Corrosion Test Method for Hot-Dip Galvanized Steel Pipes
By constructing multi-field coupled corrosion test conditions, the problem of a single corrosion test environment for hot-dip galvanized steel pipes in the existing technology is solved. This enables the analysis of the unique failure mechanism of the zinc layer under multi-field coupled environment, and improves the guiding value of the test results and the ability to optimize the process.
Patent Information
- Application Number
- CN202611071230.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-07-20
AI Technical Summary
Existing corrosion testing methods for hot-dip galvanized steel pipes fail to simultaneously consider the multi-field coupling effects of the internal gas pipeline medium, external soil medium, and operating stress on corrosion behavior. Furthermore, corrosion data is disconnected from process parameters, making it difficult to optimize the galvanizing process and predict service life.
Multi-field coupled corrosion test conditions were constructed, including gas medium inside the pipe, soil medium outside the pipe, and stress corrosion environment. By applying predetermined stress to the sample and measuring the corrosion rate and electrochemical performance, the mapping relationship between galvanizing process parameters, zinc layer thickness grade and corrosion performance was established.
This improved the environmental realism and acceleration rate of corrosion tests, revealed the unique failure mechanism of zinc layers under multi-field coupling environments, and provided a theoretical basis for process optimization and lifetime prediction.
Smart Images

Figure CN122591534B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of corrosion testing technology, and more specifically, relates to a corrosion testing method for hot-dip galvanized steel pipes. Background Technology
[0002] Hot-dip galvanized steel pipes are widely used in urban gas pipeline construction due to their excellent corrosion resistance and relatively economical cost. During the service life of gas pipelines, the inner and outer walls of the steel pipes are simultaneously subjected to different corrosive environments: the inner wall is in long-term contact with the transported medium (gas containing corrosive components such as CO2, H2S, and water vapor), while the outer wall is buried in a complex and variable soil environment (affected by factors such as acidity, alkalinity, moisture content, and salinity). Simultaneously, the pipe wall is subjected to continuous stress under operating internal pressure and external loads. The coupling effect of these multiple factors leads to complex corrosion behavior of the galvanized layer, and the corrosion mechanism differs significantly from that in a single atmospheric or soil environment.
[0003] Currently, corrosion testing methods for hot-dip galvanized steel pipes mainly focus on general atmospheric environment corrosion simulation. For example, existing technologies have disclosed accelerated corrosion testing methods for simulating hot-dip galvanized steel corrosion in inland industrial atmospheric environments, employing an alternating cycle of sulfur dioxide corrosion testing and humidity testing; similarly, methods for simulating accelerated corrosion testing of hot-dip galvanized steel in coastal industrial atmospheric environments have been disclosed, using alternating cycles of sulfur dioxide corrosion testing and salt spray, dry, and humidity corrosion testing. However, these existing methods all simulate a single external atmospheric environment and fail to simultaneously consider the multi-field coupling effects of the internal transport medium of the gas pipeline, the external soil medium, and operating stress on corrosion behavior.
[0004] Furthermore, the corrosion data established by existing accelerated corrosion testing methods are mostly isolated environmental-corrosion rate correspondences. They do not systematically correlate corrosion data with hot-dip galvanizing process parameters (such as galvanizing temperature, immersion time, alloy composition, etc.) and zinc layer structural characteristics (such as thickness grade, alloy layer morphology). As a result, the test results are difficult to use to optimize and improve the galvanizing process, and cannot provide differentiated life prediction basis for gas pipeline networks under different service conditions. Summary of the Invention
[0005] The purpose of this application is to provide a corrosion testing method for hot-dip galvanized steel pipes, so as to solve the technical problems in the prior art where the corrosion testing environment for hot-dip galvanized steel pipes for gas pipelines is singular and the corrosion data is disconnected from the process parameters.
[0006] To achieve the above objectives, the technical solution adopted in this application is: to provide a corrosion test method for hot-dip galvanized steel pipes, comprising: S1: Obtain hot-dip galvanized steel pipe samples for gas pipelines produced by different galvanizing process parameters, determine the zinc layer thickness grade and characterize the zinc layer microstructure of each sample, and divide the samples into multiple thickness grade groups according to the zinc layer thickness. S2: Construct multi-field coupled corrosion test conditions that simultaneously cover the corrosion environment of gas medium inside the pipe, the corrosion environment of soil medium outside the pipe, and the stress corrosion environment. Place the samples of each thickness grade group under the multi-field coupled corrosion test conditions for accelerated corrosion, and take out the samples in batches at predetermined time intervals. The corrosion environment of the gas medium inside the pipe includes acidic gas components and moisture that are corrosive to the zinc layer, the corrosion environment of the soil medium outside the pipe includes simulated soil with different pH, water content and salt content, and the stress corrosion environment is achieved by applying stress in a predetermined direction to the sample. S3: The corrosion rate of the extracted samples was measured, the electrochemical corrosion performance was tested, and the microstructure and composition of the corrosion products were analyzed. Based on the analysis results, the delamination failure characteristics and failure evolution law of zinc layers of different thickness grades under the multi-field coupled corrosion test conditions were determined. S4: Link and store the galvanizing process parameters, zinc layer thickness grade, corrosion test condition parameters, measured corrosion rate and corresponding delamination failure characteristics of each sample to establish a corrosion data set for characterizing the mapping relationship between process, structure and corrosion performance.
[0007] In one possible implementation, in S2, the corrosive environment of the gas medium inside the pipe and the corrosive environment of the soil medium outside the pipe act on the sample in an alternating cycle. In one alternating cycle, the inner wall of the sample is first exposed to the corrosive environment of the gas medium inside the pipe while the outer wall is isolated from the simulated soil. Then, the outer wall of the sample is buried in the simulated soil while the inner wall is no longer exposed to the corrosive environment of the gas medium inside the pipe. This alternating cycle is repeated until the accelerated corrosion test ends.
[0008] In one possible implementation, in S2, the stress corrosion environment is constructed by applying a periodically varying internal pressure load to the inner cavity of the sample. The internal pressure load oscillates between a predetermined lower pressure limit and a predetermined upper pressure limit according to a set waveform, so as to simultaneously simulate the effect of pressure fluctuations during the operation of a gas pipeline on the corrosion behavior of the zinc layer.
[0009] In one possible implementation, during the accelerated corrosion process of S2, for each thickness grade group, when the first visible corrosion red rust spot appears on the zinc layer surface of any sample in that group, the moment when the first visible corrosion red rust spot appears is recorded as the initial corrosion start time of that thickness grade group, and this initial corrosion start time is used as the basis for adjusting the sample removal frequency of that group in subsequent accelerated corrosion tests.
[0010] In one possible implementation, in S3, the failure evolution law is determined by classifying the samples taken from each batch into the early corrosion stage, the intermediate corrosion stage, and the late corrosion stage according to the chronological order, and making a longitudinal comparison of the delamination failure characteristics of samples in different corrosion stages within the same thickness grade group to identify the movement trajectory of the corrosion front that advances layer by layer from the zinc layer surface inward.
[0011] In one possible implementation, during the longitudinal comparison process, if the incremental advance depth of the corrosion front between two adjacent corrosion stages of a certain thickness grade group continues to increase, then the zinc layer of that thickness grade is determined to have entered the corrosion acceleration stage; if the incremental advance depth continues to decrease, then the zinc layer of that thickness grade is determined to have entered the corrosion decay stage; based on the determination result, the corrosion process of the thickness grade group is divided into the initial incubation stage, the accelerated expansion stage, and the decay stabilization stage.
[0012] In one possible implementation, in S3, the microstructure and composition analysis of the corrosion products further includes observing the interface morphology between the corrosion product layer and the remaining zinc layer, and determining whether the corrosion type of the zinc layer of this thickness is uniform corrosion or localized corrosion based on the degree of undulation of the interface profile; when it is determined to be localized corrosion, the depth and opening size of the localized corrosion pit are further measured, and the localized corrosion sensitivity coefficient of the zinc layer is calculated based on the depth and opening size.
[0013] In one possible implementation, in S3, after completing the layered failure characteristic analysis of all thickness grade groups, a horizontal comparison is made between the failure evolution laws of different thickness grade groups. Based on the horizontal comparison results, the corrosion test duration corresponding to the first exposure of the alloy layer in the zinc layer in each thickness grade group is identified, and this duration is marked as the critical time for protective failure of the zinc layer of that thickness grade.
[0014] In one possible implementation, in S4, after establishing the corrosion data set, the following is also performed: normalizing the corrosion rate of each thickness grade group with the corresponding initial zinc layer thickness to obtain the corrosion rate ratio per unit zinc layer thickness, and performing a multiple regression correlation between this ratio and the zinc bath temperature and immersion time in the corresponding zinc plating process parameters to obtain a ranking of the influence factors describing the degree of influence of process parameters on the corrosion rate per unit thickness.
[0015] One possible implementation also includes: S5: Obtain the actual galvanizing process parameter records and preset service life requirements of each pipe section in the target gas pipeline network, match the corrosion rate data corresponding to the actual galvanizing process parameters from the corrosion data set, and determine whether the corrosion margin of the pipe section is sufficient under the preset service life requirements based on the matching results. If it is insufficient, provide process improvement suggestions for adjusting the zinc bath temperature or immersion time in the galvanizing process parameters of the pipe section.
[0016] The beneficial effects of the corrosion test method for hot-dip galvanized steel pipes provided in this application are as follows: Compared with the prior art, the corrosion test method for hot-dip galvanized steel pipes in this application firstly involves sample preparation and grouping steps. By obtaining gas pipe samples produced with different galvanizing process parameters (such as zinc bath temperature, immersion time, alloy composition, etc.), the zinc layer thickness grade and microstructure characterization of each sample are determined, and the samples are divided into multiple grade groups according to thickness, thereby incorporating galvanizing production variables into the scope of investigation at the source of the test.
[0017] Then, an accelerated corrosion test was conducted, constructing a three-field coupled test condition that simultaneously covers the corrosion environment of the gas medium inside the pipe (including acidic gas components and moisture that are corrosive to the zinc layer), the corrosion environment of the soil medium outside the pipe (including simulated soils with different pH, moisture content and salinity), and the stress corrosion environment (applying stress to the sample in a predetermined direction). Samples of each thickness grade were placed in this environment for accelerated corrosion and were taken out in batches at predetermined time intervals. This step is a comprehensive simulation scheme designed for the actual service conditions of gas pipes, including the contact of the inner wall of the pipe with corrosive gas medium, the outer wall of the pipe being buried in a complex soil environment and the continuous stress of the pipe wall under the action of internal pressure and external loads. It overcomes the limitation of simulating only a single atmospheric environment. By simultaneously superimposing the three fields of the chemical medium inside the pipe, the electrochemical medium of the soil outside the pipe and the mechanical load, the environmental realism and acceleration rate of the accelerated corrosion test are significantly improved.
[0018] Next, the failure mechanism analysis step is carried out. The extracted samples are subjected to corrosion rate measurement, electrochemical corrosion performance test and microstructure and composition analysis of corrosion products. Based on this, the delamination failure characteristics and failure evolution law of zinc layers of different thicknesses under multi-field coupling conditions are determined. This step is different from the existing technology that only focuses on the overall corrosion rate of zinc layer. Instead, it examines the differentiated response behavior of each layer of zinc layer from the outside to the inside (outer zinc layer, intermediate alloy layer, inner coating substrate interface) during the corrosion process, thereby revealing the unique failure mechanism of high-thickness zinc layers in the multi-field coupling environment of gas.
[0019] Finally, a database was constructed to associate and store the galvanizing process parameters, zinc layer thickness grades, corrosion test conditions, measured corrosion rates, and corresponding delamination failure characteristics of each sample, thus establishing a corrosion data set for characterizing the mapping relationship between process, structure, and corrosion performance.
[0020] This approach identifies structural differences in samples at the source of the process and exposes these differences in corrosion behavior under multi-field coupled conditions. Corrosion behavior is then deconstructed into the differentiated failure contributions of each layer structure. Finally, a systematic data mapping relationship is established between process parameters, structural characteristics, and corrosion performance. By constructing a corrosion test environment that couples the gas inside the pipe, the soil outside the pipe, and stress, the accelerated corrosion test conditions more closely resemble the actual internal and external comprehensive service environment of gas pipelines, significantly improving the guiding value of the test results for actual operating conditions. Through layered failure characteristic analysis of zinc layers of different thicknesses, the differentiated failure behavior and interaction laws of each layer structure during the corrosion process can be systematically elucidated, providing a theoretical basis for optimizing the anti-corrosion design of high-thickness zinc layers. By establishing a systematic correlation database of galvanizing process parameters, zinc layer structural characteristics, and corrosion performance, corrosion test results can be directly fed back from back-end failure evaluation to front-end process optimization. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 A flowchart illustrating the corrosion testing method for hot-dip galvanized steel pipes provided in this application embodiment. Detailed Implementation
[0023] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of this application.
[0024] It should be noted that when a component is referred to as being "fixed to" or "set on" another component, it can be directly on or indirectly on that other component. When a component is referred to as being "connected to" another component, it can be directly connected to or indirectly connected to that other component.
[0025] It should be understood that the terms "length", "width", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0026] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0027] Please see Figure 1 The corrosion test method for hot-dip galvanized steel pipes provided in this application is now described. A corrosion test method for hot-dip galvanized steel pipes includes: S1: Obtain hot-dip galvanized steel pipe samples for gas pipelines produced by different galvanizing process parameters, determine the zinc layer thickness grade and characterize the zinc layer microstructure of each sample, and divide the samples into multiple thickness grade groups according to the zinc layer thickness. S2: Construct multi-field coupled corrosion test conditions that simultaneously cover the corrosion environment of gas medium inside the pipe, the corrosion environment of soil medium outside the pipe, and the stress corrosion environment. Place the samples of each thickness grade group under the multi-field coupled corrosion test conditions for accelerated corrosion, and take out the samples in batches at predetermined time intervals. Among them, the gas medium corrosion environment inside the pipe includes acidic gas components and moisture that are corrosive to the zinc layer, the soil medium corrosion environment outside the pipe includes simulated soil with different pH, water content and salt content, and the stress corrosion environment is achieved by applying stress in a predetermined direction to the sample. S3: The corrosion rate of the extracted samples was measured, the electrochemical corrosion performance was tested, and the microstructure and composition of the corrosion products were analyzed. Based on the analysis results, the delamination failure characteristics and failure evolution law of zinc layers of different thickness grades under multi-field coupled corrosion test conditions were determined. S4: Link and store the galvanizing process parameters, zinc layer thickness grade, corrosion test condition parameters, measured corrosion rate and corresponding delamination failure characteristics of each sample to establish a corrosion data set for characterizing the mapping relationship between process, structure and corrosion performance.
[0028] The corrosion test method for hot-dip galvanized steel pipes provided in this application, compared with the prior art, firstly involves sample preparation and grouping steps. By obtaining gas pipe samples produced with different galvanizing process parameters (such as zinc bath temperature, immersion time, alloy composition, etc.), the zinc layer thickness grade and microstructure characterization of each sample are determined, and the samples are divided into multiple grade groups according to thickness, thereby incorporating galvanizing production variables into the scope of investigation at the source of the test.
[0029] Then, an accelerated corrosion test was conducted, constructing a three-field coupled test condition that simultaneously covers the corrosion environment of the gas medium inside the pipe (including acidic gas components and moisture that are corrosive to the zinc layer), the corrosion environment of the soil medium outside the pipe (including simulated soils with different pH, moisture content and salinity), and the stress corrosion environment (applying stress to the sample in a predetermined direction). Samples of each thickness grade were placed in this environment for accelerated corrosion and were taken out in batches at predetermined time intervals. This step is a comprehensive simulation scheme designed for the actual service conditions of gas pipes, including the contact of the inner wall of the pipe with corrosive gas medium, the outer wall of the pipe being buried in a complex soil environment and the continuous stress of the pipe wall under the action of internal pressure and external loads. It overcomes the limitation of simulating only a single atmospheric environment. By simultaneously superimposing the three fields of the chemical medium inside the pipe, the electrochemical medium of the soil outside the pipe and the mechanical load, the environmental realism and acceleration rate of the accelerated corrosion test are significantly improved.
[0030] Next, the failure mechanism analysis step is carried out. The extracted samples are subjected to corrosion rate measurement, electrochemical corrosion performance test and microstructure and composition analysis of corrosion products. Based on this, the delamination failure characteristics and failure evolution law of zinc layers of different thicknesses under multi-field coupling conditions are determined. This step is different from the existing technology that only focuses on the overall corrosion rate of zinc layer. Instead, it examines the differentiated response behavior of each layer of zinc layer from the outside to the inside (outer zinc layer, intermediate alloy layer, inner coating substrate interface) during the corrosion process, thereby revealing the unique failure mechanism of high-thickness zinc layers in the multi-field coupling environment of gas.
[0031] Finally, a database was constructed to associate and store the galvanizing process parameters, zinc layer thickness grades, corrosion test conditions, measured corrosion rates, and corresponding delamination failure characteristics of each sample, thus establishing a corrosion data set for characterizing the mapping relationship between process, structure, and corrosion performance.
[0032] This approach identifies structural differences in samples at the source of the process and exposes these differences in corrosion behavior under multi-field coupled conditions. Corrosion behavior is then deconstructed into the differentiated failure contributions of each layer structure. Finally, a systematic data mapping relationship is established between process parameters, structural characteristics, and corrosion performance. By constructing a corrosion test environment that couples the gas inside the pipe, the soil outside the pipe, and stress, the accelerated corrosion test conditions more closely resemble the actual internal and external comprehensive service environment of gas pipelines, significantly improving the guiding value of the test results for actual operating conditions. Through layered failure characteristic analysis of zinc layers of different thicknesses, the differentiated failure behavior and interaction laws of each layer structure during the corrosion process can be systematically elucidated, providing a theoretical basis for optimizing the anti-corrosion design of high-thickness zinc layers. By establishing a systematic correlation database of galvanizing process parameters, zinc layer structural characteristics, and corrosion performance, corrosion test results can be directly fed back from back-end failure evaluation to front-end process optimization.
[0033] The following is a specific implementation process of the above embodiments.
[0034] First, sample preparation, testing, and grouping were carried out. For sample preparation, hot-dip galvanized steel pipes for urban gas transmission were selected. Two types of core galvanizing process variables were set, with the zinc bath temperature controlled at 440–460℃ and the immersion time of the steel pipe at 60–180s. Multiple groups of test pipes were prepared by cross-matching parameters. For zinc layer testing, the thickness of the zinc layer in the complete area of the pipe wall was measured using a coating thickness gauge. The microstructure of the alloy layering inside the zinc layer was observed using a metallographic microscope, and the morphology was recorded simultaneously. Based on the measured zinc layer thickness, three sample groups were divided into three categories: thin zinc layer group (40–70 μm), medium thick zinc layer group (80–120 μm), and high thick zinc layer group (130–160 μm). Each group of samples was independently numbered and filed.
[0035] Then, a multi-field coupled accelerated corrosion test was conducted: The overall test cycle is 90 days, with sampling at 5 fixed points: day 7, day 15, day 30, day 60, and day 90. The two environments, gas inside the pipe and soil outside the pipe, are used for 12-hour alternating cycles.
[0036] The corrosion environment inside the pipe is a corrosion mixture with natural gas as the base, with CO2 accounting for 3% of the volume and H2S accounting for 0.05% of the volume. The medium is saturated with water vapor, and the environment is kept at a constant temperature of 30℃ and a relative humidity of 95%. The mixture is continuously introduced into the inner cavity of the steel pipe for the first 6 hours of the single cycle, and the outer wall of the steel pipe is isolated from the soil. Three types of simulated soil were prepared for the external soil corrosion environment, with a pH range of 4.5 to 8.5, a moisture content of 12% to 28%, and a soluble salt content of 0.2% to 1.5% by mass. Six hours after a single circulation, the outer wall of the steel pipe was completely buried in the simulated soil, and the ventilation of the inner cavity was stopped. The stress-corrosion coupling condition is to continuously apply periodically fluctuating internal pressure to the inner cavity of the steel pipe, with a pressure variation range of 0.2 to 0.4 MPa and a complete cycle of a single pressure rise and fall of 30 minutes, simulating the daily gas supply pressure fluctuation of the pipeline network.
[0037] Next, we will analyze the multi-dimensional testing and failure patterns of the samples: Each batch of samples is subjected to three types of tests, and the corrosion is divided into early, middle and late stages based on the corrosion duration: 7-15 days is the early stage, 30-60 days is the middle stage, and 90 days is the late stage.
[0038] The corrosion rate was detected by weighing the sample before and after corrosion using the weight loss method, with a weighing accuracy of 0.1 mg, and the annual corrosion rate was calculated in μm / a. Electrochemical performance testing was conducted using a conventional three-electrode testing system, with a potential scan range of -1.2V to 0.2V and a scan rate of 0.5mV / s, to collect characteristic data of zinc layer electrochemical corrosion. Microscopic failure analysis involves observing the morphology of the interface between the zinc layer and corrosion products using scanning electron microscopy, and analyzing the elemental composition of the corrosion products using energy dispersive spectroscopy. The depth of the corrosion interface advancing inward at different corrosion stages is measured, and the longitudinal corrosion changes of the same thickness group are compared to summarize the characteristics of the evolution of delamination failure.
[0039] Finally, a multi-dimensional correlation erosion data set was constructed: A standardized data table was established, with five major categories of parameters linked and stored together to form a complete mapping database. This database includes galvanizing process parameters, zinc layer structure parameters, corrosion environment parameters, corrosion performance parameters, and failure characteristic parameters. Galvanizing process parameters include zinc bath temperature and immersion time of the steel pipe; zinc layer structure parameters include zinc layer thickness range and internal alloy layer thickness; corrosion environment parameters include the proportion of acidic components in the fuel gas, soil pH / moisture content / salt content, and circulating internal pressure range; corrosion performance parameters include annual corrosion rate and corrosion interface penetration depth; and failure characteristic parameters include corrosion type and corrosion duration corresponding to the initial exposure of the alloy layer.
[0040] Furthermore, the database supports cross-sectional comparison and retrieval of data from samples with different processes and zinc layer thicknesses.
[0041] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S2, the corrosion environment of the gas medium inside the pipe and the corrosion environment of the soil medium outside the pipe act on the sample in an alternating cycle. In one alternating cycle, the inner wall of the sample is first exposed to the corrosion environment of the gas medium inside the pipe while the outer wall is isolated from the simulated soil. Then, the outer wall of the sample is buried in the simulated soil while the inner wall is no longer exposed to the corrosion environment of the gas medium inside the pipe. This alternating cycle is repeated until the accelerated corrosion test ends.
[0042] Within an alternating cycle, the inner wall of the sample is first exposed to the corrosive environment of the combustion gas medium inside the pipe, namely, a mixture of acidic gas components and moisture that are corrosive to the zinc layer, while the outer wall of the sample is isolated from the simulated soil medium. After a predetermined time, the process switches to the next state, burying the outer wall of the sample in the simulated soil, while the inner wall is no longer exposed to the corrosive environment of the combustion gas medium inside the pipe. This alternating cycle is repeated until the entire accelerated corrosion test cycle is completed. The introduction of this alternating cycle mode further refines the corrosion test conditions in step two in terms of time sequence. Existing multi-environment coupling often adopts a simultaneous action approach, while this implementation adopts a time-division alternating strategy.
[0043] In actual service, the internal transport conditions (pressure, flow rate, and medium composition) and the external soil environment (alternating wet and dry conditions, water level fluctuations) of gas pipelines are not constant but vary periodically with seasons, gas load, and climatic conditions. By alternating the corrosive environments inside and outside the pipeline, the coupled erosion state of internal and external media during the alternation of transport and shutdown conditions, and wet and dry seasons, can be simulated more realistically. Simultaneously, the alternating cycle mode ensures that the inner and outer walls of the sample are alternately subjected to corrosive media over time, avoiding the interference of corrosion products that might result from simultaneous exposure, and making the test results closer to the intermittent corrosion characteristics of actual pipelines.
[0044] The duration of the alternating cycle can be flexibly set according to the actual simulated working conditions, such as 24 hours, 48 hours or 72 hours as a complete cycle; it can also be set to an asymmetrical cycle, that is, the exposure time of the inner wall is not equal to the exposure time of the outer wall, in order to simulate the actual working conditions of long-term operation and short-term shutdown of the pipeline.
[0045] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S2, the stress corrosion environment is constructed by applying a periodically changing internal pressure load to the inner cavity of the sample. The internal pressure load changes back and forth between a predetermined lower pressure limit and a predetermined upper pressure limit according to a set waveform, so as to simultaneously simulate the influence of pressure fluctuations during the operation of the gas pipeline on the corrosion behavior of the zinc layer.
[0046] An internal pressure load, varying cyclically between a predetermined lower pressure limit and a predetermined upper pressure limit according to a set waveform (such as a sine wave, triangular wave, or square wave), is applied to the inner cavity of the sample to create a stress corrosion environment. The periodic variation of this internal pressure load simulates the periodic pressure fluctuations within a gas pipeline caused by factors such as gas load fluctuations and pressure regulating device operation during actual operation. This implementation concretizes the overarching concept of applying stress in a predetermined direction to the sample in step two into a periodically varying internal pressure load, expanding from static stress loading to dynamic stress loading.
[0047] In actual gas pipelines, the pressure inside the pipe is not constant during service. Urban gas networks exhibit a clear periodic fluctuation, with lower pressure during peak gas consumption periods (morning, noon, and evening) and higher pressure during off-peak periods. Studies show that the effect of periodically fluctuating stress on zinc corrosion behavior differs significantly from that of constant stress: stress fluctuations cause repeated rupture and repair of the protective corrosion product film on the zinc surface, accelerating the penetration and diffusion of corrosive media. By applying periodically varying internal pressure loads in experiments, the coupled effect of chemical corrosion by the gas medium inside the pipe and the mechanical damage caused by pressure fluctuations can be simulated simultaneously, further improving the realism of accelerated corrosion simulation.
[0048] Among them, the waveform of the internal pressure load can be selected according to the actual pipeline pressure fluctuation characteristics, such as using the measured pressure curve as the loading spectrum; the frequency of pressure change can be adjusted according to the simulation object, such as simulating the daily fluctuation of the urban pipeline network (with a period of 24 hours) or the weekly fluctuation of the long-distance pipeline (with a period of 7 days).
[0049] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, during the accelerated corrosion process of S2, for each thickness grade group, when the first visible corrosion red rust spot appears on the zinc layer surface of any sample in that group, the moment when the first visible corrosion red rust spot appears is recorded as the initial corrosion start time of that thickness grade group, and this initial corrosion start time is used as the basis for adjusting the sample removal frequency of that group in subsequent accelerated corrosion tests.
[0050] During the accelerated corrosion test, for each thickness group, the surface condition of the zinc layer on the samples in that group was continuously observed. When the first visible red rust spots appeared on the zinc layer surface of any sample in that group, this moment was recorded as the initial corrosion start time for that thickness group. Subsequently, using this time point as a reference, the sampling frequency of subsequent samples in that group was adjusted; for example, the sampling frequency could be lower before the appearance of red rust, and higher after the appearance of red rust. This operation introduces an event-driven dynamic sampling mechanism into the accelerated corrosion process in step two.
[0051] Zinc coatings of different thicknesses exhibit varying corrosion resistance, with significant differences in their initial corrosion initiation times (the appearance of red rust in thicker zinc coatings is typically much later than in thinner coatings). Applying a uniform, fixed sampling frequency to all thickness groups could lead to a mismatch, with thinner zinc coatings already fully corroded in the later stages of the test while thicker coatings are still in the early stages of corrosion, reducing the comparability of the test data. By dynamically adjusting the sampling frequency based on the appearance of red rust, sufficient samples can be obtained for analysis in each thickness group before corrosion initiation, during the initial corrosion stage, and in the fully developed corrosion stage, making the corrosion evolution data of each group more complete and comparable over time. Furthermore, the first visible red rust spot serves as a direct and repeatable indicator, accurately identifiable without the need for complex instruments, offering excellent operational convenience.
[0052] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S3, the failure evolution law is determined by classifying the samples taken from each batch into the early corrosion stage, the middle corrosion stage, and the late corrosion stage according to the chronological order. The layered failure characteristics of samples in different corrosion stages within the same thickness grade group are compared longitudinally to identify the movement trajectory of the corrosion front that advances layer by layer from the zinc layer surface inward.
[0053] In the failure mechanism analysis of S3, the samples were first classified into three time intervals—early corrosion stage, intermediate corrosion stage, and late corrosion stage—according to the order in which they were taken out. Then, for samples from different corrosion stages within the same thickness group, their layered failure characteristics were compared longitudinally. That is, from early to intermediate to late stage, the process of zinc layer corrosion from the surface inward was observed step by step to identify the movement trajectory of the corrosion front (i.e., the interface between the deepest corrosion point and the uncorroded area) in the zinc layer thickness direction.
[0054] Current technologies for evaluating zinc layer corrosion often employ endpoint evaluation methods, which involve measuring the total corrosion amount or average corrosion rate at the end of the test. This method fails to reveal the evolution of corrosion over time or distinguish the differences in corrosion mechanisms at different stages. By dividing samples into early, middle, and late stages according to time and comparing them longitudinally, the dynamic process of the corrosion front gradually advancing from the zinc layer surface to the inner alloy layer can be visually presented. This process-tracking analysis method allows researchers to clearly grasp when, where, and how zinc layers of various thicknesses fail during the corrosion process, providing temporal data support for revealing the delamination failure mechanism of high-thickness zinc layers.
[0055] Please see Figure 1As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, during the longitudinal comparison process, if the incremental advance depth of the corrosion front between two adjacent corrosion stages of a certain thickness grade group continues to increase, it is determined that the zinc layer of that thickness grade has entered the corrosion acceleration stage; if the incremental advance depth continues to decrease, it is determined that the zinc layer of that thickness grade has entered the corrosion decay stage; based on the determination results, the corrosion process of the thickness grade group is divided into the initial incubation stage, the accelerated expansion stage, and the decay stabilization stage.
[0056] The increment of the corrosion front depth between two adjacent corrosion stages is the difference between the corrosion depth of the later stage and the previous stage. If the increment of the corrosion front depth for a certain thickness group continuously increases in multiple consecutive stages, it is determined that the zinc layer of that group has entered the corrosion acceleration stage; if the increment of the corrosion front depth continuously decreases, it is determined that it has entered the corrosion decay stage. Based on the above determination results, the entire corrosion process of this thickness group is divided into three characteristic stages: the initial incubation stage (corrosion begins but at a low rate), the accelerated propagation stage (corrosion rate continuously increases), and the decay and stabilization stage (corrosion rate gradually slows down and tends to stabilize).
[0057] The corrosion behavior of galvanized layers is not uniform but exhibits distinct stages. In the early stages of corrosion, the protective oxide film on the zinc surface is not completely destroyed, resulting in a low corrosion rate (incubation stage). With the accumulation of corrosion products and continuous erosion by the environmental medium, the corrosion rate rapidly increases after the protective film ruptures (accelerated propagation stage). When the corrosion front advances to the vicinity of the zinc-alloy interface, the density of the corrosion product layer and the corrosion resistance of the alloy layer may cause the corrosion rate to level off again (decay and stabilization stage). By quantitatively determining the transition points of each stage, the corrosion kinetic curves of zinc layers of different thicknesses can be accurately characterized, providing staged kinetic parameters for establishing a corrosion rate database and offering more refined segmented input data for subsequent lifetime prediction models.
[0058] Please see Figure 1 As a specific embodiment of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S3, the microstructure and composition analysis of corrosion products also includes observing the interface morphology between the corrosion product layer and the remaining zinc layer, and determining whether the corrosion type of the zinc layer of this thickness is uniform corrosion or localized corrosion based on the degree of undulation of the interface profile; when it is determined to be localized corrosion, the depth and opening size of the localized corrosion pit are further measured, and the localized corrosion sensitivity coefficient of the zinc layer is calculated based on the depth and opening size.
[0059] During the microscopic morphology and composition analysis of corrosion products in S3, the focus is on observing the interface morphology between the corrosion product layer and the remaining zinc layer, using microscopic analysis techniques such as scanning electron microscopy. After observation, the degree of undulation of the interface contour is used for judgment; if the interface contour is relatively flat with minimal undulation, the corrosion type of the zinc layer at this thickness level is determined to be uniform corrosion; if the interface contour has severe undulation and obvious pitting features, it is determined to be localized corrosion. When localized corrosion is determined, the depth and opening size of the localized corrosion pits are further measured, and the localized corrosion sensitivity coefficient of the zinc layer is calculated based on the ratio of depth to opening size or other preset formulas. The larger the coefficient, the higher the sensitivity of the zinc layer to localized corrosion.
[0060] Uniform corrosion and localized corrosion are two completely different corrosion failure modes. Uniform corrosion can be easily addressed by increasing the zinc layer thickness, while localized corrosion (such as pitting corrosion) is sudden and insidious, and is a major risk source for sudden gas pipeline leaks. Current technologies for determining the type of zinc layer corrosion rely heavily on empirical qualitative observations, lacking quantitative indicators.
[0061] The objective determination of corrosion type was achieved by observing the degree of undulation in the interface contour, and the quantitative evaluation of localized corrosion tendency was achieved by calculating the localized corrosion sensitivity coefficient. This quantitative indicator can be directly written into the corrosion dataset, providing a quantitative basis for assessing localized corrosion risk under different galvanizing process parameters.
[0062] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S3, after completing the layer failure characteristic analysis of all thickness grade groups, the failure evolution law between different thickness grade groups is compared horizontally. Based on the horizontal comparison results, the corrosion test duration corresponding to the first exposure of the alloy layer in the zinc layer in each thickness grade group is identified, and this duration is marked as the critical time for the protective failure of the zinc layer of that thickness grade.
[0063] After completing the layered failure characteristic analysis for all thickness grade groups, a horizontal comparison operation was further performed: the failure evolution patterns of different thickness grade groups (such as low thickness group, medium thickness group, and high thickness group) were compared side by side. Through horizontal comparison, the corrosion test duration (i.e., the time interval from the start of the test to the first exposure of the alloy layer to the corrosive medium) corresponding to the first appearance of the zinc layer in each thickness grade group was identified, and this duration was marked as the critical time for protective failure of the zinc layer of that thickness grade.
[0064] The zinc coating of hot-dip galvanized steel pipes consists of an outer pure zinc layer and an inner zinc-iron alloy layer. These two layers have fundamentally different corrosion resistance and protective mechanisms. The pure zinc layer primarily protects the substrate through cathodic protection via sacrificial anodes, while the alloy layer serves a dual function of cathodic protection and physical barrier. When the corrosion front penetrates the outer pure zinc layer and exposes the inner alloy layer for the first time, it signifies a fundamental shift in the zinc coating's protective mechanism (from single sacrificial anode protection to a composite mechanism of alloy layer barrier protection + sacrificial anode protection). This critical time for protective failure is a key indicator for evaluating the protective performance of zinc coatings of different thicknesses. By comparing this critical time across different thickness groups, we can quantitatively answer the engineering question of how much increasing the zinc coating thickness extends the critical time for protective failure, providing direct data support for the design of galvanized coating thickness in gas pipelines.
[0065] Please see Figure 1 As a specific implementation of the corrosion test method for hot-dip galvanized steel pipes provided in this application, in S4, after establishing the corrosion data set, the following is also performed: the corrosion rate of each thickness grade group is normalized with the corresponding initial zinc layer thickness to obtain the corrosion rate ratio per unit zinc layer thickness, and the ratio is correlated with the zinc bath temperature and immersion time in the corresponding galvanizing process parameters to obtain the ranking of influence factors describing the degree of influence of process parameters on the corrosion rate per unit thickness.
[0066] After establishing the corrosion dataset in S4, further data processing operations are performed: First, the corrosion rate measured for each thickness group is normalized to the corresponding initial zinc layer thickness—that is, the corrosion rate is divided by the initial zinc layer thickness to obtain the corrosion rate ratio per unit zinc layer thickness. This ratio eliminates the influence of the zinc layer thickness itself on the absolute value of the corrosion rate, reflecting the corrosion resistance per unit thickness of the zinc layer. Then, this ratio is subjected to a multiple regression correlation analysis with the zinc bath temperature and immersion time in the corresponding galvanizing process parameters. By comparing the regression coefficients, the ranking of the influencing factors of each process parameter on the corrosion rate per unit thickness is obtained.
[0067] The lack of quantitative correlation between corrosion data and process parameters in existing technologies has resulted in experimental results being unable to provide feedback for process optimization, a long-standing technical challenge. This implementation eliminates the interference of zinc layer thickness—a structural factor—on corrosion rate data through normalization, ensuring that the corrosion rate truly reflects the intrinsic corrosion resistance of the zinc layer material rather than the physical barrier effect of zinc layer thickness. Based on this, a multiple regression correlation is performed between the normalized corrosion rate and key process parameters such as zinc bath temperature and immersion time. This quantitatively reveals which process parameter has the greatest impact on corrosion resistance and how much adjustment to the process parameter can lead to a significant improvement in corrosion resistance. The ranking of influencing factors provides clear direction and quantitative basis for process optimization in galvanizing production lines.
[0068] As a specific embodiment of the corrosion test method for hot-dip galvanized steel pipes provided in this application, it also includes: S5: Obtain the actual galvanizing process parameter records and preset service life requirements of each pipe section in the target gas pipeline network, match the corrosion rate data corresponding to the actual galvanizing process parameters from the corrosion data set, and determine whether the corrosion margin of the pipe section is sufficient under the preset service life requirements based on the matching results. If it is insufficient, provide process improvement suggestions for adjusting the zinc bath temperature or immersion time in the galvanizing process parameters of the pipe section.
[0069] After completing all testing and database construction steps, the application steps are further executed. The actual galvanizing process parameters (such as zinc bath temperature and immersion time during actual production) and preset service life requirements for each pipe section in the target gas pipeline network are obtained. From the established corrosion dataset, corrosion rate data corresponding to the actual galvanizing process parameters and zinc layer thickness level are matched. Based on the matched corrosion rate and the designed wall thickness of the pipe section, it is determined whether the corrosion margin (i.e., the designed corrosion allowance) of the pipe section under the preset service life requirements is sufficient. That is, if corrosion continues at this rate until the preset service life end, whether the remaining wall thickness can still meet the strength requirements. If the corrosion margin is insufficient, process improvement suggestions are given to adjust the zinc bath temperature or immersion time in the galvanizing process parameters of the pipe section.
[0070] This approach elevates the established four-dimensional correlation database from an experimental tool to an engineering application tool, achieving a complete technical closed loop from laboratory testing to engineering practice. Traditionally, corrosion test results often remain at the research report level, making it difficult to directly translate them into engineering decision-making data. Through this implementation method, pipeline operators can directly match the corresponding corrosion rate from the database based on the actual production process parameters recorded for each batch of steel pipes and determine whether it meets specific service life requirements. If the predicted corrosion margin for a batch of steel pipes is insufficient, the database can also clearly indicate specific improvement directions, such as how much the zinc bath temperature should be increased or how much the immersion time should be extended. This provides a scientific basis for differentiated material selection and process traceability management of gas pipeline networks, enabling corrosion testing to truly serve engineering practice.
[0071] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A corrosion test method for hot-dip galvanized steel pipes, characterized in that, include: S1: Obtain hot-dip galvanized steel pipe samples for gas pipelines produced by different galvanizing process parameters, determine the zinc layer thickness grade and characterize the zinc layer microstructure of each sample, and divide the samples into multiple thickness grade groups according to the zinc layer thickness. S2: Construct multi-field coupled corrosion test conditions that simultaneously cover the corrosion environment of gas medium inside the pipe, the corrosion environment of soil medium outside the pipe, and the stress corrosion environment. Place the samples of each thickness grade group under the multi-field coupled corrosion test conditions for accelerated corrosion, and take out the samples in batches at predetermined time intervals. The corrosion environment of the gas medium inside the pipe includes acidic gas components and moisture that are corrosive to the zinc layer, the corrosion environment of the soil medium outside the pipe includes simulated soil with different pH, water content and salt content, and the stress corrosion environment is achieved by applying stress in a predetermined direction to the sample. S3: The extracted samples were subjected to corrosion rate determination, electrochemical corrosion performance testing, and microstructure and composition analysis of corrosion products. Based on the analysis results, the delamination failure characteristics and failure evolution law of zinc layers of different thickness grades under the multi-field coupled corrosion test conditions were determined. The samples extracted in each batch were classified into early corrosion stage, mid-corrosion stage, and late corrosion stage according to time sequence. The delamination failure characteristics of samples of different corrosion stages within the same thickness grade group were compared longitudinally to identify the movement trajectory of the corrosion front in the zinc layer thickness direction. The corrosion front is the interface between the deepest point reached by corrosion and the uncorroded area. By quantitatively determining the transition nodes of each stage, the corrosion kinetic curves of zinc layers of different thickness grades can be accurately characterized, providing staged kinetic parameters for establishing a corrosion rate database and providing more refined segmented input data for subsequent lifetime prediction models. S4: The zinc plating process parameters, zinc layer thickness grade, corrosion test condition parameters, measured corrosion rate and corresponding delamination failure characteristics of each sample are associated and stored to establish a corrosion data set for characterizing the mapping relationship between process, structure and corrosion performance. S5: Obtain the actual galvanizing process parameter records and preset service life requirements of each pipe section in the target gas pipeline network. Match the corrosion rate data corresponding to the actual galvanizing process parameters from the corrosion data set. Determine whether the corrosion margin of the pipe section is sufficient under the preset service life requirements based on the matching results. If it is insufficient, provide process improvement suggestions for adjusting the zinc bath temperature or immersion time in the galvanizing process parameters of the pipe section. Whether the corrosion margin is sufficient is whether the remaining wall thickness can still meet the strength requirements when the corrosion continues at the preset service life end.
2. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, In S2, the corrosive environment of the gas medium inside the pipe and the corrosive environment of the soil medium outside the pipe act on the sample in an alternating cycle. In one alternating cycle, the inner wall of the sample is first exposed to the corrosive environment of the gas medium inside the pipe while the outer wall is isolated from the simulated soil. Then, the outer wall of the sample is buried in the simulated soil while the inner wall is no longer exposed to the corrosive environment of the gas medium inside the pipe. This alternating cycle is repeated until the accelerated corrosion test ends.
3. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, In S2, the stress corrosion environment is constructed by applying a periodically varying internal pressure load to the inner cavity of the sample. The internal pressure load changes back and forth between a predetermined lower pressure limit and a predetermined upper pressure limit according to a set waveform, so as to simultaneously simulate the effect of pressure fluctuations during the operation of the gas pipeline on the corrosion behavior of the zinc layer.
4. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, During the accelerated corrosion process of S2, for each thickness grade group, when the first visible red rust spot appears on the zinc layer surface of any sample in the group, the moment when the first visible red rust spot appears is recorded as the initial corrosion start time of that thickness grade group, and this initial corrosion start time is used as the basis for adjusting the sample removal frequency of that group in subsequent accelerated corrosion tests.
5. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, During the longitudinal comparison, if the incremental advance depth of the corrosion front between two adjacent corrosion stages in a certain thickness grade group continues to increase, it is determined that the zinc layer of that thickness grade has entered the corrosion acceleration stage; if the incremental advance depth continues to decrease, it is determined that the zinc layer of that thickness grade has entered the corrosion decay stage; based on the determination results, the corrosion process of the thickness grade group is divided into the initial incubation stage, the accelerated expansion stage, and the decay stabilization stage.
6. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, In S3, the microstructure and composition analysis of the corrosion products also includes observing the interface morphology between the corrosion product layer and the remaining zinc layer, and determining whether the corrosion type of the zinc layer of this thickness is uniform corrosion or localized corrosion based on the degree of undulation of the interface profile; when it is determined to be localized corrosion, the depth and opening size of the localized corrosion pit are further measured, and the localized corrosion sensitivity coefficient of the zinc layer is calculated based on the depth and opening size.
7. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, In S3, after completing the layered failure characteristic analysis of all thickness grade groups, the failure evolution law between different thickness grade groups is compared horizontally. Based on the horizontal comparison results, the corrosion test duration corresponding to the first exposure of the alloy layer in the zinc layer in each thickness grade group is identified, and this duration is marked as the critical time for protective failure of the zinc layer of that thickness grade.
8. The corrosion test method for hot-dip galvanized steel pipes as described in claim 1, characterized in that, In S4, after establishing the corrosion data set, the following steps are performed: the corrosion rate of each thickness grade group is normalized with the corresponding initial zinc layer thickness to obtain the corrosion rate ratio per unit zinc layer thickness, and this ratio is correlated with the zinc bath temperature and immersion time in the corresponding zinc plating process parameters to obtain the ranking of influence factors describing the degree of influence of process parameters on the corrosion rate per unit thickness.