A eucalyptus-based high-pressure hard carbon anode material and its thermo-mechanical coupling densification preparation method

By employing a thermo-mechanical coupling densification method, the problems of low density and low initial efficiency of eucalyptus-based hard carbon materials were solved, and high-density hard carbon materials were prepared, thereby improving the volumetric energy density and electrochemical performance of sodium-ion batteries.

CN122520032BActive Publication Date: 2026-11-10WUZHOU TONGCHUANG NEW ENERGY MATEIALS CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610608047.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-05-06
Publication Date
2026-11-10
Estimated Expiration
2046-05-06

AI Technical Summary

Technical Problem

Existing technologies for preparing eucalyptus-based hard carbon materials suffer from low tap density and compaction density, resulting in insufficient volumetric energy density and low initial efficiency in sodium-ion batteries. Existing methods offer limited improvement or may even impair electrochemical performance.

Method used

A thermo-mechanical coupling densification method was adopted to prepare eucalyptus-based high-pressure hard carbon anode material by hot-pressing a pre-carbonized eucalyptus intermediate under specific temperature and pressure conditions, combined with acid washing and high-temperature carbonization. The densification of the material was achieved by utilizing the specific fiber structure and lignin/cellulose ratio of eucalyptus.

Benefits of technology

The material significantly improves the tap density of hard carbon powder and the compaction density of electrode sheets, thereby increasing the initial coulombic efficiency. It exhibits good rate performance and cycle stability at high current densities, making it suitable for high volumetric energy density sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of electrode material technology, and relates to a eucalyptus-based high-pressure hard carbon anode material and its thermo-mechanical coupling densification preparation method. The method includes: cleaning, drying, crushing, and sieving eucalyptus wood, followed by pre-carbonization at 400-650℃ under inert gas protection to obtain a eucalyptus pre-carbonized intermediate; placing the intermediate into a mold, heating to 180-450℃ under inert gas protection and applying a pressure of 5-80 MPa for thermo-mechanical coupling densification treatment, followed by crushing, grinding, acid washing to remove impurities, drying, and then high-temperature carbonization at 1000-1600℃ to obtain the eucalyptus-based high-pressure hard carbon anode material. This invention utilizes the plasticity of the eucalyptus pre-carbonized intermediate within a specific temperature window, and significantly improves the tap density and electrode compaction density of the hard carbon material through hot-press densification, while effectively reducing the specific surface area, thereby simultaneously improving the initial coulombic efficiency and endowing the material with excellent rate performance and cycle stability, making it suitable for high volumetric energy density sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrode material technology, and relates to a eucalyptus-based high-pressure hard carbon anode material and its thermo-mechanical coupling densification preparation method. Background Technology

[0002] Sodium-ion batteries have shown great promise in large-scale energy storage due to their abundant resources and low cost. Hard carbon materials, with their suitable sodium storage platform and high specific capacity, are considered one of the most promising anode materials for sodium-ion batteries. Currently, hard carbon materials are mostly prepared by using various biomass (such as coconut shells, bamboo, straw, walnut shells, etc.) as precursors through high-temperature carbonization.

[0003] Eucalyptus, a fast-growing, high-yielding, and widely planted forest tree, produces processing residues (such as sawdust) that are potential high-quality hard carbon precursors, offering advantages such as wide availability, low cost, high carbon content, and relatively controllable ash content. However, regardless of whether eucalyptus or other biomass is used, existing technologies for preparing hard carbon generally suffer from a key drawback: low tap density and compacted density. This directly leads to low capacity per unit volume of the electrode, severely limiting the volumetric energy density of sodium-ion batteries.

[0004] Existing methods for increasing hard carbon density (such as optimizing the carbonization process and mechanically compressing the final carbon powder) often have limited effectiveness or impair electrochemical performance (such as reducing initial efficiency and damaging the structure). In particular, for specific raw materials like eucalyptus, there is no effective method to simultaneously address the related issues of low density and low initial efficiency by introducing a specific physical field during the critical intermediate stage of its conversion into hard carbon.

[0005] Therefore, for eucalyptus, a specific and promising biomass raw material, how to significantly improve the compaction density of its derived hard carbon materials without sacrificing its inherent electrochemical performance advantages, so as to prepare a negative electrode material with excellent comprehensive performance suitable for high volumetric energy density sodium-ion batteries, has become an urgent problem to be solved. Summary of the Invention

[0006] To address the aforementioned problems, this invention provides a eucalyptus-based high-pressure hard carbon anode material and its thermo-mechanical coupling densification preparation method, specifically including the following steps:

[0007] Step 1: The eucalyptus wood is washed, dried, crushed and sieved in sequence to obtain eucalyptus wood powder with a particle size of 50-500 mesh. Under the protection of inert gas, the temperature is raised to 400-650℃ at a heating rate of 1-10℃ / min and held for 0.5-4h to obtain eucalyptus pre-carbonized intermediate. During this stage, lignin and other components undergo pyrolysis and preliminary aromatization.

[0008] Preferably, the eucalyptus wood includes, but is not limited to, eucalyptus sawdust, branches, trunks, and other processing residues.

[0009] Preferably, the particle size of the eucalyptus wood powder is 100-300 mesh.

[0010] Preferably, the heating rate is 2-5℃ / min.

[0011] Preferably, the temperature is 450-550℃.

[0012] Preferably, keep warm for 1-2 hours.

[0013] Step 2: The eucalyptus pre-carbonized intermediate is loaded into a mold, and under the protection of inert gas, a pressure of 5-80 MPa is applied and heated to 180-450℃. The temperature and pressure are maintained for 0.5-5 hours, and then the pressure is released and cooled to obtain a densified block.

[0014] The densified bulk material is mechanically crushed and ground, then mixed with acid at a ratio of 1g:(2-15)mL. The mixture is stirred at 60-90℃ for 2-6 hours to remove potassium, calcium and other ash. The material is then washed with deionized water until neutral, dried, placed in a tube furnace, and heated to 1000-1600℃ at a rate of 1-10℃ / min under inert gas protection. The temperature is maintained for 1-6 hours, and the material is naturally cooled to obtain eucalyptus-based high-pressure hard carbon anode material.

[0015] Preferably, the acid solution is a 1-5 mol / L hydrochloric acid aqueous solution or a sulfuric acid aqueous solution, and most preferably a 1-2 mol / L hydrochloric acid aqueous solution.

[0016] Preferably, the pressure is 10-30 MPa.

[0017] Preferably, the temperature is heated to 250-350℃.

[0018] Preferably, heat preservation and pressure maintenance should be carried out for 1-2 hours.

[0019] Preferably, the heating rate is 2-5℃ / min.

[0020] Preferably, the temperature is raised to 1200-1400℃.

[0021] Preferably, keep warm for 2-4 hours.

[0022] The present invention has the following advantages:

[0023] (1) High compaction density and high tap density: The tap density of the hard carbon powder prepared by this method can be significantly improved, which in turn enables the electrode sheet prepared by it to achieve a higher compaction density under the same rolling process, which directly helps to improve the volumetric energy density of sodium-ion batteries.

[0024] (2) Improve the first coulombic efficiency: While achieving the increase in density, the first charge and discharge coulombic efficiency of the material is also improved simultaneously.

[0025] (3) Excellent rate performance and cycle stability: The material has good capacity retention at high current densities and stable long-term cycle performance.

[0026] The above advantages come from:

[0027] Advantages (1) (High density): mainly derived from the biomass precursors provided by eucalyptus with specific fiber structure and lignin / cellulose ratio; thermo-mechanical coupling densification is carried out at a specific stage, and the plasticity of eucalyptus pre-carbonized intermediates at a specific temperature window is utilized to achieve effective compression of the structure through pressure.

[0028] Advantage (2) (High initial efficiency): This mainly stems from the fact that the hot-pressing densification process effectively reduces macropores and mesopores in the material, thereby significantly reducing the specific surface area. A lower specific surface area means that during the first charge and discharge process, there are fewer active sites that react with the electrolyte to form a solid electrolyte interphase (SEI) film, reducing irreversible sodium consumption and thus improving the initial coulombic efficiency. The low ash content of eucalyptus raw materials and their high purity after acid washing also provide a basis for this.

[0029] Advantages (3) (Good rate and cycle performance): Carbon materials derived from eucalyptus trees usually have a carbon layer structure suitable for sodium ion insertion / extraction. Moderate hot pressing conditions avoid serious damage to the carbon skeleton and maintain the structural integrity and ion transport channels of the material. Detailed Implementation

[0030] The technical solutions in the embodiments of the invention are described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] Example 1

[0032] Step 1: The eucalyptus wood chips are washed, dried, crushed, and sieved through a 200-mesh sieve. Then, under argon protection, the temperature is increased to 500°C at a rate of 5°C / min and held for 2 hours to obtain the eucalyptus pre-carbonized intermediate.

[0033] Step 2: The eucalyptus pre-carbonized intermediate is loaded into a mold, and under argon protection, a pressure of 20 MPa is applied and heated to 300°C. The temperature and pressure are maintained for 2 hours, then the pressure is released, cooled, crushed, and ground. It is then mixed with 1 mol / L hydrochloric acid aqueous solution at a ratio of 1 g: 9 mL, stirred at 80°C for 4 hours, washed with deionized water until neutral, dried, placed in a tube furnace, and heated to 1300°C at a heating rate of 5°C / min under argon protection. The temperature is maintained for 3 hours, and after natural cooling, the eucalyptus-based high-pressure hard carbon anode material E-S1 is obtained.

[0034] Example 2

[0035] The difference from Example 1 is that a pressure of 10 MPa was applied and heated to 250°C, and the temperature and pressure were maintained for 1.5 hours to obtain eucalyptus-based high-pressure hard carbon anode material E-S2.

[0036] Example 3

[0037] The difference from Example 1 is that a pressure of 30 MPa was applied and heated to 350°C, and the temperature and pressure were maintained for 2.5 hours to obtain eucalyptus-based high-pressure hard carbon anode material E-S3.

[0038] Comparative Example 1

[0039] The difference from Example 1 is that the hot pressing densification operation is not performed, that is, the heating and pressure application steps are not performed, resulting in hard carbon material E-D1.

[0040] Comparative Example 2

[0041] The difference from Example 1 is that the original amount of coconut shells was used to obtain hard carbon material C-S1.

[0042] Comparative Example 3

[0043] First, hard carbon material E-D1 was prepared according to the method of Comparative Example 1. It was then pressed into sheets by applying a pressure of 20 MPa at room temperature, and then crushed, ground and sieved to obtain hard carbon material E-D2.

[0044] Experimental Example 1

[0045] The tap density, electrode compaction density, specific surface area, initial coulombic efficiency, and reversible capacity of Examples 1-3 and Comparative Examples 1-3 were tested respectively.

[0046] Tap density test:

[0047] Instrument: Tap density meter (if conforming to GB / T 5162 or ASTM B527 standards).

[0048] Procedure: Take a sample of a certain mass (e.g., 10.00 g) and pour it into a clean, dry graduated cylinder. Fix the cylinder on a tapped density meter and vibrate it at a fixed frequency and height until the powder volume no longer changes significantly. Record the final volume. Tapped density = Powder mass (g) / Tapped volume (cm³) 3 Each sample was tested three times and the average value was taken.

[0049] Electrode preparation and compaction density testing:

[0050] Electrode slurry preparation: The sample, conductive agent (Super P), and binder (sodium carboxymethyl cellulose CMC and styrene-butadiene rubber SBR) were mixed at a mass ratio of 8:1:1. Deionized water was added as a solvent, and the mixture was thoroughly stirred on a planetary mixer until a homogeneous slurry was formed. The slurry was evenly coated onto a copper foil current collector and dried in an oven at 80°C for at least 12 hours. The dried electrode sheets were then rolled using a roller press under a pressure of 15 MPa. They were then punched into 12 mm diameter discs using a precision punching machine, and the mass (m) of each electrode sheet was weighed using a precision balance.

[0051] Thickness and compaction density calculation: Measure the thickness (h) and diameter (d) of the rolled electrode sheet (excluding the copper foil thickness) using a micrometer. Compaction density = m / [π×(d / 2)] 2 ×h).

[0052] Specific surface area and pore size analysis:

[0053] Instrument: Physical adsorption apparatus (Micromeritics ASAP 2460).

[0054] Procedure: Approximately 0.1 g of sample was taken and degassed under vacuum at 120°C for 6 h to remove surface adsorbates. Nitrogen adsorption-desorption tests were then performed at liquid nitrogen temperature (77 K). The specific surface area was calculated using the BET (Brunauer-Emmett-Teller) model.

[0055] Electrochemical performance testing (assembling a CR2032 coin cell)

[0056] 1. Battery assembly (performed in an argon-filled glove box):

[0057] Working electrode: the hard carbon electrode sheet prepared above.

[0058] Counter electrode / reference electrode: Sodium metal sheet.

[0059] Diaphragm: Glass fiber diaphragm (such as Whatman GF / D).

[0060] Electrolyte: 1M NaPF6 dissolved in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio 1:1), with 5% fluoroethylene carbonate (FEC) added.

[0061] Assembly sequence: negative electrode shell → hard carbon electrode sheet → electrolyte (add appropriate amount) → separator (wet with electrolyte) → sodium sheet → gasket → spring sheet → positive electrode shell. Tighten and seal using a button cell sealing machine.

[0062] 2. Electrochemical testing:

[0063] Testing equipment: LAND or LAND series battery testing system.

[0064] First Coulomb efficiency test:

[0065] Charge / discharge procedure: After standing for 10 minutes, discharge at a constant current density of 0.1C (1C=300mA / g) to 0.01V, then discharge at a constant voltage at that potential until the current drops to 0.01C, and record the discharge capacity (initial sodium intercalation capacity). Subsequently, charge at a constant current of 0.1C to 2.0V, and record the charging capacity (initial sodium deintercalation capacity).

[0066] Calculation: Initial Coulomb efficiency = (Initial charge capacity / Initial discharge capacity) × 100%.

[0067] Reversible capacity:

[0068] After the first charge and discharge cycle, the battery was subjected to constant current charge and discharge test at a current density of 0.1C, and the stable reversible capacity at 0.1C was recorded after 5 cycles.

[0069] Table 1 Experimental Results

[0070] Tap density Electrode compaction density Specific surface area First Coulomb efficiency Reversible capacity <![CDATA[(g / cm 3 )]]> <![CDATA[(g / cm 3 )]]> <![CDATA[(m 2 / g)]]> (%) (mAh / g, 0.1C) E-S1 0.86 1.26 8.5 89.5 313 E-S2 0.79 1.19 10.8 91.8 309 E-S3 0.87 1.27 8.0 90.0 315 E-D1 0.69 1.01 16.0 82.0 320 C-S1 0.82 1.20 9.2 86.0 290 E-D2 0.76 1.08 19.5 78.5 298

[0071] Table 1 shows that, compared to E-S1 and E-D1, when using the same eucalyptus raw materials, introducing a hot-pressing step significantly improves density and initial efficiency. Comparing E-S1 and C-S1, even with the same hot-pressing process, the final material properties differ depending on the raw materials, indicating that using eucalyptus as a precursor combined with this hot-pressing process can produce specific and superior overall effects (such as higher compaction density and volume). E-S1 is superior to E-D2, which involves post-processing eucalyptus carbonized material, in both density and initial efficiency, proving that "hot pressing during the pre-carbonization and plasticization stage" has a fundamental advantage over "post-pressing of hard and brittle carbon powder." Examples 1-3 show the adjustable range and optimization direction of hot-pressing parameters (temperature, pressure), and the parameters in Example 1 (300℃, 20MPa) show a good balance in the eucalyptus system.

[0072] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for thermo-mechanical coupling densification of a eucalyptus-based high-pressure hard carbon anode material, characterized in that, Includes the following steps: Step 1: The eucalyptus wood is washed, dried, crushed and sieved in sequence. Under the protection of inert gas, it is heated to 400-650℃ at a heating rate of 1-10℃ / min and held at that temperature for 0.5-4h to obtain the eucalyptus pre-carbonized intermediate. Step 2: The eucalyptus pre-carbonized intermediate is loaded into a mold and subjected to a pressure of 5-80 MPa at 180-450℃ under inert gas protection for 0.5-5 hours. It is then crushed and ground, mixed with acid solution at a ratio of 1g:(2-15)mL, stirred at 60-90℃ for 2-6 hours, washed and dried, and placed under inert gas protection. The temperature is then increased to 1000-1600℃ at a rate of 1-10℃ / min and held for 1-6 hours. After natural cooling, the eucalyptus-based high-pressure hard carbon anode material is obtained.

2. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, The heating rate described in steps one and two is 2-5℃ / min.

3. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, The temperature in step one is 450-550℃.

4. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, Keep warm for 1-2 hours in step one.

5. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, The acid solution mentioned in step two is a 1-5 mol / L hydrochloric acid aqueous solution or sulfuric acid aqueous solution.

6. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 5, characterized in that, The acid solution is a 1-3 mol / L hydrochloric acid aqueous solution.

7. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, The pressure mentioned in step two is 10-30 MPa.

8. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, In step two, heat to 250-350℃.

9. The thermo-mechanical coupling densification preparation method of a eucalyptus-based high-pressure hard carbon anode material according to claim 1, characterized in that, In step two, the temperature is raised to 1200-1400℃ and held for 2-4 hours.

10. Eucalyptus-based high-pressure hard carbon anode material prepared by the method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Preparation method of sodium ion battery negative electrode based on eucalyptus derived hard carbon

    CN120749122A

  • Hard carbon negative electrode active material and preparation and application thereof

    CN121134726A