A method for controlling the heat transfer properties of a fluorine-free mold flux for high-titanium steel continuous casting.

By preparing CaO-Al2O3-based fluorine-free continuous casting protective slag for high-titanium steel and controlling the crystallization heat transfer characteristics of the slag film, the problems of SiO2 interface reaction and fluoride corrosion in traditional protective slags were solved, achieving efficient heat transfer control and environmentally friendly billet production.

CN123060065APending Publication Date: 2026-11-10NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611184030.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the continuous casting process of high titanium steel, the high SiO2 content in traditional protective slag leads to the reaction at the steel-slag interface, resulting in unstable slag film composition and surface defects of the billet. Fluorine-containing protective slag corrodes equipment and pollutes the environment. Heat transfer control is insufficient, and the composition design lacks predictive means at the microstructure level, resulting in long adjustment cycles and low efficiency.

Method used

Using CaO-Al2O3-based high-titanium steel fluorine-free continuous casting protective slag, transparent or translucent glassy slag blocks are prepared by controlling the composition ratio and process steps, including ball milling, melting, rapid cooling, drying, crushing and grinding. The crystallization heat transfer characteristics of the slag film are regulated, and TiO2 is used to replace CaF2 to control the slag film thickness, porosity and surface roughness. The composition is optimized by combining molecular dynamics simulation.

Benefits of technology

It eliminates fluoride corrosion, reduces surface defects in cast billets, improves heat transfer regulation, simplifies operation procedures, enhances batch reproducibility and composition optimization efficiency, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060065A_ABST
    Figure CN123060065A_ABST
Patent Text Reader

Abstract

This invention discloses a method for controlling the heat transfer properties of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film. In this invention, TiO2 completely replaces CaF2, eliminating the corrosion of equipment, environmental pollution, and health hazards to operators caused by fluorides, while reducing the dependence on special environmental protection equipment in the continuous casting process. By strictly limiting the SiO2 content to the range of 3%–5%, the interfacial reaction between Ti in the steel and SiO2 in the protective slag is significantly suppressed, preventing the slag film composition from deteriorating due to the reaction. Through TiO2-induced perovskite as the dominant precipitated crystalline phase, the crystallinity concentration and structural stability of the slag film are improved, while the surface roughness, apparent porosity, and true porosity of the slag film are increased. This reduces the interfacial contact area between the slag film and the copper wall and the internal thermal conductivity, effectively controlling the steady-state heat flux density, thereby reducing the probability of surface cracks and steel leakage in the cast billet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of continuous casting technology in iron and steel metallurgy, specifically a method for controlling the heat transfer characteristics of a fluorine-free protective slag for high-titanium steel continuous casting and its slag film. Background Technology

[0002] High-titanium steel, due to its high strength, good corrosion resistance, and excellent low-temperature performance, has been widely used in aerospace, automotive, chemical, and medical fields. However, during the continuous casting process of high-titanium steel, the Ti in the steel undergoes a significant interfacial reaction with the SiO2 in the protective slag, leading to changes in the composition and deterioration of the protective slag's properties, and further causing surface defects in the cast billet, even resulting in leaks in severe cases. To mitigate the adverse effects of the steel-slag reaction, researchers have developed CaO-Al2O3-based protective slags for high-titanium steel. CaF2 is often added as a flux to improve its physicochemical properties.

[0003] However, existing fluorine-containing protective slags release fluorides at high temperatures, corroding equipment and polluting the environment; traditional protective slags have a high SiO2 content, which easily reacts with Ti in steel at the interface, leading to unstable slag film composition and surface defects in the billet; fluorine-containing slag systems rely on multiphase competitive crystallization to control heat transfer, resulting in limited slag film thickening and porosity improvement, and insufficient heat flow suppression capability in the later stages; the design of protective slag composition lacks predictive means at the microstructure level, and formula optimization mainly relies on empirical trial and error of macroscopic heat flow testing, which has a long adjustment cycle and low efficiency. Summary of the Invention

[0004] The purpose of this invention is to provide a method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film in order to solve the problems mentioned above.

[0005] The technical solution adopted in this invention is as follows: a fluorine-free continuous casting protective slag for high-titanium steel, comprising: CaO: 28%–30%, Al2O3, etc. 3: 26%–28%, TiO 2: 8%–10%, SiO 2: 3%~5%, BaO: 10%~12%, Na2O: 8%~10%, B2O 3: 8%–11%.

[0006] In a preferred embodiment, a method for preparing a fluorine-free continuous casting protective slag for high-titanium steel includes the following steps: S1: Weigh the chemically pure raw materials according to the mass percentage, put the weighed raw materials into a high-performance ball mill, and mix and stir at a speed of 300-400 r / min for 30-45 min to obtain a uniformly mixed powder; S2: Load the mixed powder into a high-purity graphite crucible, place it in an induction furnace, heat it to 1400-1450℃ at a heating rate of 5-8℃ / min, hold it for 20-30min, and stir it with a molybdenum rod every 5min during the holding period. Each stirring lasts for 30-60s to homogenize the melt composition. S3: Quickly pour the completely molten liquid protective slag into deionized water at 25°C for water quenching and rapid cooling to obtain transparent or translucent glassy slag blocks. S4: Place the glassy slag block obtained by water quenching into an oven and dry it at 105-110℃ for 12-24 hours. Then use a jaw crusher to crush the dried slag block into particles with a particle size of less than 5mm. S5: Place the crushed granules in a planetary ball mill and grind for 20-30 minutes. Pass the granules through a 200-mesh standard sieve and take the sieve-passing material and seal it in a sealed container to obtain the finished product of high-titanium steel fluorine-free continuous casting protective slag.

[0007] In a preferred embodiment, in step S1, the amount of Na2CO3 weighed needs to be converted based on the target mass fraction of Na2O (8%–10%), with a conversion factor of 1.71 (the molecular weight ratio of Na2CO3 to Na2O). All weighed raw materials are loaded into the grinding jar of a high-performance ball mill. The ball mill speed is set to 300–400 r / min, and mixing is continued for 30–45 minutes until the powder components achieve a uniform dispersion at the microscopic scale. After mixing, the powder is removed and placed in a sealed bag for later use to prevent the fine powder from absorbing moisture or introducing impurities.

[0008] In a preferred embodiment, in step S2, the uniformly mixed powder is transferred to a high-purity graphite crucible, with the powder filling volume controlled to approximately 2 / 3 of the crucible's volume to prevent overflow during heating expansion. The graphite crucible containing the powder is placed in the center of the heating coil of the induction furnace. After closing the furnace door, the heating program is started, with the heating rate set to 5°C / min to 8°C / min, gradually increasing the furnace temperature from room temperature to the target melting temperature of 1400°C to 1450°C. After reaching the target temperature, a holding stage is entered, maintaining the holding time for 20 to 30 minutes to ensure that the powder fully melts and forms a uniform liquid phase at this temperature. During the holding period, a molybdenum stirring rod is inserted into the crucible every 5 minutes to manually stir the melt, with each stirring lasting 30 to 60 seconds. The molybdenum rod should avoid touching the crucible wall when inserting and removing it to prevent crucible breakage and the introduction of impurities. Throughout the heating and heat preservation process, the power output of the induction furnace must remain stable. A small amount of inert gas can be introduced into the furnace as a protective atmosphere to suppress the volatilization of some oxides or unexpected valence state changes at high temperatures.

[0009] In a preferred embodiment, in step S3, the graphite crucible containing the fully molten protective slag is quickly removed from the induction furnace and placed over a stainless steel container filled with sufficient deionized water. The liquid slag is then poured in a thin, uniform stream into the room-temperature deionized water for rapid cooling. During the water quenching process, the liquid slag solidifies rapidly in a very short time. Due to the rapid cooling effect, a large amount of the high-temperature structure of the melt is frozen, resulting in a transparent or translucent glassy slag block. The key to the water quenching operation is controlling the pouring speed. It is necessary to avoid the liquid flow being too coarse, which would lead to insufficient quenching and formation of crystalline phases, and to prevent it from being too fine, which would cause splashing and spraying. The pouring process should be completed continuously within a few seconds. After quenching, the glassy slag block is removed from the water, allowed to drain naturally, and then transferred to a clean tray for further processing.

[0010] In a preferred embodiment, in step S4, the glassy slag obtained from water quenching is evenly spread on a tray and placed in a forced-air drying oven at a temperature of 105℃~110℃ for 12h~24h to completely remove the moisture adhering to and absorbed during the water quenching process. After drying, the slag is removed and allowed to cool naturally to room temperature before being fed into a jaw crusher. The distance between the two jaw plates of the crusher is adjusted to a suitable position so that the output particle size is controlled below 5mm. The crushing operation should be carried out in stages, with larger slag particles being coarsely crushed first, followed by fine crushing by adjusting the jaw plate distance. The crushing chamber should be cleaned promptly after each crushing to avoid residual material mixing into the next batch of samples. Because B2O3 has a certain degree of hygroscopicity, the crushed granules need to be transferred to the next grinding step in a timely manner or temporarily stored in a dryer, and should not be exposed to air for too long.

[0011] In a preferred embodiment, in step S5, the slag particles with a diameter less than 5 mm after crushing and sieving are fed into a planetary ball mill for fine grinding. The ball mill speed is set to 200 r / min to 300 r / min, and the grinding time is 20 min to 30 min. The grinding jar and grinding balls are made of zirconium oxide or corundum to reduce the introduction of metal impurities during the grinding process. After grinding, the powder is removed and poured into a standard 200-mesh vibrating sieve for sieving. The sieve is vibrated continuously for no less than 10 min until the amount of material passing through the sieve no longer increases significantly. The fine powder passing through the 200-mesh sieve is collected and placed in a double-layer sealed bag. After the air inside the bag is expelled, it is sealed, and then covered with a light-proof container with a desiccant. Finally, the high-titanium steel fluorine-free continuous casting protective slag is obtained. The finished product should be labeled with the formula number and preparation date and stored in a cool, dry place for later use.

[0012] In a preferred embodiment, a method for controlling the heat transfer properties of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film includes the following steps: S1: The basicity of the protective slag, CaO / Al2O3, is controlled between 1.00 and 1.15, and the mass fraction of TiO2 is set to 8% to 10%, while the mass fraction of SiO2 is limited to 3% to 5%. This serves as the basic composition framework, so that perovskite CaTiO3 becomes the dominant precipitated crystalline phase during the solidification process of the slag, replacing the multiphase competitive precipitation pathways of borate and aluminate in the fluorine-containing slag system. This establishes a crystallization heat transfer control basis with a single crystalline phase as the core.

[0013] S2: By adjusting the mass fractions of BaO, Na2O, and B2O3 to within the ranges of 10%–12%, 8%–10%, and 8%–11%, respectively, the polymerization degree and ion migration ability of the slag are controlled, enabling the liquid slag to quickly form an initial solidified shell after contacting the water-cooled copper probe, and to complete the initial growth of the slag film thickness within a time window of 20s–40s. The peak heat flux density is controlled between 0.85 MW / m² and 0.92 MW / m² to avoid excessively high initial heat transfer shock.

[0014] S3: After the slag film growth enters the steady-state stage of 40s to 80s, the perovskite crystal layer gradually thickens due to the increased TiO2 content, so that the solid slag film thickness reaches 2.8cm to 3.0cm at 80s. At the same time, by controlling the cooling intensity, the surface roughness Sa of the slag film in contact with the copper wall is stabilized in the range of 18μm to 20μm, the apparent porosity is maintained at 1.8vol% to 2.0vol%, and the true porosity is maintained at 5.0% to 5.5%, thereby increasing the interfacial contact thermal resistance and the internal radiation thermal resistance of the slag film.

[0015] S4: Molecular dynamics simulations were used to pre-obtain the coordination number distribution of Al-O, Ti-O, and Si-O atom pairs and the Al-O tetrahedron under the target composition. Structural unit ratio, when Q³, Q 4 , When the total proportion of highly polymerized structural units exceeds 40%, the high-temperature liquid slag corresponding to this composition is determined to have high phonon transport efficiency, ensuring a peak heat flux density of not less than 0.85 MW / m² to meet initial lubrication requirements; simultaneously, based on simulation results... Tetrahedron proportion and The relative changing trend of the octahedral proportion can be used to predict the precipitation tendency of perovskite and serve as a structural basis for fine-tuning the composition.

[0016] S5: When the measured steady-state heat flux density deviates from the target range of 0.52 MW / m² to 0.56 MW / m², adjust the TiO2 content by increasing or decreasing it by 0.5% to 1.0% within the range of 8% to 10%, and correspondingly adjust the CaO content to maintain constant alkalinity. This will change the amount of perovskite crystals, thereby altering the porosity and roughness of the slag film, until the heat flux density returns to the target range. If the heat flux density is too low, appropriately reduce the TiO2 content to reduce the slag film thickness and porosity. If it is too high, increase the TiO2 content to enhance the inhibitory effect of the crystalline layer on heat transfer.

[0017] S6: After each composition adjustment, the slag film thickness and true porosity are re-measured, and the steady-state heat flux density at 80s is used as the final evaluation index. When the heat flux density at that time is stable at 0.52 MW / m²~0.56 MW / m², the slag film thickness reaches more than 2.8cm, and the true porosity is higher than 5.0%, it is determined that the heat transfer characteristics of the slag system have reached the target state, and the composition scheme can be put into practical application as the preferred formula under this continuous casting condition.

[0018] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. In this invention, TiO2 completely replaces CaF2, eliminating the corrosion of equipment, environmental pollution, and health hazards to operators caused by fluorides, while reducing the reliance on special environmental protection equipment in the continuous casting process. By strictly limiting the SiO2 content to the range of 3% to 5%, the interfacial reaction between Ti in the steel and SiO2 in the protective slag is significantly suppressed, preventing the slag film composition from deteriorating due to the reaction. TiO2 induces perovskite as the dominant precipitated crystalline phase, improving the crystallinity concentration and structural stability of the slag film, while increasing the surface roughness, apparent porosity, and true porosity of the slag film. This reduces the interfacial contact area between the slag film and the copper wall and the internal thermal conductivity, effectively controlling the steady-state heat flux density, thereby reducing the probability of surface cracks and steel leakage in the cast billet.

[0019] 2. In this invention, while ensuring the initial heat transfer capacity in the liquid-slag stage, the thermal resistance control capability of the slag film in the later stage of solidification is improved, realizing active intervention in the heat transfer process. This preparation method uses conventional equipment and process routes, improving operational convenience and batch reproducibility, and reducing manufacturing costs and process complexity. This control method uses the coordination number output by molecular dynamics simulation and... Using distribution as a basis for composition adjustment improves the targeting and efficiency of composition optimization, and reduces the number of trials and errors and the time cost associated with relying on experience. Replacing CaF2 with TiO2 in this slag system with CaF2 based on fluorine-containing slag also improves the degree of polymerization and phonon transport efficiency of the melt. Attached Figure Description

[0020] Figure 1The X-ray diffraction pattern of the water-quenched slag of this invention; Figure 2 This is a schematic diagram of the crystallizer slag film heat flow simulator of the present invention; Figure 3 This is a schematic diagram of the slag film thickness measurement position according to the present invention; Figure 4 This is a graph showing the change in heat flux density over time for different protective slag samples in this invention. Figure 5 This is a graph showing the change in the thickness of the solid slag film over time in this invention. Figure 6 The X-ray diffraction pattern of the solid slag film containing fluorine protective slag in this invention; Figure 7 The X-ray diffraction pattern of the solid slag film of the fluorine-free titanium-containing protective slag in this invention; Figure 8 This is a diagram showing the measurement location of the slag film surface roughness and the false-color morphology obtained by laser confocal imaging in this invention. Figure 9 This is a comparison diagram of the surface roughness of different solid slag films of protective slag in this invention; Figure 10 This is a comparison diagram of the apparent porosity of different solid slag films of protective slag in this invention; Figure 11 This is a comparison diagram of the true porosity of different solid slag films of protective slag in this invention; Figure 12 This is a graph showing the change in the apparent comprehensive thermal conductivity of the solid slag film over time in this invention. Figure 13 This is a molecular dynamics simulation result of the atomic configuration of a typical protective slag melt in this invention; Figure 14 The diagram shows the coordination number distribution curves of Al-O, Ca-O, Si-O, and Ti-O atomic pairs in different protective slag melts in this invention. Figure 15 This is a diagram showing the coordination number distribution of Al-F, Ca-F, and Si-F atomic pairs in the fluorine-containing protective slag melt of this invention. Figure 16 This is a statistical distribution diagram of the coordination numbers of Al-O, Al-F, and Ti-O as a function of composition in this invention; Figure 17 The Al-O tetrahedron in this invention Distribution pattern of structural units as composition changes; Figure 18 This is a schematic diagram of the overall process principle in this invention. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0022] Example: Refer to Figure 1-18 A fluorine-free continuous casting protective slag for high-titanium steel, comprising: CaO: 28%–30%, Al2O3, etc. 3: 26%–28%, TiO 2: 8%–10%, SiO 2: 3%~5%, BaO: 10%~12%, Na2O: 8%~10%, B2O 3: 8%–11%.

[0023] A method for preparing a fluorine-free continuous casting protective slag for high-titanium steel includes the following steps: S1: Weigh the chemically pure raw materials according to the mass percentage, put the weighed raw materials into a high-performance ball mill, and mix and stir at a speed of 300-400 r / min for 30-45 min to obtain a uniformly mixed powder; S2: Load the mixed powder into a high-purity graphite crucible, place it in an induction furnace, heat it to 1400-1450℃ at a heating rate of 5-8℃ / min, hold it for 20-30min, and stir it with a molybdenum rod every 5min during the holding period. Each stirring lasts for 30-60s to homogenize the melt composition. S3: Quickly pour the completely molten liquid protective slag into deionized water at 25°C for water quenching and rapid cooling to obtain transparent or translucent glassy slag blocks. S4: Place the glassy slag block obtained by water quenching into an oven and dry it at 105-110℃ for 12-24 hours. Then use a jaw crusher to crush the dried slag block into particles with a particle size of less than 5mm. S5: Place the crushed granules in a planetary ball mill and grind for 20-30 minutes. Pass the granules through a 200-mesh standard sieve and take the sieve-passing material and seal it in a sealed container to obtain the finished product of high-titanium steel fluorine-free continuous casting protective slag.

[0024] In step S1, the amount of Na2CO3 weighed needs to be converted based on the target mass fraction of Na2O (8%–10%), with a conversion factor of 1.71 (the molecular weight ratio of Na2CO3 to Na2O). All weighed raw materials are then placed into the grinding jar of a high-performance ball mill. The ball mill speed is set to 300–400 r / min, and mixing is continued for 30–45 minutes until the powder components achieve a uniform dispersion at the microscopic scale. After mixing, the powder is removed and placed in a sealed bag for later use to prevent moisture absorption or the introduction of impurities.

[0025] In step S2, the uniformly mixed powder is transferred to a high-purity graphite crucible, with the powder filling volume controlled to approximately 2 / 3 of the crucible's volume to prevent overflow during heating expansion. The graphite crucible containing the powder is placed in the center of the heating coil of the induction furnace. After closing the furnace door, the heating program is started, with the heating rate set to 5℃ / min~8℃ / min, gradually increasing the furnace temperature from room temperature to the target melting temperature of 1400℃~1450℃. After reaching the target temperature, a holding stage is initiated, maintaining the holding time for 20min~30min to ensure that the powder fully melts and forms a uniform liquid phase at this temperature. During the holding period, a molybdenum stirring rod is inserted into the crucible every 5min to manually stir the melt, with each stirring lasting 30s~60s. The molybdenum rod should avoid touching the crucible wall when inserting and removing it to prevent crucible breakage and the introduction of impurities. Throughout the heating and heat preservation process, the power output of the induction furnace must remain stable. A small amount of inert gas can be introduced into the furnace as a protective atmosphere to suppress the volatilization of some oxides or unexpected valence state changes at high temperatures.

[0026] In step S3, the graphite crucible containing the fully melted protective slag is quickly removed from the induction furnace and placed over a stainless steel container filled with sufficient deionized water. The liquid slag is then poured in a thin, uniform stream into the room-temperature deionized water for rapid cooling. During the water quenching process, the liquid slag solidifies rapidly in a very short time. Due to the rapid cooling effect, a large amount of the high-temperature structure of the melt is frozen, resulting in transparent or translucent glassy slag blocks. The key to the water quenching operation is controlling the pouring speed. It is necessary to avoid the liquid flow being too coarse, which would lead to insufficient quenching and formation of crystalline phases, and to prevent it from being too fine, which would cause splashing and spraying. The pouring process should be completed continuously within a few seconds. After quenching, the glassy slag blocks are removed from the water, allowed to drain naturally, and then transferred to a clean tray for further processing.

[0027] In step S4, the glassy slag obtained from water quenching is evenly spread on a tray and placed in a forced-air drying oven at 105℃~110℃ for 12h~24h to completely remove the moisture adhering to and absorbed during water quenching. After drying, the slag is removed and allowed to cool naturally to room temperature before being fed into a jaw crusher. The distance between the two jaw plates of the crusher is adjusted to a suitable position so that the output particle size is controlled below 5mm. The crushing operation should be carried out in stages. Larger slag particles are coarsely crushed first, and then the jaw plate distance is adjusted for fine crushing. The crushing chamber should be cleaned in time after each crushing to avoid residual material from mixing into the next batch of samples. Because B2O3 has a certain degree of hygroscopicity, the crushed particles need to be transferred to the next grinding step in time or temporarily stored in a dryer. They should not be exposed to air for too long.

[0028] In step S5, the crushed and sieved slag particles with a diameter less than 5mm are fed into a planetary ball mill for fine grinding. The ball mill speed is set to 200r / min to 300r / min, and the grinding time is 20min to 30min. The grinding jar and grinding balls are made of zirconium oxide or corundum to reduce the introduction of metal impurities during the grinding process. After grinding, the powder is removed and poured into a standard 200-mesh vibrating screen for sieving. The screen is vibrated continuously for no less than 10min until the amount of material passing through the screen no longer increases significantly. The fine powder passing through the 200-mesh screen is collected and placed in a double-layer sealed bag. After the air inside the bag is expelled, it is sealed, and then covered with a light-proof container with a desiccant. Finally, the high-titanium steel fluorine-free continuous casting protective slag is obtained. The finished product should be labeled with the formula number and preparation date and stored in a cool, dry place for later use.

[0029] Experimental example: In this application, protective slag samples were prepared using chemically pure reagents such as CaO, Al2O3, CaF2, TiO2, SiO2, Na2CO3, B2O3, and BaCO3, with Na2CO3 and BaCO3 replacing Na2O and BaO, respectively. The compositions of the prepared fluorine-containing and fluorine-free CaO-Al2O3-based protective slags are shown in Table 1. The chemically pure reagents were mixed and stirred for half an hour using a high-performance ball mill to ensure homogeneity. The stirred sample was then placed in a high-purity graphite crucible and heated to 1400℃ in an induction furnace to melt the sample, holding it at that temperature for 20 minutes. During the holding period, the sample was stirred every five minutes to ensure uniform composition. The liquid protective slag was then rapidly poured into water and quickly quenched to obtain a completely glassy phase. Subsequently, the sample was crushed, ground, and sieved through a 200-mesh sieve.

[0030] Table 1 Flux CaO <![CDATA[Al2O3]]> <![CDATA[TiO2]]> <![CDATA[Na2O]]> <![CDATA[SiO2]]> BaO <![CDATA[CaF2]]> <![CDATA[B2O3]]> A 30 27 - 10 5 12 5 11 B 27 25 - 10 5 12 10 11 C 30 28 4 10 5 12 - 11 D 28 26 8 10 5 12 - 11 The water-quenched slag was then tested using X-ray diffraction (XRD, Rigaku TTRⅢ), and the results are as follows: Figure 1 As shown, the XRD curve of the water-quenched slag shows a relatively obvious "bun peak" and no obvious sharp characteristic peaks were found, indicating that the prepared water-quenched slag samples are all glass phases, which means that the sample composition is relatively uniform.

[0031] Slag film heat flux density analysis: The heat flux density was determined using an HF-200 crystallizer slag film heat flux simulator. A schematic diagram of the equipment is shown below. Figure 2 As shown. During the test, 350g of carbon-free protective slag was first placed into a high-purity graphite crucible with an inner diameter of 55mm. Then, the crucible was placed in a vertical furnace with a Si2Mo heating rod, heated to 1400℃, and held for 10 minutes to ensure complete melting. Then, the water-cooled copper probe was immersed in the molten slag pool.

[0032] A water-cooled copper probe, 35 mm in length and 20 mm in width and height, was vertically immersed in the liquid slag. The cooling water flow rate inside the copper probe was 200 L / h, and the immersion depth was approximately 18 mm. After the experiment, the slag film solidified on the copper probe was recovered. The heat flux density of the slag film was calculated using the temperature difference between the inlet and outlet water of the water-cooled copper probe. The inlet water temperature was approximately 35℃ ± 0.5℃. The formula for calculating the heat flux density is shown in Equation 1.

[0033] (1) in, Heat flux density, W / m 2 W represents the cooling water flow rate inside the copper probe, in kg / s. The inlet and outlet water temperature difference of the copper probe is kJ; F is the effective heat transfer area of ​​the copper probe, m². 2 C represents the specific heat capacity of water, kJ / (kg·K). To further analyze the changes in the structure and properties of the slag film, immersion times of the water-cooled copper probe were set at 20s, 40s, 45s, 60s, and 80s, respectively.

[0034] Slag film structure measurement: Solid slag film is a key medium in the heat transfer process within the mold, and its structural characteristics directly affect its total thermal resistance and heat flow transfer behavior. The heat transfer capacity of the slag film is not only related to its material composition but also closely related to its thickness, crystalline mineral phases, surface morphology, and pore structure. Therefore, slag film structure analysis is an important foundation for understanding the differences in heat transfer among different protective slags.

[0035] Slag film thickness measurement: The thickness of the slag film determines the heat transfer distance. A pointed outside micrometer was used to measure the slag film thickness. A wide-faced solid slag film was selected for measurement. The average of six tests for each sample was taken as the slag film thickness. The test locations were as follows: Figure 3 As shown.

[0036] The mineral phase composition reflects the solidification and crystallization characteristics of the slag film. As the immersion time increases, a stable air gap forms between the water-cooled copper probe and the solid slag film. At this point, reheat crystallization occurs, and the slag film continues to thicken while the crystals gradually grow. The solid slag film with a higher proportion of crystalline layer is taken, ground into powder, and passed through a 200-mesh sieve. X-ray diffraction (XRD, Bruker D8 ADVANCE, Germany) is then used to identify the crystalline phases in the slag film.

[0037] Surface roughness measurement: Surface roughness affects the contact state between the slag film and the copper probe. A solid slag film immersed for 45 seconds was used, and the surface roughness of the surface in contact with the copper probe was measured using a laser confocal microscope (LSM 800, ZEISS, Germany). LSM can perform "optical slicing" of samples through Z-axis scanning and 3D construction (Z-Stack) to analyze the three-dimensional structure of samples, the spatial distribution of target molecules, etc. When using it to measure surface roughness, linear roughness... More susceptible to the influence of "which line to select, scanning direction, and local random peaks and valleys"; surface roughness The method uses area data, which has a larger sampling range and is generally more representative of the overall surface condition. Therefore, this application prioritizes the use of surface roughness parameters. Equation 2 represents the surface roughness. The continuous form of (area arithmetic mean height) calculation.

[0038] in It is the sampling area. This refers to the height deviation of the surface relative to the average surface. Before calculating the roughness, the original 3D data is first leveled. The leveling method selects the smallest square plane, and the leveling operation is performed by difference (suitable for small tilt angles) to eliminate the overall tilt of the sample and establish a uniform reference plane. Subsequently, a spatial filter (used to remove noise) is applied to the surface data, and the NM point filling function is used to replace non-measured points (nearest neighbor interpolation). After completing the above preprocessing, the surface roughness parameters are calculated based on the processed surface data. .

[0039] Porosity measurement: Porosity affects the density and thermal conductivity of slag films. The apparent porosity and true porosity of solid slag films are key structural parameters that determine their heat transfer performance, directly influencing the heat transfer path, thermal resistance, and transient heat flow within the slag film. The specific steps for determining apparent porosity are as follows: First, dry the sample at 105~110℃ to constant weight and record its dried mass. Subsequently, the impregnation solution was slowly injected under vacuum conditions (<20 mmHg) to saturate the pores inside the sample; finally, the suspended mass of the saturated sample in the impregnation solution was weighed. And the mass in the air The formula for calculating apparent porosity is shown in Equation 3.

[0040] True porosity is calculated as the difference between the apparent density (Da) of the solid slag film and the true density (Dt) of the slag film after grinding it into 200-mesh powder. True density refers to the actual mass of a unit volume of solid material in an absolutely dense state, that is, the density after removing internal pores or voids between particles. This experiment used a true density meter (AccuPyc 1340, Micromeritics, USA) for measurement. The formula for calculating true porosity is shown in Equation 4.

[0041] In the formula, This difference is 1cm 3 The non-porous object is larger than 1cm 3 How much of a porous object is there?

[0042] Calculation of apparent overall thermal conductivity: To compare the overall heat transfer capacity of slag films from different samples, the apparent comprehensive thermal conductivity of the slag films was calculated to characterize the influence of slag film solidification structure factors on thermal conductivity values ​​at different times. According to Fourier's heat conduction equation, within an object, consider two parallel planes perpendicular to the direction of heat conduction, separated by a distance h, with temperatures T1 and T2 respectively (assuming T1 > T2). If the area of ​​each plane is S, at time... Heat passing through the internal surface area S Satisfy the following expression 5: In the formula For heat flow, This is the thermal conductivity (also known as the thermal conductivity coefficient) of the material. When the temperature difference between two planes separated by a unit length is numerically equal to the temperature difference of one unit, the heat passing through a unit area per unit time is expressed in W·m³. -1 ·K -1 By converting the left and right sides of equation 5, we can obtain formula 6 for calculating thermal conductivity.

[0043] (6) Since this application only measures the liquid slag temperature, probe cooling water inlet and outlet temperatures, heat flux density, and slag film thickness, and does not directly obtain the slag film hot surface temperature, slag film cold surface temperature, and copper probe hot surface temperature, it is impossible to strictly separate the internal thermal resistance of the slag film from the slag film / copper probe interface thermal resistance. Considering that the interface thermal resistance has a significant impact on the total thermal resistance during the heat transfer process of continuous casting protective slag, this paper does not define the calculated result as the intrinsic comprehensive thermal conductivity of the slag film, but defines it as the apparent comprehensive thermal conductivity characterizing the overall heat transfer capacity of the slag film under this experimental system.

[0044] In the calculation, the cooling water outlet temperature is taken as the approximate cold end temperature. The temperature of the liquid residue was taken as the approximate temperature of the high-temperature end. Combined with the measured heat flux density and slag film thickness Calculate the apparent comprehensive thermal conductivity. Combine Equation 1 and Equation 6 for calculating heat flux density. The heat flux density in Equation 1... That is, in equation 6 Unit W / m 2 Formula 7 can be derived for calculating the apparent comprehensive thermal conductivity of the slag film.

[0045] (7) in, The apparent overall thermal conductivity of the slag film (including the thermal resistance between the copper mold and the slag film). The thickness of the slag film at the current moment, in meters (m). and These represent the liquid slag temperature and the copper probe outlet temperature, respectively, in kJ. It should be noted that the values ​​calculated in this paper... The apparent comprehensive thermal conductivity is obtained based on the experimental temperature difference approximation. This parameter reflects the overall heat transfer capacity of the slag film under this experimental system and can be used for cross-sectional comparisons under the same experimental conditions, but it is not equivalent to the true comprehensive thermal conductivity determined solely by the intrinsic properties of the slag film material.

[0046] Molecular dynamics simulation: The effects of CaF2 and TiO2 on the microstructure of CaO-Al2O3-based protective slag were studied using Scigress (SCIGRESS, FQS Poland Sp.zoo, Kraków, Poland) molecular dynamics software, and the influence of the two on the heat transfer mechanism of the protective slag was analyzed at the molecular structure level.

[0047] Currently, numerous studies have demonstrated that the two-body potential function Born-Mayer-Higgins (BMH) can be accurately applied to the study of protective slags in aluminate systems. For systems that are essentially multi-component ionic melts, this potential function can effectively reflect the combined effects of long-range electrostatic interactions and short-range local interactions in the ionic melt, thus making it suitable for structural simulation studies of this system. Its functional form is usually written as Equation 8.

[0048] in, Represents particles With particles In distance Interaction potential energy at time; Indicates the distance between two particles; These are the effective charges of the corresponding particles; This is a long-range coulombic interaction term used to describe the electrostatic attraction or repulsion between ions; This is a short-range exponential repulsion term, used to characterize the strong repulsive effect caused by the overlap of electron clouds when particles approach each other; This is the van der Waals dispersion term, used to describe the weak van der Waals interactions between particles. In actual calculations, its influence is small and is often ignored or set to 0. , and These are the parameters of the BMH potential.

[0049] To investigate the effect of TiO2 substitution for CaF2 on the microstructure of CaO-Al2O3-based protective slag, the systems were designed as CaO-Al2O3-SiO2-CaF2 slag systems and CaO-Al2O3-SiO2-TiO2 slag systems. The potential parameters used in this application are empirical parameters, and the parameters involved in the slag systems... and The values ​​are shown in Table 2.

[0050] Table2.ParametersfortheBMHPotentials Atom Atom (J) (1 / Å) O O 2.399e-20 5.88 O Al 1.379e-21 6.06 O Ca 1.150e-20 6.06 O Si 1.006e-21 6.06 O Ti 4.225e-21 6.06 O F 1.709e-20 5.88 Ca Ca 5.274e-21 6.25 Ca Al 5.917e-22 6.25 Ca Si 4.275e-22 6.25 Ca Ti 1.723e-21 6.25 Ca F 7.939e-21 6.06 Al Al 6.639e-23 6.25 Al Si 4.797e-23 6.25 Al Ti 1.933e-22 6.25 Al F 8.575e-22 6.06 Si Si 3.394e-23 6.25 Si Ti 1.397e-22 6.25 Si F 6.945e-22 6.06 Ti Ti 5.628e-22 6.25 Ti F 2.603e-22 6.06 F F 1.169e-20 5.88 Since the BMH potential parameters treat the melt as a completely ionic solution during the simulation, the composition range of the simulation system should be selected within the completely molten state at the corresponding temperature. Molecular dynamics simulations were performed using the MaterialsExplorer program under the NVT ensemble, i.e., calculations were conducted under the condition that the particle number N, system volume V, and temperature T remained constant. The atomic motion equations were solved using the frog-leapfrog algorithm with a time step of 1 fs (10⁻¹⁰). -15 Data is saved every 10 steps. The total number of atoms in each sample is set to approximately 6000, and its density at 1673 K is calculated using an empirical formula proposed by Mills and Keene. The composition, number of atoms, cell density, and side length of each system are shown in Table 3.

[0051] Atoms in each sample were placed in the constructed unit cells with random initial configurations, the cell volume of which was determined by the number of atoms and the system density. The initial configurations were melted at 5000 K and relaxed for 10000 fs to eliminate the influence of the initial distribution and ensure a homogeneous melt state. Subsequently, the system was continuously cooled from 5000 K to the target temperature of 1673 K over 10000 fs. Finally, the melt underwent another 10000 fs equilibrium calculation at 1673 K to obtain stable structural data. Considering that the number of atoms in the actual system far exceeds the computational scale, periodic boundary conditions were applied in all directions of the simulation cell to construct an equivalent infinite system without boundaries, thereby improving the reliability of the calculation results.

[0052] Example Result Analysis: 1. Heat flux density analysis: The curves showing the change in heat flux density over time through different sample slag films at 1400℃ using a heat flux simulator are shown below. Figure 4 As shown.

[0053] The heat flux density curves of all four samples showed a pattern of rapid initial increase, gradual decrease, and eventual relative stabilization, indicating that the heat transfer behavior during slag film formation exhibits significant transient characteristics. The peak heat flux densities of samples A and B were 0.949 MW / m² and 0.982 MW / m², respectively, while those of samples C and D were 0.869 MW / m² and 0.917 MW / m², respectively. At this point, the solid slag film had not yet thickened, and the air gap had not yet stabilized; therefore, the peak values ​​mainly depended on the heat transfer capacity of the liquid melt.

[0054] The main differences between the two slag systems lie in the post-peak decay process and the steady-state heat flux density in the later stages. The heat flux densities of samples A and B at 45 s were 0.620 MW / m² and 0.668 MW / m², respectively, significantly higher than those of samples C and D (0.579 MW / m² and 0.539 MW / m²), indicating that the fluorine-free titanium-containing slag has stronger heat transfer control capabilities after slag film formation. Sample D, in particular, despite its high peak value, exhibited the most significant post-peak decay, demonstrating strong heat transfer capacity in the early stages followed by a rapid increase in thermal resistance in the later stages.

[0055] 2. The analysis of the evolution law of solid slag film specifically includes: 2-1. Slag film thickness analysis: Test results of solid slag film thickness at different times are as follows Figure 5 As shown in the figure, the slag film thickness of the four samples at different times all showed a monotonically increasing trend, indicating that within the experimental range, the solid slag film was always in a continuous growth process.

[0056] It is worth noting that although all four curves show an increase over time, their slopes are not constant. Overall, the thickness increases rapidly in the 20–40 s stage, while the increase slows down in the 60–80 s stage, indicating that the slag film growth rate gradually decreases over time. The initial stage of slag film formation exhibits strong growth driving force, but in the later stages, with the increase in film thickness, changes in temperature gradient, and increased thermal resistance, the slag film thickness increase trend tends to level off.

[0057] The comparison results of different samples show that the slag film thickness at each time point follows a consistent pattern, exhibiting the order D>C>A>B. This indicates that the slag film formed by titanium-containing fluorine-free slag is generally thicker than that of fluorine-containing titanium-free slag. In the fluorine-containing group, the slag film thickness of A is consistently higher than that of B, indicating that a higher CaF2 content is not conducive to slag film thickening. Studies have shown that with increasing CaF2 content, fluoride ions in the CaO-Al2O3-CaF2 slag system with high Al2O3 content gradually transform from a network-breaking effect to a certain network-forming effect, thereby slowing down the crystallization trend. In this slag system, when the CaF2 mass fraction increases from 5% to 10%, the slag film thickness increases from 1.93 cm to 2.75 cm (an increase of 0.82 cm) and from 1.72 cm to 2.46 cm (an increase of 0.74 cm) respectively within the time interval of 20–80 s. The results show that with increasing CaF2 content, the slag film thickening rate decreases and gradually flattens out. It should be noted that this pattern is closely related to the main crystal phase type and structural evolution path of the specific slag system. Therefore, in different protective slag systems, the final effect of increased fluorine content on slag film thickness still needs to be analyzed in conjunction with actual mineral phase results.

[0058] To analyze the mineral phase composition and crystal structure characteristics of the protective slag film, X-ray diffraction (XRD) was used to perform phase analysis on the slag film sample. Figure 6 The XRD patterns of samples A and B are shown, and their crystal phase types are basically the same.

[0059] It can be seen that the CaO-Al2O3-based slag system did not precipitate the gunmetal crystals commonly found in the traditional CaO-SiO2-CaF2 system. The main crystalline phases in the fluorine-containing slag film are Ca3B2O6 (3CaO·B2O3, PDF#99-000-3622) and BaAl2O4 (BaO·Al2O3, PDF#04-010-4310). This indicates that in the current system, the effect of F− on the slag film is not achieved by promoting gunmetal crystal precipitation, but rather by affecting the degree of polymerization of the melt structure, thereby affecting the crystallization ability. This point will be discussed in subsequent MD simulations.

[0060] Figure 7 The XRD diffraction results of the titanium-containing fluorine-free slag film are shown. Phase identification shows that the main crystalline phases in the slag film of sample C include Ca3B2O6, BaAl2O4 and CaTiO3 (CaO·TiO2, PDF#03-065-3287), while only the CaTiO3 crystalline phase was detected in the slag film of sample D.

[0061] As the Ti content increases, the crystallization pathway of the slag film gradually shifts from a multi-phase coexistence to a single crystalline system dominated by perovskite. Compared to sample C, the crystallization process of sample D is more concentrated, and a CaTiO3-based lattice framework is more easily formed at the interface with the copper probe, thereby improving the growth and maintenance of the crystalline layer. Because the CaTiO3-dominated precipitated mineral phase enables the slag film to complete crystalline layer growth more quickly during solidification, its crystallization ability is stronger, thus sample D ultimately forms a slag film thicker than C. Conversely, the coexistence of borates, aluminates, and perovskites in sample C indicates multiple competing crystallization pathways in its crystallization process, which is not conducive to the rapid establishment of a single stable crystalline layer; therefore, its slag film thickness is less than that of sample D.

[0062] The heat flux density results show that the titanium-containing fluorine-free slag exhibits a lower heat flux density in the later stages, while its corresponding slag film thickness is significantly greater. This indicates that the increased thermal resistance caused by the thicker slag film is one of the important reasons for its suppressed heat transfer performance in the later stages. However, slag film thickness is not the only controlling factor; further comprehensive analysis of its heat transfer behavior, incorporating surface roughness, porosity, and mineral phase evolution, is still needed.

[0063] 2-2. Surface roughness analysis: Figure 8 The image shows a pseudo-color view of the broad slag film obtained by scanning sample D using a laser confocal microscope. The four locations for measuring surface roughness of the slag are shown in the figure. Eight different locations on the broad slag film were selected, and their average value was used as the measured surface roughness value. The effective scanning field of view for each pseudo-color view is 5mm × 5mm. The color scale (Z-axis) on the right characterizes the relative height of the slag film surface, in μm. The warm and cool variations in the color spectrum establish a visual mapping of height.

[0064] The extracted pseudo-color topography images show that the surface of the central region of the slag film (B, C, F, G) is relatively smooth, while the edge and corner regions near the boundary (A, D, E, H) exhibit more dramatic topographic undulations, with local maximum peak heights exceeding 400 μm. This difference is mainly attributed to the different cooling rates. Compared to the smooth one-dimensional heat transfer at the probe center, the boundary regions experience intense two-dimensional or even three-dimensional heat dissipation, leading to a sharp increase in their local cooling rates. As Cho et al. pointed out, thermal contraction under intense cooling results in a high concentration of thermal stress, causing severe "shrinkage warping" of the solidified slag film at the geometric boundaries. These towering microscopic protrusions formed at the edges inevitably lead to the generation of uneven, wide air gaps between the slag film and the cold wall, thus profoundly affecting the local interfacial thermal resistance of the boundary region.

[0065] The contact state between the slag film and the copper wall directly affects the interfacial heat transfer efficiency. Therefore, the surface roughness of the solid slag film was measured, and the average value obtained from the scanning is shown below. Figure 9As shown.

[0066] The surface roughness of the slag film from different samples follows the order D>C>A>B, indicating that the initial film formed by titanium-containing fluorine-free slag is significantly rougher than that formed by fluorine-containing titanium-free slag. It should be noted that the surface roughness mainly forms during the initial solidification stage, rather than being directly caused by the continued growth of the slag film later. Since the surface roughness of the titanium-containing fluorine-free slag film is higher than that of the fluorine-containing titanium-free slag film, the titanium-containing fluorine-free protective slag should exhibit better performance in controlling heat flux density and preventing longitudinal cracks in high-titanium steel billets.

[0067] 2-3. Porosity Analysis: Apparent porosity is a key indicator characterizing the surface compactness of the protective slag film and its interfacial contact with the copper wall. To compare the differences in microscopic compactness of protective slag films with different compositions, the apparent porosity of each sample's slag film was tested and statistically analyzed. The results are as follows: Figure 10 As shown.

[0068] It can be seen that the apparent porosity of the four samples follows the order D>C>A>B, with corresponding values ​​of 1.85 vol%, 1.81 vol%, 1.78 vol%, and 1.63 vol%, respectively. This indicates significant differences in the open pore structure on the slag film surface among the different samples. Overall, the apparent porosity of C and D is higher than that of A and B, indicating that their surfaces are more prone to forming open pores and local voids, thereby reducing the actual contact area between the slag film and the copper plate and increasing the interfacial thermal resistance. Combined with the heat flux density results, it can be seen that samples with higher apparent porosity usually exhibit lower heat flux density in the later stages, indicating that interfacial air gaps are one of the important reasons for inhibiting heat transfer. At the same time, the apparent porosity results are basically consistent with the surface roughness results in terms of overall trend, indicating that the unevenness of the cold end interface of the slag film is not only related to surface undulations but also closely related to the open pore structure. When both surface roughness and apparent porosity increase simultaneously, the interfacial contact state further deteriorates, and the heat transfer capacity weakens accordingly.

[0069] Unlike surface roughness and apparent porosity, true porosity primarily reflects the density and thermal resistance changes within the slag film. The true porosity of slag films from different samples was measured and analyzed, and the results are as follows: Figure 11 As shown.

[0070] The true porosity of the four samples followed the order D>C>A>B, with corresponding values ​​of 5.32 vol%, 4.73 vol%, 4.58 vol%, and 3.82 vol%, respectively. This indicates that pores and air gaps are more easily formed inside the titanium-containing fluorine-free slag film, especially in sample D, which has the most developed pores. As the true porosity increases, the number of low-thermal-conductivity gas phase regions inside the slag film increases, the apparent density decreases, and the overall thermal conductivity weakens. The fluorine-containing titanium-free slag has a more dense structure, a continuous and complete heat transfer path, and higher thermal conductivity. In contrast, the volume shrinkage caused by crystal precipitation during the solidification process of the fluorine-free titanium-containing slag is more significant, easily forming a large number of closed pores and micro-defects inside, further increasing the heat transfer resistance, resulting in a weaker overall heat transfer capacity of the slag film. Apparent porosity mainly affects interfacial thermal resistance, while true porosity mainly affects the internal thermal conductivity of the slag film; both together determine the overall heat transfer capacity of the slag film.

[0071] 2-4. Apparent comprehensive thermal conductivity analysis: Figure 12 The figure shows the variation of the apparent comprehensive thermal conductivity of the slag film of different samples over time. It can be seen that the apparent comprehensive thermal conductivity of all four samples is within the range of... Within the range, but the trends of change are significantly different. Overall, A, C and D increase with time, while sample B remains basically stable after 40s.

[0072] In the initial stage of slag film solidification (20s), for fluorine-containing protective slag films, sample B exhibited the highest overall thermal conductivity, followed by sample A. This is mainly because B was almost entirely glassy, ​​with no crystals precipitating in the short term, resulting in weak phonon scattering and the highest apparent overall thermal conductivity. Sample A, however, showed a stronger heat flux density decay than B, making it easier to form a crystal lattice in the slag film during the initial stage. The volume shrinkage accompanying crystallization created microscopic air gaps within the slag film, leading to a less significant increase in its thermal conductivity. Although samples A and C had similar heat flux density decay capabilities, A had lower interfacial thermal resistance and lower internal thermal resistance within the slag film, ultimately resulting in a slightly higher apparent overall thermal conductivity for A compared to C. In the titanium-containing group, samples C and D both showed an initial decrease followed by an increase, but C was higher than D at all times, reaching its highest value at 80s. Although the precipitation of CaTiO3 in D is more concentrated, its slag film is thicker, rougher, and has more air gaps, resulting in greater interfacial and internal thermal resistance, ultimately leading to the lowest apparent overall thermal conductivity. While the crystalline layer has high thermal conductivity, the increased gaps between crystals increase radiative thermal resistance, thus reducing its overall macroscopic thermal conductivity and improving heat transfer control.

[0073] Therefore, the apparent overall thermal conductivity of the slag film is determined by crystallization behavior, slag film thickness, interface morphology, and pore structure, and no single factor can completely determine the overall heat transfer capacity. In the early stage of slag film formation, strong crystallization ability is beneficial to improving the apparent overall thermal conductivity of the slag film, while greater thickness, higher roughness, and porosity have a more profound impact on weakening heat transfer performance.

[0074] 3. Molecular dynamics simulation: The melt structure of CaO-Al2O3-based slag systems with different CaF2 and TiO2 contents was simulated using Scigress software. Figure 13 The figure shows the atomic configuration obtained after simulation of a typical slag sample. The coordination environment and Q of the protective slag melt structure are analyzed. i The distribution of structural units characterizes the degree of polymerization of the slag, reflecting the structural connectivity, ion migration ability, and crystallization tendency of the melt. These microstructural features collectively determine the heat transfer behavior during solidification. Since each system contains approximately 6000 atoms, it is difficult to directly analyze the structural properties of the melt based on atomic configuration; mathematical and statistical analysis is required.

[0075] 3-1. Coordination Number (CNs) Analysis: Integrating the radial distribution function (RDF) curves yields the coordination information between each atom pair. Figure 14 The curves show the coordination number distribution functions of Al-O, Ca-O, Si-O, and Ti-O atomic pairs in the four samples.

[0076] It can be seen that within a certain range, the average coordination number remains constant, meaning there is a plateau on the CNs curve, which also reflects the short-range ordering characteristic of the melt structure. The wider and gentler this plateau, the more stable the structural unit formed by this coordination. It can be seen that the first plateau of the Al-O curve appears near 4, indicating that it is mainly composed of [missing information - likely a specific type of coordination unit]. It exists in tetrahedral form. With decreasing CaF2 and increasing TiO2, the plateau of the CNs curve narrows, and the upward slope appears earlier and steeper. In the aluminate network, Al... 3+ The formation of a tetrahedron requires the consumption of metal cations (such as Ca) in the system. 2+ Charge compensation is performed by introducing Ti into [TiO2]. x The formation of polyhedra intensifies the competition between free oxygen ions and charge-compensating cations in the system, forcing some Al to transform to higher coordination states (such as 5-coordinate or 6-coordinate), which is reflected in the curve as a narrowing of the plateau and an earlier rise.

[0077] The CNs curves of Ca-O, across all compositions, exhibit a continuous, steep rise without a distinct plateau, indicating that the Ca-O bond exhibits purely ionic characteristics and lacks a stable structure. Ca consistently acts as an active network modifier, working with O atoms to increase the likelihood of disrupting the network structure within the system. In the Si-O CNs curves, all samples show a broad and horizontal first plateau near the 4-axis, indicating that Si atoms and O atoms form a highly stable bond. With decreasing F and increasing Ti, Si-O exhibits a tendency to transform into a more complex structure, exhibiting a tetrahedral structure. In the CNs curve, the ordinate value of the first plateau is about 5. As the TiO2 content increases, the plateau becomes narrower and the upward slope increases, indicating that not only are more Ti-O structural units formed in the sample, but the network structure also tends to become more complex. This trend is conducive to the formation of Ti-related local enrichment and provides a structural basis for the subsequent precipitation of CaTiO3.

[0078] To reveal the regulatory mechanism of fluoride ions on the micro-coordination environment and network structure of molten slag, the coordination number distribution functions of Al-F, Ca-F, and Si-F atom pairs in the fluorine-containing system were calculated. The results are as follows: Figure 15 As shown.

[0079] It can be seen that with the increase of fluorine, the coordination number of Ca-F is the highest and increases the most significantly, indicating that in the melt, F- preferentially interacts with the network modifier Ca. 2+ Coordination occurs, forming free ionic clusters. The values ​​of both Al-F and Si-F atom pairs increase, with Al-F showing a higher value than Si-F, indicating that fluoride ions actively participate in coordination with aluminum ions. As the fluorine content increases, Al-O bonds are replaced by Al-F bonds, promoting the formation of [AlO3F]. 4- The formation of polyhedral structural units.

[0080] To further analyze the effects of changes in CaF2 and TiO2 content on Al-O, Ti-O, and Al-F coordination, the coordination number distribution was statistically analyzed to obtain the actual coordination situation in the system. The results are as follows: Figure 16 As shown.

[0081] It can be seen that Al in the four samples IV Al has always accounted for the vast majority. III And Al V Secondly, Al VI The smallest proportion indicates that Al mainly exists in a four-coordinate structure in this system. As the CaF2 content increases, the proportion of Al in system B increases. IV The proportion decreased while Al III Significant increase, and free F -The proportion decreased and F Ⅰ The proportion increased, and F Ⅱ There was also a slight increase, indicating that the increase in fluoride ions replaced oxygen, forming more Al-F-Al structures, which bonded with aluminum to form [AlO3F] in the CaO-Al2O3-based slag system. 4- The tetrahedral structure, connected to the silicon-oxygen tetrahedra to form a network, weakens ion migration. The network-forming effect of fluorine weakens the crystallization ability of the protective slag, while in sample A, Al constitutes a relatively large proportion. V And Al VI The external body, which is connected by ionic bonds, exists in the gaps of the network. This is not conducive to the formation of the network structure, resulting in low resistance to ion migration and enhanced crystallization performance. This is why sample A has a stronger crystallization ability than sample B.

[0082] It is worth noting that, comparing the fluorine-containing group (samples A and B, with increasing F content) and the fluorine-free group (samples C and D, with increasing Ti content), the Al content in the fluorine-free group... Ⅲ The proportion is significantly lower, and AI V With Al Ⅵ The proportion of [specific component] increases with increasing TiO2 content. For example... Figure 17 As shown, the coordination of Ti atoms in the melt is mainly due to Ti Ⅳ Ti V and Ti Ⅵ Composition, in which Ti V It accounts for the largest proportion. As the TiO2 content increases, Ti... Ⅳ The proportion increased while Ti Ⅵ The proportions show the opposite trend, indicating that the proportion of [TiO6] octahedra in the system has decreased while the proportion of [TiO4] tetrahedra has increased, and the proportions of [TiO4] tetrahedra, [SiO4] tetrahedra, and [AlO4] tetrahedra are also increasing. - Tetrahedra have the same network building ability and can connect with surrounding Si-O or Al-O tetrahedra through bridging oxygen to form Ti-O-Si or Ti-O-Al bridging bonds. They are directly integrated into the three-dimensional network framework of the slag, which increases the degree of polymerization of the system. This indicates that increasing the content of CaF2 and TiO2 can make the melt structure more complex.

[0083] 3-2.Q i Distribution analysis: To further investigate the influence of the degree of melt polymerization of CaF2 and TiO2, Q was analyzed. i The distribution of structural units, where i represents the number of bridging oxygen (BO) atoms connected to the central Al atom, such as... Figure 17 As shown.

[0084] For the fluorine-containing group (samples A and B, with increasing F content) and Q0 To Q 3 The proportion decreased, Q 4 and Q 5 The increased proportion of fluoride ions indicates that the increased fluoride ion content polymerized the Al-O structure, which is consistent with FAN's findings. For the fluoride-free group (samples C and D), Q increased with increasing Ti content. 0 Q 1 Q 2 The proportion of Q is decreasing. 3 Q 4 Q 5 The distributions show opposite trends, indicating a tendency for simple structural units to transform into complex structural units, with an increasing degree of polymerization in the melt. The degree of micro-polymerization in the melt directly affects the phonon transport efficiency; the higher the degree of polymerization, the stronger the heat transfer capacity of the liquid slag. This explains why, on the heat flux density curve, the peak heat flux density is B>A>D>C. The degree of polymerization in the melt also affects ion migration; the higher the degree of polymerization, the greater the resistance to ion migration in the liquid slag. This also explains why the slag film growth rate of sample B is weaker than that of sample A.

[0085] A method for controlling the heat transfer characteristics of slag film in a fluorine-free continuous casting protective slag for high-titanium steel includes the following steps: S1: The basicity of the protective slag, CaO / Al2O3, is controlled between 1.00 and 1.15, and the mass fraction of TiO2 is set to 8% to 10%, while the mass fraction of SiO2 is limited to 3% to 5%. This serves as the basic composition framework, so that perovskite CaTiO3 becomes the dominant precipitated crystalline phase during the solidification process of the slag, replacing the multiphase competitive precipitation pathways of borate and aluminate in the fluorine-containing slag system. This establishes a crystallization heat transfer control basis with a single crystalline phase as the core.

[0086] S2: By adjusting the mass fractions of BaO, Na2O, and B2O3 to within the ranges of 10%–12%, 8%–10%, and 8%–11%, respectively, the polymerization degree and ion migration ability of the slag are controlled, enabling the liquid slag to quickly form an initial solidified shell after contacting the water-cooled copper probe, and to complete the initial growth of the slag film thickness within a time window of 20s–40s. The peak heat flux density is controlled between 0.85 MW / m² and 0.92 MW / m² to avoid excessively high initial heat transfer shock.

[0087] S3: After the slag film growth enters the steady-state stage of 40s to 80s, the perovskite crystal layer gradually thickens due to the increased TiO2 content, so that the solid slag film thickness reaches 2.8cm to 3.0cm at 80s. At the same time, by controlling the cooling intensity, the surface roughness Sa of the slag film in contact with the copper wall is stabilized in the range of 18μm to 20μm, the apparent porosity is maintained at 1.8vol% to 2.0vol%, and the true porosity is maintained at 5.0% to 5.5%, thereby increasing the interfacial contact thermal resistance and the internal radiation thermal resistance of the slag film.

[0088] S4: Molecular dynamics simulations were used to pre-obtain the coordination number distribution of Al-O, Ti-O, and Si-O atom pairs and the Al-O tetrahedron under the target composition. Structural unit ratio, when Q³, Q 4 Q 5 When the total proportion of highly polymerized structural units exceeds 40%, the high-temperature liquid slag corresponding to this composition is determined to have high phonon transport efficiency, ensuring a peak heat flux density of not less than 0.85 MW / m² to meet initial lubrication requirements; simultaneously, based on simulation results... Tetrahedron proportion and The relative changing trend of the octahedral proportion can be used to predict the precipitation tendency of perovskite and serve as a structural basis for fine-tuning the composition.

[0089] S5: When the measured steady-state heat flux density deviates from the target range of 0.52 MW / m² to 0.56 MW / m², adjust the TiO2 content by increasing or decreasing it by 0.5% to 1.0% within the range of 8% to 10%, and correspondingly adjust the CaO content to maintain constant alkalinity. This will change the amount of perovskite crystals, thereby altering the porosity and roughness of the slag film, until the heat flux density returns to the target range. If the heat flux density is too low, appropriately reduce the TiO2 content to reduce the slag film thickness and porosity. If it is too high, increase the TiO2 content to enhance the inhibitory effect of the crystalline layer on heat transfer.

[0090] S6: After each composition adjustment, the slag film thickness and true porosity are re-measured, and the steady-state heat flux density at 80s is used as the final evaluation index. When the heat flux density at that time is stable at 0.52 MW / m²~0.56 MW / m², the slag film thickness reaches more than 2.8cm, and the true porosity is higher than 5.0%, it is determined that the heat transfer characteristics of the slag system have reached the target state, and the composition scheme can be put into practical application as the preferred formula under this continuous casting condition.

[0091] Data Analysis: Using fluorine-containing and fluorine-free high-titanium steel protective slags as the research object, and combining heat flux density testing, slag film structure characterization, and molecular dynamics simulation, the influence of compositional changes on slag film evolution and heat transfer mechanism was systematically analyzed. The conclusions can be summarized as follows: (1) When the mass fraction of CaF2 increases from 5% to 10%, the maximum heat flux density of the protective slag increases from 0.949 MW·m -2 Increased to 0.982 MW·m -2 The steady-state heat flux density is 0.620 MW·m -2 Increased to 0.668 MW·m -2 When the TiO2 mass fraction increased from 4% to 8%, the maximum heat flux density increased from 0.869 MW·m -2 Increased to 0.917 MW·m -2 The steady-state heat flux density is 0.579 MW·m -2 Reduced to 0.539 MW·m -2 This indicates that the initial heat transfer capacity of fluorine-containing slag is stronger than that of titanium-containing slag. The heat flux decay of the non-fluorine titanium-containing slag after the peak is more significant, and the steady-state heat flux density is lower, indicating that this type of slag system has a stronger heat transfer control capability in the later stage of solidification.

[0092] (2) The slag film thickness of different slag systems showed a consistent increasing trend over time, but the rate of increase differed. The overall thickness order was: D>C>A>B. Taking 20 s, 40 s, 60 s, and 80 s as time nodes, the slag film thickness of titanium-containing slag was higher than that of fluorine-containing slag. The highest thickness of sample D was 3.03 cm, while the slag film thickness of sample A was more significant, increasing from 1.93 cm at 20 s to 2.75 cm at 80 s, an increase of 0.82 cm. In terms of crystalline mineral phases, with the increase of TiO2 content, the crystallization path of the slag film gradually changed from the multiphase competitive precipitation of borate (Ca3B2O6) and aluminate (BaAl2O4) to a single crystalline phase dominated by perovskite (CaTiO3). The addition of TiO2 enhanced the heat transfer control capability of the protective slag in the later stage of solidification.

[0093] (3) The surface roughness of the fluorine-free titanium-containing protective slag can reach 19.62 μm, which is significantly higher than the 14.32 μm of the 10% CaF2 sample. At the same time, its apparent porosity increases from 1.63 vol% to 1.85 vol%, and its true porosity also increases from 3.82 vol% to 5.32 vol%. The increase in surface roughness and apparent porosity increases the interfacial thermal resistance, while the increase in true porosity indicates that the slag film develops more low thermal conductivity air gaps, resulting in its stronger heat transfer control ability than that of the fluorine-containing protective slag.

[0094] (4) As the slag film grows, the apparent comprehensive thermal conductivity of all samples shows an increasing trend, and is in a state of... Within the range, the solid slag films of samples A and C exhibited similar heat transfer capabilities after 60s of solidification, while the overall thermal conductivity of sample D remained relatively low. This indicates that TiO2 replacing CaF2 resulted in a lower apparent overall thermal conductivity of the protective slag film and enhanced heat transfer control.

[0095] (5) Molecular dynamics simulation results show that in CaO-Al2O3-CaF2 based and CaO-Al2O3-TiO2 based slag systems, the CNs values ​​of Al-O, Ca-O, Si-O, and Ti-O all increase with the increase of CaF2 and TiO2 content. The increase of F content leads to an increase in Al... Ⅳ The proportion decreased while Al Ⅲ The increase is significant, and more Al-F-Al structures are formed, with F bonding with Al to form [AlO3F]. 4- This promotes phonon transport. With increasing TiO2 content, the proportion of [TiO6] octahedra decreases while the proportion of [TiO4] tetrahedra increases, thus improving the Q of Al-O. 0 Q 1 Q 2 The number of simple structural units decreases while the number of complex structural units increases, resulting in an increased phonon transport capacity in the liquid slag, manifested as a higher peak heat flux density in sample D compared to sample C.

[0096] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the term "comprising" or any other variations thereof is intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.

[0097] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A fluorine-free continuous casting protective slag for high-titanium steel, characterized in that: include: CaO: 28%–30%, Al2O 3: 26%~28%, TiO 2: 8%~10%, SiO 2: 3%–5%, BaO: 10%–12%, Na2O: 8%–10%, B2O 3: 8%–11%.

2. The method for preparing a fluorine-free continuous casting protective slag for high-titanium steel according to claim 1, characterized in that: The method includes the following steps: S1: Weigh the chemically pure raw materials according to the mass percentage, put the weighed raw materials into a high-performance ball mill, and mix and stir at a speed of 300-400 r / min for 30-45 min to obtain a uniformly mixed powder; S2: Load the mixed powder into a high-purity graphite crucible, place it in an induction furnace, heat it to 1400-1450℃ at a heating rate of 5-8℃ / min, hold it for 20-30min, and stir it with a molybdenum rod every 5min during the holding period. Each stirring lasts for 30-60s to homogenize the melt composition. S3: Quickly pour the completely molten liquid protective slag into deionized water at 25°C for water quenching and rapid cooling to obtain transparent or translucent glassy slag blocks. S4: Place the glassy slag block obtained by water quenching into an oven and dry it at 105-110℃ for 12-24 hours. Then use a jaw crusher to crush the dried slag block into particles with a particle size of less than 5mm. S5: Place the crushed granules in a planetary ball mill and grind for 20-30 minutes. Pass the granules through a 200-mesh standard sieve and take the sieve-passing material and seal it in a sealed container to obtain the finished product of high-titanium steel fluorine-free continuous casting protective slag.

3. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: In step S1, the amount of Na2CO3 weighed needs to be converted based on the target mass fraction of Na2O of 8% to 10%, and the conversion factor is the molecular weight ratio of Na2CO3 to Na2O of 1.

71. All the weighed raw materials are loaded into the grinding jar of a high-performance ball mill. The ball mill speed is set to 300 r / min to 400 r / min, and the mixture is continuously stirred for 30 min to 45 min until the powder of each component reaches a uniform dispersion state at the microscale.

4. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: In step S2, the uniformly mixed powder is transferred into a high-purity graphite crucible, with the powder filling amount controlled to about 2 / 3 of the crucible volume to prevent overflow during heating expansion. The graphite crucible containing the powder is placed in the center of the heating coil of the induction furnace. After closing the furnace door, the heating program is started, with the heating rate set to 5℃ / min~8℃ / min, so that the furnace temperature gradually increases from room temperature to the target melting temperature of 1400℃~1450℃. After reaching the target temperature, the holding stage is entered, and the holding time is maintained for 20min~30min to ensure that the powder is fully melted at this temperature and forms a uniform liquid phase.

5. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: In step S3, the graphite crucible containing the fully melted protective slag is quickly removed from the induction furnace and aligned with a stainless steel container containing sufficient deionized water. The liquid slag is then poured into the room-temperature deionized water in a thin, uniform stream for rapid cooling.

6. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: In step S4, the glassy slag block obtained by water quenching is evenly spread out in a tray and placed in a forced-air drying oven to be continuously dried at a temperature of 105℃~110℃ for 12h~24h to completely remove the moisture that adhered to and absorbed during the water quenching process.

7. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: In step S5, the crushed and sieved slag particles with a particle size of less than 5 mm are fed into a planetary ball mill for fine grinding. The ball mill speed is set to 200 r / min to 300 r / min, and the grinding time is 20 min to 30 min. The grinding jar and grinding balls are made of zirconium oxide or corundum.

8. The method for controlling the heat transfer characteristics of a fluorine-free continuous casting protective slag for high-titanium steel and its slag film according to claim 1, characterized in that: Includes the following steps: S1: The basicity of the protective slag, CaO / Al2O3, is controlled between 1.00 and 1.15, and the mass fraction of TiO2 is set to 8% to 10%, while the mass fraction of SiO2 is limited to 3% to 5%. This serves as the basic composition framework, so that perovskite CaTiO3 becomes the dominant precipitated crystalline phase during the solidification process of the slag, replacing the multiphase competitive precipitation pathways of borates and aluminates in the fluorine-containing slag system. This establishes a crystallization heat transfer control basis with a single crystalline phase as the core. S2: By adjusting the mass fractions of BaO, Na2O, and B2O3 to within the ranges of 10%–12%, 8%–10%, and 8%–11%, respectively, the polymerization degree and ion migration ability of the slag are controlled, enabling the liquid slag to quickly form an initial solidified shell after contacting the water-cooled copper probe, and to complete the initial growth of the slag film thickness within a time window of 20s–40s, thereby controlling the peak heat flux density between 0.85MW / m and 0.92 MW / m to avoid excessively high initial heat transfer shock. S3: After the slag film growth enters the steady-state stage of 40s to 80s, the perovskite crystal layer gradually thickens due to the increased TiO2 content, so that the solid slag film thickness reaches 2.8cm to 3.0cm at 80s. At the same time, by controlling the cooling intensity, the surface roughness Sa of the slag film in contact with the copper wall is stabilized in the range of 18m to 20m, the apparent porosity is maintained at 1.8vol% to 2.0vol%, and the true porosity is maintained at 5.0% to 5.5%, thereby increasing the interfacial contact thermal resistance and the internal radiation thermal resistance of the slag film. S4: Molecular dynamics simulations were used to pre-obtain the coordination number distribution of Al-O, Ti-O, and Si-O atom pairs and the Al-O tetrahedron under the target composition. Structural unit ratio, when Q, Q 4 , When the total proportion of highly polymerized structural units exceeds 40%, the high-temperature liquid slag corresponding to this composition is deemed to have high phonon transport efficiency, ensuring a peak heat flux density of not less than 0.85 MW / m to meet initial lubrication requirements; simultaneously, based on simulation results... Tetrahedron proportion and The relative changing trend of the octahedral proportion can be used to predict the precipitation tendency of perovskite and serve as a structural basis for fine-tuning the composition. S5: When the measured steady-state heat flux density deviates from the target range of 0.52 MW / m to 0.56 MW / m, the TiO2 content is increased or decreased by 0.5% to 1.0% within the range of 8% to 10%, and the CaO content is adjusted accordingly to maintain constant alkalinity. This changes the amount of perovskite crystals, thereby altering the porosity and roughness of the slag film, until the heat flux density returns to the target range. If the heat flux density is too low, the TiO2 content should be appropriately reduced to decrease the slag film thickness and porosity; if it is too high, the TiO2 content should be increased to enhance the inhibitory effect of the crystalline layer on heat transfer. S6: After each composition adjustment, the slag film thickness and true porosity are re-measured, and the steady-state heat flux density at 80s is used as the final evaluation index. When the heat flux density at that time is stable at 0.52 MW / m to 0.56 MW / m, the slag film thickness reaches more than 2.8cm, and the true porosity is higher than 5.0%, it is determined that the heat transfer characteristics of the slag system have reached the target state, and the composition scheme can be put into practical application as the preferred formula under the continuous casting condition.