A wO3 / pdO composite material, a preparation method thereof and application thereof in a hydrogen sensor
By loading ultra-small PdO nanoparticles onto the surface of WO3 nanowires to form a pn heterojunction, the problems of high operating temperature and insufficient catalytic activity of existing WO3/PdO composite materials in hydrogen sensors are solved, enabling rapid response and stable detection of low-concentration hydrogen.
Patent Information
- Application Number
- CN202611224605.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing WO3/PdO composite materials used in hydrogen sensors suffer from problems such as high optimal operating temperature, unsatisfactory PdO particle size and dispersion state, low utilization of catalytic active sites, insufficient response recovery speed and long-term stability, making it difficult to meet the requirements for real-time monitoring and safety early warning of hydrogen leaks.
A combination of hydrothermal, chemical reduction and calcination methods was used to prepare WO3/PdO composite materials. By uniformly loading ultra-small PdO nanoparticles on the surface of WO3 nanowires, pn heterojunctions were formed, which enhanced catalytic activity and interfacial charge transport processes.
The optimal operating temperature of the sensor has been lowered, the response value and selectivity to hydrogen have been improved, the response speed and recovery speed have been enhanced, and the long-term stability and repeatability of the sensor have been ensured, making it suitable for real-time detection and safety early warning of low-concentration hydrogen.
Smart Images

Figure CN123059697A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hydrogen sensing and detection technology, and more specifically, to a WO3 / PdO composite material, its preparation method, and its application in hydrogen sensors. Background Technology
[0002] Hydrogen, as a highly efficient and clean secondary energy source, has broad application prospects in fuel cells, hydrogen energy storage, chemical production, metallurgy, and aerospace. However, hydrogen is colorless, odorless, has low density, diffuses rapidly, has low ignition energy, and readily forms explosive mixtures with air. Once a leak occurs, it is difficult to detect in time, easily leading to combustion or explosion accidents. Therefore, achieving rapid, accurate, and stable detection of hydrogen is of great significance for ensuring safety during hydrogen production, storage, transportation, and use.
[0003] Currently, hydrogen detection methods mainly include gas chromatography, optical analysis, electrochemical methods, catalytic combustion, and semiconductor gas sensing. While gas chromatography and some optical analysis methods offer high detection accuracy and selectivity, they generally suffer from problems such as expensive equipment, large size, complex operation, and difficulty in achieving real-time online detection. Electrochemical and catalytic combustion methods, although widely used, still have limitations in long-term stability, anti-interference capabilities, miniaturization, and low power consumption. In contrast, metal oxide semiconductor gas sensors, due to their simple structure, low cost, ease of integration, and fast response, have become an important research direction in the field of hydrogen detection.
[0004] Among numerous metal-oxide-semiconductor materials, WO3 is a typical n-type semiconductor material with advantages such as tunable bandgap, good chemical stability, low cost, non-toxicity, and high surface activity. Furthermore, it undergoes significant surface reactions and changes in electrical properties under the influence of hydrogen gas, thus attracting widespread attention in the field of hydrogen sensing. Existing research has shown that WO3 can be fabricated into various micro / nano structures such as nanowires, nanorods, nanosheets, nanoneedles, and nanofibers. These structures can enhance sensing performance by increasing specific surface area and the number of active sites.
[0005] However, pure WO3 materials still have significant shortcomings in practical applications. For example, they typically operate at high temperatures, have limited response values to hydrogen, lack ideal selectivity, and are easily affected by factors such as environmental humidity, making it difficult to meet the demands for highly sensitive, fast-response, and highly stable hydrogen detection in complex scenarios. To improve the performance of WO3-based sensing materials, researchers often employ strategies such as nanostructure design, noble metal modification, and heterostructure construction. Among these, noble metal modification can utilize its excellent catalytic activity to promote the adsorption, dissociation, and overflow of hydrogen molecules; heterostructures can effectively improve the sensor's response sensitivity and selectivity by controlling carrier distribution through interfacial charge transfer and built-in electric fields.
[0006] Palladium oxide (PdO), as an important p-type semiconductor oxide, possesses good catalytic activity and hydrogen sensitivity. When PdO is combined with n-type WO3, a pn heterojunction can be formed at the interface, thereby improving the hydrogen sensing performance of WO3-based materials to some extent. Previous studies have shown that PdO can promote the catalytic dissociation of hydrogen molecules and lower the activation energy of surface reactions. The heterojunction formed by WO3 and PdO also helps to regulate the interfacial barrier and carrier migration behavior, enhancing the material's response to hydrogen. For example, a fruit-leaf-shaped PdO / WO3 composite material has shown a high response to 100 ppm hydrogen at 120℃, indicating that PdO loading has a positive effect on improving the hydrogen-sensing performance of WO3.
[0007] However, existing WO3 / PdO composite materials still have the following shortcomings: First, the optimal operating temperature is still relatively high, which is not conducive to reducing device power consumption and improving safety. Second, the particle size, dispersion state, and interfacial contact between PdO and WO3 in existing composite materials are still not ideal, resulting in the failure to fully utilize the catalytic active site utilization and heterojunction synergistic effect. Third, there is still room for improvement in the comprehensive performance of response value, response recovery speed, long-term stability, and selectivity, making it difficult to better meet the application requirements of real-time monitoring and safety early warning of hydrogen leaks.
[0008] Therefore, the present invention proposes a novel WO3 / PdO composite material, which has significant practical implications. Summary of the Invention
[0009] In view of this, the present invention proposes a method for preparing WO3 / PdO composite material, aiming to solve at least one of the problems in the background art.
[0010] This invention proposes a method for preparing WO3 / PdO composite materials, including the following preparation steps: Take Na2WO4·2H2O and K2SO4, add them to water and stir to dissolve. Then adjust the pH of the solution to 1.5, stir and mix to obtain the first mixed solution. The first solution was subjected to a first heating treatment, and after the treatment, it was washed and dried to obtain WO3 nanowires. The WO3 nanowires and PdCl2 were added to water and ultrasonically dispersed to obtain a second mixed solution; Sodium borohydride aqueous solution was added to the second mixed solution and stirred to react. After the reaction was completed, the mixture was centrifuged and the precipitate was added to water and ultrasonically dispersed to obtain a suspension. The suspension was subjected to rotary evaporation and then dried to obtain a WO3 / PdO precursor material; the WO3 / PdO precursor material was subjected to a second heat treatment to obtain the WO3 / PdO composite material.
[0011] Preferably, the molar ratio of Na2WO4·2H2O to K2SO4 is 2:1.
[0012] Preferably, the heating temperature of the first heat treatment is 180°C and the heating time is 24 hours.
[0013] Preferably, in the WO3 / PdO composite material, the number of Pd atoms accounts for 1-2 at of the total number of Pd and W atoms.
[0014] Preferably, the concentration of the sodium borohydride aqueous solution is 0.1 mol / L.
[0015] Preferably, the stirring time of the stirring reaction is 1 hour, and the stirring environment is an ice bath.
[0016] Preferably, the rotary evaporation temperature is 200°C and the rotation speed is 300 r / min.
[0017] Preferably, the heating temperature of the second heat treatment is 400°C and the heating time is 2 hours.
[0018] The present invention also proposes a WO3 / PdO composite material prepared by the preparation method described above.
[0019] This invention also proposes an application of WO3 / PdO composite material in hydrogen sensing and detection.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention combines the catalytic activity of PdO with the gas-sensing properties of WO3 by loading ultra-small PdO nanoparticles onto the surface of WO3 nanowires. PdO promotes the adsorption and dissociation of hydrogen molecules, lowers the activation energy of the surface reaction, and thus enables the sensor to achieve a high response at a lower temperature. Compared with the high operating temperature of some existing WO3-based hydrogen sensing materials, this invention effectively reduces the optimal operating temperature, decreases device energy consumption, and improves the safety of hydrogen detection.
[0021] 2. In this invention, PdO nanoparticles are uniformly loaded onto the surface of WO3 nanowires, increasing the number of catalytically active sites favorable for hydrogen reactions. Simultaneously, the pn heterojunction formed between PdO and WO3 can modulate the interfacial barrier and carrier migration behavior, amplifying the resistance change signal induced by hydrogen. Therefore, the WO3 / PdO composite material prepared in this invention exhibits a high response value to hydrogen, meeting the requirements for low-concentration hydrogen detection and rapid early warning.
[0022] 3. Because the composite material prepared by this invention has a high specific surface area and abundant mesoporous structure, it is beneficial to the diffusion, adsorption and desorption of hydrogen molecules; at the same time, the catalytic effect of PdO can accelerate the surface reaction process. Therefore, the hydrogen sensor prepared by this invention has good response speed and recovery speed, and is suitable for real-time detection applications.
[0023] 4. This invention utilizes the catalytic selectivity of PdO and the synergistic effect of the WO3 / PdO heterostructure to improve the material's sensitivity to hydrogen and reduce interference from other gases on the detection results. Simultaneously, the prepared composite material has a stable structure, with PdO and WO3 fully bonded, thus the sensor exhibits good repeatability and long-term stability, which is beneficial for continuous monitoring.
[0024] 5. This invention achieves a more thorough interfacial contact between PdO and WO3 by controlling the size of PdO nanoparticles and their dispersion state on the surface of WO3 nanowires. This technical feature not only helps to exert the catalytic activity of PdO, but also enhances the charge regulation effect at the heterojunction interface, thereby further improving the overall gas-sensing performance of the material. Attached Figure Description
[0025] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 Transmission electron microscope (TEM) image of WO3 / PdO nanowire sample provided in an embodiment of the present invention; Figure 2 The response and recovery diagrams of WO3 / PdO materials to 50ppm H2 at different loadings and temperatures provided in this embodiment of the invention; Figure 3 The graph shows the long-term stability test of the WO3 / PdO 1.5at% nanowire gas sensor provided in this embodiment of the invention against 50 ppm H2 at 105 °C for 30 days.
[0026] Figure 4The dynamic response curve of the WO3 / PdO 1.5at% nanowire gas sensor provided in this embodiment of the invention to 10-50 ppm H2 at 105 °C. Detailed Implementation
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.
[0028] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0029] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0030] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0031] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0032] This invention provides a method for preparing a WO3 / PdO composite material, comprising the following preparation steps: Take Na2WO4·2H2O and K2SO4, add them to water and stir to dissolve. Then adjust the pH of the solution to 1.5, stir and mix to obtain the first mixed solution. The first solution was subjected to a first heating treatment, and after the treatment, it was washed and dried to obtain WO3 nanowires. The WO3 nanowires and PdCl2 were added to water and ultrasonically dispersed to obtain a second mixed solution; Sodium borohydride aqueous solution was added to the second mixed solution and stirred to react. After the reaction was completed, the mixture was centrifuged and the precipitate was added to water and ultrasonically dispersed to obtain a suspension. The suspension was subjected to rotary evaporation and then dried to obtain a WO3 / PdO precursor material; the WO3 / PdO precursor material was subjected to a second heat treatment to obtain the WO3 / PdO composite material.
[0033] Specifically, after dissolving Na2WO4·2H2O and K2SO4 in water and adjusting the pH of the solution to 1.5, the pH of the solution was adjusted to 1.5 by adding 2 mol / L dilute hydrochloric acid dropwise.
[0034] Specifically, the first solution is subjected to a first heating treatment. After the treatment, during washing and drying, it is washed three times alternately with anhydrous ethanol and deionized water, and then dried at 80°C for 12 hours.
[0035] Specifically, when the WO3 nanowires and PdCl2 were added to water for ultrasonic dispersion, the ultrasonic dispersion power was 70% and the dispersion time was 1 hour.
[0036] Specifically, the centrifugation speed was 7830 r / min and the centrifugation time was 10 min. After centrifugation, the precipitate was washed three times with anhydrous ethanol and deionized water, and then added to water for ultrasonic dispersion. The ultrasonic dispersion power was 70% and the dispersion time was 1 h.
[0037] Specifically, the suspension is subjected to rotary evaporation, and after the process, the evaporated solid product is dried at 80°C for 12 hours.
[0038] It is understood that this invention employs a combination of hydrothermal, chemical reduction, and calcination methods to prepare WO3 / PdO composite nanomaterials. In this composite material, ultra-small PdO nanoparticles are uniformly loaded on the surface of WO3 nanowires, which not only provide more catalytic active sites but also form an effective pn heterojunction structure with WO3, thereby significantly enhancing the adsorption, dissociation, and interfacial charge transport processes of hydrogen molecules.
[0039] Understandably, this invention combines the catalytic activity of PdO with the gas-sensing properties of WO3 by loading ultra-small PdO nanoparticles onto the surface of WO3 nanowires. PdO can promote the adsorption and dissociation of hydrogen molecules, reducing the activation energy of the surface reaction, thus enabling the sensor to achieve a high response at a lower temperature. Compared to the high operating temperature of some existing WO3-based hydrogen sensing materials, this invention can effectively reduce the optimal operating temperature, decrease device energy consumption, and improve the safety of use in hydrogen detection processes.
[0040] It is understood that in this invention, PdO nanoparticles are uniformly loaded onto the surface of WO3 nanowires, increasing the number of catalytically active sites favorable for hydrogen reactions. Simultaneously, the pn heterojunction formed between PdO and WO3 can modulate the interfacial barrier and carrier migration behavior, amplifying the resistance change signal induced by hydrogen. Therefore, the WO3 / PdO composite material prepared in this invention exhibits a high response value to hydrogen, meeting the requirements for low-concentration hydrogen detection and rapid early warning.
[0041] It is understood that the composite material prepared by this invention has a high specific surface area and abundant mesoporous structure, which is conducive to the diffusion, adsorption and desorption of hydrogen molecules; at the same time, the catalytic effect of PdO can accelerate the surface reaction process. Therefore, the hydrogen sensor prepared by this invention has good response speed and recovery speed, and is suitable for real-time detection applications.
[0042] Understandably, this invention utilizes the catalytic selectivity of PdO and the synergistic effect of the WO3 / PdO heterostructure to improve the material's sensitivity to hydrogen and reduce interference from other gases on the detection results. Simultaneously, the prepared composite material exhibits a stable structure, with PdO and WO3 fully bonded, thus the sensor demonstrates good repeatability and long-term stability, facilitating continuous monitoring.
[0043] Understandably, this invention achieves more thorough interfacial contact between PdO and WO3 by controlling the size of PdO nanoparticles and their dispersion state on the surface of WO3 nanowires. This technical feature not only helps to exert the catalytic activity of PdO but also enhances the charge regulation effect at the heterojunction interface, thereby further improving the overall gas-sensing performance of the material.
[0044] In this invention, the molar ratio of Na2WO4·2H2O and K2SO4 is 2:1.
[0045] In this invention, the heating temperature of the first heat treatment is 180°C and the heating time is 24 hours.
[0046] In this invention, the Pd atoms in the WO3 / PdO composite material account for 1-2 at% of the total number of Pd and W atoms; preferably, the Pd atoms in the WO3 / PdO composite material account for 1.5 at% of the total number of Pd and W atoms.
[0047] In this invention, the concentration of the sodium borohydride aqueous solution is 0.1 mol / L.
[0048] In this invention, the stirring time of the stirring reaction is 1 hour, and the stirring environment is an ice bath.
[0049] In this invention, the temperature of the rotary evaporation is 200°C and the rotation speed is 300 r / min.
[0050] Specifically, the suspension is poured into a beaker and then placed on a heating platform and heated by rotation at a temperature of 200°C and a speed of 300 r / min until all the liquid inside the beaker has evaporated.
[0051] In this invention, the heating temperature of the second heat treatment is 400°C and the heating time is 2 hours.
[0052] The present invention also proposes a WO3 / PdO composite material prepared by the preparation method described above.
[0053] This invention also proposes an application of WO3 / PdO composite material in hydrogen sensing and detection.
[0054] It is understandable that this invention can effectively reduce the operating temperature of the hydrogen sensor, improve the safety of the detection process, significantly improve the material's response value to low concentrations of hydrogen, and exhibit good response recovery speed, stability, and selectivity. With a PdO loading of 1.5 at%, the WO3 / PdO composite material prepared in this invention achieves a response value of 290 to 50 ppm H2 at 105℃, demonstrating excellent hydrogen sensing performance. Therefore, it has promising application prospects in the field of hydrogen leak monitoring and safety early warning.
[0055] Example 1 Pd atomic loading: Pd atoms account for 1 at of the total number of Pd and W atoms.
[0056] Preparation of WO3 nanowires: S1. Weigh 1.155g Na2WO4·2H2O and 0.3g K2SO4 into a 50mL beaker, add 20mL deionized water and stir for 1h to form a transparent solution. Add 2mol / L dilute hydrochloric acid dropwise to the solution to adjust the pH to 1.5, and continue stirring for 1h to obtain the first mixed solution. S2. Transfer the first mixed solution into a 50mL polytetrafluoroethylene-lined hydrothermal crystallization vessel, place it in an oven and heat at 180°C for 24 hours. After naturally cooling to room temperature, wash it three times with anhydrous ethanol and deionized water, and then dry it at 80°C for 12 hours.
[0057] Preparation of WO3 / PdO composite materials: S1. Weigh 250 mg of the prepared WO3 nanowire powder and 1.9 mg of PdCl2, add them to 25 mL of deionized water, and ultrasonically disperse them at 70% power for 1 h to fully mix WO3 and PdCl3 to obtain a second mixed solution. S2. Add 2.6 ml of 0.1 mol / L sodium borohydride aqueous solution dropwise to the second mixed solution and stir continuously for 1 h. After the reaction is completed, centrifuge at 7830 r / min for 10 min, wash the precipitate three times with anhydrous ethanol and deionized water, add the washed precipitate to 2 ml of water and sonicate at 70% power for 1 h to obtain a suspension. S3. Pour the suspension into a beaker, then place it on a heating platform and rotate it at 200°C and 300 r / min until all the liquid inside the beaker has evaporated. Dry the evaporated solid at 80°C for 12 hours to obtain the WO3 / PdO precursor material. Place the WO3 / PdO precursor material in a muffle furnace and calcine it at 400°C for 2 hours to obtain the WO3 / PdO composite material.
[0058] Example 2 Pd atom loading: Pd atoms account for 1.5 at of the total number of Pd and W atoms.
[0059] Preparation of WO3 nanowires: S1. Weigh 1.155g Na2WO4·2H2O and 0.3g K2SO4 into a 50mL beaker, add 20mL deionized water and stir for 1h to form a transparent solution. Add 2mol / L dilute hydrochloric acid dropwise to the solution to adjust the pH to 1.5, and continue stirring for 1h to obtain the first mixed solution. S2. Transfer the first mixed solution into a 50mL polytetrafluoroethylene-lined hydrothermal crystallization vessel, place it in an oven and heat at 180°C for 24 hours. After naturally cooling to room temperature, wash it three times with anhydrous ethanol and deionized water, and then dry it at 80°C for 12 hours.
[0060] Preparation of WO3 / PdO composite materials: S1. Weigh 250 mg of the prepared WO3 nanowire powder and 2.85 mg of PdCl2, add them to 25 mL of deionized water, and ultrasonically disperse them at 70% power for 1 h to fully mix WO3 and PdCl3 to obtain a second mixed solution. S2. Add 3.91 ml of 0.1 mol / L sodium borohydride aqueous solution dropwise to the second mixed solution and stir continuously for 1 h. After the reaction is completed, centrifuge at 7830 r / min for 10 min, wash the precipitate three times with anhydrous ethanol and deionized water, add the washed precipitate to 2 ml of water and sonicate at 70% power for 1 h to obtain a suspension. S3. Pour the suspension into a beaker, then place it on a heating platform and rotate it at 200°C and 300 r / min until all the liquid inside the beaker has evaporated. Dry the evaporated solid at 80°C for 12 hours to obtain the WO3 / PdO precursor material. Place the WO3 / PdO precursor material in a muffle furnace and calcine it at 400°C for 2 hours to obtain the WO3 / PdO composite material.
[0061] Example 3 Pd atom loading: Pd atoms account for 2 at of the total number of Pd and W atoms.
[0062] Preparation of WO3 nanowires: S1. Weigh 1.155g Na2WO4·2H2O and 0.3g K2SO4 into a 50mL beaker, add 20mL deionized water and stir for 1h to form a transparent solution. Add 2mol / L dilute hydrochloric acid dropwise to the solution to adjust the pH to 1.5, and continue stirring for 1h to obtain the first mixed solution. S2. Transfer the first mixed solution into a 50mL polytetrafluoroethylene-lined hydrothermal crystallization vessel, place it in an oven and heat at 180°C for 24 hours. After naturally cooling to room temperature, wash it three times with anhydrous ethanol and deionized water, and then dry it at 80°C for 12 hours.
[0063] Preparation of WO3 / PdO composite materials: S1. Weigh 250 mg of the prepared WO3 nanowire powder and 3.8 mg of PdCl2, add them to 25 mL of deionized water, and ultrasonically disperse them at 70% power for 1 h to fully mix WO3 and PdCl3 to obtain a second mixed solution. S2. Add 5.2 ml of 0.1 mol / L sodium borohydride aqueous solution dropwise to the second mixed solution and stir continuously for 1 h. After the reaction is completed, centrifuge at 7830 r / min for 10 min, wash the precipitate three times with anhydrous ethanol and deionized water, add the washed precipitate to 2 ml of water and sonicate at 70% power for 1 h to obtain a suspension. S3. Pour the suspension into a beaker, then place it on a heating platform and rotate it at 200°C and 300 r / min until all the liquid inside the beaker has evaporated. Dry the evaporated solid at 80°C for 12 hours to obtain the WO3 / PdO precursor material. Place the WO3 / PdO precursor material in a muffle furnace and calcine it at 400°C for 2 hours to obtain the WO3 / PdO composite material.
[0064] Effect test The WO3 / PdO composite material prepared in Example 2 was characterized and tested, and the results are as follows: Figure 1 As shown.
[0065] The performance of the WO3 / PdO composite material prepared in Example 2 was tested: Gas testing is performed using a side-heated gas sensor. First, place the WO3 / PdO composite material in a mortar and pestle, add a small amount of ethanol solution, and grind to disperse it into a uniform paste. Use a small brush to apply the paste evenly to a ceramic tube with gold electrodes. Weld the ceramic tube to a hexagonal base, and weld a nickel-chromium alloy heating wire to the center of the ceramic tube for heating with a suitable DC current. The gas sensor is now complete. Place the gas sensor on an aging bench for 48 hours, and then perform gas testing. Gas testing: A digital multimeter was used to synchronously acquire the sensor's resistance signal. In an H2 atmosphere, the sensor's resistance value gradually decreased. The sensor's resistance response value was defined as: Sr = R a / R g Where Ra and Rg are the resistance values of the sensor in air and H2 atmosphere, respectively, and the results are as follows: Figure 3-4 As shown.
[0066] like Figure 2 As shown ( Figure 2 In Figure a, WO3 / PdO 1at% nanowire, WO3 / PdO 1.5at% nanowire, and WO3 / PdO 2at% nanowire gas sensors respond to 50 ppm H2 at different temperatures; and in Figure b, the response and recovery time of the WO3 / PdO 1.5at% nanowire gas sensor to 50 ppm H2 at 105 °C. The hydrogen response values of all three materials first increase and then decrease with increasing temperature. The optimal operating temperature for the WO3 / PdO 1.5at% nanowire is 105 °C, while the optimal operating temperatures for the WO3 / PdO 1at% and WO3 / PdO 2at% nanowires are 115 °C. The material with a 1.5at% Pd loading has the highest peak response of 290, which is significantly better than the materials with 1at% and 2at% loadings. Meanwhile, the sensor's resistance drops rapidly after H2 is introduced, with a response time (time for the resistance to drop to 90% of its stable value) of approximately 30 seconds; after switching back to air, the resistance gradually recovers, with a recovery time (time for the resistance to recover to 90% of its initial value) of approximately 182 seconds, demonstrating a fast response speed and good recovery performance.
[0067] like Figure 3 As shown, during a continuous 30-day cyclic test period, the sensor's response to 50ppm H2 remained at a high level without significant attenuation, drift, or large fluctuations. This demonstrates that the hydrogen sensor prepared from this composite material has excellent long-term stability and test repeatability, and can meet the application requirements for long-term continuous monitoring of hydrogen leaks.
[0068] like Figure 4 As shown, the sensor can generate a clear and distinguishable response signal for low concentrations of H2 in the range of 10-50 ppm. The response value increases approximately linearly with the increase of H2 concentration. Moreover, the response rises rapidly each time H2 is introduced and falls back quickly after switching to air. Furthermore, the baseline remains stable without drift during the cyclic testing of different concentrations, proving that the sensor has good sensitivity and dynamic response characteristics for low concentrations of hydrogen and can achieve quantitative detection and rapid early warning of hydrogen in the range of 10-50 ppm.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a WO3 / PdO composite material, characterized in that, Including preparation steps: Take Na2WO4·2H2O and K2SO4, add them to water and stir to dissolve. Then adjust the pH of the solution to 1.5, stir and mix to obtain the first mixed solution. The first solution was subjected to a first heating treatment, and after the treatment, it was washed and dried to obtain WO3 nanowires. The WO3 nanowires and PdCl2 were added to water and ultrasonically dispersed to obtain a second mixed solution; Sodium borohydride aqueous solution was added to the second mixed solution and stirred to react. After the reaction was completed, the mixture was centrifuged and the precipitate was added to water and ultrasonically dispersed to obtain a suspension. The suspension was subjected to rotary evaporation and then dried to obtain a WO3 / PdO precursor material; the WO3 / PdO precursor material was subjected to a second heat treatment to obtain the WO3 / PdO composite material.
2. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The molar ratio of Na2WO4·2H2O to K2SO4 is 2:
1.
3. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The heating temperature for the first heat treatment is 180°C, and the heating time is 24 hours.
4. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, In the WO3 / PdO composite material, Pd atoms account for 1-2 at of the total number of Pd and W atoms.
5. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The concentration of the sodium borohydride aqueous solution is 0.1 mol / L.
6. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The stirring time for the stirring reaction was 1 hour, and the stirring environment was an ice bath.
7. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The rotary evaporation temperature is 200℃ and the rotation speed is 300 r / min.
8. The method for preparing the WO3 / PdO composite material according to claim 1, characterized in that, The second heat treatment is performed at a temperature of 400°C for 2 hours.
9. A WO3 / PdO composite material prepared by the preparation method according to any one of claims 1-8.
10. The application of the WO3 / PdO composite material as described in claim 9 in a hydrogen sensor.