A method for preparing a magnetic core-shell composite photocatalyst with enhanced magnetic field and its application.
By using a magnetic field-enhanced magnetic core-shell composite photocatalyst, combined with an external magnetic field and the spontaneous polarization of bismuth-based ferroelectric semiconductors, the problems of severe carrier recombination and easy poisoning in complex industrial flue gas environments of existing photocatalysts have been solved, achieving efficient and stable conversion of CO2 to high-value fuels and catalyst recyclability.
Patent Information
- Application Number
- CN202611322263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing photocatalysts suffer from severe carrier recombination, low light energy utilization, susceptibility to poisoning, and poor cycle stability in complex industrial flue gas environments. In particular, bismuth-based ferroelectric semiconductor materials have insufficient spin polarization regulation and anti-poisoning capabilities, making it difficult to achieve efficient and stable CO2 conversion.
A magnetic core-shell composite photocatalyst with enhanced magnetic field is used. The spin state of photogenerated carriers is controlled by an external magnetic field. Combined with the spontaneous polarization of bismuth-based ferroelectric semiconductors, the synergistic effect of magnetic field and ferroelectric polarization is used to achieve spatial separation and lifetime extension of photogenerated electrons and holes. Furthermore, the diffusion of poison molecules is prevented by the SiO2 intermediate layer, and convenient magnetic recovery performance is designed.
It significantly improves the CO2 photocatalytic reduction efficiency, enhances the adsorption and activation capacity of active sites, extends carrier lifetime, strengthens the material's resistance to poisoning, and enables convenient recovery and recycling of the catalyst.
Smart Images

Figure CN123059657A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photocatalytic carbon dioxide resource utilization technology, and more specifically to a method for preparing a magnetic core-shell composite photocatalyst with enhanced magnetic field. Background Technology
[0002] With the accelerating pace of global industrialization, the massive combustion of fossil fuels has led to a continuous rise in atmospheric CO2 concentrations. The resulting greenhouse effect and global climate change have become one of the most severe environmental challenges facing humanity. The International Energy Agency's (IEA) "Global Energy Review 2026" report shows that global energy-related CO2 emissions will increase by approximately 0.4% in 2025, the slowest growth rate since 2021, but the total still increases by approximately 145 million tons, reaching a new high of nearly 3.84 billion tons, 5% higher than the 2019 level. In the same year, the global atmospheric CO2 concentration reached a historical peak of approximately 427 ppm, about 2.4 ppm higher than in 2024 and about 50% higher than pre-industrial levels, making carbon dioxide emission reduction an urgent priority.
[0003] In my country, carbon emissions are mainly concentrated in eight key industries: power, steel, building materials, non-ferrous metals, petrochemicals, chemicals, papermaking, and aviation. Flue gas from coal-fired power plants, cement plants, and steel plants is the most concentrated source of CO2 emissions. This flue gas has a complex composition, containing not only CO2 but also various impurities such as SO2, NOx, H2O, and O2. CO2, as a major greenhouse gas, is also an important carbon resource. Converting it into high-value-added carbon-based fuels, such as CO, CH4, and CH3OH, is of significant strategic importance for alleviating the fossil fuel crisis and achieving carbon resource recycling.
[0004] To address the challenges of climate change, my country has established a "1+N" policy system for achieving carbon peaking and carbon neutrality, and urgently needs to develop efficient, stable, and industrially viable CO2 conversion technologies.
[0005] Photocatalytic CO2 reduction driven by solar energy, converting CO2 into high-value carbon-based fuels such as CO, CH4, and CH3OH, is considered an ideal way to simultaneously mitigate the greenhouse effect and solve the energy crisis. The core of photocatalytic CO2 reduction lies in developing efficient and stable photocatalytic materials. In recent years, researchers have conducted extensive work on the design of photocatalysts, including strategies such as constructing heterojunctions, controlling crystal facet exposure, and introducing defect engineering. However, problems such as severe carrier recombination, low light energy utilization, susceptibility to poisoning, and poor cycle stability still exist. For example, the Fe3O4@TiO2 magnetic photocatalyst disclosed in CN106964350A lacks a buffer layer, with the magnetic core in direct contact with the photocatalytic layer. High-temperature preparation easily leads to core oxidation and demagnetization, severe interfacial charge recombination, and the absence of a sulfur-resistant structure, making the active sites highly susceptible to poisoning by flue gas SO2. The magnetic CO2 photocatalytic material disclosed in CN112808314A uses only a single electric field to control the charge; after cyclic magnetic recovery, the shell layer easily detaches, resulting in continuous activity decay. Bismuth-based ferroelectric semiconductor materials, such as bismuth titanate Bi4Ti3O4, are also relevant. 12 ,Bi2MoO6,Bi3TiNbO9,SrBi4Ti4O 15 As a typical Aurivillius-type ferroelectric layered perovskite semiconductor, bismuth-based ferroelectric semiconductors have attracted widespread attention due to their unique layered crystal structure and spontaneous ferroelectric polarization effect. However, pure-phase bismuth-based ferroelectric semiconductors still suffer from problems such as high photogenerated carrier recombination rates, difficulty in recovering powdered catalysts, and insufficient resistance to poisoning, which severely restrict their practical application in complex industrial flue gas environments.
[0006] In recent years, external magnetic fields have been introduced into the field of photocatalysis as a non-contact control method. Studies have shown that magnetic fields can regulate the spin state of electrons in catalysts through spin polarization effects, causing photogenerated electrons and holes to have opposite spin directions, effectively suppressing carrier recombination. Magnetic fields can also regulate spin-selective electron transfer through Zeeman splitting-mediated polarization effects, thereby enhancing reaction specificity. However, most current research on magnetic field-enhanced photocatalysis relies on external magnetic field equipment to provide the magnetic field, failing to integrate magnetic components as intrinsic components of the catalyst in its design, and lacking systematic research on the synergistic effects of ferropolarization and spin polarization. Furthermore, the design of existing magnetic photocatalysts mostly uses magnetic nuclei only as a physical separation method, failing to fully utilize the intrinsic control potential of magnetic nuclei on the spin state of photogenerated carriers. Summary of the Invention
[0007] In view of this, the present invention provides a method for preparing a magnetic core-shell composite photocatalyst with enhanced magnetic field and its application. A magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst was developed and equipped with a magnetic field generating device, constructing a novel photo-magnetic-catalytic coupling system. This invention differs from traditional catalyst modification and physical separation methods by directly utilizing an external magnetic field on the magnetic photocatalytic reaction system, thereby improving catalytic efficiency by controlling the spin state of photogenerated carriers through the magnetic field.
[0008] This invention is the first to introduce the concept of external magnetic field control and ferroelectric polarization synergistically into the field of photocatalytic reduction of CO2 in flue gas. The core of this method consists of two parts: first, a magnetic field generator with uniform magnetic field distribution and adjustable intensity, suitable for photocatalytic reactors; second, a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst with excellent magnetic response characteristics and visible light response. The two work synergistically. An external magnetic field acts on the magnetic core, inducing spin polarization of the orbital electrons on the catalyst surface, causing the spin directions of photogenerated electrons and holes to be opposite. Based on the Pauli exclusion principle, this suppresses carrier recombination and prolongs the lifetime of photogenerated carriers. Simultaneously, the built-in electric field of the spontaneous polarization of the bismuth-based ferroelectric semiconductor further drives the spatial separation of photogenerated electron-hole pairs. The synergistic effect of magnetic field spin polarization and ferroelectric polarization achieves multi-dimensional control over the "spatial separation" and "lifetime extension" of photogenerated carriers. The SiO2 intermediate layer has three functions: physical isolation, robust loading, and anti-poisoning barrier, effectively preventing the diffusion of toxic molecules such as SO2 and H2S from flue gas to the active sites. Ultimately, this will enable a more efficient, stable, and recyclable photocatalytic conversion of CO2 into CO, CH4, and CH3OH in industrial flue gas environments such as coal-fired power plants, cement plants, and steel plants.
[0009] One objective of this invention is to provide a method for preparing a magnetic field-enhanced magnetic core-shell composite photocatalyst, specifically comprising the following methods:
[0010] Step 1: Preparation of magnetic nanoparticle cores; Step 2: Coat the surface of the magnetic nanoparticles with a SiO2 intermediate layer to obtain magnetic core@SiO2 core-shell nanoparticles; Step 3: The magnetic core@SiO2 core-shell nanoparticles are dispersed in a solution containing a bismuth-based ferroelectric semiconductor precursor. After a solvothermal reaction, a bismuth-based ferroelectric semiconductor photocatalytic shell is grown on the surface of the Fe3O4@SiO2 to obtain a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst.
[0011] Preferably, in step one, the magnetic nanoparticles are selected from one of Fe3O4, γ-Fe2O3, or MFe2O4, and M in MFe2O4 is selected from at least one of Co, Mn, Ni, Mg, Cu, or Zn. The magnetic nanoparticles are prepared by co-precipitation, solvothermal method, or thermal decomposition method.
[0012] The magnetic nanoparticles have a particle size of 50~500 nm, preferably 100~300 nm.
[0013] Preferably, in step two, the SiO2 intermediate layer is formed by a sol-gel method. The sol-gel method includes: dispersing the magnetic nanoparticles obtained in step one in a mixed solution of ethanol and water, adding ammonia and tetraethyl orthosilicate, stirring the mixture at 20-60°C for 2-12 hours, and then centrifuging, washing, and drying to obtain magnetic core@SiO2 core-shell nanoparticles. The mass ratio of tetraethyl orthosilicate to magnetic nanoparticles is (0.5-5):1, preferably (1-3):1. The thickness of the SiO2 intermediate layer is 5-30 nm, preferably 10-20 nm. The SiO2 intermediate layer is a dense amorphous silica layer with silanol functional groups on its surface.
[0014] Preferably, in step three, the bismuth-based ferroelectric semiconductor is Bi4Ti3O. 12 Bi2MoO6, Bi3TiNbO9 or SrBi4Ti4O 15 At least one of the following. The precursor solution is an ethylene glycol solution of a bismuth-based ferroelectric semiconductor with a concentration of 0.05~0.3M.
[0015] When the bismuth-based ferroelectric semiconductor is Bi4Ti3O 12 In this process, the precursor solution contains a bismuth source and a titanium source; the bismuth source is at least one of bismuth nitrate, bismuth chloride, or bismuth acetate; the titanium source is at least one of tetrabutyl titanate, tetraisopropyl titanate, or titanium tetrachloride; the molar ratio of the bismuth source to the titanium source is (3~5):(2~4), preferably 4:3.
[0016] When the bismuth-based ferroelectric semiconductor is Bi2MoO6, the precursor solution contains a bismuth source and a molybdenum source; the bismuth source is at least one of bismuth nitrate, bismuth chloride, or bismuth acetate; the molybdenum source is at least one of sodium molybdate or ammonium molybdate; the molar ratio of the bismuth source to the molybdenum source is (1.5~2.5):1, preferably 2:1.
[0017] When the bismuth-based ferroelectric semiconductor is Bi3TiNbO9, the precursor solution contains a bismuth source, a titanium source, and a niobium source; the bismuth source is at least one of bismuth nitrate, bismuth chloride, or bismuth acetate; the titanium source is at least one of tetrabutyl titanate, tetraisopropyl titanate, or titanium tetrachloride; the niobium source is at least one of niobium ethanol, niobium oxalate, or niobium pentachloride; the molar ratio of the bismuth source, titanium source, and niobium source is (2.5~3.5):(0.8~1.2):(0.8~1.2), preferably 3:1:1.
[0018] When the bismuth-based ferroelectric semiconductor is SrBi4Ti4O15 In this process, the precursor solution contains a strontium source, a bismuth source, and a titanium source; the strontium source is at least one of strontium nitrate or strontium chloride; the bismuth source is at least one of bismuth nitrate, bismuth chloride, or bismuth acetate; the titanium source is at least one of tetrabutyl titanate, tetraisopropyl titanate, or titanium tetrachloride; the molar ratio of the strontium source, bismuth source, and titanium source is (0.8~1.2):(3.5~4.5):(3.5~4.5), preferably 1:4:4.
[0019] The precursor solution also contains a mineralizing agent, which is at least one of sodium hydroxide, potassium hydroxide, or ammonia water, and the concentration of the mineralizing agent is 0.5~0.7 mol / L. The pH value is adjusted to 9~13.
[0020] The solvothermal reaction is carried out at a temperature of 120–240°C for 6–24 hours, preferably at 160–200°C for 12–18 hours. After the solvothermal reaction, the product is further subjected to centrifugation, washing, drying, and then calcination at 400–600°C for 2–6 hours. The calcination heating rate is 2–10°C / min, and the calcination atmosphere is air, nitrogen, or argon. The thickness of the bismuth-based ferroelectric semiconductor photocatalytic shell is 10–100 nm, preferably 20–60 nm.
[0021] Preferably, in step three, the precursor solution further contains a surfactant or dispersant, wherein the surfactant is at least one of polyvinylpyrrolidone (PVP), cetyltrimethylammonium bromide (CTAB), or polyethylene glycol (PEG), and the amount of the surfactant added is 0.5 to 5 wt%.
[0022] Preferably, in step three, after growing the bismuth-based ferroelectric semiconductor photocatalytic shell, it is further subjected to a reducing atmosphere heat treatment to increase the oxygen vacancy concentration; the reducing atmosphere heat treatment gas is an H2 / Ar mixture, the heat treatment temperature is 200~400℃, and the time is 1~4 hours.
[0023] In step three, the concentration of the magnetic core@SiO2 core-shell nanoparticles in the bismuth-based ferroelectric semiconductor precursor solution is 0.5~5 g / L.
[0024] The second objective of this invention is to provide an application of a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst in a magnetic field-enhanced photocatalytic reduction of CO2.
[0025] As can be seen from the above technical solution, compared with the prior art, the beneficial effects of the present invention are: (1) This invention utilizes the coupling between a magnetic core and an external magnetic field to regulate the separation and transport of photogenerated carriers through spin polarization, causing spin polarization of photogenerated electrons and holes. By leveraging the spin-forbidden property stipulated by the Pauli exclusion principle, the recombination of electrons and holes is suppressed at the physical level, thus extending the lifetime of photogenerated carriers and significantly improving the photocatalytic reduction efficiency of CO2. Simultaneously, the external magnetic field enhances the adsorption and activation capacity of CO2 by increasing the magnetic moment of the active sites and suppresses the competitive hydrogen evolution reaction.
[0026] (2) In this invention, the bismuth-based ferroelectric semiconductor, as an Aurivillius-type ferroelectric layered perovskite material, has a built-in electric field generated by its spontaneous polarization that can effectively drive the spatial separation of photogenerated electron-hole pairs. The ferroelectric built-in electric field of the bismuth-based ferroelectric semiconductor and the spin polarization effect of the magnetic core under the induction of an external magnetic field work synergistically to achieve multi-dimensional synergistic regulation of the "spatial separation" and "lifetime extension" of photogenerated carriers, significantly improving the photocatalytic reduction efficiency of CO2. Moreover, the photocatalytic shell of the bismuth-based ferroelectric semiconductor in this invention contains oxygen vacancy defects. Oxygen vacancies can not only serve as active sites to promote the adsorption and activation of CO2, but also enhance the magnetic response performance of the material by capturing unpaired spin electrons. In synergy with the external magnetic field, they can further promote the polarization adsorption and activation of CO2 molecules and reduce the energy barrier of the CO2 reduction reaction.
[0027] (3) The SiO2 intermediate layer in this invention has three functions: First, as a physical isolation layer, it effectively blocks the direct contact between the magnetic core and the bismuth-based ferroelectric semiconductor photocatalytic shell, avoiding the quenching of photogenerated carriers and the recombination of interface charges that may be caused by the magnetic core; Second, as a structural connection layer, its abundant silanol groups provide chemical bonding sites for the in-situ growth of bismuth-based ferroelectric semiconductors, enhancing the structural stability of the core-shell interface; Third, as an anti-poisoning protective layer, the dense SiO2 shell prevents the diffusion of poison molecules such as SO2 and H2S in flue gas to the active site through the size exclusion effect. At the same time, SiO2 itself can act as a sacrificial site to preferentially react with SO2 to generate stable sulfates, effectively delaying the poisoning and deactivation of the catalyst.
[0028] (4) The magnetic core in this invention gives the material convenient magnetic recovery performance. After the reaction is completed, the catalyst can be quickly separated and recovered by applying an external magnetic field. The recovered catalyst can be directly reused after washing and drying, and has good cycle stability. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0030] Figure 1 This is a graph showing the effect of the presence or absence of a magnetic field and an optical field on the efficiency of NiFe2O4@SiO2 / Bi2MoO6.
[0031] Figure 2 It is Fe3O4@SiO2 / Bi4Ti3O 12 The effect of the presence or absence of a magnetic field and a light field on the CO2 conversion rate.
[0032] Figure 3 It is Fe3O4@SiO2 / Bi4Ti3O 12 Sulfur resistance of materials under the influence of magnetic and light fields. Detailed Implementation
[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] This invention provides a method for preparing a magnetic core-shell composite photocatalyst with enhanced magnetic field strength. The material couples a magnetic core (selected from Fe3O4, γ-Fe2O3, or MFe2O4, where M = Co, Mn, Ni, Mg, Cu, Zn, etc.) with an applied magnetic field. This utilizes spin polarization to regulate the separation and transport of photogenerated charge carriers, effectively suppressing electron-hole recombination and extending carrier lifetime. The ferroelectric built-in electric field of the bismuth-based ferroelectric semiconductor shell synergistically enhances charge separation and transport with the magnetic field spin polarization effect. The SiO2 intermediate layer possesses triple functions: physical isolation, robust loading, and anti-poisoning barrier. The dense SiO2 shell prevents the diffusion of poison molecules such as SO2 and H2S to the active site through size exclusion effect, while also acting as a sacrificial site to preferentially react with SO2 to generate stable sulfates, effectively delaying catalyst poisoning and deactivation. The magnetic core endows the material with convenient magnetic recovery properties, allowing for rapid separation and recovery after the reaction using an applied magnetic field. This invention provides a novel material design scheme for achieving efficient, stable, and recyclable photocatalytic conversion of CO2 in complex industrial flue gas environments.
[0035] 1. Preparation of magnetic cores for magnetic nanoparticles (1) Preparation of Fe3O4 magnetic nanoparticles by coprecipitation method FeCl3·6H2O and FeC2·4H2O were weighed out in a molar ratio of 1:(1~1.5) and dissolved separately in deionized water. While stirring, the FeCl2 solution was slowly added to the FeCl3 solution, followed by dropwise addition of 10%~25% ammonia solution to adjust the pH to 8~12. The mixed solution was transferred to a hydrothermal reactor and reacted at 70~90℃ for 5~7 hours. After the reaction, the mixture was cooled to room temperature and centrifuged (3800~4500 rpm, 10~15 min). The precipitate was washed with deionized water until neutral. The resulting particles were dried in a vacuum oven at 60℃ for 12 hours to obtain Fe3O4 magnetic nanoparticles. The particle size of the obtained Fe3O4 magnetic nanoparticles was 50~500 nm, preferably 100~300 nm.
[0036] The co-precipitation method uses FeCl3·6H2O as the ferric salt and FeCl2·4H2O as the ferrous salt, with a preferred molar ratio of 1.2:1. The precipitant is ammonia, the pH value is preferably 10, the reaction temperature is preferably 80℃, and the reaction time is preferably 6 hours.
[0037] (2) Preparation of Fe3O4 magnetic nanoparticles by solvothermal method FeCl3·6H2O was weighed and dissolved in ethylene glycol, and the solution was magnetically stirred until completely dissolved. Sodium acetate was added, and stirring was continued for 30–60 min. The mixture was then transferred to a hydrothermal reactor and reacted at 180–250 °C for 8–24 hours. After the reaction was complete, the mixture was allowed to cool naturally to room temperature. The product was separated using a magnet, washed several times with ethanol and deionized water, and dried in a vacuum oven at 60 °C for 12 hours to obtain Fe3O4 magnetic nanoparticles.
[0038] In the solvothermal method, the soluble trivalent iron salt is FeCl3·6H2O, the mass ratio of ethylene glycol to iron salt is (10~30):1, the mass ratio of sodium acetate to iron salt is (2~5):1, the preferred reaction temperature is 200℃, and the preferred reaction time is 10~15 hours.
[0039] (3) Preparation of MFe2O4 magnetic nanoparticles (coprecipitation method) Weigh out water and chlorides (M = Co, Mn, Ni, Mg, Cu, Zn) and FeCl3·6H2O in a molar ratio of 2:1, and dissolve them in deionized water. While stirring, add dropwise a 2 mol / L NaOH solution to adjust the pH to 9–12. Heat and stir the mixture in a water bath at 70–90 °C for 2–4 hours. After the reaction is complete, separate the precipitate using a magnet, wash with deionized water until neutral, and dry in a vacuum oven at 60 °C for 12 hours to obtain MFe2O4 magnetic nanoparticles.
[0040] (4) Preparation of γ-Fe2O3 magnetic nanoparticles The Fe3O4 magnetic nanoparticles prepared by the above method were placed in a tube furnace and heated to 250~300℃ at a heating rate of 2℃ / min in air atmosphere, and calcined for 2~4 hours to obtain γ-Fe2O3 magnetic nanoparticles.
[0041] 2. Preparation of SiO2 Intermediate Layer Coating by Sol-Gel Method Take 0.5 g of the magnetic nanoparticles prepared above and disperse them in 30-100 mL of anhydrous ethanol, and sonicate for 20 min. Add 5-10 mL of deionized water, 2-10 mL of ammonia water and 2-4 mL of tetraethyl orthosilicate (TEOS) sequentially, and stir the reaction in a water bath at 25-60 °C for 4-12 hours. After the reaction is completed, separate the product with a magnet, wash it 3-6 times with ethanol and deionized water respectively, and dry it in a vacuum oven at 60 °C for 12 hours to obtain magnetic core@SiO2 core-shell nanoparticles.
[0042] In the sol-gel method, the volume ratio of ethanol to water is (2~8):1; the mass fraction of ammonia is 25%~28%; the volume ratio of ammonia to tetraethyl orthosilicate is (0.5~3):1; the preferred reaction temperature is 25~40℃; and the preferred reaction time is 4~8 hours.
[0043] After the magnetic core@SiO2 core-shell nanoparticles are coated, they undergo surface modification treatment. The surface modification treatment uses a silane coupling agent, which is at least one of KH-550, KH-570 or KH-792.
[0044] (1) Control of SiO2 coating thickness The thickness of the SiO2 interlayer is controlled by adjusting the amount of tetraethyl orthosilicate (TEOS) and the reaction time. The mass ratio of TEOS to magnetic nanoparticles is (0.5~5):1, preferably (1~3):1. The greater the amount of TEOS and the longer the reaction time, the greater the thickness of the SiO2 layer.
[0045] 3. Loading of bismuth-based ferroelectric semiconductor photocatalytic shell (1)Bi4Ti3O 12 load Take 0.3-0.5 g of the magnetic core@SiO2 core-shell nanoparticles prepared above and disperse them in 30-50 mL of ethylene glycol, and sonicate for 30-60 min. Weigh 3-5 mmol of Bi(NO3)3·5H2O and 2-4 mmol of tetrabutyl titanate (or tetraisopropyl titanate, titanium tetrachloride), and dissolve them in 10-20 mL of ethylene glycol, stirring for 30-60 min to form a precursor solution. Slowly add the precursor solution dropwise to the magnetic core@SiO2 suspension, add NaOH to adjust the pH of the solution to 9-13, and continue stirring for 1-2 hours. Transfer the mixed solution to a 50 mL hydrothermal reactor and react at 120-240 °C for 6-24 hours, preferably at 160-200 °C for 12-18 hours. After the reaction is complete, cool naturally to room temperature, centrifuge to separate the product, wash several times with deionized water and ethanol, and dry at 60 °C for 12 hours. The dried product was placed in a tube furnace and heated to 400-600°C at a heating rate of 2-10°C / min under air atmosphere, and calcined for 2-6 hours. It was then cooled to room temperature in the furnace to obtain the magnetic core @SiO2 / Bi4Ti3O. 12 Magnetic composite photocatalyst. The resulting Bi₄Ti₃O₂ 12 The thickness of the photocatalytic shell is 10~100nm, preferably 20~60nm.
[0046] (2) Loading of Bi2MoO6 Take 0.3–0.5 g of magnetic core@SiO2 core-shell nanoparticles and disperse them in 30–50 mL of deionized water, then sonicate for 30–60 min. Weigh 1–3 mmol of Bi(NO3)3·5H2O and 0.5–1.5 mmol of Na2MoO6·2H2O, respectively, and dissolve them in 10–20 mL of deionized water, stirring for 30–60 min to form a precursor solution. Slowly add the precursor solution dropwise to the magnetic core@SiO2 suspension and continue stirring for 1–2 hours. Transfer the mixed solution to a 50 mL hydrothermal reactor and react at 140–180 °C for 10–16 hours. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to separate the product, wash several times with deionized water and ethanol, and dry at 60 °C for 12 hours. The dried product was placed in a tube furnace and heated to 380-450°C at a heating rate of 2-10°C / min in air atmosphere. It was calcined for 2-4 hours and then cooled to room temperature with the furnace to obtain the magnetic core@SiO2 / Bi2MoO6 magnetic composite photocatalyst.
[0047] (3) Loading of Bi3TiNbO9 Take 0.3–0.5 g of magnetic core@SiO2 core-shell nanoparticles and disperse them in 30–50 mL of deionized water, then sonicate for 30–60 min. Weigh 2–4 mmol of Bi(NO3)3·5H2O, 0.5–1.5 mmol of tetrabutyl titanate, and 0.5–1.5 mmol of NbCl5, and dissolve them in 10–20 mL of ethylene glycol, stirring for 30–60 min to form a precursor solution. Slowly add the precursor solution dropwise to the magnetic core@SiO2 suspension, add NaOH to adjust the pH of the solution to 9–13, and continue stirring for 1 hour. Transfer the mixed solution to a 50 mL hydrothermal reactor and react at 150–250 °C for 10–16 hours. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to separate the product, wash several times with deionized water and ethanol, and dry at 60 °C for 12 hours. The dried product was placed in a tube furnace and heated to 450-550°C at a heating rate of 2-10°C / min under air atmosphere. It was calcined for 2-4 hours and then cooled to room temperature with the furnace to obtain the magnetic core@SiO2 / Bi3TiNbO9 magnetic composite photocatalyst.
[0048] (4) SrBi4Ti4O 15 load Take 0.3–0.5 g of magnetic core@SiO2 core-shell nanoparticles and disperse them in 30–50 mL of deionized water, then sonicate for 30–60 min. Weigh 3–5 mmol of Bi(NO3)3·5H2O, 0.5–1.5 mmol of Sr(NO3)2, and 3–5 mmol of tetrabutyl titanate, and dissolve them in 10–20 mL of ethylene glycol, stirring for 30–60 min to form a precursor solution. Slowly add the precursor solution dropwise to the magnetic core@SiO2 suspension, add NaOH to adjust the pH of the solution to 9–13, and continue stirring for 1 hour. Transfer the mixed solution to a 50 mL hydrothermal reactor and react at 150–250 °C for 10–16 hours. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to separate the product, wash several times with deionized water and ethanol, and dry at 60 °C for 12 hours. The dried product was placed in a tube furnace and heated to 400-700°C at a heating rate of 2-10°C / min under air atmosphere, and calcined for 4-6 hours. It was then cooled to room temperature in the furnace to obtain the magnetic core @SiO2 / SrBi4Ti4O. 15 Magnetic composite photocatalyst.
[0049] 4. Post-treatment and oxygen-vacancy regulation The calcined product was placed in a tube furnace and heated to 200-400°C at a heating rate of 2-10°C / min under an H2 / Ar mixed gas atmosphere (5% H2 volume fraction) for 1-4 hours. After furnace cooling to room temperature, an oxygen-vacancy-rich magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst was obtained. The oxygen vacancy concentration could be controlled by adjusting the heat treatment temperature and time, and was found to be 0.5-5 at%.
[0050] 5. Surface modification treatment Before loading bismuth-based ferroelectric semiconductors, magnetic core@SiO2 core-shell nanoparticles can undergo surface modification: The magnetic core@SiO2 core-shell nanoparticles are dispersed in anhydrous ethanol, and a silane coupling agent (at least one of KH-550, KH-570, or KH-792) is added. The mixture is stirred and refluxed in a 60°C water bath for 4–8 hours. After the reaction, the product is separated using a magnet, washed 3–5 times with ethanol and deionized water, and dried in a 60°C vacuum oven for 12 hours to obtain silane coupling agent-modified magnetic core@SiO2 core-shell nanoparticles.
[0051] 6. Application of magnetic field-enhanced photocatalytic reduction of CO2 The magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst prepared above was applied to the magnetic field-enhanced photocatalytic reduction of CO2 reaction. The specific method is as follows: Weigh 100–800 mg of catalyst and place it in a quartz tube gas-phase reactor. Add appropriate amounts of quartz wool to both sides of the catalyst to secure it and prevent it from being blown away. Transfer the reactor to a sealed photoreactor and purge with N2 gas for 20–60 min to purge air from the reactor. Use a 300 W xenon lamp (equipped with an AM 1.5G filter) as the light source, with a light intensity of 100–500 mW / cm². 2 Preferably, it is 200~300 mW / cm 2 Permanent magnets or electromagnets are placed on both sides of the reactor to provide an external magnetic field of 0.05~2 T, preferably 0.1~1 T. The reaction is carried out at 15~80℃ (preferably 20~60℃) and 0.1~2 MPa (preferably 0.1~1 MPa), with light and magnetization time of 1~12 hours. After the reaction, the gaseous products are analyzed by gas chromatography. CO and CH4 are the main reduction products, and small amounts of at least one of CH3OH, HCOOH, or C2H5OH may also be present. After the reaction, the catalyst is magnetically separated and recovered using an external magnetic field, with a recovery rate of over 90%. The recovered catalyst can be directly reused after washing and drying.
[0052] After the reaction, the catalyst is magnetically separated and recovered using an external magnetic field, with a recovery rate of 90% to 99%. The recovered catalyst is washed with ethanol and deionized water, dried at 60°C, and then reused directly. After being reused 5 to 10 times, the catalytic activity still retains more than 80% of the initial activity.
[0053] Example 1 Fe3O4@SiO2 / Bi4Ti3O 12 Taking the preparation method of magnetic composite photocatalyst as an example, it includes the following steps: Step 1: Preparation of Fe3O4 magnetic nanoparticles Weigh out 12 mmol of FeCl3·6H2O and 10 mmol of FeCl2·4H2O at a molar ratio of 1.2:1, and dissolve them separately in 50 mL of deionized water. While stirring, slowly add the FeCl2 solution to the FeCl3 solution, then add 25% ammonia solution dropwise to adjust the pH to 10. Transfer the mixed solution to a hydrothermal reactor and react at 80 °C for 6 hours. After the reaction, cool to room temperature, separate by centrifugation (4000 rpm, 10 min), and wash the precipitate with deionized water until neutral. Dry the obtained particles in a vacuum oven at 60 °C for 12 hours to obtain Fe3O4 magnetic nanoparticles. The particle size of the obtained Fe3O4 magnetic nanoparticles is 100–300 nm.
[0054] Step 2: Preparation of SiO2 Intermediate Layer Coating via Sol-Gel Method 0.5 g of the Fe3O4 magnetic nanoparticles obtained in step one were dispersed in a mixed solution of 80 mL ethanol and 20 mL deionized water and ultrasonically dispersed for 15 min. 2 mL of 25% ammonia and 2 mL of tetraethyl orthosilicate (TEOS) were added, and the mixture was stirred in a 30°C water bath for 6 hours. After the reaction, the product was separated using a magnet, washed three times with ethanol and deionized water respectively, and dried in a 60°C vacuum oven for 12 hours to obtain Fe3O4@SiO2 core-shell nanoparticles. The thickness of the obtained SiO2 intermediate layer was 10–20 nm.
[0055] Step 3: Bi4Ti3O 12 Loading of photocatalytic shell 0.3 g of the Fe3O4@SiO2 core-shell nanoparticles obtained in step two were dispersed in 30 mL of ethylene glycol and ultrasonically dispersed for 30 min. 4 mmol of Bi(NO3)3·5H2O and 3 mmol of tetrabutyl titanate were weighed and dissolved in 10 mL of ethylene glycol, and stirred for 30 min to form a precursor solution. The precursor solution was slowly added dropwise to the Fe3O4@SiO2 suspension, and NaOH was added to adjust the pH to 13. Stirring was continued for 1 hour. The mixed solution was transferred to a 50 mL hydrothermal reactor and reacted at 180 °C for 16 hours. After the reaction, the mixture was allowed to cool naturally to room temperature, and the product was separated by centrifugation. The product was washed several times with deionized water and ethanol, and dried at 60 °C for 12 hours. The dried product was placed in a tube furnace and calcined at 500 °C at a heating rate of 5 °C / min for 4 hours under air atmosphere. The furnace was then cooled to room temperature to obtain Fe3O4@SiO2 / Bi4Ti3O2. 12 Magnetic composite photocatalyst. The resulting Bi₄Ti₃O₂ 12 The thickness of the photocatalytic shell is 20~60nm.
[0056] Step 4: Apply the magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst obtained in Step 3 to the magnetic field-enhanced photocatalytic reduction of CO2 reaction. Weigh 300 mg of catalyst and place it in a quartz tube gas-phase reactor. Add appropriate amounts of quartz wool to both sides of the catalyst to secure it and prevent it from being blown away. Transfer the reactor to a sealed photoreactor and purge with N2 gas for 20–60 min to purge air from the reactor. Use a 300 W xenon lamp (with an AM 1.5G filter) as the light source, with a light intensity of 300 mW / cm². 2 Permanent magnets or electromagnets were placed on both sides of the reactor to provide an external magnetic field of 0.1 T. The reaction was carried out at room temperature (25℃) and 0.1 MPa, with irradiation and magnetization time of 10 hours. After the reaction, the gaseous products were analyzed by gas chromatography. CO and CH4 were the main reduction products, and small amounts of CH3OH, HCOOH, or C2H5OH may also be present. After the reaction, the catalyst was magnetically separated and recovered using an external magnetic field, with a recovery rate of over 90%. The recovered catalyst can be directly reused after washing and drying.
[0057] Example 2 A method for preparing a CoFe2O4@SiO2 / Bi2MoO6 magnetic composite photocatalyst includes the following steps: Step 1: Preparation of CoFe2O4 magnetic nanoparticles (coprecipitation method) Weigh out 20 mmol of CoCl₂·6H₂O and 10 mmol of FeCl₃·6H₂O at a molar ratio of 2:1, and dissolve them in 100 mL of deionized water. While stirring, add dropwise a 2 mol / L NaOH solution to adjust the pH to 11. Heat and stir the mixture in an 80°C water bath for 2 hours. After the reaction is complete, separate the precipitate using a magnet and wash with deionized water until neutral. Dry the resulting particles in a 60°C vacuum oven for 12 hours to obtain CoFe₂O₄ magnetic nanoparticles.
[0058] Step 2: Preparation of SiO2 Intermediate Layer Coating via Sol-Gel Method 0.5 g of the CoFe2O4 magnetic nanoparticles obtained in step one were dispersed in a mixed solution of 80 mL ethanol and 20 mL deionized water and ultrasonically dispersed for 15 min. 2 mL of 25% ammonia and 2.5 mL of tetraethyl orthosilicate (TEOS) were added, and the mixture was stirred in a 30°C water bath for 6 hours. After the reaction was complete, the product was separated using a magnet, washed three times with ethanol and deionized water respectively, and dried in a 60°C vacuum oven for 12 hours to obtain CoFe2O4@SiO2 core-shell nanoparticles.
[0059] Step 3: Loading the Bi2MoO6 photocatalytic shell 0.3 g of Fe3O4@SiO2 core-shell nanoparticles were dispersed in 30 mL of deionized water and ultrasonically dispersed for 30 min. 2 mmol of Bi(NO3)3·5H2O and 1 mmol of Na2MoO4·2H2O were weighed and dissolved in 10 mL of deionized water, and stirred for 30 min to form a precursor solution. The precursor solution was slowly added dropwise to the CoFe2O4@SiO2 suspension, and stirring was continued for 1 hour. The mixed solution was transferred to a 50 mL hydrothermal reactor and reacted at 160 °C for 12 hours. After the reaction, the mixture was allowed to cool naturally to room temperature, and the product was separated by centrifugation. The product was washed several times with deionized water and ethanol, and dried at 60 °C for 12 hours. The dried product was placed in a tube furnace and calcined at 400 °C at a heating rate of 5 °C / min for 2 hours under air atmosphere. The furnace was then cooled to room temperature to obtain the CoFe2O4@SiO2 / Bi2MoO6 magnetic composite photocatalyst.
[0060] Step 4: Apply the magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst obtained in Step 3 to the magnetic field-enhanced photocatalytic reduction of CO2 reaction. Weigh 400 mg of catalyst and place it in a quartz tube gas-phase reactor. Add appropriate amounts of quartz wool to both sides of the catalyst to secure it and prevent it from being blown away. Transfer the reactor to a sealed photoreactor and purge with N2 gas for 20–60 minutes to remove air from the reactor. Use a 300 W xenon lamp (with an AM 1.5G filter) as the light source, with a light intensity of 300 mW / cm². 2 Permanent magnets or electromagnets were placed on both sides of the reactor to provide an external magnetic field of 0.2 T. The reaction was carried out at room temperature (25℃) and 0.1 MPa, with illumination and magnetization time of 12 hours. After the reaction, the gaseous products were analyzed by gas chromatography. CO and CH4 were the main reduction products, and small amounts of CH3OH, HCOOH, or C2H5OH may also be present. After the reaction, the catalyst was magnetically separated and recovered using an external magnetic field, with a recovery rate of over 90%. The recovered catalyst can be directly reused after washing and drying.
[0061] Comparative Example 1 The difference from Comparative Example 2 is that, under the same conditions, without the application of an external magnetic field, the yields of CO and CH4 were significantly lower than those of the experimental group with the application of a magnetic field, indicating that the external magnetic field has a significant enhancing effect on photocatalytic CO2 reduction through spin polarization.
[0062] Example 3 A Fe3O4@SiO2 / Bi4Ti3O 12 The preparation method of the magnetic composite photocatalyst differs from that of Example 1 in that the SiO2 intermediate layer in step two is formed by sol-gel coating: 0.5 g of the Fe3O4 magnetic nanoparticles obtained in step one are dispersed in 50 mL of anhydrous ethanol and ultrasonically dispersed for 20 min. Then, 5 mL of deionized water, 2 mL of ammonia, and 2 mL of tetraethyl orthosilicate (TEOS) are added sequentially, and the mixture is stirred and reacted in a 50 °C water bath for 8 hours. After the reaction, the product is separated using a magnet, washed three times with ethanol and deionized water respectively, and dried in a 60 °C vacuum oven for 12 hours to obtain Fe3O4@SiO2 core-shell nanoparticles. The remaining steps are the same as in Example 1.
[0063] Example 4 A method for preparing a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst with oxygen vacancy regulation differs from Examples 1, 2, and 3 in that, after step three, the calcined product is placed in a tube furnace and heated to 350°C at a heating rate of 5°C / min under an H2 / Ar mixed gas atmosphere (H2 volume fraction 5%) for 2 hours. The product is then cooled to room temperature with the furnace to obtain a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst rich in oxygen vacancies.
[0064] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0065] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a magnetic core-shell composite photocatalyst with enhanced magnetic field strength, characterized in that, Includes the following steps: Step 1: Preparation of magnetic nanoparticles; Step 2: Coat the surface of the magnetic nanoparticles with a SiO2 intermediate layer to obtain magnetic core@SiO2 core-shell nanoparticles; Step 3: Disperse the magnetic core@SiO2 core-shell nanoparticles in a bismuth-based ferroelectric semiconductor precursor solution, add a mineralizer to adjust the pH value, and grow a bismuth-based ferroelectric semiconductor photocatalytic shell on the surface of the magnetic core@SiO2 core-shell nanoparticles through a solvothermal reaction to obtain a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst.
2. The preparation method according to claim 1, characterized in that, In step one, the magnetic nanoparticles are selected from one of Fe3O4, γ-Fe2O3 or MFe2O4, and the particle size of the magnetic nanoparticles is 50~500 nm.
3. The preparation method according to claim 1, characterized in that, The M in MFe2O4 is selected from at least one of Co, Mn, Ni, Mg, Cu, or Zn.
4. The preparation method according to claim 1, characterized in that, In step one, the magnetic nanoparticles are prepared by co-precipitation, solvothermal method or thermal decomposition method.
5. The preparation method according to claim 1, characterized in that, In step two, the SiO2 intermediate layer is formed by coating with a sol-gel method, and the thickness of the SiO2 intermediate layer is 5~30nm.
6. The preparation method according to claim 1, characterized in that, In step three, the bismuth-based ferroelectric semiconductor is Bi4Ti3O. 12 Bi2MoO6, Bi3TiNbO9 or SrBi4Ti4O 15 At least one of the following, wherein the precursor solution is an ethylene glycol solution of a bismuth-based ferroelectric semiconductor with a concentration of 0.05-0.3M; the mineralizing agent is at least one of sodium hydroxide, potassium hydroxide, or ammonia water; and the pH value is adjusted to 9-13.
7. The preparation method according to claim 1, characterized in that, In step three, the temperature of the solvothermal reaction is 120~240℃ and the reaction time is 6~24h. After the solvothermal reaction is completed, the product is further centrifuged, washed, dried, and then calcined at 400~600℃ for 2~6h, with the calcination heating rate being 2~10℃ / min.
8. The preparation method according to claim 1, characterized in that, In step three, the concentration of the magnetic core@SiO2 core-shell nanoparticles in the bismuth-based ferroelectric semiconductor precursor solution is 0.5-5 g / L.
9. The application of the magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst prepared by any one of claims 1-8 in the magnetic field-enhanced photocatalytic reduction of CO2 reaction.
10. The application according to claim 9, characterized in that, The application involves placing a magnetic core@SiO2 / bismuth-based ferroelectric semiconductor magnetic composite photocatalyst in a quartz tube gas-phase reactor, transferring the reactor to a sealed photoreactor, introducing N2 gas to purge the air from the reactor, and using a 300 W xenon lamp as the light source with a light intensity of 100~500 mW / cm². 2 Permanent magnets or electromagnets are placed on both sides of the reactor to provide an external magnetic field of 0.05~2 T. The reaction is carried out at 15~80℃ and 0.1~2 MPa, and the illumination and magnetization time is 1~12h.
Citation Information
Patent Citations
Simple preparation method for Fe3O4@C@TiO2 magnetic separation photocatalyst
CN106964350A
Preparation method and application of photocatalyst material with magnetic core-shell structure
CN112808314A