A one-step etching solution composition for ITO-Cu
By designing a one-step etching solution composition for ITO-Cu containing specific components, continuous etching of ITO-Cu stacked gates was achieved, solving the problems of cumbersome step-by-step etching process and high equipment cost, improving production efficiency and controllability of etching morphology, while ensuring electrical performance.
Patent Information
- Application Number
- CN202611347449.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-09-02
AI Technical Summary
The existing etching process for ITO-Cu stacked gates is cumbersome, requiring separate steps for Cu wet etching and ITO dry etching, resulting in low production efficiency, high equipment costs, and difficulty in ensuring the controllability of the etching morphology and electrical performance.
A one-step etching solution composition for ITO-Cu is used, which contains a specific proportion of hydrogen peroxide, ethylenediaminetetraacetic acid, imidazole, benzotriazole, phosphoric acid, sulfuric acid, gallic acid and guanine. The continuous etching of ITO-Cu is achieved by spray etching, which ensures the controllability of the etching morphology and electrical performance.
The etching process was simplified, production efficiency was improved, equipment costs were reduced, and the good morphology and electrical properties of the ITO-Cu film after etching were ensured by optimizing the composition ratio of the etching solution.
Smart Images

Figure CN122941417B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal film etching technology, and more specifically to an ITO-Cu one-step etching solution composition. Background Technology
[0002] In the manufacturing process of TFT-LCDs (Thin Film Transistor Liquid Crystal Displays), the gate metal layer is one of the key structures determining device performance and manufacturing costs. With the development of large-size, high-resolution display panels, the RC delay problem of gate signal transmission has become increasingly prominent. To reduce gate resistance, Cu (copper), with its low resistivity (approximately 1.7 μΩ·cm), has gradually replaced traditional metals such as Mo (molybdenum) and Al (aluminum) to become the mainstream conductive material for large-size TFT-LCD gates.
[0003] However, using Cu as the gate metal layer presents two major problems: first, the adhesion between Cu and the glass substrate is poor, making it prone to peeling or delamination in subsequent processes; second, Cu atoms easily diffuse into adjacent semiconductor or insulating layers under high temperature or electric field conditions, leading to increased leakage current and threshold voltage drift, severely affecting the electrical reliability of the TFT. To address these issues, existing technologies typically add a transition layer with good adhesion and barrier properties between the Cu layer and the substrate, forming a stacked gate structure.
[0004] Indium tin oxide (ITO), as a highly doped N-type semiconductor material, not only possesses excellent conductivity and high visible light transmittance, but also exhibits good adhesion to glass substrates and provides some barrier to Cu atom diffusion. Therefore, the ITO-Cu stack structure is considered one of the feasible alternatives to the traditional Mo-Cu stack structure. Using an ITO-Cu stack gate allows for low-resistance signal transmission using Cu while leveraging ITO to enhance interface adhesion and suppress Cu diffusion.
[0005] In existing TFT manufacturing processes, the patterning of ITO-Cu stacked gates typically employs a step-by-step etching process. The first step uses wet etching to etch the Cu layer, and the second step switches to dry etching to etch the ITO layer.
[0006] The main drawbacks of this step-by-step etching process are: (1) complicated process steps: the etching equipment and etching gas / solution system need to be switched between the two etching steps, which increases the process time and equipment occupation and reduces production efficiency; (2) high equipment cost: wet etching and dry etching require separate equipment, which increases the equipment investment of the production line and the area occupied by the clean room, and the maintenance cost also increases accordingly.
[0007] Therefore, how to simplify the etching process of ITO-Cu stacked gates, integrate the originally independent Cu wet etching and ITO dry etching into a continuous one-step etching process, reduce process steps and switching between different etching systems, improve the controllability of etching morphology, and at the same time ensure the electrical performance and reliability of the gate after etching has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0008] To address the shortcomings of existing technologies, this invention provides an ITO-Cu one-step etching solution composition, which is designed to etch ITO-Cu in one step, effectively improving the overall etching efficiency and reducing production costs.
[0009] To achieve the above objectives, the present invention provides the following technical solution: A one-step ITO-Cu etching solution composition, comprising the following raw materials in the indicated mass percentages: 14%-20% hydrogen peroxide, 0.12%-0.18% ethylenediaminetetraacetic acid, 0.15%-0.4% imidazole, 0.2%-0.45% benzotriazole, 2.2%-3% triethanolamine, 2%-5% weak organic acid, 0.4%-0.8% phosphoric acid, 0.8%-1.6% sulfuric acid, 1%-3% triethylene glycol, 0.15%-0.18% gallic acid, 0.02%-0.05% guanine, with the balance being water; wherein the mass percentage ratio of phosphoric acid to sulfuric acid is 1:2, the total mass percentage of imidazole and benzotriazole is 0.6%, and the total mass percentage of gallic acid and guanine is 0.2%.
[0010] Preferably, the weak organic acid is at least one of tartaric acid, citric acid, malic acid, and salicylic acid.
[0011] Preferably, the etching method of the etching solution composition is spray etching.
[0012] Preferably, the etching temperature of the etching solution composition is 30°C.
[0013] Preferably, the etching solution composition maintains an etching time of 50% over-etching during etching.
[0014] This invention provides an ITO-Cu one-step etching solution composition, which has the following advantages compared with the prior art: The present invention provides an etching solution composition based on a hydrogen peroxide system, which can etch ITO-Cu in one step, reducing the number of etching steps for ITO-Cu. Furthermore, by setting and limiting the proportions of components such as imidazole, benzotriazole, phosphoric acid, sulfuric acid, gallic acid, and guanine, the final etch morphology can be effectively controlled, reducing the "ITO tail" after etching. At the same time, it ensures good side etching amount (S / E) and better side etching angle (T / A), comprehensively improving the technical effect of one-step etching of ITO-Cu film. Attached Figure Description
[0015] Figure 1 This is a cross-sectional SEM image of the substrate after etching with etchant S1 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 2 This is a top-view SEM image of the substrate after etching with etchant S1 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 3 This is a cross-sectional SEM image of the substrate after etching with etchant S2 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 4 This is a top-view SEM image of the substrate after etching with etchant S2 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 5 This is a cross-sectional SEM image of the substrate after etching with etchant S3 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 6 This is a top-view SEM image of the substrate after etching with etchant S3 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 7 This is a cross-sectional SEM image of the substrate after etching with etchant S4 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 8 This is a top-view SEM image of the substrate after etching with etchant S4 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 9 This is a cross-sectional SEM image of the substrate after etching with etchant S5 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 10 This is a top-view SEM image of the substrate after etching with etchant S5 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 11 This is a cross-sectional SEM image of the substrate after etching with etchant D1 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 12 This is a top-view SEM image of the substrate after etching with etchant D1 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 13This is a cross-sectional SEM image of the substrate after etching with etchant D2 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 14 This is a top-view SEM image of the substrate after etching with etchant D2 in an embodiment of the present invention, where 1 represents ITO tailing; Figure 15 This is a cross-sectional SEM image of the substrate after etching with etchant D3 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 16 This is a top-view SEM image of the substrate after etching with etchant D3 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 17 This is a cross-sectional SEM image of the substrate after etching with etchant D4 in this embodiment, where 1 represents S / E and 2 represents T / A. Figure 18 This is a top-view SEM image of the substrate after etching with etchant D4 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 19 This is a cross-sectional SEM image of the substrate after etching with etchant D5 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 20 This is a top-view SEM image of the substrate after etching with etchant D5 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 21 This is a cross-sectional SEM image of the substrate after etching with etchant D6 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 22 This is a top-view SEM image of the substrate after etching with etchant D6 in an embodiment of the present invention, where 1 represents ITO tailing. Figure 23 This is a cross-sectional SEM image of the substrate after etching with etchant D7 in this embodiment, where 1 represents S / E and 2 represents T / A; Figure 24 This is a top-view SEM image of the substrate after etching with etchant D7 in an embodiment of the present invention, where 1 represents ITO tailing. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0017] Citric acid was chosen as the weak organic acid in the following examples, and some of the components are abbreviated as follows: Hydrogen peroxide (H2O2); ethylenediaminetetraacetic acid (EDTA); benzotriazole (BTA); triethanolamine (TEA); triethylene glycol (TEG); gallic acid (GA).
[0018] The meanings of the abbreviations for the items detected in the following examples are as follows: S / E (Side Etching) – The distance from the lower edge of Cu to the outermost edge of the upper PR (Photoresist); T / A (side etching angle) – the angle formed by the straight line connecting the upper edge and the lower edge of Cu and the horizontal line at the bottom of Cu; ITO trailing edge – the distance from the lower edge of Cu to the outermost edge of the bottom ITO layer.
[0019] Example
[0020] Prepare different etching solutions according to the mass percentage of each component in Table 1 below (the remainder is water): Table 1
[0021] Different etching solutions were prepared according to Table 1 above, and then the following etching tests were performed: 1. Testing method: Etching substrate: Cu / ITO (copper / indium tin oxide) 4500 / 150A; Etching conditions: Etching machine, temperature 30℃, spray pressure 0.1MPa, substrate size 5cm×5cm, etching time O / E 50% (O / E Over Etch, etching time is 50% over-etching); 2. Test Results: The specific results are shown in Table 2 below: Table 2
[0022] Combined with Table 2 above and Figures 1-10 It can be seen that the etching effects of etching solutions S1, S2, S3, S4 and S5 are relatively stable, ensuring a small S / E value and a large T / A value, while controlling a small ITO tail, ensuring the smoothness of the etched morphology and no ITO residue after etching.
[0023] The addition of sulfuric acid was omitted in etching solution D1, and the morphology after etching is as follows. Figure 11 and Figure 12 As shown, there is ITO residue, and the overall morphology after etching is poor, with a large S / E value and a significantly prolonged ITO tail, which seriously affects the etching effect.
[0024] The ratio of phosphoric acid to sulfuric acid in etching solution D2 was 1:1, resulting in a poor morphology after etching, with a large amount of ITO residue, making it impossible to measure ITO tailing, and the T / A value was significantly reduced. The ratio of phosphoric acid to sulfuric acid in etching solution D3 was 1:3, resulting in poor morphology after etching, with ITO residue, decreased T / A value and increased ITO tailing. The total amount of imidazole and BTA in the etching solution D4 was 0.35%. The final morphology after etching showed severe side etching and ITO residue. The final T / A ratio was low, while ITO tailing increased. The total amount of imidazole and BTA in etching solution D5 is 0.85%. The final morphology after etching is step-like with no ITO residue, but the T / A ratio is low and the ITO tailing is significantly improved compared with S1-S5. The total amount of GA and guanine in the etching solution D6 was 0.17%. The final morphology after etching was serrated with no ITO residue, but the S / E value was large and the ITO tailing value was also large. The addition of guanine was omitted in the etching solution D7, and the amount of GA added was adjusted to 0.20%. The final etching result was severe side etching with a large amount of ITO residue, making it impossible to measure ITO tailing, and the S / E value increased significantly.
[0025] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A one-step ITO-Cu etching solution composition, characterized in that, The composition comprises the following raw materials in the following mass percentages: hydrogen peroxide 14%-20%, ethylenediaminetetraacetic acid 0.12%-0.18%, imidazole 0.15%-0.4%, benzotriazole 0.2%-0.45%, triethanolamine 2.2%-3%, citric acid 2%-5%, phosphoric acid 0.4%-0.8%, sulfuric acid 0.8%-1.6%, triethylene glycol 1%-3%, gallic acid 0.15%-0.18%, guanine 0.02%-0.05%, with the balance being water; The mass percentage ratio of phosphoric acid to sulfuric acid is 1:2, the total mass percentage of imidazole and benzotriazole is 0.6%, and the total mass percentage of gallic acid and guanine is 0.2%.
2. The composition according to claim 1, characterized in that: The etching method of the etching solution composition is spray etching.
3. The composition according to claim 1, characterized in that: The etching temperature of the etching solution composition is 30°C.
4. The composition according to claim 1, characterized in that: The etching solution composition maintains an etching time of 50% over-etching during etching.
Citation Information
Patent Citations
Etching composition and method for manufacturing conducting film