A sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer for the cathode of a layered oxide sodium-ion battery, its preparation method and application.
By preparing an amorphous or near-amorphous sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer on the surface of the positive electrode of a layered oxide sodium-ion battery, the problem of surface structural instability of the layered oxide sodium-ion battery at high potentials was solved, and the chemical stability and performance of the battery were improved.
Patent Information
- Application Number
- CN202611264866.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-08-20
AI Technical Summary
During the high-potential sodium-ion battery cathode process, surface lattice oxygen activation, phase structure rearrangement, surface crack propagation, and transition metal dissolution are prone to occur, leading to electrolyte oxidative decomposition and increased interfacial impedance. At the same time, there are problems such as poor air stability and pH increase during slurry processing.
An amorphous or near-amorphous sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is adopted. A glass network is formed by Si-O tetrahedra, which are combined with BO and PO units to form a multi-element glass network. Al and F elements are introduced to improve the density and adhesion of the network structure, promote the formation of a stable surface layer rich in NaF, and enable sodium ion conduction, thereby achieving chemical stability and interface flexibility.
It significantly improves the air stability of layered oxide cathodes, suppresses surface phase transitions and transition metal dissolution under high-voltage cycling, reduces battery impedance, and enhances the battery's long-cycle stability, high-temperature storage stability, and safety.
Smart Images

Figure CN122822761B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of sodium-ion battery cathode materials, and relates to a sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer for a layered oxide sodium-ion battery cathode, its preparation method, and its application. Background Technology
[0002] Layered oxide cathodes possess high operating voltage, high compaction density, and large reversible capacity, making them important candidate materials for high-energy-density sodium-ion batteries. However, during high-potential desodium removal, these materials are prone to surface lattice oxygen activation, phase rearrangement, surface crack propagation, and transition metal dissolution, which in turn trigger electrolyte oxidative decomposition and increased interfacial impedance. Simultaneously, residual alkaline species such as NaOH and Na₂CO₃ are often present on the surface of layered oxide particles, resulting in poor air stability, increased pH during slurry processing, and exacerbated side reactions during storage and cycling.
[0003] While traditional simple oxide coatings can isolate the electrolyte from direct contact with the positive electrode surface to a certain extent, they often have two problems: first, the ionic conductivity is low, and thick coatings will significantly increase polarization; second, a single inorganic layer is brittle and it is difficult to simultaneously suppress residual alkali, buffer surface structural stress, and adapt to the high-voltage interface chemical environment.
[0004] Therefore, a composite protective layer that combines chemical buffering capacity, certain sodium ion conductivity, and interfacial flexibility is needed to stabilize the surface of the high-voltage layered oxide cathode, reduce battery impedance, and improve battery cycle performance. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer for the positive electrode of a layered oxide sodium-ion battery, its preparation method, and its application.
[0006] In the sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer of this invention, Si acts as a glass network forming body in the form of Si-O tetrahedra. It can form an amorphous or near-amorphous BP-Si multi-element glass network together with BO and PO units, providing a chemically stable and continuous surface barrier for the positive electrode. Simultaneously, the introduction of Al helps improve the density and adhesion of the network structure, while the introduction of F improves the compatibility of the protective layer with the electrolyte environment and promotes the formation of a stable NaF-rich surface layer. The introduction of Na enables the protective layer to maintain electronic insulation while possessing a certain sodium ion conductivity. This invention utilizes the chemical stability of the boron-phosphorus-silicon composite network, the enhancing effect of aluminum and fluorine on structural and interfacial bonding, and the compensating effect of sodium on ion conductivity to achieve multifunctional protection of the high-voltage layered oxide positive electrode surface. Therefore, it can simultaneously achieve the triple functions of adsorbing residual alkali, buffering structural stress, and suppressing side reactions during high-voltage cycling.
[0007] The protective layer has the following characteristics: First, the amorphous or near-amorphous structure helps to avoid lattice mismatch and stress concentration; second, the glassy network can react with or adsorb residual alkali, reducing the alkalinity of the cathode particle surface; third, the F-containing component helps to further form a stable NaF-rich interface in the electrolyte environment; fourth, the thin-layer coating can suppress surface phase transition and transition metal dissolution without significantly increasing charge transfer impedance.
[0008] The objective of this invention can be achieved through the following methods: In a first aspect, the present invention provides a sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer, the chemical composition of which is Na a Al b B c P d Si e O f F g The elements Na, Al, B, P, Si, O, and F are all present, where a, b, c, d, e, and g are all greater than 0, and satisfy the following atomic ratios: 0.1 ≤ a ≤ 3.0, 0.1 ≤ b ≤ 2.0, 0.1 ≤ c ≤ 3.0, 0.1 ≤ d ≤ 3.0, 0.1 ≤ e ≤ 3.0, 0.01 ≤ g ≤ 1.0. f is the number of oxygen atoms required to satisfy the valence equilibrium of each element.
[0009] The protective layer of this invention must contain an appropriate amount of Si to form a glass network, reducing the risk of local dissolution, cracking, and interface exposure of the Si-free coating under high voltage and trace water environments; however, excessively high Si content may also reduce Na content. + It increases migration ability and polarization.
[0010] As one embodiment of the present invention, the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is amorphous or near-amorphous and has a thickness of 2 nm-30 nm.
[0011] Secondly, the present invention provides a method for preparing the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer, comprising: uniformly mixing phosphorus source, boron source, aluminum source, silicon source, fluorine source and sodium source in a solution, followed by drying and heat treatment to form the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer in situ.
[0012] As one embodiment of the present invention, the phosphorus source is selected from one or more of sodium dihydrogen phosphate, sodium metaphosphate, and polyphosphates; the boron source is selected from one or more of boric acid and sodium tetraborate; the aluminum source is selected from one or more of aluminum isopropoxide, aluminum sec-butoxide, and boehmite; the silicon source is selected from one or more of tetraethyl orthosilicate, sodium silicate, and silica sol; the fluorine source is selected from one or more of ammonium fluoride, sodium fluoride, and fluorinated organosilanes; and the sodium source is selected from one or more of sodium dihydrogen phosphate, sodium metaphosphate, sodium tetraborate, sodium silicate, sodium fluoride, and sodium acetate.
[0013] As one embodiment of the present invention, the temperature of the heat treatment is 250℃-450℃.
[0014] Thirdly, the present invention provides the application of the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer in the preparation of layered oxide sodium-ion battery cathode materials and sodium-ion batteries.
[0015] As one embodiment of the present invention, the layered oxide sodium-ion battery cathode material includes a layered oxide cathode active material and a sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer coated on its surface.
[0016] As one embodiment of the present invention, the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is 0.1%-3.0% of the mass of the layered oxide positive electrode active material.
[0017] As one embodiment of the present invention, the layered oxide positive electrode active material is Na. x TMO2, where 0.60≤x≤1.20, and TM is selected from two or more of Ni, Mn, Fe, Cu, Co, Mg, Ti, and Li.
[0018] As one embodiment of the present invention, the preparation method of the layered oxide sodium-ion battery cathode material includes the following steps: dispersing the layered oxide cathode active material in a solvent, and sequentially adding a phosphorus source, a boron source, an aluminum source, a silicon source, a fluorine source and a sodium source to form a precursor solution; after stirring, evaporation and drying, a coated precursor powder is obtained; and then heat-treated to obtain the final product.
[0019] As one embodiment of the present invention, the solvent includes an alcohol / water mixed solvent.
[0020] As one embodiment of the present invention, the heat treatment temperature is 250℃-450℃, the time is 1-8 hours, and the atmosphere is one of air, oxygen, argon or a mixture thereof.
[0021] As one embodiment of the present invention, the sodium-ion battery includes the layered oxide sodium-ion battery positive electrode material, negative electrode, separator and electrolyte.
[0022] As one embodiment of the present invention, the negative electrode is selected from one or more of hard carbon, soft carbon or amorphous carbon.
[0023] The air stability, long-cycle stability, high-temperature storage stability, and safety of the sodium-ion battery of this invention are evaluated according to the method described in the specific embodiments, and the specific improvement is illustrated by the measured data of the examples and comparative examples.
[0024] Compared with the prior art, the present invention has the following beneficial effects: 1. In the sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer of this invention, Si forms a Si-O tetrahedral glass network, which, together with BO and PO units, constitutes an amorphous or near-amorphous BP-Si multi-element glass network, providing a chemically stable and continuous surface barrier for the positive electrode. Furthermore, the introduction of Al helps improve the density and adhesion of the network structure, while the introduction of F improves the compatibility of the protective layer with the electrolyte environment and promotes the formation of a stable NaF-rich surface layer. The introduction of Na enables the protective layer to maintain electronic insulation while possessing a certain sodium ion conductivity. Compared to a protective layer without Si, the protective layer of this invention can further improve the battery's capacity retention and reduce impedance growth.
[0025] 2. The sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer of the present invention can significantly improve the air stability of the layered oxide cathode and reduce the residual alkali content on the surface. On the other hand, it can suppress surface phase transition, lattice oxygen activation and transition metal dissolution under high voltage cycling, while reducing electrolyte oxidation and decomposition, reducing gas evolution and interfacial impedance growth, thereby improving the long-cycle stability, high-temperature storage stability and safety of the battery. Attached Figure Description
[0026] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 This is a schematic diagram of the structure of the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer covering layered oxide particles of the present invention; Figure 2 This is a schematic diagram of the process for forming a protective layer using a solution precursor method and medium-low temperature heat treatment; Figure 3 This is a schematic diagram comparing the capacity retention of Example 1 and the uncoated comparative sample after high-pressure cycling. Figure 4 Here is a high-resolution transmission electron microscope image of the near-surface of the layered oxide particles coated in Example 1; Figure 5 Here is a high-resolution transmission electron microscope image of the near-surface of the layered oxide particles coated in Example 2; Figure 6 Here is a high-resolution transmission electron microscope image of the near-surface of the layered oxide particles coated in Example 3; Figure reference numerals: 1-core particle, 2-sodium aluminum boron phosphide silicon oxyfluorine glass protective layer, 3-sodium ion channel. Detailed Implementation
[0027] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The following examples are implemented under the premise of the technical solution of the present invention, providing detailed implementation methods and specific operating procedures, which will help those skilled in the art to further understand the present invention. It should be noted that the scope of protection of the present invention is not limited to the following embodiments; any adjustments and improvements made under the concept of the present invention are all within the scope of protection of the present invention.
[0028] Characterization and Electrochemical Testing Methods Protective layer composition: The contents of Na, Al, B, P, and Si were determined by ICP-OES, and the F content and elemental chemical states were determined by XPS. Atomic ratios were normalized to P=1.00, and the average and sample standard deviation of n=3 independent batches were reported. The amorphous nature of the protective layer was confirmed by a combination of XRD and selected area electron diffraction.
[0029] Battery assembly: The mass ratio of positive electrode active material, conductive carbon black, and PVDF is 92:4:4, the areal density of the positive electrode active material is 10.2±0.3 mg / cm², and the compacted density is 3.10±0.07 g / cm³. The mass ratio of hard carbon:conductive carbon black:CMC:SBR is 94:2:2:2, and the N / P ratio is 1.10. A 16 μm PP / PE / PP three-layer separator is used, with an electrolyte injection volume of 2.5 g / Ah, to assemble a 1 Ah soft-pack battery. After electrolyte injection, the battery is allowed to stand at 25℃ for 12 h, and then formed by two cycles of 0.1C charge / discharge with a constant voltage cutoff current of 0.05C. Cycling is performed using 0.5C charge / 0.5C discharge at 25℃, with n=3 independent batteries per group.
[0030] High-temperature storage and EIS testing: Fully charged batteries were stored at 55℃ for 168 hours. EIS was measured before and after storage at 25℃ and open-circuit potential, with frequencies ranging from 100 kHz to 10 mHz and an AC disturbance amplitude of 5 mV. The equivalent circuit Rs-(Rct∥CPE)-W was used to fit Rct. A greater change in Rct before and after storage indicates that the surface of the cathode material is more susceptible to damage.
[0031] Example 1 Na, a P2 / O3 mixed-phase layered oxide, was selected. 0.90 [Cu 0.22 Fe 0.30 Mn 0.48 O2 is used as the positive electrode active material.
[0032] refer to Figure 2The procedure is as follows: 100 g of the positive electrode active material is dispersed in a mixed solvent of ethanol / deionized water at a volume ratio of 8:2. Based on a final coating weight of 1.0 wt%, 0.54 g of sodium dihydrogen phosphate, 0.20 g of boric acid, 0.34 g of aluminum isopropoxide, 0.49 g of tetraethyl orthosilicate, 0.06 g of ammonium fluoride, and 0.12 g of anhydrous sodium acetate are added sequentially as sodium source compensators. After stirring at room temperature for 4 hours, the solvent is evaporated under reduced pressure, and the material is vacuum dried at 80°C for 12 hours. Subsequently, it is heat-treated at 350°C in air for 3 hours to obtain a positive electrode material with a 5 nm thick amorphous sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer (the structure of the protective layer is shown in the figure). Figure 1 As shown, the electron microscope image is as follows: Figure 4 As shown, it is divided into an internal crystalline region and a surface amorphous coating region. According to the amount of material fed and normalized with P=1.00, the nominal atomic ratio of Na:Al:B:P:Si:F is 1.32:0.37:0.72:1.00:0.52:0.36.
[0033] The material was mixed with a conductive agent and a binder in a mass ratio of 92:4:4 to form a slurry, which was then coated onto aluminum foil. This slurry was then used in conjunction with a hard carbon negative electrode to assemble a full cell. The results were as follows: Figure 3 As shown, it exhibits a higher capacity retention rate when cycling at a cutoff voltage of 4.35 V; Table 1 shows a smaller impedance increase.
[0034] Example 2 O3 type NaNi was selected 0.33 Fe 0.33 Mn 0.33 O2 is used as the positive electrode active material.
[0035] Based on a final coating weight of 0.5 wt%, 0.24 g of sodium metaphosphate, 0.10 g of anhydrous sodium tetraborate, 0.06 g of boehmite, 0.24 g of 30 wt% silica sol, and 0.04 g of sodium fluoride were used as precursors, dispersed in an isopropanol / water mixture, and coated onto the material surface. After heat treatment at 300℃ for 2 hours in air atmosphere, an 18 nm thick amorphous surface protective layer was obtained. Near-surface electron micrographs of the particles are shown below. Figure 5 As shown. The nominal atomic ratio of Na:Al:B:P:Si:F normalized to P=1.00 is 1.83:0.43:0.85:1.00:0.51:0.41.
[0036] The material was used in half-cell and full-cell tests. The results in Table 1 show that its capacity retention was improved and its high-voltage cycling stability was better than that of the uncoated sample.
[0037] Example 3 Na[Ni] was selected 0.40 Fe 0.20 Mn 0.40O2 is used as the positive electrode active material.
[0038] Based on a final coating weight of 2.0 wt%, 0.92 g of sodium trimetaphosphate, 0.33 g of boric acid, 1.11 g of aluminum sec-butoxide, 2.30 g of sodium silicate nonahydrate, and 0.13 g of ammonium fluoride were selected as precursors and mixed at the molecular level in an ethanol system. After evaporation and drying, the mixture was heat-treated at 400℃ for 5 hours to obtain a 25 nm thick near-amorphous protective layer. The near-surface electron microscopy image of the particles is shown below. Figure 6 As shown. The nominal atomic ratio of Na:Al:B:P:Si:F normalized to P=1.00 is 2.80:0.50:0.59:1.00:0.90:0.39.
[0039] This embodiment is more suitable for high-voltage systems above 4.45 V, and can significantly reduce interface degradation after high-temperature storage.
[0040] Comparative Example 1 Using uncoated Na 0.90 [Cu 0.22 Fe 0.30 Mn 0.48 O2 cathode material was used to assemble a full cell. The test results are shown in Table 1. Under the same high voltage window, the capacity decayed faster and the impedance increased more significantly during cycling.
[0041] Comparative Example 2 A single fluorine-free coating containing only phosphorus and silicon oxides was used as a control. 0.58 g of ammonium dihydrogen phosphate and 0.84 g of tetraethyl orthosilicate were used, with a P:Si atomic ratio of 1.00:0.80 and a coating weight of 1.0 wt%. The results are shown in Table 1. Although it showed some improvement in air stability, the interfacial impedance increased significantly during high-pressure cycling, and its inhibitory effect on transition metal dissolution was weaker than that of the multi-element sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer of this invention.
[0042] Comparative Example 3 Comparative Example 3 used the same cathode substrate, drying, heat treatment, and battery testing conditions as Example 1. The difference was that tetraethyl orthosilicate was not added to Comparative Example 3; to ensure the total amount of non-oxygen elements was comparable to that of Example 1, the remaining precursors were scaled up using the same coefficient of 1.14, using 0.62 g of sodium dihydrogen phosphate, 0.23 g of boric acid, 0.39 g of aluminum isopropoxide, 0.07 g of ammonium fluoride, and 0.14 g of anhydrous sodium acetate. The nominal atomic ratio of Na:Al:B:P:F, normalized to P=1.00, was 1.32:0.37:0.72:1.00:0.36. The results are shown in Table 1. Due to the lack of Si, the protective layer of Comparative Example 3 could not form Si-O tetrahedra, resulting in an inability to effectively address issues such as localized dissolution, cracking, and interface exposure in high-voltage and trace-water environments. Furthermore, it could not react or adsorb effectively with residual alkali, leading to reduced capacity retention and significant impedance growth.
[0043] Table 1 Results of Cyclic and Impedance Tests
[0044] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. The application of a sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer for a layered oxide sodium-ion battery cathode in the preparation of layered oxide sodium-ion battery cathode materials, characterized in that, The chemical composition of the sodium aluminum boron phosphate silicon oxyfluorine glass protective layer is Na a Al b B c P d Si e O f F g Based on atomic ratios, the following conditions must be met: 0.1≤a≤3.0, 0.1≤b≤2.0, 0.1≤c≤3.0, 0.1≤d≤3.0, 0.1≤e≤3.0, 0.01≤g≤1.0, where f is the number of oxygen atoms required to satisfy the valence equilibrium of each element. The sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is amorphous or near-amorphous.
2. The application according to claim 1, characterized in that, The thickness of the sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is 2 nm-30 nm.
3. The application according to claim 1, characterized in that, The layered oxide sodium-ion battery cathode material includes a layered oxide cathode active material and a sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer coated on its surface.
4. The application according to claim 3, characterized in that, The sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer comprises 0.1%-3.0% of the mass of the layered oxide positive electrode active material; the layered oxide positive electrode active material is Na... x TMO2, wherein 0.60≤x≤1.20, and TM is selected from two or more of Ni, Mn, Fe, Cu, Co, Mg, Ti, and Li.
5. The application according to claim 3, characterized in that, The preparation method of the layered oxide sodium-ion battery cathode material includes the following steps: dispersing the layered oxide cathode active material in a solvent, and sequentially adding phosphorus source, boron source, aluminum source, silicon source, fluorine source and sodium source to form a precursor solution; after stirring, evaporation and drying, a coated precursor powder is obtained; and then heat treatment is performed to obtain the final product.
6. The application according to claim 5, characterized in that, The phosphorus source is selected from one or more of sodium dihydrogen phosphate, sodium metaphosphate, and polyphosphates; the boron source is selected from one or more of boric acid and sodium tetraborate; the aluminum source is selected from one or more of aluminum isopropoxide, aluminum sec-butoxide, and boehmite; the silicon source is selected from one or more of tetraethyl orthosilicate, sodium silicate, and silica sol; the fluorine source is selected from one or more of ammonium fluoride, sodium fluoride, and fluorinated organosilanes; the sodium source is selected from one or more of sodium dihydrogen phosphate, sodium metaphosphate, sodium tetraborate, sodium silicate, sodium fluoride, and sodium acetate; the heat treatment temperature is 250℃-450℃, the time is 1-8 hours, and the atmosphere is air, oxygen, argon, or a mixture thereof; the solvent includes an alcohol / water mixed solvent.
7. The application of a sodium-aluminum-boron-phosphorus-silicon-oxygen-fluorine glass protective layer for the positive electrode of a layered oxide sodium-ion battery in the preparation of sodium-ion batteries, characterized in that, The chemical composition of the sodium aluminum boron phosphate silicon oxyfluorine glass protective layer is Na a Al b B c P d Si e O f F g Based on atomic ratios, the following conditions must be met: 0.1≤a≤3.0, 0.1≤b≤2.0, 0.1≤c≤3.0, 0.1≤d≤3.0, 0.1≤e≤3.0, 0.01≤g≤1.0, where f is the number of oxygen atoms required to satisfy the valence equilibrium of each element. The sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer is amorphous or near-amorphous.
8. The application according to claim 7, characterized in that, The sodium-ion battery includes a layered oxide sodium-ion battery positive electrode material, a negative electrode, a separator, and an electrolyte; the layered oxide sodium-ion battery positive electrode material includes a layered oxide positive electrode active material and a sodium aluminum boron phosphorus silicon oxyfluorine glass protective layer coated on its surface; the negative electrode is amorphous carbon.
9. The application according to claim 8, characterized in that, The negative electrode is selected from hard carbon and soft carbon.
Citation Information
Patent Citations
High-nickel ternary lithium battery positive electrode material with stability and preparation method thereof
CN108550790A
Sodium-ion battery positive electrode material as well as preparation method and application thereof
CN117594778A