechanical properties of recombinant collagen hydrogels while maintaining the triple helix structure and self-assembly ability of layered fibers. The method involves preparing hydrogels using methacrylated recombinant collagen, comprising: Methacrylic anhydride was added to the recombinant collagen solution at a rate of 1.4~2 μL / min, and the reaction and displacement were carried out to obtain recombinant collagen with the ability to self assemble layered fibers. The molar ratio of methacrylic anhydride to amino groups in recombinant collagen is 8-12:1.
[0022] Beneficial effects of the present invention This invention creatively introduces a recombinant collagen hydrogel with a triple helix structure and layered fiber self-assembly forming periodic light and dark striped fibers through photocrosslinking. It also verifies that the triple helix structure and self-assembly ability of the recombinant collagen before and after chemical modification are not significantly different.
[0023] Compared to most recombinant collagen hydrogels, the recombinant collagen hydrogel prepared in this way possesses a biomimetic structure—a triple helix structure—and self-assembles into periodic light and dark striped fibers resembling type I collagen. In addition to these capabilities, it also possesses certain mechanical properties—it can be 3D printed to create models with relatively complex shapes. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the collagen structure.
[0025] Figure 2 This is a schematic diagram of the collagen structure after the folded regions have been removed.
[0026] Figure 3SDS-PAGE images of whole cells after cell lysis and supernatant collected by centrifugation; 1 and 2 in the figure correspond to the sequence V-P10BP10 in whole cells and supernatant, respectively; M: protein marker.
[0027] Figure 4 SDS-PAGE of target proteins eluted by V-P10BP10 at 50mM, 400mM, and 500mM imidazole concentrations in lanes 2-4. M: protein marker.
[0028] Figure 5 The images show SDS-PAGE and MALDI-TOF sequences of collagen with V-domain after trypsin digestion. In Figure A, 1 represents the SDS-PAGE of P10BP10, and M stands for protein marker. Figure B shows the MALDI-TOF sequence, verifying that the molecular weight of the expressed recombinant collagen matches the theoretical value.
[0029] Figure 6 The full wavelength spectrum, thermochromic curve, and first derivative plot of the thermochromic curve of the designed recombinant type I collagen P10BP10 are shown.
[0030] Figure 7 The triple helix extent of RCMA-1 and RCMA-2 samples and unmodified recombinant collagen (RC) was compared.
[0031] Figure 8 This paper presents the fibrous structure of type I collagen with periodic light and dark stripes formed by the self-assembly of three samples: RC, RCMA-1, and RCMA-2, and uses ImageJ to measure the statistical graph of the width of the light and dark stripes.
[0032] Figure 9 To verify the degree to which the side chain amino groups of the two samples, RCMA-1 and RCMA-2, were substituted by methacrylic anhydride (MA).
[0033] Figure 10 The state of the sample before and after photocrosslinking was recorded in a 2 mL glass bottle.
[0034] Figure 11 To record the appearance after gelation in a 1.5ml plastic EP tube and removal with tweezers.
[0035] Figure 12 Macrorheology was used to characterize RCMA-1 and RCMA-2 hydrogels, including amplitude scanning, frequency scanning, and viscosity scanning spectra.
[0036] Figure 13 The internal three-dimensional structural features of three samples: RC, RCMA-1, and RCMA-2.
[0037] Figure 14 This test was conducted to verify the thermal stability of the RCMA-2 sample.
[0038] Figure 15 Characterization of successful methacrylation of RCMA-2 samples was performed, including 1H NMR and Fourier transform infrared spectroscopy.
[0039] Figure 16 Comparative spectra of the mechanical properties of three hydrogels, RCMA-2, GelMA-1, and GelMA-2, including amplitude scan, frequency scan, and viscosity scan.
[0040] Figure 17 Images of models printed using RCMA-2 samples as 3D printing ink are recorded and displayed.
[0041] Figure 18 The results of cytotoxicity and proliferation experiments on RCMA-1 and RCMA-2 samples are shown in Figure A, where live and dead cell staining is shown; Figures B and C show the 24-hour toxicity of RCMA-1 and RCMA-2 samples; and Figure D shows the cell proliferation experiment of RCMA-1 and RCMA-2 samples. Detailed Implementation
[0042] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explanation of the present invention and are not intended to limit the present invention.
[0043] Culture medium: LB medium (g / L): tryptone 10, yeast extract 5, NaCl 10, pH 7.0; TB medium (g / L): tryptone 12, yeast extract 24, glycerol 4 mL, KH2PO4 2.31, K2HPO4 12.54 Cultivation method (shake flask fermentation): Aspirate 50 μL of bacterial culture from the glycerol tube containing the target gene into 5 mL of LB (Amp resistant) and incubate overnight at 37 °C and 200 r / min. Transfer 1% of the culture to 100 mL of TB fermentation broth (Amp resistant) and incubate at 37 °C and 200 r / min for 24 h. Then add IPTG to a final concentration of 1 mmol / L and ferment at 25 °C and 200 r / min for 10 h, followed by fermentation at 15 °C for 14 h.
[0044] Protein purification methods: After fermentation, the bacterial culture was collected, centrifuged at 4 ℃ and 10,000 rpm for 5 min, the supernatant was discarded, and the bacterial precipitate was collected. After disruption, the precipitate was centrifuged at 4 ℃ and 10,000 rpm for 20 min and filtered through a 0.45 μm aqueous filter membrane. Then, it was filtered using a His Trap filter. TM HP affinity purification was performed using 5 mL of buffer A (20 mmol / L Na₂HPO₄, 20 mmol / L NaH₂PO₄, 500 mmol / L NaCl, 10 mmol / L Iminazole, pH 7.4), followed by loading at a flow rate of 3 mL / min. After loading, a gradient elution was performed using elution buffer B (20 mmol / L Na₂HPO₄, 20 mmol / L NaH₂PO₄, 500 mmol / L NaCl, 500 mmol / L Iminazole, pH 7.4) to obtain the target protein. The purification status was analyzed using SDS-PAGE.
[0045] Trypsin digestion: The purified collagen was digested with trypsin and digested on a shaker at 25 °C for 24 h. The purity was verified by SDS-PAGE analysis.
[0046] Desalination freeze-drying method: The enzyme digestion reaction product was desalted using HiTrap Desalting with ultrapure water as the mobile phase at a flow rate of 5 mL / min. The peak sample was collected, verified by SDS-PAGE, and then freeze-dried under vacuum at -50 °C.
[0047] Identification of the triple helix structure and stability of the samples: Circular dichroism (CD) chromatography was used for identification. The specific steps were as follows: the lyophilized sample was dissolved in 10 mmol / L, pH 7.4 sodium phosphate buffer to a concentration of 1 mg / mL, equilibrated at 4 °C for 24 h, and then subjected to CD chromatography. The CD spectra from 190 to 260 nm were measured at 4 °C at 1 nm intervals, with an average scan time of 5 s. The thermochromic curve was obtained by monitoring the CD signal at 223 nm, increasing the temperature from 10 °C to 80 °C at a rate of 10 °C / h, equilibrating for 8 s at each temperature, and determining the melting temperature (…). T m The temperature data is obtained by taking the first derivative of the fitted thermal curve, and this temperature data represents the stability of the sample.
[0048] Methods for determining molecular weight using MALDI-TOF-MS (ultrafleXtreme) mass spectrometry: The lyophilized sample was dissolved in water to a concentration of 1 mg / mL, and the molecular weight was determined using a MALDI-TOF-MS (ultrafleXtreme) mass spectrometer. The matrix used was DHAP (2-acetylresorcinol, combined with ethanol and diammonium hydrogen citrate), and the operation was performed in linear mode.
[0049] MA-type reaction process: The recombinant collagen with the correct test results was dissolved in PB at a concentration of 2 mM. Methacrylic anhydride was added at a molar ratio of N (recombinant collagen side chain amino group) to methacrylic anhydride (MA) of 1:10. During the reaction, the pH was adjusted using 200 mM sodium hydroxide to maintain the reaction system at 7.0~7.4. After the reaction was completed, the mixture was diluted ten times the volume of the reaction system and dialyzed. After dialyzing for 48 hours to ensure that impurities and unreacted MA were completely removed, the mixture was lyophilized. The lyophilized powder was stored at -80℃ for later use.
[0050] Photocrosslinking process: After MA conversion, collagen was dissolved in PB, and a photocrosslinking agent (LAP) was added to it at a working concentration of 10 mg / mL. The hydrogel was prepared by crosslinking under 405 nm blue-violet visible light at room temperature.
[0051] Determination of MA residue: High performance liquid chromatography (HPLC) was used to detect and analyze the residual amount of MA in the reaction system. The mobile phase used was acetonitrile and 0.1% trifluoroacetic acid. The method used acetonitrile to perform gradient elution of the reaction system to detect the peak. The detector wavelength was selected as 220 nm, and the reaction temperature was controlled at 35 °C.
[0052] Indicators of successful MA conversion: The obtained reaction system was analyzed using proton nuclear magnetic resonance (NMR) spectroscopy and Fourier transform infrared spectroscopy (FTIR). The NMR spectrometer used was an AVANCE NEO 600MHz, the reaction temperature was room temperature, and the test results were processed and analyzed using MestReNova software. The Fourier transform infrared spectroscopy recording range was 4000–400 cm⁻¹. -1 Resolution better than 0.5 cm -1 The scans were performed 32 times at room temperature.
[0053] Transmission electron microscope: A collagen solution of a specific concentration was prepared and assembled at 4°C for 4 days. 5 μL of the assembled collagen solution was dropped onto a copper grid, and after adsorption for 45 seconds, the collagen solution was absorbed using filter paper. Then, 5 μL of 0.75% phosphotungstic acid was used for negative staining for 20 seconds. The stain was then absorbed using filter paper, and the sample was dried before observation and imaging using a Hitachi H-7650 transmission electron microscope at 80 kV.
[0054] Scanning electron microscope: After freeze-drying in a vacuum freeze dryer, the samples were placed on aluminum foil that had been fixed with double-sided tape. After sputtering gold for 40 seconds, the samples were transferred to a scanning electron microscope for imaging. The samples were observed and photographed using a Hitachi SU1510 scanning electron microscope at an accelerating voltage of 5 kV.
[0055] Macrorheological scanning: The viscoelastic properties of the hydrogel samples were evaluated using a rheometer. The testing system employed a cone-plate geometry. First, strain scanning experiments were used to determine the linear viscoelastic region (LVE), with a fixed frequency of 1 Hz and a continuous gradient variation in strain amplitude (0.1% to 1000%). After determining the LVE range, two stages of system testing were conducted: (1) a frequency scanning stage, maintaining a constant shear strain of 1% within the frequency range of 1-100 Hz; and (2) a steady-state viscosity test stage, applying a strain of 0.1-100 s. -1 The gradient shear rate was determined. The dynamic storage modulus (G'), loss modulus (G''), and viscosity were quantitatively characterized using the above experimental scheme.
[0056] Substitutability: The degree of substitution was quantitatively analyzed using the 2,4,6-trinitrobenzenesulfonic acid (TNBS) colorimetric method. The sample was dissolved in 0.1 mol / L sodium bicarbonate buffer to prepare a final concentration of 1.6 mg / mL. 0.2% (w / v) TNBS reagent (2,4,6-trinitrobenzenesulfonic acid) was added to each sample, and the reaction was carried out at 37 °C for 3 hours. At the end of the reaction, 1 mol / L hydrochloric acid and 10% (w / v) sodium dodecyl sulfate (SDS) were added to terminate the chemical reaction. The absorbance of the sample was finally measured at 335 nm, and a working curve was established by comparing the absorbance with a gradient concentration of glycine standard solutions for comparative analysis. 3D printing: The 3D model was designed and generated using AutoCAD software (SolidWorks), saved as a stereolithography (STL) file, and then layered and cut in the Z direction using Orixell Master software to form a digital pattern. Printing was performed using a commercial DLP 3D printer (PBP-R2, Otrixell Life Science, China), equipped with a 405 nm ultraviolet LED light source and an 8520 × 4320 pixel resolution.
[0057] Cellular experiments: The cytotoxicity of the hydrogel was assessed using the CCK-8 assay. NIH-3T3 mouse fibroblasts were injected at a concentration of 2 × 10⁻⁶ cells / mL. 3Cells were seeded at a density of [number] cells / well in 96-well plates and incubated at 37°C with 5% CO2 for 24 hours. 100 μL of hydrogel extract at different dilutions (1:1000, 1:500, 1:200, 1:100, v / v) was added to each well, while an equal volume of DMEM was added to the control wells. After another 24 hours of incubation, the medium was replaced with 10% CCK-8 solution, and the plates were incubated at 37°C with 5% CO2 in the dark for 1 hour. The absorbance at 450 nm was measured using a multi-functional microplate reader, and cell viability was calculated. All experiments were repeated three times. The proliferation experiment was similar, simply extending the time interval for sampling.
[0058] Example 1: Design of collagen sequences Design as Figure 1 The collagen amino acid sequence is shown. The amino acid sequence of the first repeating sequence is shown in SEQ ID NO.3 (named P10).
[0059] The introduction of the folding domain (amino acid sequence shown in SEQ ID NO.1) in the collagen sequence can assist collagen in folding to form a triple helix structure; the introduction of the collagen domain (abbreviated as B, amino acid sequence shown in SEQ ID NO.2) is achieved through protein computational analysis and thermal stability prediction. Analysis of the α1 chain of type II collagen was performed, and predicted proteins were selected. T m Sequence B, with a high tendency for triple helix extension close to 37℃, was selected. An LVPRGSP restriction site was added between the folded region and the first repeat sequence to facilitate subsequent restriction enzyme cleavage to remove the folded region. Considering that a proline residue at the end of the sequence might be detrimental to protein expression, an additional glycine residue G was added to the end of the collagen amino acid sequence.
[0060] Example 2: Construction of recombinant plasmids and recombinant bacteria (1) Construction of recombinant plasmids Starting from the recombinant collagen sequence V-P10BP10 (amino acid sequence as shown in SEQ ID NO.4) and its nucleotide sequence (nucleotide sequence as shown in SEQ ID NO.5) obtained in Example 1, when synthesizing the nucleotide sequence of the protein single chain, the base GC was introduced at the 5' flanking end, and bases GC were introduced at the 5' and 3' ends, respectively. Nco I and Bam HI restriction site Nco The nucleotide sequence of the I restriction site is CCATGG. Bam The nucleotide sequence of the HI restriction site is GGATCC. The synthesized genes were then inserted into the pColdIII plasmid (purchased from Genewiz). Nco I and BamBetween HI, sequencing verification yielded the correct recombinant plasmid.
[0061] (2) Construction of recombinant strains Transform the correctly sequenced recombinant plasmids from step (1) into... E. coli BL21 (DE3) competent cells were spread on LB agar plates containing ampicillin, cultured and screened, and then preserved in glycerol tubes to obtain recombinant bacteria containing recombinant collagen, which were named [missing name]. E. coli BL21 (DE3)-V-P10BP10.
[0062] Example 3: Expression, purification, and enzymatic digestion of collagen sequences The recombinant bacteria obtained in Example 2 E. coli BL21(DE3)-V-P10BP10 was cultured in shake flasks. After cell collection, lysis, and centrifugation, the SDS-PAGE results of whole cells and supernatant are as follows: Figure 3 As shown. The supernatant is retrieved using His Trap. TM HP 5 mL was used for affinity purification, and samples were collected at imidazole concentrations of 50 mmol / L, 400 mmol / L, and 500 mmol / L. The samples were verified as the target protein by SDS-PAGE, and the results are as follows. Figure 4 As shown.
[0063] To remove the folded domain, a trypsin cleavage site, LVPRGSP, was introduced between the repeat sequence and the folded domain during sequence design. The pure collagen domain structure was obtained by digestion with trypsin.
[0064] Under the action of trypsin, the V-domain is digested into multiple short peptides containing 2-20 amino acid residues. If the collagen domain folds correctly into a rigid triple helix structure under the action of the V-domain, it will not be digested by trypsin in a short time. After enzymatic digestion, desalting is performed to remove the short peptides, finally yielding collagen P10BP10 (results after enzymatic digestion are shown in the figure). Figure 2 (As shown). Verification via SDS-PAGE yielded the following results. Figure 5 As shown in Figure A, the purity is greater than 95%. The validated protein was desalted, lyophilized, and weighed to obtain its yield. The yield of recombinant collagen P10BP10 was 46.3 mg / L.
[0065] Example 4: MALDI-TOF Identification The collagen P10BP10 protein obtained after enzymatic digestion and desalting in Example 3 was lyophilized. The lyophilized samples were then dissolved in water to prepare 1 mg / mL solutions, and the molecular weight was determined using a MALDI-TOF-MS (ultrafleXtreme) mass spectrometer. The matrix used was DHAP (2-acetylresorcinol, combined with ethanol and diammonium citrate), and the operation was performed in linear mode. The results confirmed that the obtained collagen molecular weight matched the theoretical value. Figure 5 As shown in B.
[0066] Example 5: Circular dichroism characterization of collagen and its sequence structure To confirm the secondary structure of the collagen domain, the lyophilized collagen P10BP10 sample after enzymatic digestion and desalting in Example 3 was prepared into a 1 mg / mL solution using 10 mmol / L sodium phosphate buffer and equilibrated at 4°C for 24 h. After equilibration, full-wavelength scanning was performed using circular dichroism spectroscopy.
[0067] The results are as follows Figure 6 As shown, P10BP10 exhibits a characteristic positive absorption peak at 223 nm, indicating that collagen P10BP10 correctly folds into a triple helix structure with the assistance of the V-domain. The thermochromatograms at 223 nm from 4℃ to 80℃ were monitored using circular dichroism spectroscopy, and the collagen's... T m Value, P10BP10 T m The value is 53℃. The above results indicate that the collagen sequence designed in this invention can fold correctly to form a triple helix structure and has good thermal stability.
[0068] Example 6: Preparation of methacrylated recombinant collagen by MA conversion 1. Preparation of recombinant collagen hydrogels that first self-assemble and then methacrylamide. The purified lyophilized recombinant collagen (P10BP10) was treated with 10 mmol·L⁻¹ pH 7.0 solution. -1 Phosphate buffer is prepared to a concentration of 2 mmol / L. -1 The recombinant collagen solution was placed in a 4°C environment for 3 days to self-assemble. After assembly, methacrylic anhydride was added at a molar ratio of 10:1 to the amino groups in the recombinant collagen. The reaction temperature was 35°C, and the shaking speed was 200 rpm·min. -1 The addition rate of methacrylic anhydride was 1.4-2 μL / min; During the reaction, the pH was adjusted to be stable at 7.4 using 200 mM NaOH. After the reaction, the reaction system was replaced with 10 times the volume of phosphate buffer to remove unreacted methacrylic anhydride and impurities, resulting in a recombinant collagen protein that was first self-assembled and then methacrylated (named RCMA-1). The RCMA-1 sample was prepared to a concentration of 40 mg / mL, and a photocrosslinking agent (LAP) was added to it at a working concentration of 10 mg / mL. Under the action of 405 nm blue-violet visible light for 30 s, the RCMA-1 solution was crosslinked to form an RCMA-1 hydrogel.
[0069] 2. Preparation of recombinant collagen hydrogels that are first methacrylated and then self-assembled The purified lyophilized recombinant collagen (P10BP10) was treated with 10 mmol·L⁻¹ pH 7.0. -1 Phosphate buffer is prepared to a concentration of 2 mmol / L. -1 The recombinant collagen solution was prepared by adding methacrylic anhydride at a molar ratio of 10:1 to the amino groups in the recombinant collagen, at a reaction temperature of 35°C, and a shaking speed of 200 rpm·min. -1 The addition rate of methacrylic anhydride was 1.4-2 μL / min; During the reaction, the pH was adjusted to a stable 7.4 using 200 mM NaOH. After the reaction, the reaction system was replaced with 10 times the volume of phosphate buffer to remove unreacted methacrylic anhydride and impurities. After replacement, the collagen was placed in a 4°C environment for self-assembly for 3 days to obtain recombinant collagen that was first methacrylated and then self-assembled (named RCMA-2). The RCMA-2 sample was prepared to a concentration of 40 mg / mL, and a photocrosslinking agent (LAP) was added to it at a working concentration of 10 mg / mL. Under the action of 405 nm blue-violet visible light for 30 s, RCMA-2 was crosslinked to form RCMA-2 hydrogel.
[0070] Example 7: Circular dichroism spectroscopy characterization of the effect of self-assembly and methacrylation sequence on triple helices Recombinant collagen RC (unmethacrylated recombinant collagen), RCMA-1, and RCMA-2 were prepared according to Example 6. The effects of different self-assembly and methacrylation sequences on the degree of triple helix of the recombinant collagen were characterized by circular dichroism spectroscopy.
[0071] The results are as follows Figure 7As shown, measurements of the three samples (RC, RCMA-1, and RCMA-2) across all wavelengths revealed positive absorption peaks near 223 nm for both RCMA-1 and RCMA-2 solutions, with similar peaks to the unmodified recombinant collagen. This indicates that the modified recombinant collagen can still correctly fold into a triple helix structure. Furthermore, the MRE values of the two samples near 223 nm are clearly similar, suggesting that the difference in the self-assembly and methacrylylation sequence has no significant impact on the formation of the triple helix structure in recombinant collagen.
[0072] Example 8: Transmission electron microscopy characterization of the effect of self-assembly and methacrylation sequence on collagen self-assembly To verify whether the assembly of RCMA-1 and RCMA-2 was affected compared to RC, transmission electron microscopy (TEM) was used to observe the assembly of these three samples in solution and to measure the bandwidth of bright and dark fringes. The results are as follows: Figure 8 As shown.
[0073] The results showed that RC, RCMA-1, and RCMA-2 all formed fibrous structures with periodic bright and dark stripes. Furthermore, the morphology of the three samples was highly similar to that of natural type I collagen fibers. The bandwidth of the bright and dark stripes in each sample was measured using ImageJ. The distribution of the measurement results is shown below. Figure 8 As shown.
[0074] The fringe widths of RC are 10.74 ± 1.16 nm and 23.19 ± 1.39 nm, respectively; the fringe widths of RCMA-1 are 10.96 ± 1.11 nm and 22.46 ± 1.65 nm, respectively; and the fringe widths of RCMA-2 are 11.01 ± 1.32 nm and 23.16 ± 1.56 nm, respectively.
[0075] The above data indicate that methacrylylation modification has no significant effect on the stripe width of the recombinant collagen assembly product. Notably, the observed light and dark stripe widths correspond to the viscous module (approximately 10 nm) and functional module (approximately 24.9 nm) in the theoretical model of collagen molecules, respectively, further verifying the ultrastructural characteristics of recombinant collagen.
[0076] Example 9: Effect of self-assembly and methacrylation sequence on the degree of amino substitution of collagen side chains The degree of substitution of amino groups on the side chains of recombinant collagen molecules was quantified by trinitrobenzenesulfonic acid (TNBS) analysis, and the results are as follows: Figure 9 As shown in the figure. Based on the fitting results of the glycine concentration standard curve, the substitution degrees of RCMA-1 and RCMA-2 were calculated to be 82% and 87%, respectively.
[0077] The above results indicate that the RCMA-2 sample has more exposed side chain amino groups, while the RCMA-1 sample may have had a relatively low substitution efficiency due to the superposition of sticky ends during the self-assembly process, which prevented the predetermined reactive groups from fully participating in the substitution reaction. This result is consistent with the theoretical results.
[0078] Example 10: Effect of self-assembly and methacrylation sequence on the macroscopic properties of recombinant collagen hydrogels RCMA-1 and RCMA-2 schematic diagrams are shown below Figure 10 As shown.
[0079] The results showed that both RCMA-1 and RCMA-2 were initially in a liquid state, tilted against the glass dish, with their liquid surfaces remaining horizontal. After adding a photocrosslinking agent and irradiating with 405 nm blue-violet visible light for 30 seconds, both samples maintained a flat meniscus interface in contact with the bottom of the glass tube. When the test tube was inverted, the samples were confirmed to have completed the gelation process, forming a hydrogel with a rigid network structure. This hydrogel adhered firmly to the base of the tube without displacement, confirming the directional controllability of mechanical stability.
[0080] Based on Example 6, the concentration of the sample before photocrosslinking was increased to 60 mg / mL, which allows the hydrogel to be picked up with tweezers. An expanded image of the hydrogel surface morphology is shown below. Figure 11 exhibit.
[0081] Example 11: Effect of self-assembly and methacrylation sequence on the mechanical properties of recombinant collagen hydrogels Tested using a rheometer, such as Figure 12 As shown, the storage modulus (G′) of RCMA-1 and RCMA-2 hydrogels is stable in the viscoelastic linear region (LVR) during strain scanning, with values of 6.8 Pa and 101 Pa, respectively, exhibiting the characteristics of viscoelastic solids.
[0082] Frequency scanning shows that G′>G′′, indicating that elasticity dominates. In the 1-100 Hz range, G′ of both increases with frequency, with RCMA-1 at 3000 Pa and RCMA-2 at 4200 Pa at 100 Hz.
[0083] Viscosity tests revealed the shear-thinning behavior of the samples. RCMA-2 exhibited higher zero-shear viscosity, stronger structural stability, and higher instantaneous stiffness under impact. Therefore, overall, RCMA-2 outperformed RCMA-1 in both storage modulus and initial shear stress, demonstrating superior mechanical properties.
[0084] Example 12: Effect of self-assembly and methacrylation sequence on the internal three-dimensional pore structure of recombinant collagen hydrogels The three-dimensional microstructures of the lyophilized RC, RCMA-1, and RCMA-2 samples were observed using scanning electron microscopy (SEM). Figure 13 As shown, at 1200× magnification, the methacrylamide-treated hydrogels (RCMA-1 / RCMA-2) exhibit higher porosity and a highly interconnected network structure compared to RC. This three-dimensional porous architecture may be more conducive to cell adhesion, proliferation, and nutrient transport. Example 13: Effect of methacrylation on the thermal stability of recombinant collagen As can be seen from Example 11, the RCMA-2 hydrogel exhibits superior mechanical properties compared to the RCMA-1 hydrogel, despite both possessing a biomimetic structure. Therefore, subsequent research will primarily focus on the RCMA-2 hydrogel.
[0085] The thermal change temperatures of recombinant collagen before and after methacrylation were investigated using circular dichroism spectroscopy, and the results are as follows: Figure 14 As shown in the figure. It can be seen from the figure that, compared to unmodified recombinant collagen RC, RCMA-2... T m It decreased slightly (by 11°C, from 53°C to 42°C), but it is still higher than the human physiological temperature of 37°C, so it can still maintain the unique triple helix structure of recombinant collagen within a certain temperature range.
[0086] Example 14: Verification of successful substitution reaction between methacrylic anhydride and the amino groups on the side chains of recombinant collagen. The successful methacrylation of recombinant collagen (RC) was confirmed by ¹H NMR and FT-IR analysis, as shown in the results. Figure 15 As shown.
[0087] 1 ¹H NMR showed that, compared to the unmodified sample, the chemically modified recombinant collagen sample exhibited new characteristic peaks around 5.4 ppm and 5.8 ppm. These peaks, compared to those reported in the literature, are methacrylamide proton peaks, indicating successful methacrylation. The FT-IR spectroscopy detection range was 4000-400 cm⁻¹. -1 Within the range, compared with the infrared spectrum of unmodified collagen, the recombinant collagen after methacrylation showed a higher intensity at 1730 cm⁻¹. -1 The characteristic peak appearing nearby is due to the formation of the amide bond C=O. At 1130 cm⁻¹ -1The new characteristic peaks appearing nearby are due to the ester groups (COC) generated after the substitution reaction of methacrylic anhydride with the amino groups on the side chains of recombinant collagen. In summary, the new characteristic peaks appearing in the chemically modified spectra by ¹H NMR and FT-IR confirm the successful insertion of methacrylic anhydride.
[0088] Example 15: Comparison of mechanical properties between RCMA-2 hydrogel and GelMA samples 1. Preparation of GelMA-1 The purchased gelatin was dissolved in 10 mmol·L⁻¹ solution at pH 7.0. -1 Phosphate buffer was prepared as a 25.9 mg / mL solution (same as 2 mM RCMA-2). Methacrylic anhydride was added at a molecular ratio of 10:1. The reaction temperature was 35℃, the shaking speed was 200 rpm·min-1, and the addition rate of methacrylic anhydride was 1.4-2 μL / min.
[0089] During the reaction, the pH was adjusted to a stable 7.4 using 200 mM NaOH. After the reaction, the reaction system was displaced with 10 times its volume of phosphate buffer to remove unreacted methacrylic anhydride and impurities. After displacement, the GelMA-1 sample was prepared to a concentration of 40 mg / mL, and a photocrosslinking agent (LAP) with a working concentration of 10 mg / mL was added. The GelMA-1 was then induced to form a hydrogel under 405 nm blue-violet visible light for 30 s.
[0090] 2. Preparation of GelMA-2 The purchased gelatin was dissolved in 10 mmol·L⁻¹ solution at pH 7.0. -1 Phosphate buffer was prepared to a concentration of 100 mg / mL. 8 mL of methacrylic anhydride was added to the gelatin solution at a rate of 0.5 mL / min. The reaction temperature was 35°C, and the shaking speed was 200 rpm·min. -1 .
[0091] During the reaction, the pH was adjusted to a stable level of 7.4 using 200 mM NaOH. After the reaction, the solution was transferred to a dialysis tube (10 kDa MWCO) and dialyzed against deionized water at 25°C for 3 days. Fresh deionized water was used daily to completely remove salts and MA. GelMA-2 was obtained by lyophilization. The sample was prepared at a concentration of 40 mg / mL, and a photocrosslinking agent (LAP) was added at a working concentration of 10 mg / mL. Exposure to 405 nm blue-violet visible light for 30 s induced the formation of a hydrogel from GelMA-2.
[0092] 3. Comparison of mechanical properties Rheological testing of RCMA-2, GelMA-1 and GelMA-1 as follows Figure 16 As shown, the results indicate that RCMA-2 and GelMA-2 exhibit typical viscoelastic solid properties, with storage modulus (G′) significantly higher than dissipation modulus (G′′) within the LVR (G′ being 102 Pa and 417 Pa, respectively). RCMA-2 withstands a critical strain of 40%, while GelMA-2 withstands a strain as high as 300%.
[0093] Frequency scanning revealed that at 100 Hz, both RCMA-2 and GelMA-2 exhibited a G′ of ~3000 Pa, forming a stable elastic network, while GelMA-1, due to G′′>G′, consistently remained a viscous solution. Viscosity tests showed that all three exhibited significant shear-thinning behavior, with viscosity decreasing as the shear rate increased.
[0094] In summary, GelMA-2 exhibits the highest mechanical strength, followed by RCMA-2, with GelMA-1 being the weakest. Particularly noteworthy is that, at the same initial reaction concentration, RCMA-2 demonstrates superior mechanical properties compared to GelMA-1, indicating its potential application in tissue engineering.
[0095] Example 16: 3D Printed Model Successfully printed general-purpose supports such as triangles, pentagons, hexagons, and cylinders, as well as complex structures such as hearts, pentagrams, and serrated edges. Figure 17 As shown, the high printability of RCMA-2 ink in DLP 3D printing was verified. Its uniformity was further evaluated by adding riboflavin and methylene blue dye. All experiments demonstrated that RCMA-2 possesses stable printing performance and can be used as a reliable bio-ink for DLP 3D printing.
[0096] Example 17: Cytotoxicity of methacrylated recombinant collagen hydrogel The in vitro cytotoxicity of RCMA-1 and RCMA-2 hydrogels was evaluated using the CCK-8 assay. Figure 18 (As shown in Figures B and C). NIH-3T3 cells were cultured in two different hydrogel extracts for 24 hours, and the cell viability of all groups exceeded 100%, indicating that RCMA hydrogel has excellent biocompatibility.
[0097] To verify the cell proliferation capacity within the RCMA hydrogel, live / dead cell staining and CCK-8 assay were performed. Figure 18 A, Figure 18 D), NIH-3T3 cells (approximately 2 × 10⁻⁶) 4 Cells / mL were cultured in a medium containing hydrogel extract. Live / dead staining fluorescence imaging showed a significant increase in cell density over time. Figure 18 A), CCK-8 experiment ( Figure 18D) Further confirmation showed that cell activity in both hydrogel groups increased in a time-dependent manner within 1-5 days. The results consistently indicated that both RCMA-1 and RCMA-2 hydrogels exhibited excellent biocompatibility and significantly promoted cell proliferation.
[0098] The sequence involved in this invention: SEQ ID NO.1: Amino acid sequence of V-domain ADEQEEKAKVRTELIQELAQGLGGIEKKNFPTLGDEDLDHTYMTKLLTYLQEREQAENSWRKRLLKGIQDHALD SEQ ID NO.2: Amino acid sequence of collagen domain B GPRGEQGPQGLPGKDGEAGAQGPAGPMGPAGFPGERGEKGEPGTQGAKGDRGETGPVGPRGERGEAGPAGKDGERGPVGPA SEQ ID NO.3: (GPP) 10 amino acid sequence GPPGPPGPPGPPGPPGPPGPPGPPGPPGPP SEQ ID NO.4: Amino acid sequence of V-P10BP10 ADEQEEKAKVRTELIQELAQGLGGIEKKNFPTLGDEDLDHTYMTKLLTYLQEREQAENSWRKRLLKGIQDHALDLVPRGSPGPPGPPGPPGPPGPPGPPGPPGPPGPPGPP GPRGEQGPQGLPGKDGEAGAQGPAGPMGPAGFPGERGEKGEPGTQGAKGDRGETGPVGPRGERGEAGPAGKDGERGPVGPAGPPGPPGPPGPPGPPGPPGPPGPPGPPGPPG SEQ ID NO.5: Nucleotide sequence of V-P10BP10 GCAGACGAACAGGAAGAGAAAGCCAAAGTGCGCACCGAGCTGATTCAGGAACTGGCACAGGGCCTGGGCGGCATTGAAAAGAAGAATTTCCCGACCCTGGGCGATGAGGACCTGGACCACACCTATATGACCAAGCTGCTGACCTACCTGCAGGAACGCGAGCAGGC CGAAAATAGCTGGCGTAAGCGCCTGCTGAAAGGCATTCAGGATCATGCCCTGGATCTGGTTCCGCGTGGTAGCCCTGGTCCGCCGGGCCCGCCGGGCCCTCCGGGCCCGCCGGGTCCGCCGGGTCCGCCGGGCCCGCCGGGCCCTCCGGGTCCGCCGGGCCCGCCGG GTCCGCGTGGTGAACAGGGTCCGCAGGGTCTGCCGGGTAAGGACGGTGAAGCAGGTGCACAGGGTCCTGCAGGCCCTATGGGTCCGGCAGGTTTTCCGGGTGAACGCGGTGAAAAAGGCGAACCGGGTACCCAGGGTGCAAAAGGTGATCGTGGCGAAACAGGTCCG GTTGGCCCTCGTGGTGAACGTGGTGAGGCAGGTCCGGCCGGCAAAGATGGTGAGCGCGGTCCTGTTGGTCCGGCAGGTCCGCCGGGTCCGCCGGGTCCGCCGGGTCCGCCTGGTCCGCCGGGTCCGCCGGGTCCGCCGGGTCCGCCGGGTCCGCCGGGTCCCGCCGGGT Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.
Claims
1. A method for preparing recombinant collagen with the ability to self-assemble layered fibers, characterized in that, Including the following steps: Methacrylic anhydride was added to the recombinant collagen solution at a rate of 1.4~2 μL / min, and the reaction and displacement were carried out to obtain recombinant collagen with the ability to self assemble layered fibers. The molar ratio of methacrylic anhydride to amino groups in recombinant collagen is 8-12:
1.
2. The method according to claim 1, characterized in that, Recombinant collagen has the following structure: From the N-terminus to the C-terminus, the sequence consists of the first repeat sequence, the collagen domain, and the second repeat sequence. Optionally, the amino acid sequences of the first repeat sequence and the second repeat sequence are as shown in SEQ ID NO.3; Optionally, the amino acid sequence of the collagen domain is shown in SEQ ID NO.
2.
3. The method according to any one of claims 1 to 2, characterized in that, The recombinant collagen also has a folded domain attached to its N-terminus; the amino acid sequence of the folded domain is shown in SEQ ID NO.1; Optionally, there is an enzyme cleavage site between the folded domain and the first repeat sequence, and the amino acid sequence of the enzyme cleavage site is LVPRGSP.
4. The method according to any one of claims 1 to 3, characterized in that, The reaction temperature was 35~40 ℃, the rotation speed was 200~220 rpm, and the pH was 7.0~7.
4.
5. Recombinant collagen with layered fiber self-assembly ability prepared by the method according to any one of claims 1 to 4.
6. A recombinant collagen hydrogel, characterized in that, It is prepared from the recombinant collagen with layered fiber self-assembly capability as described in claim 5; Optionally, the recombinant collagen hydrogel is prepared by: dissolving recombinant collagen in a buffer solution, adding methacrylic anhydride, and reacting to obtain methacrylic anhydride-modified recombinant collagen; using buffer replacement and self-assembly to obtain methacrylamide-self-assembled recombinant collagen; adding a photocrosslinking agent to form a recombinant collagen hydrogel through photocrosslinking.
7. The application of the recombinant collagen with layered fiber self-assembly capability as described in claim 5 or the recombinant collagen hydrogel as described in claim 6 in the fields of biology, food, chemical industry, medicine, biomaterials, tissue engineering, or cosmetics.
8. The application according to claim 7, characterized in that, The applications include: using recombinant collagen with the ability to self-assemble layered fibers to prepare drug delivery materials, three-dimensional scaffold materials, hemostatic materials, tissue filler materials, and biosensors.
9. A recombinant collagen product, characterized in that, The product contains the recombinant collagen with layered fiber self-assembly capability as described in claim 5 or the recombinant collagen hydrogel as described in claim 6.
10. A method for improving the mechanical properties of recombinant collagen hydrogels while maintaining the triple helix structure and layered fiber self-assembly ability of recombinant collagen, characterized in that, Hydrogels were prepared using methacrylated recombinant collagen, including: Methacrylic anhydride was added to the recombinant collagen solution at a rate of 1.4~2 μL / min, and the reaction and displacement were carried out to obtain recombinant collagen with the ability to self assemble layered fibers. The molar ratio of methacrylic anhydride to amino groups in recombinant collagen is 10:1.