Edge-emitting semiconductor laser and its fabrication method

By employing a combined structure of optical dielectric reflective film and metal reflective film in the edge-emitting semiconductor laser, the problems of low absorption, high reflection, low stress and high reliability of reflective composite films are solved, thereby improving the stability and reliability of the laser.

CN122763153BActive Publication Date: 2026-11-17EVERBRIGHT INST OF SEMICON PHOTONICS CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611223566.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17
Estimated Expiration
2046-08-13

AI Technical Summary

Technical Problem

Existing edge-emitting semiconductor lasers have shortcomings in achieving a balance between low absorption, high reflection, low stress, and high reliability of reflective composite films.

Method used

The reflective composite film structure is adopted, including an optical medium reflective film and a metal reflective film. The optical medium reflective film is close to the rear cavity surface of the light-emitting body, while the metal reflective film is far away from the light-emitting body. Most of the laser light is reflected by the optical medium reflective film, and the remaining light is reflected by the metal reflective film, which reduces the impact of heat on the rear cavity surface. The interfacial adhesive layer improves the bonding stability of the film layers.

Benefits of technology

This achieves low absorption, high reflection, low stress, and high reliability of the reflective composite film, reducing the risk of back cavity surface heating and improving the stability and reliability of the laser.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122763153B_ABST
    Figure CN122763153B_ABST
Patent Text Reader

Abstract

This invention provides a side-emitting semiconductor laser and its fabrication method. The side-emitting semiconductor laser includes: a light-emitting body having a front cavity surface and a rear cavity surface disposed opposite to each other along the cavity length direction; and a reflective composite film covering the rear cavity surface. The reflective composite film includes: an optical dielectric reflective film comprising a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction, wherein the refractive index of the second optical dielectric film is different from that of the first optical dielectric film; and a metal reflective film located on the side of the optical dielectric reflective film opposite to the light-emitting body along the cavity length direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and more specifically to a side-emitting semiconductor laser and its fabrication method. Background Technology

[0002] The edge-emitting semiconductor light-emitting structure includes a semiconductor substrate layer, a lower confinement layer, a lower waveguide layer, an active layer, an upper waveguide layer, and an upper confinement layer stacked in the fast axis direction. The front cavity surface of the edge-emitting semiconductor light-emitting structure is covered with an anti-reflection film, and the rear cavity surface of the edge-emitting semiconductor light-emitting structure is covered with a reflective film. Summary of the Invention

[0003] The technical problem addressed by this application is how to balance the advantages of low absorption, high reflection, low stress, and high reliability of reflective composite films.

[0004] This application provides a side-emitting semiconductor laser, which includes a light-emitting body and a reflective composite film. The light-emitting body has a front cavity surface and a rear cavity surface disposed opposite to each other along the cavity length direction, and the reflective composite film covers the rear cavity surface. The reflective composite film includes an optical dielectric reflective film and a metal reflective film. The optical dielectric reflective film includes a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction. The refractive index of the second optical dielectric film is different from that of the first optical dielectric film. The metal reflective film is located on the side of the optical dielectric reflective film opposite to the light-emitting body along the cavity length direction.

[0005] Optionally, the absorption rate of the optical medium reflective film is lower than that of the metal reflective film.

[0006] Optionally, the optical thickness of the single-layer first optical dielectric film in the cavity length direction is 0.5 to 1.5 times λ0 / 4; the optical thickness of the single-layer second optical dielectric film in the cavity length direction is 0.5 to 1.5 times λ0 / 4; where λ0 is the center wavelength of the emitted light from the edge-emitting semiconductor laser.

[0007] Optionally, the refractive index of the second optical dielectric film is greater than that of the first optical dielectric film; the material of the second optical dielectric film includes any one of ZnSe, ZnS, and Ge; wherein, when the material of the second optical dielectric film is ZnSe or ZnS, the material of the first optical dielectric film is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, and Ca-doped or Ba-doped YbF3; when the material of the second optical dielectric film is Ge, the material of the first optical dielectric film is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, Ca-doped or Ba-doped YbF3, ZnSe, or ZnS.

[0008] Optionally, the thickness of the metal reflective film in the cavity length direction is 50nm~250nm.

[0009] Optionally, the material of the metal reflective film can be Au or Ag.

[0010] Optionally, the reflective composite film further includes a first optical medium adhesive layer, which is located between the optical medium reflective film and the light-emitting body along the cavity length direction and is in contact with a first optical medium film of the optical medium reflective film and the light-emitting body. The material of the first optical medium adhesive layer is different from the material of the first optical medium film.

[0011] Optionally, the material of the first optical medium adhesive layer is Y2O3, Al2O3, ZnSe or ZnS.

[0012] Optionally, the thickness of the first optical medium adhesive layer along the cavity length direction is 10nm~30nm.

[0013] Optionally, the reflective composite film further includes a first metal adhesive layer, which is located between and in contact with the metal reflective film and the optical medium reflective film; wherein the adhesive strength between the materials of the first metal adhesive layer and the optical medium reflective film is greater than the adhesive strength between the materials of the metal reflective film and the optical medium reflective film, the reflectivity of the material of the first metal adhesive layer is less than the reflectivity of the material of the metal reflective film, and the dimension of the first metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

[0014] Optionally, the material of the first metal adhesive layer is Ti or Cr.

[0015] Optionally, the thickness of the first metal adhesive layer along the cavity length direction is 2nm~10nm.

[0016] Optionally, the reflective composite film may also include an insulating dielectric protective layer, which is located on the side of the metal reflective film opposite to the optical dielectric reflective film along the cavity length direction.

[0017] Optionally, the reflective composite film further includes a second metal adhesive layer, which is located between and in contact with the metal reflective film and the insulating dielectric protective layer; wherein the adhesive strength between the materials of the second metal adhesive layer and the insulating dielectric protective layer is greater than the adhesive strength between the materials of the metal reflective film and the insulating dielectric protective layer, the reflectivity of the material of the second metal adhesive layer is less than the reflectivity of the material of the metal reflective film, and the dimension of the second metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

[0018] Optionally, the optical thickness of the reflective composite film along the cavity length direction is less than or equal to 2λ0, where λ0 is the center wavelength of the emitted light from the edge-emitting semiconductor laser.

[0019] Optionally, the edge-emitting semiconductor laser also includes an anti-reflection composite film covering the front cavity surface; wherein the anti-reflection composite film includes an optical dielectric anti-reflection film and a second optical dielectric adhesive layer located between the optical dielectric anti-reflection film and the light-emitting body.

[0020] Optionally, the material of the second optical medium adhesive layer is Y2O3, Al2O3, ZnSe or ZnS.

[0021] Optionally, the thickness of the second optical medium adhesive layer along the cavity length direction is 10nm~30nm.

[0022] This application also provides a method for fabricating a side-emitting semiconductor laser, comprising: forming a light-emitting body having a front cavity surface and a rear cavity surface disposed opposite to each other along the cavity length direction; and forming a reflective composite film covering the rear cavity surface; wherein forming the reflective composite film includes: forming an optical dielectric reflective film covering the rear cavity surface, the optical dielectric reflective film including a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction, the refractive index of the second optical dielectric film being different from that of the first optical dielectric film; and forming a metal reflective film on the side of the optical dielectric reflective film opposite to the light-emitting body along the cavity length direction.

[0023] Optionally, the preparation method further includes: before forming the optical medium reflective film, forming a first optical medium adhesive layer covering the rear cavity surface, wherein the material of the first optical medium adhesive layer is different from the material of the first optical medium film, and the first optical medium adhesive layer is in contact with a layer of the first optical medium film of the optical medium reflective film and the light-emitting body.

[0024] Optionally, the preparation method further includes: before forming the metal reflective film, forming a first metal adhesive layer on the side of the optical medium reflective film away from the light-emitting body, wherein the adhesive strength between the material of the first metal adhesive layer and the material of the optical medium reflective film is greater than the adhesive strength between the material of the metal reflective film and the material of the optical medium reflective film, the reflectivity of the material of the first metal adhesive layer is less than the reflectivity of the material of the metal reflective film, and the dimension of the first metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

[0025] Optionally, the preparation method further includes: forming a second metal adhesive layer on the side of the metal reflective film opposite to the optical medium reflective film along the cavity length direction; forming an insulating medium protective layer on the side of the second metal adhesive layer opposite to the metal reflective film along the cavity length direction; wherein the adhesive strength between the materials of the second metal adhesive layer and the insulating medium protective layer is greater than the adhesive strength between the materials of the metal reflective film and the insulating medium protective layer, the reflectivity of the material of the second metal adhesive layer is less than the reflectivity of the material of the metal reflective film, and the dimension of the second metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

[0026] Optionally, the preparation method further includes: forming an antireflection composite film covering the front cavity surface, and including: forming a second optical medium adhesive layer covering the front cavity surface; and forming an optical medium antireflection film on the side of the second optical medium adhesive layer away from the light-emitting body along the cavity length direction.

[0027] The technical solution of this invention has the following beneficial effects: The edge-emitting semiconductor laser provided by this invention includes a reflective composite film comprising an optical dielectric reflective film and a metal reflective film. The optical dielectric reflective film is positioned closer to the back cavity surface of the light-emitting body than the metal reflective film. This closer proximity reflects most of the laser light from the back cavity surface, reducing the light intensity reaching the metal reflective film. The metal reflective film reflects any remaining light transmitted through the optical dielectric reflective film. Because the metal reflective film is farther from the light-emitting body than the optical dielectric reflective film, it reduces the heat generated by the metal reflective film's light absorption, thus minimizing the risk of overheating at the back cavity surface. Furthermore, the optical dielectric reflective film has a lower absorptivity and generates less heat, reducing its impact on the back cavity surface temperature. Therefore, the thermal influence of the reflective composite film on the back cavity surface temperature is reduced. Secondly, while ensuring high reflectivity, the presence of the metal reflective film simplifies the need for a large thickness of the optical dielectric reflective film along the cavity length, reducing stress accumulation and minimizing the likelihood of cracking or delamination. In summary, it can combine the advantages of low absorption, high reflection, low stress, and high reliability of reflective composite films. Attached Figure Description

[0028] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0029] Figure 1 This is a schematic diagram of a side-emitting semiconductor laser according to an embodiment of this application; Figure 2 For along Figure 1 Cross-sectional view of the secant line MN; Figure 3 This is a schematic diagram of a side-emitting semiconductor laser according to another embodiment of this application; Figure 4 For along Figure 3 Cross-sectional view of the cutting line M1-N1; Figures 5 to 9 This is a schematic diagram illustrating the fabrication process of a side-emitting semiconductor laser according to another embodiment of this application; Figures 10 to 14 This is a schematic diagram illustrating the fabrication process of a side-emitting semiconductor laser according to another embodiment of this application; Figure 15 This is a schematic diagram showing the variation of reflectivity and absorptivity of the reflective composite film of the edge-emitting semiconductor laser with wavelength in this embodiment; Figure 16 This is a schematic diagram illustrating the variation of reflectivity and absorptivity of the reflective film of a side-emitting semiconductor laser as a function of wavelength, in a comparative example. Detailed Implementation

[0030] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0032] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0033] One embodiment of the present invention provides a side-emitting semiconductor laser, referenced to... Figures 1 to 4 ,include: The light-emitting body has a front cavity surface and a rear cavity surface that are arranged opposite to each other along the length of the cavity; A 400mm reflective composite film covers the rear cavity surface; The reflective composite film 400 includes: The optical dielectric reflective film 420 includes a first optical dielectric film 4201 and a second optical dielectric film 4202 alternately stacked in the cavity length direction Y, wherein the refractive index of the second optical dielectric film 4202 is different from that of the first optical dielectric film 4201; and The metal reflective film 440 is located on the side of the optical medium reflective film 420 that is opposite to the light-emitting body along the cavity length direction Y.

[0034] In this embodiment, the reflective composite film 400 includes an optical medium reflective film 420 and a metal reflective film 440. The optical medium reflective film 420 is closer to the rear cavity surface of the light-emitting body than the metal reflective film 440. The optical medium reflective film 420, being closer to the rear cavity surface, reflects most of the laser light from the rear cavity surface, reducing the light intensity reaching the metal reflective film 440 from the rear cavity surface. The metal reflective film 440 reflects the remaining light transmitted through the optical medium reflective film 420. Because the metal reflective film 440 is farther from the light-emitting body than the optical medium reflective film 420, the heat generated by the metal reflective film 440's light absorption can be reduced, thus decreasing the temperature impact on the rear cavity surface. Furthermore, the optical medium reflective film 420 has a lower absorptivity and generates less heat, reducing its influence on the temperature of the rear cavity surface. Therefore, the temperature of the rear cavity surface is less affected by the heat generated by the reflective composite film 400, reducing the risk of overheating. Secondly, while ensuring high reflectivity of the reflective composite film 400, the presence of the metal reflective film 440 necessitates a smaller thickness of the optical medium reflective film 420 along the cavity length Y, reducing stress accumulation and minimizing the likelihood of cracking or delamination. In summary, this approach achieves a balance between the advantages of low absorption, high reflectivity, low stress, and high reliability of the reflective composite film 400.

[0035] In this embodiment, the side-emitting semiconductor laser can be a side-emitting quantum cascade semiconductor laser. The emission band of the side-emitting semiconductor laser can be the long infrared band, such as 8 micrometers to 12 micrometers.

[0036] A quantum cascade laser (QCL) is a unipolar semiconductor laser that primarily operates in the long infrared band. The resonant cavity of a QCL is typically a Fabry-Perot cavity, constructed from cleaved cavity surfaces. The active layer of a QCL consists of periodic units stacked in the fast axis Z-axis, with hundreds to thousands of periodic units per layer. Each periodic unit includes a gain region and an injection region. The gain region employs a multi-quantum-well design, forming an upper laser level, a lower laser level, and a rapidly evacuated lower level. The injection region is a doped superlattice used for efficient electron transport.

[0037] The operating principle of a quantum cascaded laser is based on interband transitions between conduction bands and subbands in the gain region. Driven by an external electric field, an electron is injected into the upper laser level in the gain region and radiatively transitions to the lower laser level, emitting a photon. The lower laser level is rapidly evacuated through phonon scattering, achieving population inversion. The electron then enters the upper laser level of the gain region in the next periodic unit via the injection region; a single electron can generate photons multiple times, forming a cascaded gain. This design allows the wavelength to depend only on the thickness of the quantum well, supporting high-power output at room temperature.

[0038] In other embodiments, the edge-emitting semiconductor laser may not be an edge-emitting quantum cascade semiconductor laser, but other types of edge-emitting semiconductor lasers.

[0039] In this embodiment, reference Figures 1 to 4 The light-emitting body includes a lower confinement layer 130, a lower buffer layer 141, an active layer 151, an upper buffer layer 161, an upper confinement layer 171, and a contact layer 181 stacked sequentially along the fast axis direction Z. The lower buffer layer 141, active layer 151, upper buffer layer 161, upper confinement layer 171, and contact layer 181 are located on one side of the lower confinement layer 130 along the fast axis direction Z. The light-emitting body also includes an insulating confinement layer 194 located on one side of the lower confinement layer 130 along the fast axis direction Z. The insulating confinement layer 194 is located on both sides of the lower buffer layer 141, active layer 151, upper buffer layer 161, upper confinement layer 171, and contact layer 181 along the slow axis direction X. The light-emitting body also includes a front electrode 200 located on the side of the contact layer 181 opposite to the upper confinement layer 171 and on the side of the insulating confinement layer 194 opposite to the lower confinement layer 130. The light-emitting body also includes an insulating layer 193 located between the insulating limiting layer 194 and the front electrode 200.

[0040] refer to Figures 1 to 4 The light-emitting body also includes a semiconductor substrate layer 100 located on the side of the lower confinement layer 130 opposite to the lower buffer layer 141.

[0041] refer to Figures 1 to 4 The light-emitting body also includes a back electrode 210 located on the side of the lower confinement layer 130 opposite to the lower buffer layer 141. For example, see reference. Figure 1 and Figure 2 The back electrode 210 is located on the side of the semiconductor substrate 100 opposite to the lower confinement layer 130. (Reference) Figure 1 and Figure 2 The light-emitting body may further include a buffer layer 110 located between the semiconductor substrate layer 100 and the lower confinement layer 130. (Reference) Figure 3 and Figure 4 In a side-emitting semiconductor laser, a semiconductor substrate layer may not be provided, and the back electrode 210 is in contact with the lower confinement layer 130.

[0042] In some embodiments, the semiconductor substrate 100 is an N-type InP substrate.

[0043] In some embodiments, the material of the buffer layer 110 is N-type InP.

[0044] In some embodiments, the edge-emitting semiconductor laser is an edge-emitting quantum cascade semiconductor laser, and the lower confinement layer 130, lower buffer layer 141, upper buffer layer 161, upper confinement layer 171 and contact layer 181 have the same doping type. For example, the lower confinement layer 130, lower buffer layer 141, upper buffer layer 161, upper confinement layer 171 and contact layer 181 are N-type doped, and Si elements may be doped in the lower confinement layer 130, lower buffer layer 141, upper buffer layer 161, upper confinement layer 171 and contact layer 181.

[0045] In some embodiments, the material of the lower limiting layer 130 is, for example, N-type InP. The material of the upper limiting layer 171 is, for example, N-type InP. The material of the lower buffer layer 141 is, for example, N-type In. x2 Ga 1-x2 As y2 The material of the upper buffer layer 161 can be, for example, N-type In. x2 Ga 1-x2 As y2 .

[0046] In other embodiments, the lower confinement layer 130 and the lower buffer layer 141 have the same doping type, the upper buffer layer 161, the upper confinement layer 171 and the contact layer 181 have the same doping type, and the lower confinement layer 130 and the upper confinement layer 171 have opposite doping types.

[0047] In some embodiments, the active layer 151 includes a quantum barrier layer and a quantum well. The quantum well can be made of In... x3 Ga 1-x3 As y3 The material of the quantum barrier layer can be In x4 Al 1-x4 As y4 .

[0048] In some embodiments, the side-emitting semiconductor laser is a side-emitting quantum cascade laser, and the active layer 151 includes periodic units stacked in the fast axis direction Z, for example, the active layer 151 consists of hundreds to thousands of periodic units, each periodic unit including a gain region and an injection region. The gain region employs a multi-quantum-well design to form an upper laser level, a lower laser level, and a rapidly evacuated lower level; the injection region is a doped superlattice, and the injection region is used for efficient electron transport.

[0049] In some embodiments, the material of the insulating confinement layer 194 includes Fe-doped InP.

[0050] In some embodiments, the material of the insulating layer 193 may be silicon oxide, silicon nitride, silicon oxynitride, or silicon oxycarbide.

[0051] In some embodiments, the optical thickness of the reflective composite film 400 along the cavity length direction Y is less than or equal to 2λ0, where λ0 is the center wavelength of the light emitted by the edge-emitting semiconductor laser. While ensuring high reflectivity of the reflective composite film 400, the thickness of the optical medium reflective film 420 along the cavity length direction Y is not required to be too large due to the presence of the metal reflective film 440, thus reducing the total thickness of the reflective composite film 400 along the cavity length direction Y.

[0052] In this embodiment, the absorption rate of the optical medium reflective film 420 is less than that of the metal reflective film 440. Specifically, the absorption rate of the light emitted by the light-emitting subject by the optical medium reflective film 420 is less than that of the light emitted by the light-emitting subject by the metal reflective film 440.

[0053] In this embodiment, the optical medium reflective film 420 plays a reflective role through optical interference effect. The optical medium reflective film 420 near the rear cavity surface reflects most of the laser light from the rear cavity surface, reduces the light intensity reaching the metal reflective film 440 from the rear cavity surface, improves the overall reflectivity of the reflective composite film 400, and reduces the impact of the heat generated by the metal reflective film 440 absorbing light on the temperature of the rear cavity surface.

[0054] In some embodiments, the optical thickness of the monolayer first optical dielectric film 4201 in the cavity length direction Y is 0.5 to 1.5 times λ0 / 4; the optical thickness of the monolayer second optical dielectric film 4202 in the cavity length direction Y is 0.5 to 1.5 times λ0 / 4; wherein λ0 is the center wavelength of the emitted light of the edge-emitting semiconductor laser.

[0055] In some embodiments, the optical thickness of the optical dielectric reflective film 420 in the cavity length direction Y is greater than or equal to 0.5 times λ0. Maintaining a certain distance between the metal reflective film 440 and the rear cavity surface of the light-emitting body further reduces the impact of the heat generated by the metal reflective film 440 absorbing light on the temperature of the rear cavity surface, thereby reducing the risk of overheating of the rear cavity surface. Furthermore, the optical thickness of the optical dielectric reflective film 420 in the cavity length direction Y is greater than or equal to 0.5 times λ0 and less than or equal to 1.5 times λ0.

[0056] The optical dielectric reflective film 420 is made of a low-absorption transparent dielectric material. For example, the optical dielectric reflective film 420 is made of a low-absorption transparent dielectric material suitable for the long-wave infrared band. This helps to reduce the absorption of laser light by the optical dielectric reflective film 420, reduce back cavity surface heating, and improve the stability of the side-emitting semiconductor laser under high power, high temperature rise, or long-term operating conditions. For example, the optical dielectric reflective film 420 is made of a low-absorption transparent dielectric material with an absorption rate of less than 1%. Specifically, the absorption rate of the low-absorption transparent dielectric material for the light emitted by the light-emitting body is less than 1%.

[0057] In some embodiments, the refractive index of the second optical dielectric film 4202 is greater than that of the first optical dielectric film 4201. The material of the second optical dielectric film 4202 includes any one of ZnSe, ZnS, and Ge. Specifically, when the material of the second optical dielectric film 4202 is ZnSe or ZnS, the material of the first optical dielectric film 4201 is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, and Ca-doped or Ba-doped YbF3; when the material of the second optical dielectric film 4202 is Ge, the material of the first optical dielectric film 4201 is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, Ca-doped or Ba-doped YbF3, ZnSe, or ZnS.

[0058] In some embodiments, the thickness of the metal reflective film 440 in the cavity length direction Y is 50 nm to 250 nm. A thickness greater than or equal to 50 nm in the cavity length direction Y of the metal reflective film 440 reduces the risk of light leakage; a thickness less than or equal to 250 nm in the cavity length direction Y of the metal reflective film 440 reduces material costs; and a thickness of 50 nm to 250 nm in the cavity length direction Y of the metal reflective film 440 optimizes both material cost and the risk of light leakage.

[0059] In some embodiments, the metal reflective film 440 is made of Au or Ag. This improves the reflectivity of the metal reflective film 440. The material of the metal reflective film 440 is not limited to these.

[0060] In some embodiments, for light emitted by the light-emitting body, the reflectivity of the metal reflective film 440 is greater than that of the optical medium reflective film 420, or the reflectivity of the metal reflective film 440 is equal to that of the optical medium reflective film 420, or the reflectivity of the metal reflective film 440 is less than that of the optical medium reflective film 420.

[0061] In some embodiments, the dimension of the optical medium reflective film 420 along the cavity length direction is greater than the dimension of the metal reflective film 440 along the cavity length direction.

[0062] In some embodiments, reference Figure 2 and Figure 4 The reflective composite film 400 further includes a first optical medium adhesive layer 410. The first optical medium adhesive layer 410 is located along the cavity length Y between the optical medium reflective film 420 and the light-emitting body, and is in contact with a first optical medium film 4201 of the optical medium reflective film 420 and the light-emitting body. The material of the first optical medium adhesive layer 410 is different from the material of the first optical medium film 4201. The first optical medium adhesive layer 410 is used to improve the interfacial bonding performance between the optical medium reflective film 420 and the light-emitting body, reducing the risk of the optical medium reflective film 420 detaching from the rear cavity surface.

[0063] In some embodiments, the adhesive strength between the material of the first optical dielectric adhesive layer 410 and the material of the light-emitting body is greater than the adhesive strength between the material of the first optical dielectric film 4201 and the material of the light-emitting body. The adhesive strength between the material of the first optical dielectric adhesive layer 410 and the material of the light-emitting body is greater than the adhesive strength between the material of the second optical dielectric film 4202 and the material of the light-emitting body.

[0064] In some embodiments, the first optical dielectric adhesive layer 410 is made of a low-absorption transparent dielectric material, such as a low-absorption transparent dielectric material suitable for the long-wave infrared band. This helps reduce the absorption of laser light by the first optical dielectric adhesive layer 410, reduces back cavity surface heating, and improves the stability of the side-emitting semiconductor laser under high power, high temperature rise, or long-term operating conditions. The first optical dielectric adhesive layer 410 is made of a low-absorption transparent dielectric material with an absorption rate of less than 1%. Specifically, the absorption rate of the low-absorption transparent dielectric material for the light emitted by the light-emitting body is less than 1%.

[0065] In some embodiments, the material of the first optical medium adhesive layer 410 is Y2O3, Al2O3, ZnSe or ZnS.

[0066] In some embodiments, when the first optical dielectric film 4201 is selected from Y2O3, Al2O3, ZnSe or ZnS, the adhesion strength between the material of the first optical dielectric film 4201 and the material of the light-emitting body is good, and the first optical dielectric adhesive layer 410 may not be used.

[0067] When the first optical medium adhesive layer 410 is provided, the material of the optical medium reflective film 420 can be selected from a wide range.

[0068] In some embodiments, the thickness of the first optical dielectric adhesive layer 410 along the cavity length direction Y is less than the thickness of the monolayer first optical dielectric film 4201 along the cavity length direction Y. The thickness of the first optical dielectric adhesive layer 410 along the cavity length direction Y is less than the thickness of the monolayer second optical dielectric film 4202 along the cavity length direction Y. For example, the thickness of the first optical dielectric adhesive layer 410 along the cavity length direction Y is 10 nm to 30 nm.

[0069] In some embodiments, reference Figure 2 and Figure 4 The reflective composite film 400 further includes a first metal adhesive layer 430, which is located between and in contact with both the metal reflective film 440 and the optical medium reflective film 420. The adhesive strength between the materials of the first metal adhesive layer 430 and the optical medium reflective film 420 is greater than that between the materials of the metal reflective film 440 and the optical medium reflective film 420. The reflectivity of the material of the first metal adhesive layer 430 is less than that of the material of the metal reflective film 440, and the dimension of the first metal adhesive layer 430 along the cavity length direction is smaller than that of the metal reflective film 440 along the cavity length direction. The first metal adhesive layer 430 improves the adhesion between the optical medium reflective film 420 and the metal reflective film 440, reducing the risk of peeling due to interface mismatch between the two films.

[0070] In some embodiments, the material of the first metal adhesive layer 430 is Ti or Cr.

[0071] In some embodiments, the thickness of the first metal adhesive layer 430 along the cavity length direction Y is less than the thickness of the metal reflective film 440 along the cavity length direction Y. For example, the thickness of the first metal adhesive layer 430 along the cavity length direction Y is 2nm to 10nm, such as 2nm, 4nm, 6nm, 8nm, or 10nm. While meeting the adhesion performance requirements of the first metal adhesive layer 430, the first metal adhesive layer 430 is not excessively large, thus reducing the overall size of the reflective composite film 400 along the cavity length direction.

[0072] In some embodiments, reference Figure 2 and Figure 4 The reflective composite film 400 also includes an insulating dielectric protective layer 460, which is located on the side of the metal reflective film 440 facing away from the optical dielectric reflective film 420 along the cavity length direction Y. The insulating dielectric protective layer 460 is used to protect the metal reflective film 440 and reduce the risk of the metal reflective film 440 being oxidized, contaminated, or corroded by the environment. The thickness of the insulating dielectric protective layer 460 in the cavity length direction Y can be set according to actual protection requirements, and this embodiment does not impose a specific limitation.

[0073] In some embodiments, the material of the insulating dielectric protective layer 460 may be silicon oxide, silicon nitride, silicon oxynitride, or silicon oxycarbide.

[0074] In some embodiments, reference Figure 2 and Figure 4 The reflective composite film 400 further includes a second metal adhesive layer 450, which is located between and in contact with both the metal reflective film 440 and the insulating dielectric protective layer 460. The adhesive strength between the materials of the second metal adhesive layer 450 and the insulating dielectric protective layer 460 is greater than that between the materials of the metal reflective film 440 and the insulating dielectric protective layer 460. The reflectivity of the material of the second metal adhesive layer 450 is less than that of the material of the metal reflective film 440, and the dimension of the second metal adhesive layer 450 along the cavity length direction is smaller than that of the metal reflective film 440 along the cavity length direction. The second metal adhesive layer 450 improves the adhesion between the insulating dielectric protective layer 460 and the metal reflective film 440, reducing the risk of peeling due to interface mismatch between the two layers.

[0075] In some embodiments, the material of the second metal adhesive layer 450 is Ti or Cr.

[0076] In some embodiments, the thickness of the second metal adhesive layer 450 along the cavity length direction Y is less than the thickness of the metal reflective film 440 along the cavity length direction Y. For example, the thickness of the second metal adhesive layer 450 along the cavity length direction Y is 2nm to 10nm, such as 2nm, 4nm, 6nm, 8nm, or 10nm. While meeting the adhesion performance requirements of the second metal adhesive layer 450, the second metal adhesive layer 450 is not excessively large, thus reducing the overall size of the reflective composite film 400 along the cavity length direction.

[0077] The present invention improves the bonding stability between different film layer interfaces by setting a first optical medium adhesive layer 410 between the light-emitting body and the optical medium reflective film 420, setting a first metal adhesive layer 430 between the metal reflective film 440 and the optical medium reflective film 420, and setting a second metal adhesive layer 450 between the metal reflective film 440 and the insulating medium protective layer 460. This reduces the risk of film peeling, cracking and delamination, and is beneficial to improving the reliability of the reflective composite film 400 during long-term operation.

[0078] In some embodiments, reference Figure 2 and Figure 4The edge-emitting semiconductor laser also includes an antireflection composite film 300 covering the front cavity surface. The antireflection composite film 300 includes an optical dielectric antireflection film 320 and a second optical dielectric adhesive layer 310 located between the optical dielectric antireflection film 320 and the light-emitting host. The second optical dielectric adhesive layer 310 improves the interface compatibility between the optical dielectric antireflection film 320 and the light-emitting host, enhances the adhesion of the optical dielectric antireflection film 320, and reduces the risk of cracking, peeling, or delamination of the optical dielectric antireflection film 320. The second optical dielectric adhesive layer 310 and the optical dielectric antireflection film 320 are made of different materials.

[0079] In some embodiments, the antireflective coating 320 and the second optical dielectric adhesive layer 310 are made of a low-absorption transparent dielectric material. For example, the antireflective coating 320 and the second optical dielectric adhesive layer 310 are made of a low-absorption transparent dielectric material suitable for the long-wave infrared band. This helps to reduce the absorption of laser light by the antireflective coating 320 and the second optical dielectric adhesive layer 310, reduce front cavity surface heating, and improve the stability of the side-emitting semiconductor laser under high power, high temperature rise, or long-term operating conditions. For example, the second optical dielectric adhesive layer 310 is made of a low-absorption transparent dielectric material with an absorption rate of less than 1%. Specifically, the absorption rate of the low-absorption transparent dielectric material for the light emitted by the light-emitting body is less than 1%.

[0080] In some embodiments, the transmittance of the material of the optical medium antireflection film 320 is greater than the transmittance of the material of the second optical medium adhesive layer 310. For example, for light emitted by the light-emitting subject, the transmittance of the material of the optical medium antireflection film 320 is greater than the transmittance of the material of the second optical medium adhesive layer 310. The adhesive strength between the material of the second optical medium adhesive layer 310 and the material of the light-emitting subject is greater than the adhesive strength between the material of the optical medium antireflection film 320 and the material of the light-emitting subject.

[0081] In some embodiments, the material of the second optical medium adhesive layer 310 is Y2O3, Al2O3, ZnSe or ZnS.

[0082] In some embodiments, the thickness of the second optical medium adhesive layer 310 along the cavity length direction Y is less than the thickness of the optical medium antireflection film 320 along the cavity length direction Y. For example, the thickness of the second optical medium adhesive layer 310 along the cavity length direction is 10 nm to 30 nm.

[0083] In some embodiments, the optical dielectric antireflection film 320 is used to reduce the reflectivity of the front cavity surface. The optical dielectric antireflection film 320 can be a transparent dielectric layer. The materials of the optical dielectric antireflection film 320 include Y2O3, Al2O3, ZnSe, ZnS, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, and Ca-doped or Ba-doped YbF3.

[0084] It should be noted that when the material of the optical medium antireflection film 320 is Y2O3, Al2O3, ZnSe or ZnS, the adhesion strength between the material of the optical medium antireflection film 320 and the material of the light-emitting body is good, so the second optical medium adhesive layer 310 is not required.

[0085] When the second optical medium adhesive layer 310 is provided, the material of the optical medium antireflection film 320 can be selected from a wide range.

[0086] The thickness of the optical medium antireflective coating 320 along the cavity length Y can be designed according to the target operating wavelength, target reflectivity, and refractive index of the coating material.

[0087] Figure 15 This is a schematic diagram showing the variation of reflectivity and absorptivity of the reflective composite film of the edge-emitting semiconductor laser with wavelength in this embodiment. Figure 16 This is a schematic diagram illustrating the variation of reflectivity and absorptivity of the reflective film of the side-emitting semiconductor laser as a function of wavelength in a comparative example. (Reference) Figure 15 and Figure 16 When the center wavelength of the light emitted by the semiconductor laser is 9 micrometers, the reflective composite film of this application can significantly reduce the absorption rate and increase the reflectivity of the reflective composite film. Specifically, the absorption rate of the reflective composite film is reduced from 2.5% to 0.4%, and the reflectivity of the reflective composite film is increased from 97.5% to 99.6%.

[0088] This application does not limit the center wavelength of the light emitted by the edge-emitting semiconductor laser.

[0089] Another embodiment of this application provides a method for fabricating a side-emitting semiconductor laser, comprising: forming a light-emitting body having a front cavity surface and a rear cavity surface disposed opposite to each other along the cavity length direction; and forming a reflective composite film covering the rear cavity surface; wherein forming the reflective composite film comprises: forming an optical dielectric reflective film covering the rear cavity surface, the optical dielectric reflective film comprising a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction, the refractive index of the second optical dielectric film being different from that of the first optical dielectric film; and forming a metal reflective film on the side of the optical dielectric reflective film opposite to the light-emitting body along the cavity length direction.

[0090] The following references Figures 5 to 9 This paper details a method for fabricating a side-emitting semiconductor laser. Figures 5 to 8 The process of forming a luminescent host.

[0091] refer to Figure 5A buffer layer 110 is formed on one side of the semiconductor substrate 100 along the fast axis direction Z; a lower confinement layer 130, a lower buffer material layer 140, an active material layer 150, an upper buffer material layer 160, an upper confinement material layer 170 and a contact material layer 180 are sequentially formed on the side of the buffer layer 110 away from the semiconductor substrate 100.

[0092] The process for forming the lower confinement layer 130, the lower buffer material layer 140, the active material layer 150, the upper buffer material layer 160, the upper confinement material layer 170, and the contact material layer 180 includes an epitaxial growth process.

[0093] refer to Figure 6 and Figure 7 A mask layer 190 is formed on the side of the contact material layer 180 opposite to the upper limiting material layer 170. Figure 6 Using mask layer 190 as a mask, contact material layer 180, upper confinement material layer 170, upper buffer material layer 160, active material layer 150 and lower buffer material layer 140 are etched, so that the lower buffer material layer 140 forms lower buffer layer 141. Figure 7 ), so that the active material layer 150 forms the active layer 151 ( Figure 7 ), so that the upper buffer material layer 160 forms the upper buffer layer 161 ( Figure 7 ), so that the upper limiting material layer 170 forms the upper limiting layer 171 ( Figure 7 ), so that the contact material layer 180 forms the contact layer 181 ( Figure 7 ).

[0094] The descriptions of the lower limiting layer 130, lower buffer layer 141, active layer 151, upper buffer layer 161, upper limiting layer 171 and contact layer 181 are as described in the foregoing embodiments.

[0095] The material of the mask layer 190 can be an insulating dielectric material, such as silicon oxide.

[0096] refer to Figure 8 , Figure 8 In order to be in Figure 7 Based on the schematic diagram, an insulating limiting layer 194 is formed on both sides of the contact layer 181, the upper limiting layer 171, the upper buffer layer 161, the active layer 151, and the lower buffer layer 141 along the slow axis direction X, and on one side of the lower limiting layer 130 along the fast axis direction Z.

[0097] The process for forming the insulating confinement layer 194 includes an epitaxial growth process. The description of the insulating confinement layer 194 refers to the foregoing embodiments.

[0098] refer to Figure 8An insulating layer 193 is formed on the side of the insulating limiting layer 194 opposite to the lower limiting layer 130; a front electrode 200 is formed, which is located on the side of the contact layer 181 opposite to the upper limiting layer 171 and on the side of the insulating limiting layer 194 opposite to the lower limiting layer 130.

[0099] The insulating layer 193 is located between the insulating limiting layer 194 and the front electrode 200. The insulating layer 193 and the front electrode 200 are described with reference to the foregoing embodiment.

[0100] refer to Figure 8 A back electrode 210 is formed, which is located on the side of the semiconductor substrate 100 away from the lower confinement layer 130.

[0101] The back electrode 210 is described with reference to the foregoing embodiment.

[0102] Figure 8 This forms the luminescent main body. A description of the luminescent main body is provided below. Figure 1 and Figure 2 Corresponding implementation examples.

[0103] refer to Figure 9 A reflective composite film 400 is formed covering the rear cavity surface.

[0104] The process for forming the reflective composite film 400 can be either an evaporation coating process or a sputtering coating process.

[0105] The formation of the reflective composite film 400 includes: forming an optical medium reflective film 420 covering the rear cavity surface, the optical medium reflective film 420 including a first optical medium film 4201 and a second optical medium film 4202 alternately stacked in the cavity length direction Y, the refractive index of the second optical medium film 4202 being different from the refractive index of the first optical medium film 4201; and forming a metal reflective film 440 on the side of the optical medium reflective film 420 away from the light-emitting body along the cavity length direction Y.

[0106] The description of the optical medium reflective film 420 and the metal reflective film 440 is the same as that in the foregoing embodiments.

[0107] In some embodiments, forming the reflective composite film 400 further includes forming a first optical medium adhesive layer 410 covering the rear cavity surface before forming the optical medium reflective film 420, the first optical medium adhesive layer 410 being described with reference to the description of the foregoing embodiments.

[0108] The description of the first optical medium adhesive layer 410 is as described in the foregoing embodiment.

[0109] In some embodiments, forming the reflective composite film 400 further includes forming a first metal adhesive layer 430 on the side of the optical medium reflective film 420 away from the light-emitting body before forming the metal reflective film 440.

[0110] The description of the first metal adhesive layer 430 is as described in the foregoing embodiment.

[0111] In some embodiments, forming the reflective composite film 400 further includes: forming a second metal adhesive layer 450 on the side of the metal reflective film 440 opposite to the optical medium reflective film 420 along the cavity length direction Y; and forming an insulating medium protective layer 460 on the side of the second metal adhesive layer 450 opposite to the metal reflective film 440 along the cavity length direction Y.

[0112] The description of the second metal adhesive layer 450 and the insulating dielectric protective layer 460 is the same as that in the foregoing embodiments.

[0113] refer to Figure 9 This forms an antireflective composite membrane 300 covering the front cavity surface.

[0114] The antireflection composite film 300 covering the front cavity surface includes: forming a second optical dielectric adhesive layer 310 covering the front cavity surface; and forming an optical dielectric antireflection film 320 on the side of the second optical dielectric adhesive layer 310 opposite to the light-emitting body along the cavity length direction Y. The description of the second optical dielectric adhesive layer 310 and the optical dielectric antireflection film 320 refers to the foregoing embodiment.

[0115] Figures 10 to 14 This article details another fabrication method for edge-emitting semiconductor lasers. Figures 10 to 13 The process of forming a luminescent host.

[0116] refer to Figure 10 A buffer layer 110 is formed on one side of the semiconductor substrate layer 100 along the fast axis direction Z; an etch barrier layer 120, a lower confinement layer 130, a lower buffer material layer 140, an active material layer 150, an upper buffer material layer 160, an upper confinement material layer 170 and a contact material layer 180 are sequentially formed on the side of the buffer layer 110 away from the semiconductor substrate layer 100.

[0117] The etch stop layer 120 may be made of a semiconductor material, and the material of the etch stop layer 120 may be different from the material of the lower confinement layer 130 and the material of the buffer layer 110, and the material of the etch stop layer 120 may be different from the material of the semiconductor substrate layer 100. For example, the material of the etch stop layer 120 may be InGaAs.

[0118] refer to Figure 11A mask layer 190 is formed on the side of the contact material layer 180 opposite to the upper limiting material layer 170. The contact material layer 180, the upper limiting material layer 170, the upper buffer material layer 160, the active material layer 150 and the lower buffer material layer 140 are etched using the mask layer 190 as a mask, so that the lower buffer material layer 140 forms a lower buffer layer 141, the active material layer 150 forms an active layer 151, the upper buffer material layer 160 forms an upper buffer layer 161, the upper limiting material layer 170 forms an upper limiting layer 171, and the contact material layer 180 forms a contact layer 181.

[0119] The descriptions of the lower limiting layer 130, lower buffer layer 141, active layer 151, upper buffer layer 161, upper limiting layer 171 and contact layer 181 are as described in the foregoing embodiments.

[0120] refer to Figure 12 An insulating limiting layer 194 is formed on both sides of the contact layer 181, the upper limiting layer 171, the upper buffer layer 161, the active layer 151, and the lower buffer layer 141 along the slow axis direction X, and on one side of the lower limiting layer 130 along the fast axis direction Z.

[0121] The description of the insulating limiting layer 194 is the same as that in the foregoing embodiment.

[0122] refer to Figure 12 An insulating layer 193 is formed on the side of the insulating limiting layer 194 opposite to the lower limiting layer 130; a front electrode 200 is formed, which is located on the side of the contact layer 181 opposite to the upper limiting layer 171 and on the side of the insulating limiting layer 194 opposite to the lower limiting layer 130.

[0123] The insulating layer 193 is located between the insulating limiting layer 194 and the front electrode 200. The insulating layer 193 and the front electrode 200 are described with reference to the foregoing embodiment.

[0124] refer to Figure 13 Remove the semiconductor substrate layer 100 and the buffer layer 110 until the etch stop layer 120 is exposed; remove the etch stop layer 120 to expose the lower confinement layer 130.

[0125] refer to Figure 13 After removing the etch barrier layer 120, a back electrode 210 is formed. The back electrode 210 is located on the side of the semiconductor substrate layer 100 away from the lower confinement layer 130.

[0126] The back electrode 210 is described with reference to the foregoing embodiment.

[0127] Figure 13 This forms the luminescent main body. A description of the luminescent main body is provided below. Figure 3 and Figure 4 Corresponding implementation examples.

[0128] refer to Figure 14 A reflective composite film 400 is formed covering the rear cavity surface; an antireflective composite film 300 is formed covering the front cavity surface.

[0129] The process for forming the reflective composite film 400 is described in the foregoing embodiments. The process for forming the antireflective composite film 300 is described in the foregoing embodiments.

[0130] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A side-emitting semiconductor laser, characterized in that, include: The light-emitting body has a front cavity surface and a rear cavity surface that are arranged opposite to each other along the length of the cavity; A reflective composite film covers the rear cavity surface, and the optical thickness of the reflective composite film along the cavity length direction is less than or equal to 2λ0, where λ0 is the center wavelength of the light emitted by the edge-emitting semiconductor laser. The reflective composite film includes: An optical dielectric reflective film comprises a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction, wherein the refractive index of the second optical dielectric film is greater than that of the first optical dielectric film, the optical thickness of the optical dielectric reflective film along the cavity length direction is greater than or equal to 0.5 times λ0 and less than or equal to 1.5λ0, and the absorption rate of the optical dielectric reflective film for light emitted by the light-emitting body is less than 1%; and A metal reflective film is located on the side of the optical medium reflective film that is opposite to the light-emitting body along the cavity length direction; Wherein, the absorptivity of the optical medium reflective film is less than that of the metal reflective film; the dimension of the optical medium reflective film along the cavity length direction is greater than that of the metal reflective film along the cavity length direction; The reflective composite film further includes: An insulating dielectric protective layer is located on the side of the metal reflective film that is opposite to the optical dielectric reflective film along the cavity length direction; A first metal adhesive layer is located between and in contact with the metal reflective film and the optical medium reflective film. The adhesive strength between the materials of the first metal adhesive layer and the optical medium reflective film is greater than the adhesive strength between the materials of the metal reflective film and the optical medium reflective film. The reflectivity of the material of the first metal adhesive layer is less than the reflectivity of the material of the metal reflective film. The dimension of the first metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction. A second metal adhesive layer is located between and in contact with the metal reflective film and the insulating dielectric protective layer. The adhesive strength between the materials of the second metal adhesive layer and the insulating dielectric protective layer is greater than the adhesive strength between the materials of the metal reflective film and the insulating dielectric protective layer. The reflectivity of the material of the second metal adhesive layer is less than the reflectivity of the material of the metal reflective film. The dimension of the second metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

2. The edge-emitting semiconductor laser according to claim 1, characterized in that, The optical thickness of the first single-layer optical dielectric film in the cavity length direction is 0.5 to 1.5 times λ0 / 4; the optical thickness of the second single-layer optical dielectric film in the cavity length direction is 0.5 to 1.5 times λ0 / 4; where λ0 is the center wavelength of the emitted light from the edge-emitting semiconductor laser.

3. The edge-emitting semiconductor laser according to claim 1, characterized in that, The material of the second optical dielectric film includes any one of ZnSe, ZnS, and Ge; Wherein, when the material of the second optical dielectric film is ZnSe or ZnS, the material of the first optical dielectric film is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, and Ca-doped or Ba-doped YbF3; when the material of the second optical dielectric film is Ge, the material of the first optical dielectric film is Y2O3, Al2O3, YF3, YbF3, BaF2, Ca-doped or Ba-doped YF3, Ca-doped or Ba-doped YbF3, ZnSe or ZnS.

4. The edge-emitting semiconductor laser according to claim 1, characterized in that, The thickness of the metal reflective film in the cavity length direction is 50nm~250nm.

5. The edge-emitting semiconductor laser according to claim 1, characterized in that, The material of the metal reflective film is Au or Ag.

6. The edge-emitting semiconductor laser according to claim 1, characterized in that, The reflective composite film further includes: A first optical medium adhesive layer is located between the optical medium reflective film and the light-emitting body along the cavity length direction and is in contact with a layer of the first optical medium film of the optical medium reflective film and the light-emitting body. The material of the first optical medium adhesive layer is different from the material of the first optical medium film.

7. The edge-emitting semiconductor laser according to claim 6, characterized in that, The material of the first optical medium adhesive layer is Y2O3, Al2O3, ZnSe or ZnS.

8. The edge-emitting semiconductor laser according to claim 6, characterized in that, The thickness of the first optical medium adhesive layer along the cavity length direction is 10nm~30nm.

9. The edge-emitting semiconductor laser according to claim 1, characterized in that, The material of the first metal adhesive layer is Ti or Cr.

10. The edge-emitting semiconductor laser according to claim 1, characterized in that, The thickness of the first metal adhesive layer along the length of the cavity is 2nm to 10nm.

11. The edge-emitting semiconductor laser according to claim 1, characterized in that, The edge-emitting semiconductor laser also includes an anti-reflection composite film covering the front cavity surface; The antireflective composite film includes an optical medium antireflective film and a second optical medium adhesive layer located between the optical medium antireflective film and the light-emitting body.

12. The edge-emitting semiconductor laser according to claim 11, characterized in that, The material of the second optical medium adhesive layer is Y2O3, Al2O3, ZnSe or ZnS.

13. The edge-emitting semiconductor laser according to claim 11, characterized in that, The thickness of the second optical medium adhesive layer along the cavity length direction is 10nm~30nm.

14. A method for fabricating a side-emitting semiconductor laser, characterized in that, include: A light-emitting body is formed, wherein the light-emitting body has a front cavity surface and a rear cavity surface that are arranged opposite to each other along the cavity length direction; as well as A reflective composite film is formed covering the rear cavity surface; The optical thickness of the reflective composite film along the cavity length direction is less than or equal to 2λ0, where λ0 is the center wavelength of the light emitted by the edge-emitting semiconductor laser. The formation of the reflective composite film includes: An optical dielectric reflective film is formed covering the rear cavity surface. The optical dielectric reflective film comprises a first optical dielectric film and a second optical dielectric film alternately stacked along the cavity length direction. The refractive index of the second optical dielectric film is greater than that of the first optical dielectric film. The optical thickness of the optical dielectric reflective film along the cavity length direction is greater than or equal to 0.5 times λ0 and less than or equal to 1.5λ0. The absorption rate of the optical dielectric reflective film for light emitted by the light-emitting body is less than 1%. A metal reflective film is formed on the side of the optical medium reflective film opposite to the light-emitting body along the cavity length direction; wherein the absorptivity of the optical medium reflective film is less than that of the metal reflective film; and the dimension of the optical medium reflective film along the cavity length direction is greater than that of the metal reflective film along the cavity length direction. Prior to forming the metal reflective film, a first metal adhesive layer is formed on the side of the optical medium reflective film facing away from the light-emitting body. The adhesive strength between the materials of the first metal adhesive layer and the optical medium reflective film is greater than the adhesive strength between the materials of the metal reflective film and the optical medium reflective film. The reflectivity of the material of the first metal adhesive layer is less than the reflectivity of the material of the metal reflective film. The dimension of the first metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction. A second metal adhesive layer is formed on the side of the metal reflective film opposite to the optical medium reflective film along the cavity length direction; An insulating dielectric protective layer is formed on the side of the second metal adhesive layer opposite to the metal reflective film along the cavity length direction; Wherein, the bonding strength between the material of the second metal adhesive layer and the material of the insulating dielectric protective layer is greater than the bonding strength between the material of the metal reflective film and the material of the insulating dielectric protective layer, the reflectivity of the material of the second metal adhesive layer is less than the reflectivity of the material of the metal reflective film, and the dimension of the second metal adhesive layer along the cavity length direction is smaller than the dimension of the metal reflective film along the cavity length direction.

15. The method for fabricating a side-emitting semiconductor laser according to claim 14, characterized in that, The formation of the reflective composite film further includes: Before forming the optical medium reflective film, a first optical medium adhesive layer is formed covering the rear cavity surface. The material of the first optical medium adhesive layer is different from the material of the first optical medium film. The first optical medium adhesive layer is in contact with a layer of the first optical medium film of the optical medium reflective film and the light-emitting body.

16. The method for fabricating a side-emitting semiconductor laser according to claim 14, characterized in that, The preparation method further includes: An antireflective composite film is formed covering the front cavity surface, and includes: Forming a second optical dielectric adhesive layer covering the front cavity surface; and An anti-reflective film is formed on the side of the second optical medium adhesive layer opposite to the light-emitting body along the cavity length direction.

Citation Information

Patent Citations

  • Semiconductor laser cavity surface coating method and semiconductor laser

    CN112342514A