A non-snow-accumulating anti-slip adhesive material, its preparation method and application
By incorporating superhydrophobic rigid anti-slip aggregate and slow-release microcapsules into the anti-slip tape, and combining it with modified HDPE substrate and acrylic pressure-sensitive adhesive, the problems of anti-slip tape being prone to brittleness at low temperatures and difficult to remove snow have been solved, achieving high adhesion and easy snow removal.
Patent Information
- Application Number
- CN202610817021.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-06-08
AI Technical Summary
Existing anti-slip tapes are prone to cracking in low-temperature environments, have poor adhesion, and are difficult to remove snow in winter, posing safety hazards.
The multi-functional anti-slip layer design includes superhydrophobic rigid anti-slip aggregate and slow-release microcapsules embedded with de-icing agent, forming a continuous interpenetrating network structure. Combined with modified HDPE substrate and acrylic pressure-sensitive adhesive, it achieves gradient functional zoning, enhancing adhesion and flexibility.
It maintains high adhesion and flexibility at low temperatures, prevents snow accumulation in light snow and facilitates the removal of heavy snow, thus improving the overall composite strength and safety of the anti-slip tape in cold environments.
Smart Images

Figure CN122648024B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of self-adhesive thermoplastic polyolefin anti-slip materials, specifically relating to a non-snow-accumulating anti-slip adhesive material, its preparation method, and its application. Background Technology
[0002] Thermoplastic polyolefin waterproofing materials are a class of sheet-like waterproofing materials based on thermoplastic polyolefin polymers, which can be heat-melted / heat-processed and are widely used in construction, transportation, and other fields. Among them, anti-slip tape is a functional roll material with a granular or special textured surface used to increase friction and prevent slippage, and is widely used in staircases, ramps, sidewalks, and other similar applications. However, in cold winter outdoor environments, ordinary anti-slip tapes face severe performance challenges. Existing anti-slip tapes typically exhibit the following problems in environments below -20°C: the chain segment movement of the substrate is hindered at low temperatures, making the material brittle and prone to cracking when bent; the adhesive layer loses its viscoelasticity at low temperatures, failing to wet the surface of the adhered object, leading to adhesion failure and tape detachment. Especially in snowy winter weather, the accumulation of snow on the surface of anti-slip adhesive materials poses a serious safety hazard. Anti-slip tape relies on hard particles to provide friction, and in heavy snow, there is a "ice embedding" problem—snow water seeps into the gaps between the particles, freezes, and forms a smooth ice layer on the surface, which adheres very firmly to the tape and is extremely difficult to remove.
[0003] To address the issues of preventing snow accumulation and ice embedding, patent CN114729228A discloses a composition for forming an anti-snow coating and an anti-snow coating. It employs a composition comprising composite particles coated with a first polymer and a coating component with reactive functional groups to form a coating that prevents snow accumulation and effectively prevents snow adhesion for extended periods, maintaining its anti-snow performance even in heavy snowfall areas. Patent CN118421141A discloses a biomimetic superhydrophobic self-cleaning anti-icing coating. It uses silica aerogel-coated titanium dioxide hydrophobic powder as a functional powder, combined with fluorocarbon resin and isocyanate to form a biomimetic superhydrophobic self-cleaning anti-icing coating. This coating forms a uniform and robust superhydrophobic coating on the substrate surface, exhibiting strong adhesion, long-lasting hydrophobicity, and self-cleaning and anti-fouling functions. Patent CN116535956B discloses a superhydrophobic anti-icing polyurethane urea elastomer coating that can be quickly applied in low-temperature environments. It involves preparing two components, mixing them evenly, coating them onto a carrier surface, and then spraying them with superhydrophobic powder to form a highly hydrophobic coating.
[0004] However, the above solutions are all improvements to individual superhydrophobic coatings or paints, and their application in prefabricated anti-slip tapes is not observed, making it difficult to bond firmly to flexible substrates. Therefore, there is an urgent need to develop snow-free anti-slip adhesive materials that possess excellent adhesion, substrate flexibility, and snow-free properties in low-temperature environments. Summary of the Invention
[0005] The purpose of this invention is to provide a non-snow-accumulating anti-slip adhesive material, its preparation method, and its application in order to solve the above-mentioned problems. This tape has the characteristics of not accumulating snow in light snow and easily removing snow in heavy snow, and can maintain high adhesion and flexibility at low temperatures.
[0006] The objective of this invention is achieved through the following technical solution:
[0007] A non-snow-accumulating anti-slip adhesive material comprises, from top to bottom, a multifunctional anti-slip layer, a substrate layer, and an adhesive layer, wherein: the multifunctional anti-slip layer includes a top layer of superhydrophobic rigid anti-slip aggregate and a bottom layer of slow-release microcapsules embedded with snow-melting agent, the two forming a continuous interpenetrating double network structure through an elastomer matrix; the substrate layer is modified HDPE; and the adhesive layer is an acrylic pressure-sensitive adhesive.
[0008] The present invention relates to an anti-slip adhesive material, the multifunctional anti-slip layer of which forms a gradient functional zone in the thickness direction, and the bottom layer is embedded with slow-release microcapsules of de-icing agent, which can release de-icing agent components when exposed to water, and can form a low freezing point salt water film at the interface between ice and snow and the anti-slip layer; the surface of the superhydrophobic hard anti-slip aggregate has a nanoscale rough structure, forming a superhydrophobic surface, achieving the effect of no snow accumulation in light snow and easy removal of heavy snow.
[0009] As a preferred technical solution of the present invention, the raw material composition of the multifunctional anti-slip layer is as follows, by weight: 40-55 parts of hard anti-slip aggregate, 5-10 parts of volcanic ash porous microspheres, 25-35 parts of organosilicon modified polyurethane prepolymer, 8-12 parts of nano silica aerogel powder, 5-8 parts of fluorocarbon modified acrylate oligomer, 10-15 parts of sustained-release microcapsules, 1.5-3.5 parts of curing agent, and 8-15 parts of diluent.
[0010] As a preferred technical solution of the present invention, the sustained-release microcapsule includes a de-icing agent core material and a wall material with sustained-release function. The de-icing agent core material is selected from acetate-based de-icing agents, and the wall material is selected from ethyl cellulose or urea-formaldehyde resin. The particle size of the sustained-release microcapsule is 50-200 μm.
[0011] As a preferred embodiment of the present invention, the hard anti-slip aggregate is selected from silicon carbide particles with a particle size of 0.5-1.2 mm;
[0012] The porous volcanic ash microspheres are selected from samples with a sieve size of 0.2-0.8 mm;
[0013] The silicone-modified polyurethane prepolymer (PUU) is selected from Wacker GENIOMER. ® Series of products;
[0014] The specific surface area of the nano-silica aerogel powder is 200-300 m². 2 / g;
[0015] The fluorocarbon modified acrylate oligomers are selected from Daikin Industries' ZEFFLE® SE-310 and SE-405.
[0016] The curing agent is selected from aliphatic or alicyclic polyisocyanates or amino resins;
[0017] The diluent is selected from one or more of butyl acetate, dimethyl carbonate, and propylene glycol methyl ether acetate.
[0018] As a preferred technical solution of the present invention, the multifunctional anti-slip layer is prepared by the following steps:
[0019] Weigh out the hard anti-slip aggregate, volcanic ash porous microspheres and sustained-release microcapsules by weight, and mix them evenly in a mixer to obtain component A;
[0020] In a dispersion tank, add silicone-modified polyurethane prepolymer and fluorocarbon-modified acrylate oligomer, stir until uniform, then add nano-silica aerogel powder and disperse at high speed, then add diluent and curing agent and continue dispersion. After uniform dispersion, degas under vacuum to obtain component B.
[0021] While stirring, pour the solid mixture of component A into the liquid of component B, stir and ensure that the solid particles are uniformly wetted and dispersed to obtain a multifunctional anti-slip coating slurry for later use.
[0022] As a preferred technical solution of the present invention, the modified HDPE substrate layer is made of a blend comprising the following components: 70-90 parts by weight of HDPE resin, 5-15 parts by weight of POE elastomer, 1-5 parts by weight of methyl vinyl silicone rubber, 2-8 parts by weight of compatibilizer, and 1-3 parts by weight of peroxide crosslinking agent.
[0023] As a preferred embodiment of the present invention, the HDPE resin has a melt index of 0.5-10.5 g / 10 min and a density of 0.95-0.97 g / cm³. 3 ;
[0024] The compatibilizer is selected from maleic anhydride-grafted polyethylene;
[0025] The peroxide crosslinking agent is selected from dicumyl peroxide and bis-tert-butyl peroxide;
[0026] The modified HDPE substrate layer is prepared by the following method: the components are premixed in a high-speed mixer in proportion, melt-blended and granulated by a twin-screw extruder, the granules are pressed into shape by a flat vulcanizing machine, the thickness is controlled, and the granules are wound up for later use.
[0027] As a preferred technical solution of the present invention, the acrylate pressure-sensitive adhesive is prepared by polymerization reaction of raw materials containing the following components: 66-78 parts by weight of soft monomer, 8-12 parts by weight of polyolefin elastomer grafted macromolecular monomer, 8-12 parts by weight of hard monomer, 2-5 parts by weight of functional monomer, 3-8 parts by weight of cold-resistant plasticizer, 0.1-0.5 parts by weight of initiator, and 0.2-1.0 parts by weight of crosslinking agent;
[0028] The polyolefin elastomer grafted macromonomer includes methacrylate-terminated ethylene / butene elastomer macromonomers.
[0029] The acrylate pressure-sensitive adhesive described above is prepared by the following method:
[0030] (1) Synthesis of acrylate prepolymer: Soft monomer, hard monomer, functional monomer, polyolefin elastomer grafted macromonomer and some initiator are added to the reactor, solvent is added, and the reaction is carried out at 70-85℃ for 3-6 hours to obtain acrylate prepolymer;
[0031] (2) Cool the obtained acrylate prepolymer to below 40°C, add cold-resistant plasticizer, remaining initiator and crosslinking agent, stir evenly to obtain the product.
[0032] A method for preparing a snow-free, anti-slip adhesive material includes the following steps:
[0033] (1) Take an HDPE film, treat it with corona on one side, then coat it with a layer of acrylic pressure-sensitive adhesive and allow it to cure semi-cured;
[0034] (2) Apply the multifunctional anti-slip coating slurry to the surface of the semi-cured acrylic pressure-sensitive adhesive of the HDPE film;
[0035] (3) After coating, let stand, sprinkle a layer of nano silica aerogel powder on the surface, and press lightly with a rubber roller so that half of the powder volume is embedded in the surface of the elastomer and the other half is exposed to form nano-scale rough protrusions.
[0036] (4) The coated material is transferred into a temperature and humidity control chamber for curing to form a flexible interpenetrating polymer network;
[0037] (5) Coat the other side of the HDPE film with acrylic pressure-sensitive adhesive, and then cover it with a release film to obtain the final product.
[0038] Further, in step (1), the thickness of the HDPE film is 0.1-0.6 mm, and the thickness of the acrylic pressure-sensitive adhesive is 0.1-0.3 mm; in step (2), the thickness of the multifunctional anti-slip layer coating slurry is controlled to be 1.2±0.1 mm; in step (3), the coating is left to stand for 15-20 minutes; in step (4), the coating is cured at 40℃ and 60% relative humidity for 1-6 hours, and the diluent completely evaporates during the curing process.
[0039] The above-mentioned application of the non-snow-accumulating anti-slip adhesive material is as an anti-slip tape.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] This invention constructs a multifunctional anti-slip layer with gradient functional zones. The bottom layer is embedded with slow-release microcapsules of snow-melting agent, which controllably release snow-melting components upon contact with water and form a low-freezing-point brine film at the ice-snow-anti-slip layer interface, weakening freeze adhesion and facilitating snow and ice removal. The surface layer of superhydrophobic hard anti-slip aggregate utilizes a nanoscale rough structure to prevent water and snow particles from spreading and penetrating, achieving the effects of preventing snow accumulation in light snow and facilitating snow removal in heavy snow. Simultaneously, the substrate is modified to improve low-temperature toughness, and a compatibilizer is used to enable hydrogen bonding or chemical bonding between the acrylic pressure-sensitive adhesive and the substrate, eliminating the weak interface between the polar adhesive layer and the non-polar substrate. Polyolefin elastomers are introduced into the pressure-sensitive adhesive, grafted with macromolecular monomers. Due to their structural similarity to the substrate, they act as molecular bridges between the adhesive layer and the substrate, helping to reduce interfacial tension, enhance low-temperature wetting and spreading capabilities, and ensure the overall composite strength of the anti-slip layer in cold environments. Attached Figure Description
[0042] Figure 1 Image of sample E1 prepared for an embodiment of the present invention;
[0043] Figure 2 The image shows a sample E1 being tested outdoors in heavy snow. Detailed Implementation
[0044] This invention provides a non-snow-accumulating anti-slip adhesive material, which has excellent adhesion, substrate flexibility and non-snow-accumulating properties in low-temperature environments. The material comprises, from top to bottom, a multifunctional anti-slip layer, a substrate layer and an adhesive layer. The multifunctional anti-slip layer includes a top layer of superhydrophobic rigid anti-slip aggregate and a bottom layer of slow-release microcapsules embedded with snow-melting agent. The two form a continuous interpenetrating double network structure through an elastomer matrix. The substrate layer is modified HDPE and the adhesive layer is acrylic pressure-sensitive adhesive.
[0045] This invention's multifunctional anti-slip layer features gradient functional zones along its thickness. Its bottom layer is embedded with slow-release microcapsules encapsulating de-icing agents. Upon contact with water, these microcapsules controllably release the de-icing agent, forming a low-freezing-point saline film at the interface between the ice / snow and the anti-slip layer. This effectively weakens the freeze-thaw adhesion between the ice and the anti-slip layer, facilitating the removal of snow and ice covering its surface. Simultaneously, the superhydrophobic rigid anti-slip aggregate in the anti-slip layer possesses a nanoscale rough structure. This superhydrophobic surface prevents liquid water and small snow particles from spreading and penetrating the micropores, reducing snow accumulation under light snowfall and facilitating overall removal during heavy snowfall due to weak interfacial bonding. This achieves both snow-proofing and easy snow removal.
[0046] This invention also improves the low-temperature toughness of the HDPE substrate by modifying it, enabling the substrate to maintain excellent flexibility and impact resistance even at extreme low temperatures. By introducing a compatibilizer, hydrogen bonds or chemical bonds are formed between the compatibilizer and the surface acrylic pressure-sensitive adhesive layer, eliminating the weak interfacial bonding between the polar adhesive and the non-polar substrate, and improving the adhesion reliability between the adhesive layer and the substrate. Furthermore, a polyolefin elastomer grafted with a macromonomer is introduced into the acrylic pressure-sensitive adhesive. The main chain segment of this macromonomer has structural similarity to the substrate and can act as a link between the adhesive, the substrate, and the adhered objects, reducing interfacial tension and enhancing the adhesive's wetting and spreading ability under low-temperature conditions, further ensuring the overall composite strength of the anti-slip layer in cold environments.
[0047] As a preferred embodiment, the raw material composition of the multifunctional anti-slip layer, by weight, is as follows: 40-55 parts of hard anti-slip aggregate, 5-10 parts of volcanic ash porous microspheres, 25-35 parts of silicone-modified polyurethane prepolymer, 8-12 parts of nano-silica aerogel powder, 5-8 parts of fluorocarbon-modified acrylate oligomer, 10-15 parts of sustained-release microcapsules, 1.5-3.5 parts of curing agent, and 8-15 parts of diluent.
[0048] Preferably, by weight, the raw material composition of the multifunctional anti-slip layer is as follows: 45-50 parts of rigid anti-slip aggregate, 6-8 parts of volcanic ash porous microspheres, 30-33 parts of silicone-modified polyurethane prepolymer, 9-11 parts of nano-silica aerogel powder, 6-8 parts of fluorocarbon-modified acrylate oligomer, 12-14 parts of slow-release microcapsules, 2.5-3.0 parts of curing agent, and 12-14 parts of diluent. More preferably, by weight, the raw material composition of the multifunctional anti-slip layer is as follows: 47 parts of rigid anti-slip aggregate, 7 parts of volcanic ash porous microspheres, 32 parts of silicone-modified polyurethane prepolymer, 10 parts of nano-silica aerogel powder, 7 parts of fluorocarbon-modified acrylate oligomer, 13 parts of slow-release microcapsules, 2.7 parts of curing agent, and 13 parts of diluent.
[0049] In a preferred embodiment, the sustained-release microcapsule includes a de-icing agent core material and a wall material with sustained-release function. The de-icing agent core material is selected from acetate-based de-icing agents, and the wall material is selected from ethyl cellulose or urea-formaldehyde resin. The particle size of the sustained-release microcapsule is 50-200 μm. Preferably, the acetate-based de-icing agent includes calcium acetate or calcium formate.
[0050] As a preferred embodiment, the sustained-release microcapsules can be prepared by the following method: grinding the de-icing agent core material to a particle size <100μm and sieving it for later use; dissolving the wall material in a solvent to prepare a solution; using a fluidized bed bottom spray coating machine, adding acetate-based de-icing agent powder into the fluidized bed and spraying the wall material solution; controlling the coating weight gain rate to reach 12-15% of the core material mass and the coating rate to reach more than 85%; drying and sieving to obtain calcium formate sustained-release microcapsules with a particle size of 50-200μm, sealing and drying them, and storing them for later use. For example, in a specific embodiment, taking the preparation of ethyl cellulose-coated calcium formate as an example, the specific preparation steps are as follows: anhydrous calcium formate is ground to a particle size <100μm and sieved for later use; ethyl cellulose is dissolved in 95% ethanol to prepare a 5% concentration solution; using a fluidized bed bottom spray coating machine, the calcium formate powder is fed into the fluidized bed, the inlet air temperature is controlled at 45-50℃, and the above wall material solution is sprayed at an atomization pressure of 0.15-0.2 MPa; the coating weight gain rate is controlled to reach 12-15% of the core material weight, and the coating rate reaches more than 85%; after drying, it is passed through a 200-mesh sieve to obtain calcium formate sustained-release microcapsules with a particle size of 50-200μm, which are then sealed and dried for storage.
[0051] As a preferred embodiment, the rigid anti-slip aggregate is selected from silicon carbide particles with a particle size of 0.5-1.2 mm and silicon carbide CAS number 409-21-2. Suitable materials include Saint-Gobain Sika® series, Shandong Jinmeng New Material JMSiC-G series, and Weifang Kaihua silicon carbide. The volcanic ash porous microspheres are selected from 0.2-0.8 mm sieved products with CAS number 1332-09-8. For example, Tengchong Yiyuan volcanic ash can be used. The silicone-modified polyurethane prepolymer (PUU) is selected from Wacker GENIOMER. ® Series of products; Nano silica aerogel powder with a specific surface area of 200-300 m² 2 / g; the fluorocarbon modified acrylate oligomer is selected from Daikin Industries ZEFFLE® SE-310 and SE-405; the curing agent is selected from aliphatic or alicyclic polyisocyanates (such as HDI trimer, IPDI trimer) or amino resins; the diluent is selected from one or more of butyl acetate, dimethyl carbonate, and propylene glycol methyl ether acetate.
[0052] As a preferred embodiment, the multifunctional anti-slip layer is prepared by the following steps: Weigh hard anti-slip aggregate, volcanic ash porous microspheres, and sustained-release microcapsules by weight, and mix them evenly in a mixer to obtain component A; add organosilicon-modified polyurethane prepolymer and fluorocarbon-modified acrylate oligomer to a dispersion tank, stir evenly, then add nano-silica aerogel powder for high-speed dispersion, then add diluent and curing agent for continued dispersion, and after even dispersion, degas under vacuum to obtain component B; while stirring, pour the solid mixture of component A into the liquid of component B, stir and ensure uniform wetting and dispersion of solid particles to obtain a multifunctional anti-slip layer coating slurry, which is then prepared for use. After coating and curing, a multifunctional anti-slip layer is formed.
[0053] As a preferred embodiment, the modified HDPE substrate layer is made of a blend comprising the following components: 70-90 parts by weight of HDPE resin, 5-15 parts by weight of POE elastomer, 1-5 parts by weight of methyl vinyl silicone rubber, 2-8 parts by weight of compatibilizer, and 1-3 parts by weight of peroxide crosslinking agent.
[0054] In a preferred embodiment of the present invention, the modified HDPE substrate layer is made of a blend comprising the following components: 75-85 parts by weight of HDPE resin, 8-12 parts by weight of POE elastomer, 2-4 parts by weight of methyl vinyl silicone rubber, 3-5 parts by weight of compatibilizer, and 2-3 parts by weight of peroxide crosslinking agent. For example, in a specific preferred embodiment, the modified HDPE substrate layer is made of a blend comprising the following components: 76.5 parts by weight of HDPE resin, 12.5 parts by weight of POE elastomer, 3.5 parts by weight of methyl vinyl silicone rubber, 4 parts by weight of compatibilizer, and 2.5 parts by weight of peroxide crosslinking agent.
[0055] In a preferred embodiment of the present invention, the HDPE resin has a melt index of 0.5-10.5 g / 10 min (weight 21.6 kg) and a density of 0.95-0.97 g / cm³. 3 Tensile yield strength ≥20MPa, elongation at break ≥280% (e.g., Daqing Petrochemical's HDPE 2200J).
[0056] In a preferred embodiment of the present invention, the POE elastomer can be commercially available Dow ENGAGE 8150 or ExxonMobil Exact 9061; the compatibilizer is selected from maleic anhydride grafted polyethylene (PE-g-MAH), for example, in a specific embodiment, commercially available ExxonMobil Exxelor PE 1040 can be used; the peroxide crosslinking agent is selected from dicumyl peroxide or di-tert-butyl peroxide.
[0057] In a preferred embodiment of the present invention, the modified HDPE substrate layer further includes pigments.
[0058] As a preferred embodiment of the present invention, the modified HDPE substrate layer is prepared by the following method: premixing each component in a high-speed mixer in proportion, melting and granulating it in a specific temperature range by a twin-screw extruder, pressing the granules into shape by a flat vulcanizing machine (or using casting film), precisely controlling the thickness (e.g., 0.1-1 mm), and winding it up for later use.
[0059] In a preferred embodiment of the present invention, the acrylate pressure-sensitive adhesive is prepared by polymerization of raw materials comprising the following components: 66-78 parts by weight of soft monomer, 8-12 parts by weight of polyolefin elastomer grafted macromonomer, 8-12 parts by weight of hard monomer, 2-5 parts by weight of functional monomer, 3-8 parts by weight of cold-resistant plasticizer, 0.1-0.5 parts by weight of initiator, and 0.2-1.0 parts by weight of crosslinking agent; wherein the polyolefin elastomer grafted macromonomer includes methacrylate-terminated ethylene / butene elastomer macromonomer;
[0060] Furthermore, the methacrylate-terminated ethylene / butene elastomer macromonomer was prepared by the following method: Under nitrogen protection, hydroxyl-terminated ethylene / butene copolymer diol (such as Kraton L-1203), methacryloyl chloride, and dry toluene were added to a reaction vessel, and triethylamine was added dropwise under ice bath conditions. The reaction was carried out at room temperature for 6-18 hours. The salt was removed by filtration, and the solvent was removed by rotary evaporation to obtain the methacrylate-terminated ethylene / butene elastomer macromonomer.
[0061] The above-mentioned acrylate pressure-sensitive adhesive was prepared by the following method:
[0062] (1) Synthesis of acrylate prepolymer: Soft monomer, hard monomer, functional monomer, polyolefin elastomer grafted macromonomer and some initiator are added to the reactor, solvent is added, and the reaction is carried out at 70-85℃ for 3-6 hours to obtain acrylate prepolymer;
[0063] (2) Cool the obtained acrylate prepolymer to below 40°C, add the cold-resistant plasticizer, the remaining initiator and crosslinking agent, and stir evenly to obtain the adhesive with a solid content of 30-55%. Preferably, the acrylate prepolymer is synthesized using a seed polymerization process.
[0064] In a preferred embodiment of the present invention, the acrylate pressure-sensitive adhesive layer is obtained by polymerization of raw materials comprising the following components: 68-72 parts by weight of soft monomer, 9-11 parts by weight of polyolefin elastomer grafted macromonomer, 8-10 parts by weight of hard monomer, 3-5 parts by weight of functional monomer, 4-6 parts by weight of cold-resistant plasticizer, 0.2-0.4 parts by weight of initiator, and 0.3-0.8 parts by weight of crosslinking agent. For example, in a specific preferred embodiment, the acrylate pressure-sensitive adhesive layer is obtained by polymerization of raw materials comprising the following components: 72 parts by weight of soft monomer, 10 parts by weight of polyolefin elastomer grafted macromonomer, 9 parts by weight of hard monomer, 4 parts by weight of functional monomer, 5 parts by weight of cold-resistant plasticizer, 0.3 parts by weight of initiator, and 0.56 parts by weight of crosslinking agent.
[0065] In a preferred embodiment of the present invention, the soft monomer is selected from one or two of isooctyl acrylate and butyl acrylate; the hard monomer is selected from one or more of methyl methacrylate, acrylonitrile, and styrene; the functional monomer is selected from one or two of acrylic acid and hydroxyethyl methacrylate; the cold-resistant plasticizer is dioctyl adipate or dioctyl sebacate; the crosslinking agent is aluminum acetylacetonate or isocyanate; and the initiator is azobisisobutyronitrile.
[0066] As a preferred embodiment of the present invention, the preparation method of the snow-free anti-slip adhesive material includes the following steps:
[0067] (1) Take an HDPE film with a thickness of 0.1-0.6 mm, treat it with corona on one side, and then apply a layer of acrylic pressure-sensitive adhesive with a thickness of 0.1-0.3 mm. Allow it to cure (touch dry but not completely cured).
[0068] (2) Apply the multifunctional anti-slip coating slurry to the surface of the semi-cured acrylic pressure-sensitive adhesive of the HDPE film, and control the thickness of the slurry coating to be 1.2±0.1 mm;
[0069] (3) After coating, let stand for 15-20 minutes, sprinkle a layer of nano silica aerogel powder on the surface, and press lightly with a rubber roller so that half of the powder volume is embedded in the surface of the elastomer and the other half is exposed, forming a lotus leaf-like nipple-shaped nano-scale rough protrusion. Due to the high density of the aggregate and the particle size being much larger than that of the microcapsules, under the leveling and micro-sinking effect in the early stage of gelation, the aggregate particles sink slightly but still partially protrude from the surface and are completely wrapped by the elastomer; while the microcapsules and volcanic ash microspheres are relatively evenly distributed throughout the entire coating thickness direction, with more of them clustered in the lower part of the coating, forming a gradient functional distribution.
[0070] (4) The coated material is transferred into a temperature and humidity control chamber for curing. It is cured at 40°C and 60% relative humidity for 1-6 hours. The diluent evaporates completely during the curing process to form a flexible interpenetrating polymer network.
[0071] (5) Coat the other side of the HDPE film with an acrylic pressure-sensitive adhesive with a thickness of 0.1-0.6 mm, and then cover it with a release film to obtain the final product.
[0072] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto. All raw materials used in the following embodiments are commercially available products. Experimental methods not specifically described in the embodiments were conducted under conventional conditions. All references to "parts" refer to parts by weight.
[0073] Preparation Example 1
[0074] Prepare multifunctional anti-slip layer slurry sample X1 according to the following steps:
[0075] (1) Preparation of sustained-release microcapsules of de-icing agent
[0076] Grind anhydrous calcium formate and pass it through a 150-mesh sieve. Collect the sieve-passing material for later use. Take ethyl cellulose (Ashland Aqualon)... TM EC-N100 was dissolved in anhydrous ethanol to prepare a 5wt% wall material solution. A fluidized bed bottom spray coating machine was used to add calcium formate powder to the fluidized bed, controlling the material temperature at 35-40℃ and the outlet air temperature at 40-48℃. The wall material solution was sprayed at an atomization pressure of 0.15-0.2 MPa. The coating weight gain was controlled to reach 13% of the core material weight, and the coating rate was above 85% to be considered qualified. After coating, fluidized drying was continued for 10-15 minutes. The material was then discharged, passed through an 80-mesh sieve, and the undersize material was collected to obtain calcium formate sustained-release microcapsules with a particle size of 50-180 μm. These were then sealed, dried, and stored for later use.
[0077] (2) Prepare components A and B
[0078] Component A (solid aggregate premix): Weigh 47 parts by weight of silicon carbide particles (Saint-Gobain Sika80). ® Component A was obtained by dry mixing 7 parts of porous volcanic rock microspheres (Tengchong Yiyuan volcanic ash) and 13 parts of pre-made calcium formate sustained-release microcapsules in a V-type mixer for 15 minutes with a particle size of 0.6-1.2 mm.
[0079] Component B (elastic superhydrophobic matrix fluid): Add 32 parts of silicone-modified polyurethane prepolymer (Wacker GENIOMER) to the dispersion tank. ® 140), 7 parts of fluorocarbon modified acrylate oligomer (DAIKIN ZEFFLE) ®SE-310), stir until homogeneous; slowly add 10 parts of hydrophobic nano-silica aerogel powder (Cabot ENOVA® IC3100), disperse at 1500 rpm for 30 min using a high-speed disperser until the fineness is <20μm; add 13 parts of butyl acetate (industrial grade) to adjust the viscosity, and then add 2.7 parts of HDI trimer curing agent (Covestro Desmodur). ® N 3390 BA), continue dispersion for 10 min; vacuum degassing for 5 min to obtain component B, with viscosity controlled at 4000-6000 mPa·s (25℃).
[0080] (3) Preparation of coating slurry: Under the stirring state of 200-300 rpm, slowly and evenly pour component A into the liquid component B. After the addition is completed, increase the speed to 500 rpm and continue stirring for 15 minutes until the system is a uniform paste without particle agglomeration. The resulting slurry is the material for surface anti-slip coating and is ready for use.
[0081] Preparation Example 2
[0082] Prepare two multifunctional anti-slip layer slurry samples X2 according to the following steps:
[0083] (1) Preparation of sustained-release microcapsules of de-icing agent
[0084] Grind anhydrous calcium acetate and pass it through a 150-mesh sieve. Collect the sieve-passing material for later use. Take ethyl cellulose (Ashland Aqualon...) TM EC-N100 was dissolved in anhydrous ethanol to prepare a 5 wt% wall material solution. A fluidized bed bottom spray coating machine was used to add calcium acetate powder to the fluidized bed, controlling the material temperature at 35-40℃ and the outlet air temperature at 40-48℃. The wall material solution was sprayed at an atomization pressure of 0.15-0.2 MPa. The coating weight gain was controlled to reach 12% of the core material weight, and the coating rate was considered qualified at over 85%. After coating, fluidized drying was continued for 10-15 minutes. The material was then discharged, passed through an 80-mesh sieve, and the undersize material was collected to obtain calcium acetate sustained-release microcapsules with a particle size of 50-180 μm. These were then sealed, dried, and stored for later use.
[0085] (2) Prepare components A and B
[0086] Component A (solid aggregate premix): Weigh 45 parts by weight of silicon carbide particles (Saint-Gobain Sika80). ® Component A was obtained by dry mixing 6 parts of porous volcanic rock microspheres (Tengchong Yiyuan volcanic ash) with a particle size of 0.6-1.2 mm and 12 parts of pre-made calcium acetate sustained-release microcapsules in a V-type mixer for 15 min.
[0087] Component B (elastic superhydrophobic matrix fluid): Add 33 parts of silicone-modified polyurethane prepolymer (Wacker GENIOMER) to the dispersion tank. ® 140), 6 parts of fluorocarbon modified acrylate oligomer (DAIKIN ZEFFLE) ® SE-310), stir until homogeneous; slowly add 9 parts of hydrophobic nano-silica aerogel powder (Cabot ENOVA® IC3100), disperse at 1500 rpm for 30 min using a high-speed disperser until the fineness is <20μm; add 12 parts of butyl acetate (industrial grade) to adjust the viscosity, and then add 2.5 parts of HDI trimer curing agent (Covestro Desmodur). ® N 3390 BA), continue dispersion for 10 min; vacuum degassing for 5 min to obtain component B, with viscosity controlled at 4000-6000 mPa·s (25℃).
[0088] (3) Preparation of coating slurry: Under the stirring state of 200-300 rpm, slowly and evenly pour component A into the liquid component B. After the addition is completed, increase the speed to 500 rpm and continue stirring for 15 minutes until the system is a uniform paste without particle agglomeration. The resulting slurry is the material for surface anti-slip coating and is ready for use.
[0089] Preparation Example 3
[0090] Prepare three multifunctional anti-slip layer slurry samples using the following steps:
[0091] (1) Preparation of sustained-release microcapsules of de-icing agent
[0092] Grind anhydrous calcium formate and pass it through a 150-mesh sieve. Collect the sieve-passing material for later use. Take ethyl cellulose (Ashland Aqualon)... TM EC-N100 was dissolved in anhydrous ethanol to prepare a 5wt% wall material solution. A fluidized bed bottom spray coating machine was used to add calcium formate powder to the fluidized bed, controlling the material temperature at 35-40℃ and the outlet air temperature at 40-48℃. The wall material solution was sprayed at an atomization pressure of 0.15-0.2 MPa. The coating weight gain was controlled to reach 15% of the core material weight, and the coating rate was considered qualified at over 85%. After coating, fluidized drying was continued for 10-15 minutes. The material was then discharged, passed through an 80-mesh sieve, and the undersize material was collected to obtain calcium formate sustained-release microcapsules with a particle size of 50-180 μm. These were then sealed, dried, and stored for later use.
[0093] (2) Prepare components A and B
[0094] Component A (solid aggregate premix): Weigh 50 parts by weight of silicon carbide particles (Saint-Gobain Sika80). ®Component A was obtained by dry mixing 8 parts of porous volcanic rock microspheres (Tengchong Yiyuan volcanic ash) and 14 parts of pre-made calcium formate sustained-release microcapsules in a V-type mixer for 15 minutes with a particle size of 0.6-1.2 mm.
[0095] Component B (elastic superhydrophobic matrix fluid): Add 33 parts of silicone-modified polyurethane prepolymer (Wacker GENIOMER) to the dispersion tank. ® 140), 8 parts of fluorocarbon modified acrylate oligomer (DAIKIN ZEFFLE) ® SE-310), stir until homogeneous; slowly add 11 parts of hydrophobic nano-silica aerogel powder (Cabot ENOVA® IC3100), disperse at 1500 rpm for 30 min using a high-speed disperser until the fineness is <20μm; add 14 parts of butyl acetate (industrial grade) to adjust the viscosity, and then add 3 parts of HDI trimer curing agent (Covestro Desmodur). ® N 3390 BA), continue dispersion for 10 min; vacuum degassing for 5 min to obtain component B, with viscosity controlled at 4000-6000 mPa·s (25℃).
[0096] (3) Preparation of coating slurry: Under the stirring state of 200-300 rpm, slowly and evenly pour component A into the liquid component B. After the addition is completed, increase the speed to 500 rpm and continue stirring for 15 minutes until the system is a uniform paste without particle agglomeration. The resulting slurry is the material for surface anti-slip coating and is ready for use.
[0097] Preparation Example 4
[0098] Compared to Preparation Example 1, this sample does not contain slow-release microcapsules for de-icing agents. All other steps are the same as in Preparation Example 1. Specifically, the following steps were followed to prepare four multifunctional anti-slip layer slurry samples:
[0099] (1) Prepare component A and component B
[0100] Component A (solid aggregate premix): Weigh 47 parts by weight of silicon carbide particles (Saint-Gobain Sika80). ® Component A was obtained by dry mixing 7 parts of porous volcanic rock microspheres (Tengchong Yiyuan volcanic ash) with a particle size of 0.6-1.2 mm in a V-type mixer for 15 min.
[0101] Component B (elastic superhydrophobic matrix fluid): same as in preparation example 1.
[0102] (2) Preparation of coating slurry: Same as in preparation example 1.
[0103] Preparation Example 5
[0104] Compared with Preparation Example 1, the raw material composition in Component B was changed, and the rigid anti-slip aggregate did not acquire hydrophobic properties. The remaining steps were the same as in Preparation Example 1. Specifically, the following steps were followed to prepare multifunctional anti-slip slurry sample X5:
[0105] (1) Preparation of slow-release microcapsules of de-icing agent: Same as preparation example 1.
[0106] (2) Prepare components A and B
[0107] Component A (solid aggregate premix): Same as preparation example 1.
[0108] Component B (conventional matrix liquid): Add 32 parts of polyurethane prepolymer (Covestro Desmophen) to the dispersion tank. ® 670), 7 parts acrylate oligomer (Wantipro from Wanhua Chemical) ® 0612 hydroxyl acrylate resin was dispersed at 1500 rpm for 30 min using a high-speed disperser until the fineness was <20 μm; 13 parts of butyl acetate (industrial grade) were added to adjust the viscosity, and then 2.7 parts of HDI trimer curing agent (Covestro Desmodur) were added. ® N 3390 BA), continue dispersion for 10 min; vacuum degassing for 5 min to obtain component B, with viscosity controlled at 4000-6000 mPa·s (25℃).
[0109] (3) Preparation of coating slurry: Same as in preparation example 1.
[0110] Preparation Example 6
[0111] The modified HDPE substrate sample Y1 was prepared according to the following steps:
[0112] (1) Prepare the raw materials according to the following formula: 76.5 parts HDPE resin (Daqing Petrochemical HDPE 2200J), 12.5 parts POE elastomer (Dow ENGAGE 8150), 3.5 parts methyl vinyl silicone rubber (CAS No.: 68037-87-6), 4 parts compatibilizer ExxonMobil Exxelor PE 1040, 2.5 parts peroxide crosslinking agent dicumyl peroxide (CAS No.: 80-43-3) and a small amount of color masterbatch.
[0113] (2) Add each component to the high-speed mixer according to the proportion, and stir for 5-10 minutes until the material is evenly mixed;
[0114] (3) The mixed materials are put into a twin-screw extruder for melt blending. The extrusion temperature is 180-210℃. The film is extruded and cast through a T-die. The film thickness is controlled at about 0.15mm. The film is then wound up for later use.
[0115] Preparation Example 7
[0116] The acrylic pressure-sensitive adhesive sample Z1 was prepared according to the following steps:
[0117] Prepare the following steps: Mix the soft monomers (36 parts isooctyl acrylate and 36 parts butyl acrylate), the hard monomers (9 parts methyl methacrylate), the functional monomers (4 parts acrylic acid), 10 parts of polyolefin elastomer grafted macromolecular monomers, and 0.2 parts of azobisisobutyronitrile (AIBN) evenly to obtain a monomer mixture for later use; add 100 parts of ethyl acetate solvent to a reaction vessel, add 8 parts of the monomer mixture to the reaction vessel, and gradually heat to 75°C under stirring conditions. Observe the reaction system and start timing from the appearance of foam, reacting for 10 minutes; add the remaining monomer mixture dropwise over 4 hours, and then keep warm for 2 hours to obtain the acrylate prepolymer; cool the obtained acrylate prepolymer to 30°C, add 5 parts of the cold-resistant plasticizer dioctyl sebacate, 0.1 parts of AIBN, and 0.56 parts of the crosslinking agent aluminum acetylacetonate, and stir evenly to obtain acrylate pressure-sensitive adhesive sample 1 for later use.
[0118] The polyolefin elastomer grafted macromonomer is a methacrylate-terminated ethylene / butene elastomer macromonomer, prepared by the following method: Under nitrogen protection, 100 parts by weight of a hydroxyl-terminated ethylene / butene copolymer diol (Kraton, brand name L-1203) with a number-average molecular weight of approximately 3000, 15 parts by weight of methacryloyl chloride, and 100 parts by weight of dry toluene were added to a reaction vessel. 10 parts by weight of triethylamine were added dropwise under ice bath conditions, and the reaction was carried out at room temperature for 12 hours. The salt was removed by filtration, and the solvent was removed by rotary evaporation to obtain the methacrylate-terminated ethylene / butene elastomer macromonomer with a yield of 86%.
[0119] Preparation Example 8
[0120] Acrylic pressure-sensitive adhesive sample Z2 was prepared. Compared with preparation example 7, no polyolefin elastomer grafted macromonomer was added to the raw materials, and all other aspects were the same as preparation example 7.
[0121] Examples 1 to 8
[0122] According to the raw material composition in Table 1, prepare a sample of non-snow-accumulating anti-slip adhesive material following the steps below:
[0123] (1) Take a 0.15 mm thick HDPE film, treat it with corona on one side, and then apply a 0.1 mm thick acrylic adhesive to it for semi-curing.
[0124] (2) Apply the multifunctional anti-slip coating slurry to the surface of the semi-cured acrylic adhesive of the HDPE film, and control the thickness of the slurry coating to 1.2 mm.
[0125] (3) After coating, let stand for 15-20 minutes, sprinkle a layer of nano silica aerogel powder on the surface, the amount of powder sprinkled is 20% of the amount of nano silica aerogel powder in component B, press lightly with a rubber roller, control the pressure, so that half of the powder volume is embedded in the surface of the elastomer and the other half is exposed, forming nano-level rough protrusions in the multifunctional anti-slip layer.
[0126] (4) The coated material is transferred into a temperature and humidity control chamber for curing. It is cured at 40°C and 60% relative humidity for 4 hours. The diluent completely evaporates during the curing process, forming a flexible interpenetrating polymer network.
[0127] (5) Coat the other side of the HDPE film with an acrylic pressure-sensitive adhesive with a thickness of 0.3 mm, and then cover it with a release film to obtain a non-snow-accumulating anti-slip adhesive material sample (E1~E8). Figure 1 This is a photograph of sample E1.
[0128] Table 1. Raw material composition of non-snow-accumulating anti-slip adhesive material
[0129]
[0130] In Table 1, substrate sample Y2 is a commercially available ordinary polyethylene film of the same specification (Guangdong Changtui Niu Film Technology Co., Ltd.); adhesive sample Z3 is a commercially available acrylic pressure-sensitive adhesive (Baolijia BLJ-532).
[0131] [Sample Performance Testing]
[0132] 1. Anti-slip performance test: Conduct a shoe-wearing slope test according to Appendix B of the anti-slip test standard DIN EN 16165:2023-02;
[0133] 2. Low temperature adhesive surface test: Cut the sample into 5cm×10cm long adhesive strips, attach them to the surface of the glass plate, and place them in a constant temperature and humidity chamber set to -40℃ for 72 hours. Observe whether the adhesive surface is peeling or easy to tear. If the adhesive surface is not peeling or easy to tear after ≥72 hours, it is considered qualified.
[0134] 3. Low temperature test: According to IEC60068-2-1:2007 "Environmental testing for electrical and electronic products - Part 2: Test methods - Test A: Low temperature", place the sample in a climate chamber at -40℃ for 288 hours and observe whether the sample shows powdering, delamination, or separation of the adhesive. The tape is qualified if there is no powdering, delamination, or separation of the adhesive.
[0135] 4. Snow accumulation prevention test: Cut the sample into 10cm×10cm blocks and fix them at a 15° angle in a -15℃ cold box environment. Spread 5 g of artificial snow powder (particle size 200-500μm) evenly from 30 cm above. After 30 minutes, observe the snow accumulation on the sample surface and calculate the snow coverage rate. A surface snow coverage rate of <10% is considered qualified.
[0136] 5. Snow Removal Simulation Test: Cut the sample into 10cm×20cm blocks, cover the sample surface with 8 layers of moist medical gauze (saturated with deionized water), freeze at -40℃ for 24 hours to form an ice layer, peel off the gauze manually, and evaluate the ease of peeling.
[0137] The test results are detailed in Table 2.
[0138] Table 2 Sample Test Results
[0139]
[0140] Note: "——" indicates that it has not been tested.
[0141] As shown in Table 2, samples E1-E3 of the embodiments of the present invention achieve the effect of preventing light snow accumulation and easily clearing heavy snow: the superhydrophobic structure makes it difficult for snow particles to adhere and accumulate, resulting in a low snow coverage rate, and the freezing cloth can be easily peeled off in one piece without ice residue. Although sample E4 maintains a certain snow-proofing ability, its de-icing performance deteriorates, requiring force to peel off and leaving a large amount of ice residue; sample E5, which lacks superhydrophobic function, has a high snow coverage rate and is difficult to de-ic. Samples E6-E8 exhibit failure phenomena such as warping and delamination at low temperatures, making it difficult to meet the requirements for use in extremely cold environments.
[0142] To further verify the practical application effect, sample E1, which had the best overall performance, was selected and subjected to outdoor testing in a natural heavy snow environment (results are shown in...). Figure 2 The results showed that after being covered by snow, the surface snow could be easily removed by hand, with no ice residue remaining on the tape surface and no ice embedded in the gaps between the anti-slip particles, demonstrating excellent snow-proof performance.
[0143] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A non-snow-accumulating, anti-slip adhesive material, characterized in that, From top to bottom, it includes a multi-functional anti-slip layer, a substrate layer, and an adhesive layer, wherein: The multifunctional anti-slip layer includes a top layer of superhydrophobic rigid anti-slip aggregate and a bottom layer of slow-release microcapsules embedded with de-icing agent. The substrate layer is modified HDPE; The adhesive layer is an acrylic pressure-sensitive adhesive; The multifunctional anti-slip layer comprises the following raw materials by weight: 40-55 parts of hard anti-slip aggregate, 5-10 parts of volcanic ash porous microspheres, 25-35 parts of silicone-modified polyurethane prepolymer, 8-12 parts of nano-silica aerogel powder, 5-8 parts of fluorocarbon-modified acrylate oligomer, 10-15 parts of sustained-release microcapsules, 1.5-3.5 parts of curing agent, and 8-15 parts of diluent. The silicone-modified polyurethane prepolymer is Wacker Geniomer. ® 140; The multifunctional anti-slip layer is prepared by the following steps: Weigh out the hard anti-slip aggregate, volcanic ash porous microspheres and sustained-release microcapsules by weight, and mix them evenly in a mixer to obtain component A; In a dispersion tank, add silicone-modified polyurethane prepolymer and fluorocarbon-modified acrylate oligomer, stir until uniform, then add nano-silica aerogel powder and disperse at high speed, then add diluent and curing agent and continue dispersion. After uniform dispersion, degas under vacuum to obtain component B. Under stirring conditions, the solid mixture of component A is poured into the liquid of component B, and the mixture is stirred to ensure that the solid particles are uniformly wetted and dispersed to obtain a multifunctional anti-slip coating slurry. After the slurry is coated and cured, a multifunctional anti-slip layer is formed. The modified HDPE substrate layer is made of a blend containing the following components: 70-90 parts by weight of HDPE resin, 5-15 parts by weight of POE elastomer, 1-5 parts by weight of methyl vinyl silicone rubber, 2-8 parts by weight of compatibilizer, and 1-3 parts by weight of peroxide crosslinking agent. The acrylic pressure-sensitive adhesive is prepared by polymerization of raw materials containing the following components: 66-78 parts by weight of soft monomer, 8-12 parts by weight of polyolefin elastomer grafted macromolecular monomer, 8-12 parts by weight of hard monomer, 2-5 parts by weight of functional monomer, 3-8 parts by weight of cold-resistant plasticizer, 0.1-0.5 parts by weight of initiator, and 0.2-1.0 parts by weight of crosslinking agent. The polyolefin elastomer grafted macromonomer includes methacrylate-terminated ethylene / butene elastomer macromonomers.
2. The non-snow-accumulating anti-slip adhesive material according to claim 1, characterized in that, The sustained-release microcapsules include a de-icing agent core material and a wall material with sustained-release function. The de-icing agent core material is selected from acetate-based de-icing agents, and the wall material is selected from ethyl cellulose or urea-formaldehyde resin. The particle size of the sustained-release microcapsules is 50-200 μm.
3. The non-snow-accumulating anti-slip adhesive material according to claim 1, characterized in that, The hard anti-slip aggregate is selected from silicon carbide particles with a particle size of 0.5-1.2 mm; The porous volcanic ash microspheres are selected from samples with a sieve size of 0.2-0.8 mm; The specific surface area of the nano-silica aerogel powder is 200-300 m². 2 / g; The fluorocarbon modified acrylate oligomers are selected from Daikin Industries' ZEFFLE® SE-310 and SE-405. The curing agent is selected from aliphatic or alicyclic polyisocyanates; The diluent is selected from one or more of butyl acetate, dimethyl carbonate, and propylene glycol methyl ether acetate.
4. The non-snow-accumulating anti-slip adhesive material according to claim 1, characterized in that, The HDPE resin has a melt flow index of 0.5-10.5 g / 10 min and a density of 0.95-0.97 g / cm³. 3 ; The compatibilizer is selected from maleic anhydride-grafted polyethylene; The peroxide crosslinking agent is selected from dicumyl peroxide and bis-tert-butyl peroxide.
5. The method for preparing a non-snow-accumulating anti-slip adhesive material as described in claim 1, characterized in that, Includes the following steps: (1) Take an HDPE film, treat it with corona on one side, then coat it with a layer of acrylic pressure-sensitive adhesive and allow it to cure semi-cured; (2) Apply the multifunctional anti-slip coating slurry to the surface of the semi-cured acrylic pressure-sensitive adhesive of the HDPE film; (3) After coating, let stand, sprinkle a layer of nano silica aerogel powder on the surface, and press lightly with a rubber roller so that half of the powder volume is embedded in the surface of the elastomer and the other half is exposed to form nano-scale rough protrusions. (4) Transfer the coated material into a temperature and humidity control chamber for curing; (5) Coat the other side of the HDPE film with acrylic pressure-sensitive adhesive, and then cover it with a release film to obtain the final product.
6. The application of the non-snow-accumulating anti-slip adhesive material as described in claim 1, characterized in that, The anti-slip adhesive material is used as an anti-slip tape.
Citation Information
Patent Citations
Preparation method of super-hydrophobic anti-icing polyurethane urea elastomer coating that can be quickly constructed under low temperature environment
CN116535956B
Bionic super-hydrophobic self-cleaning ice and snow prevention coating as well as preparation method and application thereof
CN118421141A
Waterproof and breathable coating for leather and preparation method of waterproof and breathable coating
CN119799142A