Nitrogen-oxygen separation hollow fiber membrane for simultaneous gas drying, its preparation method and application
By constructing a hydrophilic transition layer and a photothermal evaporation layer on the surface of a polyimide hollow fiber membrane, the problem of decreased gas separation performance of the polyimide hollow fiber membrane in a humid environment was solved, achieving simultaneous gas drying and nitrogen-oxygen separation, and improving the membrane's stability and self-regeneration capability.
Patent Information
- Application Number
- CN202611070991.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-07-20
AI Technical Summary
Polyimide hollow fiber membranes exhibit reduced gas separation performance in humid environments and require separate drying components, leading to system complexity and increased energy consumption.
Carboxylation modification is performed on the surface of polyimide hollow fiber membrane to construct a hydrophilic transition layer and a photothermal evaporation layer, forming a bifunctional hollow fiber composite membrane. The photothermal conversion material is used to evaporate moisture under light, thereby achieving gas drying and nitrogen-oxygen separation.
It achieves simultaneous drying of gases and separation of nitrogen and oxygen in humid environments, improves the interfacial stability and self-regeneration capability of the membrane, and avoids the peeling and static saturation failure of traditional modified coatings.
Smart Images

Figure CN122605371B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of membrane separation technology, specifically relating to a hollow fiber composite membrane, its preparation method and application, and particularly to a dual-functional hollow fiber composite membrane that combines gas drying and nitrogen-oxygen separation functions, its preparation method and application. Background Technology
[0002] Polyimide (PI) hollow fiber membranes have shown great application potential in air separation fields such as gas purification and oxygen / nitrogen enrichment due to their excellent thermal stability, mechanical strength, and good gas permeation selectivity. However, in practical industrial applications, air feedstocks often contain high humidity water vapor. When traditional hydrophobic polyimide porous membranes operate in humid environments, water vapor easily undergoes capillary condensation (i.e., pore wetting) within the membrane's micropores. This not only blocks the effective gas permeation channels but may also induce hydroplasticization of the polyimide macromolecular chains, leading to a precipitous drop in the membrane's gas permeability and nitrogen / oxygen separation selectivity.
[0003] To address the negative impact of humidity on membrane performance, drying and gas separation components can be integrated into a system, or a post-treatment drying route can be adopted. For example, US5169412A connects a membrane dryer and a membrane-air separator in series, using the permeate from the air separation membrane as the purge gas for the drying membrane, simultaneously producing dry air and nitrogen products. However, this approach uses two membrane modules, resulting in a complex system structure and requiring additional piping connections and purge gas recirculation. Another example is US4931070A, which discloses a method for first producing high-purity nitrogen from air using a membrane separation / deoxygenation system, and then dehumidifying the nitrogen using a separate membrane dryer. This approach also relies on separate drying components, increasing equipment investment and operating energy consumption.
[0004] In recent years, hollow fiber membranes with liquid water evaporation capabilities have attracted widespread attention in the field of water treatment. CN115161880A discloses a hydrophilic-hydrophobic sandwich composite photothermal fiber membrane that utilizes photothermal materials such as carbon nanotubes to absorb sunlight and convert it into heat energy, driving interfacial water evaporation for seawater desalination. CN111573780A discloses a photothermal membrane distiller that uses polydopamine and carbon materials loaded on a hollow fiber membrane, achieving 360° light absorption and efficient water evaporation through an arched structure design. Li et al. (J. Mater. Chem. A, 2021, 9, 390-399) designed a PTFE / CNT hollow fiber arched array evaporator, using hydrophilic modification to give the PTFE membrane self-water-absorbing ability, combined with the photothermal conversion of carbon nanotubes, to achieve excellent evaporation performance. However, the core function of the above technologies is to extract water from liquid water sources and vaporize it, and this has not yet been introduced into the field of gas separation membranes.
[0005] Therefore, there is an urgent need to develop an integrated technical solution based on a single fiber membrane that combines gas separation and active dehumidification functions. Summary of the Invention
[0006] The purpose of this application is to provide a hollow fiber composite membrane with both gas drying and nitrogen-oxygen separation functions and its preparation method, so as to solve the problems of reduced gas separation performance of polyimide hollow fiber membranes in humid environments and the need for separate drying components, so as to achieve simultaneous drying and nitrogen-oxygen separation of humid gas raw materials by a single membrane module.
[0007] To achieve the above objectives, this application provides the following technical solution: A method for preparing a bifunctional hollow fiber composite membrane includes the following steps: S1. The polyimide hollow fiber membrane is modified by surface carboxylation to obtain the first modified fiber membrane; S2. A hydrophilic transition layer is constructed on the surface of the first modified fiber membrane to obtain the second modified fiber membrane; S3. A photothermal evaporation layer is constructed on the surface of the second modified fiber membrane to obtain the bifunctional hollow fiber composite membrane.
[0008] This application also provides the following technical solutions: A bifunctional hollow fiber composite membrane is obtained by the aforementioned preparation method.
[0009] This application also provides the following technical solutions: The aforementioned application of bifunctional hollow fiber composite membranes in gas separation.
[0010] The technical solution provided in this application has the following beneficial effects: (1) The preparation method provided in this application involves sequentially constructing a hydrophilic transition layer and a photothermal evaporation layer on the surface of a hydrophobic base membrane (polyimide hollow fiber membrane). Figure 1 The hydrophilic transition layer can capture moisture in the gas passing through the hollow fiber membrane and transfer it to the photothermal evaporation layer through a hydrophilic polymer network. The photothermal conversion material in the photothermal evaporation layer converts light energy into heat energy under illumination, promoting moisture evaporation and thus achieving continuous and rapid gas drying.
[0011] (2) The preparation method provided in this application modifies the surface of the substrate membrane by carboxylation, generating abundant carboxyl sites in situ. This allows hydrophilic polymers to be firmly anchored to the substrate membrane surface through chemical bonds and / or hydrogen bonds. Furthermore, the photothermal evaporation layer is also constructed using hydrophilic polymers, further strengthening the bonding between functional layers. This method can significantly improve the interfacial stability of the composite membrane under high-speed airflow scouring, effectively solving the technical problem of easy peeling off of traditional modified coatings.
[0012] (3) The bifunctional hollow fiber composite membrane provided in this application preferentially traps free water in humid airflow through a hydrophilic transition layer, avoiding the condensation and plasticizing effects caused by liquid water directly intruding into the micropores of the base membrane; at the same time, the outermost photothermal conversion material captures ambient light energy or system waste heat, generating a local thermal effect, heating and vaporizing the water captured by the hydrophilic polymer and dispersing it to the external environment, forming an "inner layer water trapping" effect. The dynamic circulation mechanism of "outer layer evaporation" endows the composite membrane with the ability to capture and discharge water immediately, effectively solving the problem of static saturation failure caused by passive water absorption in traditional coatings. Invention Details 1. Terminology Explanation All patents and other publications cited herein are incorporated herein in their entirety. In the event of any conflict between any description of terminology herein and any document incorporated herein by reference, this document shall prevail.
[0014] Numerical ranges can be represented by a hyphen "-" or a tilde "~". Unless otherwise stated, the range should be understood to encompass both the endpoint values and any values in between. There are no particular restrictions on the type of numeric values within the range, including but not limited to integers, decimals, fractions, percentages, etc., unless explicitly excluded by the context or a particular numeric type is technically unavailable. The type of numeric values within the range is not limited by the specific representation of the endpoints.
[0015] The terms “including,” “containing,” and similar expressions have a non-restrictive meaning.
[0016] "Optional" is used to indicate that a certain feature (including but not limited to components, steps, parameters or structures) may be present in some embodiments, but may not appear in other embodiments, thereby providing technical flexibility for different implementations without departing from the core concept of the present invention.
[0017] "Any combination" of the enumeration items means any two or more of the enumeration items that coexist or are used together, including but not limited to any two combinations, any three combinations, any more items, and combinations of all the enumeration items, unless the context explicitly excludes it or a particular combination is technically impossible.
[0018] The use of labels such as a), b), i), ii), 1), 2), S1, S2, etc. to number the steps of a method is only for the convenience of description and reading, and does not mean that the corresponding steps must be performed in the order of the numbers, unless the text explicitly states or the information in the text can be clearly inferred that there is a logical or temporal relationship between specific steps.
[0019] The use of ordinal terms such as "first" and "second" to distinguish elements (e.g., first modified fiber membrane, second modified fiber membrane) does not imply any priority, order, or hierarchy between any two elements, but is merely used as a label.
[0020] The term "hollow fiber membrane" as used herein refers to a fibrous membrane with a hollow structure. "Hollow" means that the membrane has at least one continuously extending hollow region along its length. Hollow fiber membranes can achieve selective permeation or retention of substances through the membrane wall structure formed around the hollow regions. The membrane wall can have a porous structure, including one or more of micropores, mesopores, and macropores. Hollow fiber membranes can be used for gas separation, such as the selective separation of oxygen, nitrogen, carbon dioxide, hydrogen, helium, or other gas components; gas molecules can selectively permeate through the fiber membrane based on differences in molecular size, dissolution-diffusion differences, adsorption differences, or other mass transfer mechanisms. Unless otherwise specified, there are no particular limitations on the cross-sectional shape, fiber diameter, membrane wall thickness, pore structure type, or pore arrangement of hollow fiber membranes.
[0021] The term "polyimide" as used herein refers to a polymer containing imide structural units in its molecular chain. As an example, polyimides can be prepared by polycondensation and imidization of one or more diamine compounds with one or more dianhydride compounds. Exemplary diamine compounds include, but are not limited to, 9,9-bis(4-aminophenyl)fluorene, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and 1,3-bis(4-aminophenoxy)benzene. Exemplary dianhydride compounds include, but are not limited to, pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-oxobisphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3,3',4,4'-benzophenone tetracarboxylic dianhydride.
[0022] The "carboxylation modification" described herein refers to the process of introducing carboxyl (-COOH) functional groups onto the surface of polyimide hollow fiber membranes through chemical and / or physical means. For example, alkaline solution treatment can induce ring-opening hydrolysis of the imide rings on the fiber membrane surface, forming a carboxyl-containing polyamic acid structure and / or its partially hydrolyzed structure, thereby generating carboxyl active sites on the fiber membrane surface. These carboxyl active sites can be in free acid or salt form. Alternatively, methods such as plasma treatment, UV-initiated grafting, and chemical oxidation can be used to graft or introduce carboxyl-containing monomers or polymers capable of forming carboxyl groups onto the fiber membrane surface. After carboxylation modification, the carboxyl groups on the fiber membrane surface can serve as active sites for binding hydrophilic polymers, used in the subsequent construction of a hydrophilic transition layer.
[0023] The "hydrophilic transition layer" as described herein refers to the intermediate layer located between the base membrane (polyimide hollow fiber membrane) and the photothermal evaporation layer. The hydrophilic transition layer can be constructed by forming chemical bonds (e.g., covalent bonds, ionic bonds, coordination bonds) and / or hydrogen bonds between a hydrophilic polymer and the carboxylated modified base membrane surface. As examples, hydrophilic polymers that can be used to construct the hydrophilic transition layer include, but are not limited to, polymers containing amino, hydroxyl, or amide groups, such as polyethyleneimine, polydopamine, chitosan, polyvinyl alcohol, polyethylene glycol, and polyacrylamide.
[0024] The "photothermal evaporation layer" described in this article refers to the outermost functional layer of the bifunctional hollow fiber composite membrane, which contains at least one photothermal conversion material. The photothermal evaporation layer can also be constructed using the same or different hydrophilic polymers as the hydrophilic transition layer. These hydrophilic polymers can be used as film-forming agents, dispersing stabilizers, moisture-absorbing and wicking media, or thermal buffer materials to fix the photothermal conversion material, maintain coating uniformity, adsorb and transfer moisture, or prevent localized overheating.
[0025] The term "photothermal conversion material" as used in this article refers to a material capable of absorbing electromagnetic radiation and converting the absorbed light energy into heat energy through a non-radiative energy conversion process. The electromagnetic radiation includes, but is not limited to, ultraviolet light, visible light, and infrared light (including near-infrared light). According to the different material compositions, the photothermal conversion materials include the following categories: (1) Carbon-based materials, such as carbon black, carbon nanotubes, graphene oxide, reduced graphene oxide, mesoporous carbon, carbon quantum dots, etc., whose photothermal conversion is mainly based on non-radiative transition mechanisms; (2) Metal nanoparticles, such as gold, silver, copper, etc., whose photothermal conversion is mainly based on local surface plasmon resonance mechanisms; (3) Transition metal compounds, such as molybdenum disulfide, copper sulfide, black titanium dioxide (or reduced titanium dioxide), titanium carbide (MXene), etc., whose photothermal conversion mechanisms include band gap absorption, free electron light absorption or surface plasmon effect; (4) Organic polymer photothermal materials, such as polypyrrole, polyaniline, etc., which are conjugated conductive polymers, have broadband absorption capabilities in the near-infrared region, and achieve photothermal conversion through intramolecular photoexcitation relaxation process; (5) Macrocyclic compounds and their complexes, such as phthalocyanine, porphyrin, polyphenol-metal ion complexes, etc., whose photothermal conversion is mainly based on non-radiative decay processes after photoexcitation (including intersystem crossing, vibrational relaxation, etc.).
[0026] The term "hydrophilic polymer" as used herein refers to a class of polymeric compounds containing one or more hydrophilic groups in their molecular structure, capable of forming strong bonds with water molecules through hydrogen bonds, electrostatic interactions, or other intermolecular forces, thereby exhibiting water absorption, water solubility, or water-absorbing swelling properties. The hydrophilic groups include, but are not limited to, hydroxyl, carboxyl, amino, amide, and ether groups. Depending on their source, the hydrophilic polymers may include natural hydrophilic polymers, semi-synthetic hydrophilic polymers, and synthetic hydrophilic polymers. For example, natural hydrophilic polymers include, but are not limited to, cellulose, starch, sodium alginate, hyaluronic acid, gelatin, dextran, and chitosan; semi-synthetic hydrophilic polymers include, but are not limited to, cellulose derivatives; and synthetic hydrophilic polymers include, but are not limited to, polyvinyl alcohol, polyethylene glycol, polyethyleneimine, polyallylamine, polyvinylamine, polyacrylamide, polydopamine, and polyamide-amine dendrimers. Depending on whether the molecular chain contains ionizable groups and their charge properties, the hydrophilic polymer may include nonionic hydrophilic polymers, anionic hydrophilic polymers, cationic hydrophilic polymers, and amphoteric hydrophilic polymers.
[0027] The "aqueous coating solution" described herein refers to a liquid mixture with water as the main dispersion medium and containing the target modified component. The aqueous coating solution can be a solution, colloidal system, suspension system, or dispersion system. In addition to the target modified component, the aqueous coating solution may optionally contain crosslinking agents, dispersants, surfactants, thickeners, stabilizers, or pH adjusters to improve the uniformity, stability, and film-forming properties of the coating solution. If necessary, the coating solution can be dispersed by stirring, ultrasonication, or homogenization before use to ensure uniform distribution of the components; after coating, the aqueous medium can be removed by drying or other methods.
[0028] The "nitrogen-oxygen separation" described in this article refers to the process of selectively separating oxygen and nitrogen in a mixed gas by utilizing the difference in permeation rates of oxygen and nitrogen in the hollow fiber membrane wall. Polyimide hollow fiber membranes can preferentially allow oxygen to permeate through the membrane wall under pressure differential, thereby obtaining oxygen-rich gas or nitrogen-rich gas.
[0029] 2. Implementation Plan One embodiment of this application is as follows: A method for preparing a bifunctional hollow fiber composite membrane includes the following steps: S1. The polyimide hollow fiber membrane is modified by surface carboxylation to obtain the first modified fiber membrane; S2. A hydrophilic transition layer is constructed on the surface of the first modified fiber membrane to obtain the second modified fiber membrane; S3. A photothermal evaporation layer is constructed on the surface of the second modified fiber membrane to obtain the bifunctional hollow fiber composite membrane.
[0030] In some specific implementations, step S1 includes: hydrolyzing the surface of the polyimide hollow fiber membrane.
[0031] In some specific implementations, the hydrolysis treatment involves soaking in an alkaline solution.
[0032] In some specific embodiments, the alkaline solution is an aqueous solution of sodium hydroxide, potassium hydroxide, lithium hydroxide, or any combination thereof.
[0033] In some specific embodiments, the concentration of the alkaline solution is 0.01-5 wt%, preferably 0.01-0.5 wt%.
[0034] In some specific implementations, the hydrolysis treatment lasts for 5-30 minutes.
[0035] In some specific implementations, step S2 includes: applying a first aqueous coating solution to the first modified fiber membrane for a first coating treatment; The first aqueous coating liquid contains a first hydrophilic polymer; The first hydrophilic polymer is polyvinyl alcohol, polyethylene glycol, polyethyleneimine, polyallylamine, polyvinylamine, polyacrylamide, polydopamine, polyamide-amine dendrimer, cellulose and its derivatives, starch, sodium alginate, hyaluronic acid, gelatin, dextran, chitosan or any combination thereof.
[0036] In some specific implementations, the first hydrophilic polymer forms chemical bonds and / or hydrogen bonds with the surface of the first modified fiber membrane.
[0037] In some specific implementations, the first coating process is dip coating, spray coating, brush coating, or any combination thereof.
[0038] In some specific implementations, the first hydrophilic polymer forms chemical bonds with the surface of the first modified fiber membrane; the temperature of the first coating treatment is 60-150℃, preferably 60-80℃; and the duration of the first coating treatment is 1-24 hours, preferably 1-6 hours.
[0039] In some specific implementations, the first hydrophilic polymer does not form chemical bonds with the surface of the first modified fiber membrane; the temperature of the first coating treatment is 15-50°C, preferably 20-40°C, more preferably 25-30°C; the duration of the first coating treatment is 30 seconds to 6 hours, preferably 30-300 seconds, more preferably 30-150 seconds.
[0040] In some specific implementations, the concentration of the first hydrophilic polymer is 1-20 wt%, preferably 1-10 wt%.
[0041] In some specific implementations, step S3 includes: applying a second coating treatment to the surface of the second modified fiber membrane using a second aqueous coating liquid, followed by drying and curing treatment; The second aqueous coating liquid contains a photothermal conversion material and a second hydrophilic polymer; The photothermal conversion material is carbon black, carbon nanotubes, graphene oxide, reduced graphene oxide, mesoporous carbon, carbon quantum dots, gold nanoparticles, silver nanoparticles, copper nanoparticles, molybdenum disulfide, copper sulfide, black titanium dioxide, titanium carbide, polypyrrole, polyaniline, phthalocyanine, porphyrin, polyphenol-metal ion complex, or any combination thereof. The second hydrophilic polymer is polyvinyl alcohol, polyethylene glycol, polyethyleneimine, polyallylamine, polyvinylamine, polyacrylamide, polydopamine, polyamide-amine dendrimer, cellulose and its derivatives, starch, sodium alginate, hyaluronic acid, gelatin, dextran, chitosan or any combination thereof.
[0042] In some specific implementations, the second coating process is dip coating, spray coating, brush coating, or any combination thereof.
[0043] In some specific embodiments, the temperature of the second coating treatment is 15-50°C, preferably 20-40°C, and more preferably 25-30°C.
[0044] In some specific implementations, the duration of the second coating treatment is from 30 seconds to 6 hours, preferably 30-300 seconds, and more preferably 30-150 seconds.
[0045] In some specific embodiments, the content of the second hydrophilic polymer in the aqueous coating solution is 1-20 wt%, preferably 1-10 wt%.
[0046] In some specific implementations, the amount of the photothermal conversion material is 3 wt% of the second hydrophilic polymer.
[0047] In some specific implementations, the drying and curing temperature is 40-180℃, preferably 60-150℃.
[0048] In some specific implementations, the drying and curing process lasts for 1-24 hours, preferably 1-3 hours.
[0049] In some specific embodiments, the aqueous coating liquid further contains a crosslinking agent, a dispersant, a surfactant, a thickener, a stabilizer, a pH adjuster, or any combination thereof.
[0050] Another implementation of this application is as follows: A bifunctional hollow fiber composite membrane is obtained by any of the aforementioned preparation methods.
[0051] In some specific implementations, the composite membrane comprises, from the inside out: a support layer made of polyimide hollow fiber membrane, a hydrophilic transition layer attached to the outer surface of the support layer, and a photothermal evaporation layer attached to the outer surface of the hydrophilic transition layer.
[0052] Another implementation of this application is as follows: Application of any of the aforementioned bifunctional hollow fiber composite membranes in gas separation; wherein the bifunctional hollow fiber composite membrane is used for nitrogen and oxygen separation and simultaneous gas drying.
[0053] In some specific implementations, the dual-functional hollow fiber composite membranes are bundled and then encapsulated to form a membrane module; the membrane module includes an internally illuminated light guide structure.
[0054] In some specific embodiments, the membrane module further comprises one or more other fibers bundled together with the bifunctional hollow fiber composite membrane.
[0055] In some specific implementations, the membrane module is used in a single-stage or multi-stage series gas separation module.
[0056] In some specific implementations, the bifunctional hollow fiber composite membrane undergoes pretreatment before the nitrogen-oxygen separation operation; the pretreatment includes one or more of drying under an inert atmosphere, degassing under vacuum, and pre-pressurizing in the feed gas. Attached Figure Description
[0057] Figure 1 This is a schematic diagram of the structure of a bifunctional polyimide hollow fiber composite membrane. Detailed Implementation
[0058] The raw materials used in this application can be purchased or synthesized in-house. The following specific embodiments are used to further describe the implementation of the present invention and do not limit the scope of the invention.
[0059] Example 1 This embodiment uses the following method to prepare a nitrogen-oxygen separation hollow fiber composite membrane that can simultaneously dry gases.
[0060] (1) Preparation of polyimide hollow fiber membrane: 40 mL of m-methylphenol was added to a 250 mL round-bottom flask, followed by 9,9-bis(4-aminophenyl)fluorene (6.4207 g) and pyromellitic dianhydride (2.0088 g). The mixture was stirred in a 70 °C water bath for 30 min until completely dissolved. Then, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (4.0914 g) and 0.15 mL of isoquinoline were added, and the mixture was placed in a 160 °C oil bath for 6 h. After the reaction was complete, the viscous solution was slowly poured into an ethanol bath to precipitate filamentous precipitate. After Soxhlet extraction with methanol for 5 h, the precipitate was dried in a 60 °C oven for 12 h until constant weight was obtained to obtain polyimide. 3 g of polyimide and... N A 25 wt% spinning solution was prepared by mixing methylpyrrolidone (NMP, 9 g) and stirring in a 70°C water bath until completely dissolved, then allowed to stand for 12 h to remove bubbles. Spinning was performed using a wet-dry phase inversion process, with the core solution being an NMP / water mixture containing 10 wt% NMP. The core extrusion speed was set at 2 mL / h, and the shell extrusion speed at 10 mL / h, extruded through a 30G / 21G coaxial needle. The air gap height was controlled at 20 cm, and the collecting roller speed at 20 rpm. The resulting hydrophobic polyimide hollow fiber membrane was cleaned and dried before use.
[0061] (2) Carboxylation modification: The above polyimide hollow fiber membrane was immersed in an alkaline solution prepared by 0.025 g sodium hydroxide and 49.975 g deionized water (mass fraction of 0.05%), and allowed to stand for 10 minutes at room temperature. After being taken out, it was repeatedly rinsed with deionized water until the washing solution was neutral, thus obtaining an activated base membrane with carboxyl active sites on the surface.
[0062] (3) Hydrophilic modification: The activated base film was immersed in an aqueous coating solution prepared by 2.5 g polyvinyl alcohol and 47.5 g deionized water (mass fraction of 5%) at room temperature, and after standing for 90 seconds, it was taken out to form a hydrophilic transition layer on the surface of the base film.
[0063] (4) Photothermal modification: The hydrophilically modified base film was immersed again at room temperature in an aqueous coating solution prepared by mixing 2.5 g polyvinyl alcohol, 0.075 g carbon black nanomaterial (3 wt% of polyvinyl alcohol) and 47.425 g deionized water. After standing for 90 seconds, it was taken out and placed in an oven (60℃) for constant temperature drying for 2 hours to achieve stable cross-linking of the coating. Finally, a polyimide hollow fiber composite film with both hydrophilic and photothermal functions was obtained.
[0064] Example 2 This embodiment uses the following method to prepare a nitrogen-oxygen separation hollow fiber composite membrane that can simultaneously dry gases.
[0065] (1) Preparation of polyimide hollow fiber membrane: Same as in Example 1.
[0066] (2) Carboxylation modification: The polyimide hollow fiber membrane was immersed in an alkaline solution prepared by 0.005 g sodium hydroxide and 49.995 g deionized water (mass fraction of 0.01%), and allowed to stand for 30 minutes at room temperature. After being taken out, it was repeatedly rinsed with deionized water until the washing solution was neutral, thus obtaining an activated base membrane with carboxyl active sites on the surface.
[0067] (3) Hydrophilic modification: The activated base film was immersed in an aqueous coating solution prepared by 0.5 g polyvinyl alcohol and 49.5 g deionized water (mass fraction of 1%) at room temperature, and after standing for 150 seconds, it was taken out to form a hydrophilic transition layer on the surface of the base film.
[0068] (4) Photothermal modification: The hydrophilically modified base film was immersed again at room temperature in an aqueous coating solution prepared by mixing 0.5 g polyvinyl alcohol, 0.015 g carbon black nanomaterial (3 wt% of polyvinyl alcohol) and 49.485 g deionized water. After standing for 150 seconds, it was taken out and placed in an oven (80℃) for constant temperature drying for 3 hours to achieve stable cross-linking of the coating. Finally, a polyimide hollow fiber composite film with both hydrophilic and photothermal functions was obtained.
[0069] Example 3 This embodiment uses the following method to prepare a nitrogen-oxygen separation hollow fiber composite membrane that can simultaneously dry gases.
[0070] (1) Preparation of polyimide hollow fiber membrane: Same as in Example 1.
[0071] (2) Carboxylation modification: The polyimide hollow fiber membrane was immersed in an alkaline solution prepared by 0.25 g sodium hydroxide and 49.75 g deionized water (mass fraction of 0.5%), and allowed to stand for 5 minutes at room temperature. After being taken out, it was repeatedly rinsed with deionized water until the washing solution was neutral, thus obtaining an activated base membrane with carboxyl active sites on the surface.
[0072] (3) Hydrophilic modification: The activated base film was immersed in an aqueous coating solution prepared by 5 g polyvinyl alcohol and 45 g deionized water (mass fraction of 10%) at room temperature. After standing for 30 seconds, it was taken out and a hydrophilic transition layer was constructed on the surface of the base film.
[0073] (4) Photothermal modification: The hydrophilically modified base film was immersed again at room temperature in an aqueous coating solution prepared by mixing 5 g polyvinyl alcohol, 0.15 g carbon black nanomaterial (3 wt% of polyvinyl alcohol) and 44.85 g deionized water. After standing for 30 seconds, it was taken out and placed in an oven (150℃) for constant temperature drying for 1 hour to achieve stable cross-linking of the coating. Finally, a polyimide hollow fiber composite film with both hydrophilic and photothermal functions was obtained.
[0074] Example 4 This embodiment uses the following method to prepare a nitrogen-oxygen separation hollow fiber composite membrane that can simultaneously dry gases.
[0075] (1) Preparation of polyimide hollow fiber membrane: Same as in Example 1.
[0076] (2) Carboxylation modification: The polyimide hollow fiber membrane was immersed in an alkaline solution prepared by 0.05 g sodium hydroxide and 49.95 g deionized water (mass fraction of 0.1%), and allowed to stand for 15 minutes at room temperature. After being taken out, it was repeatedly rinsed with deionized water until the washing solution was neutral, thus obtaining an activated base membrane with carboxyl active sites on the surface.
[0077] (3) Hydrophilic modification: The activated base film was immersed in an aqueous coating solution prepared by 1.5 g polyvinyl alcohol and 48.5 g deionized water (mass fraction of 3%) at room temperature, and after standing for 60 seconds, it was taken out to form a hydrophilic transition layer on the surface of the base film.
[0078] (4) Photothermal modification: The hydrophilically modified base film was immersed again at room temperature in an aqueous coating solution prepared by mixing 1.5 g polyvinyl alcohol, 0.045 g carbon black nanomaterial (3 wt% of polyvinyl alcohol) and 48.455 g deionized water. After standing for 60 seconds, it was taken out and placed in an oven (120℃) for constant temperature drying for 2 hours to achieve stable cross-linking of the coating. Finally, a polyimide hollow fiber composite film with both hydrophilic and photothermal functions was obtained.
[0079] Comparative Example 1 Following the preparation method of Example 1, without carboxylation modification, hydrophilic modification, or photothermal modification, a pristine hydrophobic polyimide hollow fiber membrane without any surface modification was obtained.
[0080] Comparative Example 2 This comparative example does not involve hydrophilic or photothermal modification; it only modifies the polyimide hollow fiber membrane by carboxylation. The specific method is as follows: (1) Preparation of polyimide hollow fiber membrane: Same as in Example 1.
[0081] (2) Carboxylation modification: The polyimide hollow fiber membrane was immersed in an alkaline solution prepared by 0.005 g sodium hydroxide and 49.995 g deionized water (mass fraction of 0.01%), and allowed to stand for 30 minutes at room temperature. After being taken out, it was repeatedly rinsed with deionized water until the washing solution was neutral. After drying, a carboxylation modified fiber membrane without hydrophilic transition layer and photothermal evaporation layer was obtained.
[0082] Comparative Example 3 This comparative example does not involve photothermal modification; it only modifies the polyimide hollow fiber membrane by carboxylation and hydrophilicity. The specific methods are as follows: (1) Preparation of polyimide hollow fiber membrane: Same as in Example 1.
[0083] (2) Carboxylation modification: Same as in Example 1.
[0084] (3) Hydrophilic modification: The activated base film obtained in step (2) is immersed in an aqueous coating solution prepared by 2.5 g of polyvinyl alcohol and 47.5 g of deionized water (mass fraction of 5%) at room temperature. After standing for 90 seconds, it is taken out and dried to obtain a hydrophilic modified fiber film without photothermal evaporation layer.
[0085] Example 5 This embodiment is based on the preparation of a membrane module with an internally illuminated light guide structure using a dual-functional hollow fiber composite membrane.
[0086] The bifunctional hollow fiber composite membrane prepared in Example 1 was cut into appropriate lengths. Several side-emitting optical fibers (as an internally illuminated light guide structure) were selected and uniformly mixed and bundled with the composite membrane at a ratio of 1:5. The mixed fiber bundle was inserted into a transparent polycarbonate membrane shell tube, and both ends were potted and cured with epoxy resin. After curing, the end faces of both ends were cut to expose the inner cavity of the hollow fiber membrane. One end of the side-emitting optical fiber was gathered and connected to an external xenon lamp light source interface. In use, the light emitted by the external light source is guided into the interior of the membrane assembly through the side-emitting optical fiber and uniformly emitted from the sidewall of the fiber, thereby providing sufficient and uniform visible light irradiation to the photothermal evaporation layer on the outer surface of the surrounding bifunctional hollow fiber composite membrane, achieving efficient in-situ heating and dehumidification.
[0087] Example 6 In this embodiment, the fiber membranes prepared in Comparative Example 1 and Comparative Example 3 were used as test objects to conduct surface dynamic water contact angle tests. Among them, the preparation of the support layer (polyimide hollow fiber membrane), carboxylation modification and hydrophilic modification methods of Comparative Example 3 were the same as those in Example 1, which can reflect the role of the hydrophilic transition layer in the bifunctional polyimide hollow fiber composite membrane of Example 1.
[0088] The hollow fiber membrane sample to be tested was cut into 5 cm long segments and fixed flat on the stage. Using a DSA100 contact angle meter, 2 μL of deionized water was dropped onto the outer surface of the membrane using a micro-syringe. The high-speed camera system was activated, and the moment the water droplet contacted the membrane surface was recorded as 0 s. Images of the water droplet morphology were captured at 5 s, 10 s, 20 s, and 30 s. The contact angles (CA left, CA right) on the left and right sides of the water droplet were calculated using software fitting, and the average of the calculated results on both sides was taken as the dynamic water contact angle at that moment.
[0089] Table 1. Comparison Test Results of Dynamic Water Contact Angle on Surface
[0090] The test results (Table 1) show that the contact angle of the unmodified fiber membrane in Comparative Example 1 decreased only slightly from 103.6° to 102.2° within 5-30 seconds, with almost no attenuation, indicating that its strong hydrophobic properties prevent water droplets from spreading and it lacks kinetic water-trapping ability. In contrast, the contact angle of the hydrophilic modified fiber membrane in Comparative Example 3 exhibited a significant and rapid dynamic attenuation trend, rapidly decreasing from 93.4° at 5 seconds to 55.2° at 30 seconds. These results demonstrate that the preparation method provided in this application can endow polyimide hollow fiber membranes with excellent kinetic water-trapping properties, enabling efficient retention and conduction of water molecules, providing a moisture source for subsequent photothermal dehumidification.
[0091] Example 7 In this embodiment, the fiber membranes prepared in Comparative Example 1 and Example 1 were used as test objects to conduct surface photothermal conversion temperature rise tests.
[0092] The specific operation method for the surface photothermal conversion temperature rise test in this embodiment is as follows: The hollow fiber membrane sample to be tested is arranged closely and laid flat on a substrate with heat insulation properties to avoid energy loss errors caused by heat conduction from the substrate. A xenon lamp equipped with an AM 1.5G filter is used as the test light source to simulate sunlight, vertically illuminating the sample surface, and the light intensity on the membrane surface is adjusted to 100 mW / cm² using a power meter. 2 (i.e., 1 standard solar intensity). Before illumination, the initial temperature of the membrane surface is read and recorded using an infrared thermal imager; after continuous irradiation for 1 minute, the highest temperature of the membrane surface is read again using the infrared thermal imager. The temperature rise (°C) is calculated by subtracting the initial temperature from the temperature after irradiation.
[0093] Table 2. Comparison Test Results of Surface Photothermal Conversion Heating
[0094] The test results (Table 2) show that the unmodified polyimide hollow fiber membrane of Comparative Example 1, lacking photothermal components, could not generate an effective thermal effect, only heating up by 5.9°C after 1 minute of visible light irradiation, indicating that it possesses almost no photothermal conversion capability. In contrast, the bifunctional polyimide hollow fiber composite membrane of Example 1 exhibited a rapid temperature jump from 23.7°C to 42.7°C under the same conditions, a temperature increase of 19.0°C, which is 3.2 times that of Comparative Example 1. These results demonstrate that the preparation method provided in this application successfully endows the composite membrane with highly efficient photothermal conversion performance, providing sufficient thermal power for the water captured from the hydrophilic polymer, causing it to vaporize in situ and dissipate outwards, thereby achieving continuous gas drying function.
[0095] Example 8 In this embodiment, the membrane module with an internally illuminated light guide structure prepared in Example 5 (containing the dual-functional hollow fiber composite membrane prepared in Example 1, denoted as "Membrane Module 1"), the conventional module encapsulated with the original unmodified membrane of Comparative Example 1 (denoted as "Membrane Module 2"), and the membrane module encapsulated with the unmodified fiber membrane of Comparative Example 3 (denoted as "Membrane Module 3") were used as test objects to conduct simultaneous performance tests on nitrogen and oxygen separation and gas drying under humid conditions.
[0096] The specific operation method for the test in this embodiment is as follows: Simulated humid air was used as the test feed gas. The relative humidity (RH) of the feed gas entering the membrane module was controlled to be 80% by a front-end humidifier. The test environment temperature was maintained at 25℃, and the operating pressure difference between the inside and outside of the membrane housing was maintained at 0.2 MPa. During the test, for membrane module 1 containing an internally illuminated light guide structure, visible light radiation was introduced through an external LED light source interface, and the light intensity emitted from the fiber sidewall was adjusted to 100 mW / cm². 2 This ensures uniform illumination of the photothermal evaporation layer on its outer surface; membrane modules 2 and 3 are tested under normal conditions without illumination. After the test conditions stabilize, an online gas chromatograph and a trace moisture analyzer are used to measure and record the oxygen-nitrogen separation selectivity of the outlet gas on the permeate side under humid conditions, as well as the relative humidity (RH) of the outlet gas. To ensure the accuracy and repeatability of the test data, each group of membrane module samples underwent three independent parallel tests in this embodiment, and the results were taken as the average of the three parallel tests (as shown in Table 3). The nitrogen-oxygen separation selectivity (αO2 / N2) was calculated using the following formula: αO2 / N2=
[0097] In the formula, yO2 and yN2 are the volume fractions of oxygen and nitrogen in the outlet gas on the permeate side after the test stabilizes, respectively; xO2 and xN2 are the volume fractions of oxygen and nitrogen in the feed gas on the feed side, respectively.
[0098] Table 3. Comparative Test Results of Gas Separation and Drying Synchronization Performance under Humid Conditions
[0099] As shown in Table 3, under high-humidity feed gas conditions, membrane module 2 (using unmodified hydrophobic polyimide hollow fiber membrane) suffers from poor oxygen-nitrogen separation selectivity due to capillary condensation of water vapor within the micropores, leading to pore blockage. Although membrane module 3 achieves a lower outlet relative humidity of 40.2% due to the construction of a hydrophilic transition layer, the lack of a photothermal evaporation layer prevents timely removal of adsorbed moisture. The statically saturated moisture continuously wets and blocks the micropores of the base membrane, resulting in an oxygen-nitrogen separation selectivity of only 3.2, significantly inhibiting overall separation efficiency. In contrast, membrane module 1, under visible light radiation provided by an internally illuminated light guide structure, exhibits a significantly improved oxygen-nitrogen separation selectivity of 4.6, while simultaneously reducing the relative humidity of the permeate-side outlet gas to an extremely low dryness level of 7.3%. Based on the test results of Examples 6-7 above, it can be seen that the dual-functional hollow fiber composite membrane provided by this application has a dynamic cycle self-regeneration mechanism of "inner layer water capture - outer layer evaporation". Under the uniform illumination of the internal light guide structure, it can provide sufficient thermal power to trap water to achieve in-situ vaporization and dissipation, thereby effectively avoiding the wetting and blockage of the separation micropores by water vapor. This allows the membrane module to have both excellent gas separation performance and continuous gas drying function in a high humidity environment.
Claims
1. An application of a bifunctional hollow fiber composite membrane in gas separation, characterized in that, The dual-functional hollow fiber composite membrane is used for nitrogen and oxygen separation and simultaneous gas drying. The dual-functional hollow fiber composite membranes are bundled and then encapsulated to form a membrane module; the membrane module includes an internally illuminated light guide structure. The bifunctional hollow fiber composite membrane is obtained through the following steps: S1. The polyimide hollow fiber membrane is modified by surface carboxylation to obtain the first modified fiber membrane; S2. Construct a hydrophilic transition layer on the surface of the first modified fiber membrane to obtain the second modified fiber membrane; S3. A photothermal evaporation layer is constructed on the surface of the second modified fiber membrane to obtain the bifunctional hollow fiber composite membrane; Step S3 includes: applying a second coating treatment to the surface of the second modified fiber membrane using a second aqueous coating liquid, followed by drying and curing treatment; The second aqueous coating liquid contains a photothermal conversion material and a second hydrophilic polymer; The photothermal conversion material is carbon black; The second hydrophilic polymer is polyvinyl alcohol, polyethylene glycol, polyethyleneimine, polyallylamine, polyvinylamine, polyacrylamide, polydopamine, polyamide-amine dendrimer, cellulose and its derivatives, starch, sodium alginate, hyaluronic acid, gelatin, dextran, chitosan or any combination thereof; The amount of the photothermal conversion material is 3 wt% of the second hydrophilic polymer.
2. The application according to claim 1, characterized in that, Step S1 includes: hydrolyzing the surface of the polyimide hollow fiber membrane; The hydrolysis treatment involves soaking in an alkaline solution; The alkaline solution is an aqueous solution of sodium hydroxide, potassium hydroxide, lithium hydroxide, or any combination thereof.
3. The application according to claim 1, characterized in that, Step S2 includes: applying a first aqueous coating solution to the first modified fiber membrane for a first coating treatment; The first aqueous coating solution contains a first hydrophilic polymer; The first hydrophilic polymer is polyvinyl alcohol, polyethylene glycol, polyethyleneimine, polyallylamine, polyvinylamine, polyacrylamide, polydopamine, polyamide-amine dendrimer, cellulose and its derivatives, starch, sodium alginate, hyaluronic acid, gelatin, dextran, chitosan or any combination thereof.
Citation Information
Patent Citations
Photo-thermal membrane distiller and preparation method and application thereof, and water treatment equipment
CN111573780A
Batch preparation method of hydrophilic and hydrophobic sandwich structure composite photo-thermal fiber membrane
CN115161880A
Process and system for the production of dry, high purity nitrogen
US4931070A
Membrane air drying and separation operations
US5169412A
Polyimide hollow fiber membrane, preparation method and application thereof, and oxygen-containing organic gas deoxidation method and system
CN119857383A