Methods and applications for preparing high-strength, conductive carbide ceramic-metal interpenetrating phase composites using centrifugal melting and infiltration under high gravity.
By rapidly introducing molten metal into carbide porous ceramic preforms using centrifugal melting and infiltration technology under high gravity, the problems of long melting and infiltration time and difficulty in achieving synergistic performance in traditional methods have been solved. This has enabled the preparation of high-strength, high-conductivity and high-density carbide ceramic-metal interpenetrating phase composite materials with excellent dynamic and static load-bearing properties.
Patent Information
- Application Number
- CN202611035994.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-10
Smart Images

Figure CN123060086A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite materials technology, and more specifically, to a method and application for preparing high-strength, conductive carbide ceramic-metal interpenetrating phase composite materials using centrifugal melting and infiltration under high gravity. In particular, it relates to a method, material, and application of ceramic (such as chromium carbide)-based metal (such as copper) interpenetrating phase composite materials with high strength, high conductivity, high density, and high strain rate strengthening response by using high-speed centrifugation to generate high gravity to drive molten metal to rapidly enter the micron-level interconnected channels of a porous carbide ceramic preform. Background Technology
[0002] Tungsten-copper (WCu) composites combine the high melting point, high hardness, and arc erosion resistance of tungsten with the high electrical and thermal conductivity of copper, making them suitable for high-voltage electrical contacts, arc switches, thermal management components, and conductive wear-resistant structural parts. However, traditional tungsten-copper systems typically exhibit a trade-off between increased hardness and decreased electrical conductivity due to higher tungsten content. Furthermore, tungsten resources are subject to significant price fluctuations, have high density, and are difficult to process and sinter.
[0003] Chromium carbide possesses low density, high hardness, and good oxidation resistance and wear resistance. Constructing an interpenetrating phase composite material with a chromium carbide-based porous ceramic framework and a copper phase promises to achieve a comprehensive balance of electrical conductivity, wear resistance, arc erosion resistance, and load-bearing capacity while reducing tungsten content and material density. Furthermore, introducing tungsten into the chromium carbide framework allows for the control of pore connectivity, framework tortuosity, and crack propagation paths through tungsten solid solution, tungsten-enriched carbide microregions, or a network of tungsten-containing phases.
[0004] Interpenetrating phase composites refer to composite materials in which both the ceramic and metallic phases form a three-dimensional continuous network and interpenetrate each other in space. Compared with particle or short fiber reinforced composites, these materials can simultaneously obtain the hardness, wear resistance, and load-bearing capacity of the ceramic skeleton and the electrical conductivity, thermal conductivity, and toughness of the metallic phase, which is beneficial for achieving a synergistic improvement in strength, hardness, electrical conductivity, and damage tolerance.
[0005] Existing preparation methods for chromium carbide or copper chromium carbide composites mostly focus on the porous ceramic framework itself or rely on long-term pressureless melting infiltration routes that improve interfacial wetting. Porous chromium carbide preparation technologies primarily address the problem of ceramic bulk formation and do not involve the rapid filling of molten metal into micron-sized interconnected channels. While electroless copper plating or copper electroplating modification routes can improve Cr3C2-Cu interfacial wetting, they require additional electroplating steps and longer melting infiltration times. For micron-sized porous preforms containing tungsten-chromium carbide, the driving force provided by ordinary gravity and capillary action is limited, making it difficult to simultaneously achieve rapid melting infiltration, interpenetrating structural integrity, high electrical conductivity, and high Brinell hardness.
[0006] The applicant's initial technical solution focused on obtaining a porous chromium tungsten carbide preform and achieving pressureless copper infiltration through capillary action. CN201410645772 discloses a method of first chemically electroplating copper onto the surface of open-pore Cr3C2 porous ceramics, and then conventionally infiltrating at 1100–1250℃ for about 5 hours to prepare a Cr3C2-Cu three-dimensional continuous network material; this route relies on electroplating modification and long-term pressureless infiltration. CN103074534A discloses a method for preparing metal ceramics by in-situ generation of metal melt using aluminothermic reaction and infiltration into a porous ceramic blank in a hypergravity field. The core step is to prepare an aluminothermic reactant by mixing Al powder with metal oxides such as NiO, Fe2O3, Cr2O3, CrO3, MoO3, or WO3 and pressing it into a blank with a porosity of 45%–65%, which is then placed on top of the porous ceramic blank and an aluminothermic combustion reaction is initiated in a hypergravity field; after the reaction is completed, the product naturally separates into an upper layer of alumina and a lower layer of metal ceramics. This method uses Al powder / metal oxide aluminothermic reactant to initiate self-propagating aluminothermic combustion in a hypergravity field, which includes a step of removing the upper layer of alumina after the reaction. Furthermore, pressureless melting of aluminum and aluminum alloy melts easily forms a stable oxide film on their surface, and there is entry resistance in the ceramic preform channels caused by non-ideal wetting angles. Summary of the Invention
[0007] To address the problems of insufficient driving force, long infiltration time, strong dependence on chemical plating / electroplating metallization modification, difficulty in synergizing hardness and conductivity, and lack of high strain rate dynamic load-bearing capacity in existing pressureless melting infiltration methods, this invention aims to provide a method for preparing high-strength, conductive carbide ceramic-metal interpenetrating phase composite materials using centrifugal melting infiltration under hypergravity. The hypergravity field provides an external force far exceeding that of ordinary gravity, enabling the molten metal to overcome resistance from oxide films, wettability, and micron-sized pores, rapidly entering the interconnected pores of the ceramic and forming a continuous metallic phase. After cooling, a three-dimensional interpenetrating composite material of ceramic and metallic phases is obtained, solving the problem of the difficulty of traditionally non-wetting metals infiltrating into the micron-sized pores of carbide ceramics. This invention also aims to provide a carbide ceramic-metal interpenetrating phase composite material with high conductivity, hardness, density, and impact / compression load-bearing capacity, and its applications.
[0008] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing a carbide ceramic-metal interpenetrating phase composite material, comprising the following steps:
[0009] S1. Obtain a carbide porous ceramic preform with a three-dimensional continuous open-pore structure; the carbide porous ceramic preform can maintain a continuous ceramic skeleton structure at the subsequent metal infiltration temperature;
[0010] S2. The carbide porous ceramic preform, metal source, high-temperature resistant press block, and oxygen barrier layer are sequentially loaded into a metal melt crucible and sealed to obtain a crucible for melting and infiltration. Preferably, the loading is performed without chemical plating, electroplating, vapor deposition, or continuous metallization coating of the carbide porous ceramic preform. Alternatively, when it is necessary to improve the interface state of a specific metal system, the carbide porous ceramic preform is subjected to discontinuous surface activation treatment, but the discontinuous surface activation treatment does not replace the hypergravity field as the driving force for melting and infiltration.
[0011] S3. Balance the mass and center of gravity of the crucible to be melted and infiltrated and the balancing crucible; preferably, the balancing is to take another balancing crucible and load it with counterweight particles, so that the total mass of the balancing crucible and the crucible to be melted and infiltrated is the same or within the balancing error range allowed by the centrifugal device, and the centers of gravity on both sides of the rotor are consistent or substantially consistent; when the metal source is copper or copper alloy, the counterweight particles are copper particles; when the metal source is aluminum or aluminum alloy, the counterweight particles are aluminum particles; the diameter of the counterweight particles is 0.5 to 2 mm, preferably about 1 mm.
[0012] S4. Place the crucible to be melted in a heating furnace at a preset temperature and keep it in an inert atmosphere, reducing atmosphere, vacuum environment or a local low oxygen environment formed by the oxygen barrier layer to keep the metal source in a molten state.
[0013] S5. While the metal source remains in a molten state, the crucible to be melted is quickly installed into a centrifugal device under high gravity. Centrifugation is performed at a centrifugal acceleration of 750–1500 g0 for 1–10 min, allowing the molten metal to enter the interconnected pores of the carbide porous ceramic preform under the action of the high gravity field and form a continuous metal phase. Here, g0 is the standard gravitational acceleration. After centrifugation, the material is cooled to obtain a carbide ceramic-metal interpenetrating phase composite material composed of a continuous carbide ceramic framework phase and a continuous metal phase.
[0014] In a preferred embodiment, the carbide porous ceramic preform is a single-phase carbide ceramic preform or a multiphase carbide ceramic preform; the open porosity of the carbide porous ceramic preform is 40–75%, the average pore size is 0.2–50 μm, and the skeleton ligament thickness is 0.2–20 μm. Preferably, the open porosity is 50–65%, the average pore size is 0.5–5.0 μm, and the skeleton ligament thickness is 0.5–2.0 μm.
[0015] Furthermore, the carbide porous ceramic preform is a chromium carbide-based porous ceramic preform. For example, the main ceramic phases of the chromium carbide-based porous ceramic preform include Cr3C2, Cr7C3, and Cr... 23C6. Tungsten-containing chromium carbide-copper system or combination thereof. For the tungsten-containing chromium carbide-copper system, the amount of W added is preferably 10 to 50 wt.% of the chromium oxide raw material, and typical samples are denoted as (CrW10)C, (CrW25)C and (CrW50)C.
[0016] The preparation method of the carbide porous ceramic preform has no major impact on the implementation of the technical solution of this application. It can be prepared by one or more of the following methods: carbothermal reduction, gas-phase carbothermal reduction, reaction sintering, template method, pore-forming agent method, ice template method, cryogenic casting, foam replication method, gel casting method, slurry foaming method, or additive manufacturing method. In a preferred embodiment, the gas-phase carbothermal reduction stage uses a mixed atmosphere of CH4, H2, and Ar, with a typical flow rate of CH4:H2:Ar=40:180:180 sccm, and is treated at about 1150℃ for 12-20 h to achieve chromium oxide reduction and carbonization and form a three-dimensional continuous porous framework. Subsequently, wet H2 decarburization / wet hydrogen reduction, vacuum heat treatment, chemical cleaning, plasma treatment, or electrochemical surface activation can be performed to remove free carbon on the pore and framework surface and improve the subsequent melting and infiltration interface state.
[0017] In a preferred embodiment, the carbide porous ceramic preform undergoes a pretreatment before being loaded into the molten metal crucible to remove pore residues, reduce oxide film, or improve the pore interface state. This pretreatment does not serve as a source of melting infiltration driving force and may include one or more of the following processes: drying, debinding, pre-sintering, decarburization, reduction treatment, vacuum heat treatment, surface cleaning, chemical cleaning, plasma treatment, or electrochemical surface activation.
[0018] In a preferred embodiment, the metal source is one or more of copper, copper alloy, aluminum, or aluminum alloy; preferably, the metal source is one or more of electrolytic copper block, oxygen-free copper block, copper sheet, copper wire, copper granules, copper powder compact, AlSi10 alloy block, aluminum granules, or aluminum alloy block. The molten metal-resistant crucible prevents molten metal leakage under hypergravity melting conditions and reduces molten metal contamination and crucible reaction risks; the oxygen barrier layer is one of graphite paper, graphite sheet, carbon paper, or carbon felt, preferably graphite paper, used to construct a local low-oxygen isolation environment to reduce oxidation of the metal source and the preform; the high-temperature resistant press maintains the relative position of the metal source and the carbide porous ceramic preform during crucible heating, transfer, and centrifugation, and promotes the molten metal to penetrate into the carbide porous ceramic preform along the hypergravity driving direction.
[0019] Furthermore, the molten metal-resistant crucible is a boron nitride crucible; the boron nitride crucible has high-temperature resistance and leak-proof properties, and is used to prevent molten metal leakage during the melting process under 1000-1250 g / L high-gravity melting conditions; preferably, when the metal source is copper or a copper alloy, the boron nitride crucible is used to prevent copper leakage during the melting process. The high-temperature resistant briquette is a W briquette, Mo briquette, graphite briquette, alumina briquette, or other briquette that remains solid at the melting temperature of the metal source.
[0020] In step S4, the heating furnace can be one of a pit furnace, box furnace, tube furnace, vacuum furnace, or atmosphere furnace; when the metal source is copper or copper alloy, the heating temperature is 1200-1350℃, preferably 1300℃; when the metal source is aluminum or aluminum alloy, the heating temperature is 850-950℃, preferably about 900℃; the holding time is 10-60 min, preferably 30 min.
[0021] In a preferred embodiment, in step S5, the heat-insulated crucible to be melted is quickly transferred to a movable titanium alloy centrifugal sleeve and immediately installed in the centrifugal device. The movable titanium alloy centrifugal sleeve is initially vertical; after centrifugal start-up and acceleration with the rotor, it rotates approximately 90° tangentially to a horizontal position under centrifugal force, causing the crucible to change from a vertical to a horizontal position and completing the rapid centrifugal melting process. The centrifugal acceleration is 1000–1250 g₀, and the centrifugal melting time is 3–8 min; preferably, the centrifugal acceleration is 1250 g₀, and the centrifugal melting time is 5 min. The cooling method can be one of natural cooling in air, inert atmosphere cooling, reducing atmosphere cooling, furnace cooling, or forced air cooling.
[0022] Secondly, the present invention provides a carbide ceramic-metal interpenetrating phase composite material prepared by the above-described preparation method. The composite material comprises a three-dimensional continuous carbide ceramic framework phase and a continuous metal phase filling the interconnected pores of the carbide ceramic framework, wherein the carbide ceramic framework phase and the continuous metal phase form an interpenetrating phase structure. Preferably, the carbide ceramic framework phase is chromium carbide or other carbide ceramic framework phases, and the continuous metal phase is a copper phase, a copper alloy phase, an aluminum phase, or an aluminum alloy phase.
[0023] Furthermore, when the continuous metallic phase is a copper phase or a copper alloy phase, the electrical conductivity EC of the composite material is not less than 35% IACS, the Brinell hardness is not less than 220 HBW, the density is not less than 98.5%, and the electrical conductivity-hardness composite index expressed as EC×HBW is not less than 9000; when the carbide ceramic framework phase is a chromium carbide-based ceramic framework phase and the continuous metallic phase is a copper phase or a copper alloy phase, under 0.001 s⁻¹ quasi-static compression conditions and compressed to approximately 80% of the engineering strain, the maximum engineering compressive stress of the composite material in the large strain densification stage is 3000–3550 MPa; under 0.1 s⁻¹ quasi-static compression conditions and compressed to approximately 65–70% of the engineering strain, the maximum engineering compressive stress of the composite material is 1850–2400 MPa; under a dynamic compressive strain rate of 0.8 × 10³–1.35 × 10³ s⁻¹, the dynamic compressive peak engineering strength of the composite material is 800–950 MPa. MPa; Under a dynamic compressive strain rate of 4.5×103~5.5×103 s-1, the dynamic compressive peak engineering strength of the composite material is 1000~1250 MPa, and the load-bearing termination engineering strain is 0.30~0.45, wherein the load-bearing termination engineering strain refers to the engineering strain corresponding to the first drop of the dynamic compressive engineering stress to 90% of the peak engineering stress after the peak.
[0024] Finally, the present invention provides the application of the carbide ceramic-metal interpenetrating phase composite material as described above in high-voltage electrical contacts, arc-erosion resistant components, high-hardness conductive structural components, high-strain-rate impact-bearing components, high-speed load-transfer components, rail transit electrical contact components, aerospace impact-resistant conductive structural components, high-temperature conductive wear-resistant components, or metal / ceramic interpenetrating phase structural components.
[0025] Compared with the prior art, the present invention has the following technical effects:
[0026] (1) This invention utilizes a hypergravity field to provide an external force far exceeding that of ordinary gravity, enabling molten metal to overcome or reduce oxide film, wetting angle, and micron-level pore resistance in a short time, rapidly entering the interconnected pores of ceramics and forming a continuous metallic phase, thus significantly shortening the melting and infiltration cycle. Taking copper metal source as an example, after melting the copper source at 1300℃ for 30 min, only about 5 min of hypergravity centrifugation is needed to complete short-term forced melting and infiltration; compared with the applicant's previous pressureless melting and infiltration of about 5 h, the melting and infiltration stage time is shortened by about 60 times. Even including 30 min of pre-melting and holding, the total high-temperature melting and infiltration operation time is still significantly shortened.
[0027] (2) This invention can avoid or reduce the surface modification of electroless or electroplated copper, reduce the steps of plating solution preparation, plating quality control and post-treatment, and also avoid the alumina removal steps caused by the aluminothermic reaction. Wet H2 decarburization, graphite paper anti-oxidation, high temperature resistant pressing and super gravity physical drive together improve the feasibility of melting and infiltration.
[0028] (3) The present invention can achieve effective entry into aluminum alloy systems that are difficult to achieve without pressure melting. The AlSi10 sample with pressureless melting has an alumina film or alumina powder residue at the preform / AlSi10 interface, which is characterized by insufficient melting, many residual pores and weak interface bonding; after 1000g high gravity melting for 5 min, the interface oxide film is broken or weakened, the melting is more complete, the pores are significantly reduced, and the interface bonding is tighter.
[0029] (4) The samples obtained by this invention can effectively retain and fill the interpenetrating phase structure. Samples with different hypergravity accelerations and different W contents all exhibit a continuous interpenetrating phase structure, with the metallic phase fully filled and no large-sized residual pores observed, indicating that rapid hypergravity melting can maintain the continuity, integrity, and density of the interpenetrating phase structure in a short time. The conductivity of the samples obtained by this invention remains at 37.19–37.56 %IACS, and the Brinell hardness remains at 254.3–262.1 HBW. The comprehensive performance of high strength and high conductivity is higher than that of commercial tungsten copper. It is in the same high conductivity and high hardness application range as the applicant's previous pressureless melting samples (39.28–39.94 %IACS and 289.87–304.13 HBW), indicating that this invention can significantly improve melting efficiency while basically maintaining high comprehensive performance, and further obtain high strain rate and quasi-static large strain bearing capacity. The obtained S-Cu-(CrW) x C-1250 composite material at approximately 4.5 × 10 3 ~5.5×10 3 s -1 Under dynamic compression conditions, it can maintain a peak engineering strength of 1000–1250 MPa and sustain load-bearing capacity within the engineering strain range of 0.30–0.45 MPa. At 0.001 s... -1 Under quasi-static compression conditions, the maximum engineering compressive stress of the sample during the large-strain densification stage (approximately 80% of the engineering strain) is about 3.03–3.55 GPa, where S-Cu-(CrW) 50 C-1250 reached approximately 3.53 GPa; at 0.1 s -1 Under these conditions, the maximum engineering compressive stress of the sample at approximately 65–70% engineering strain is approximately 1.85–2.40 GPa. Attached Figure Description
[0030] The invention, its features and advantages will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings.
[0031] Figure 1 This is a simplified process diagram illustrating the preparation of carbide ceramic-metal interpenetrating phase composite materials using centrifugal melting and infiltration under ultragravity, as per the present invention.
[0032] Figure 2 This is a schematic cross-sectional view of the boron nitride crucible filling structure in an embodiment of the present invention.
[0033] Figure 3 This is an experimental photograph of the chromium carbide tungsten ceramic-copper interpenetrating phase composite material sample in Example 1 of the present invention.
[0034] Figure 4 Different tungsten contents (S-Cu-(CrW)) under 1250g conditions x SEM images of the surface of C-1250 samples (x = 0, 10, 25, 50) show the interpenetrating phase structure and W-containing characteristic phase distribution in the surface layer of the composite material.
[0035] Figure 5 Different tungsten contents (S-Cu-(CrW)) under 1250g conditions x The longitudinal cross-sectional SEM images of C-1250 samples (x = 0, 10, 25, 50) show the continuous interpenetrating network formed along the melting and infiltration direction and its longitudinal continuity.
[0036] Figure 6 The images show the SEM morphology of Cu-(CrW0)C samples under different centrifugation accelerators, where (a) 750g0, (b) 1000g0, and (c) 1250g0.
[0037] Figure 7 S-Cu-(CrW) x Engineering strength-engineering strain curves of C-1250 composite material (x = 0, 10, 25, 50) under different dynamic compressive strain rates.
[0038] Figure 8 S-Cu-(CrW) x C-1250 composite material (x = 0, 10, 25, 50) at 0.001 s -1 Stress-strain curves under quasi-static compression conditions.
[0039] Figure 9 These are experimental photographs of the samples obtained in Example 3 and Comparative Example 2 of the present invention.
[0040] Figure 10 Comparison of the melting infiltration interface mechanism of metal melting infiltration samples under pressureless / high gravity conditions. Detailed Implementation
[0041] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the invention.
[0042] See Figure 1 The method for preparing a carbide ceramic-metal interpenetrating phase composite material disclosed in this invention includes the following steps:
[0043] S1. Obtain a carbide porous ceramic preform with a three-dimensional continuous open-pore structure; the carbide porous ceramic preform can maintain a continuous ceramic skeleton structure at the subsequent metal infiltration temperature;
[0044] S2, see also Figure 2 The carbide porous ceramic preform, metal source, high-temperature resistant press block and oxygen barrier layer are sequentially loaded into a metal melt resistant crucible and sealed to obtain a crucible to be melted and infiltrated.
[0045] S3. Balance the mass and center of gravity of the crucible to be melted and infiltrated with the balancing crucible.
[0046] S4. Place the crucible to be melted in a heating furnace at a preset temperature and keep it in an inert atmosphere, reducing atmosphere, vacuum environment or a local low oxygen environment formed by the oxygen barrier layer to keep the metal source in a molten state.
[0047] S5. While the metal source remains in a molten state, the crucible to be melted is quickly installed into a centrifugal device under high gravity. Centrifugation is performed at a centrifugal acceleration of 750–1500 g0 for 1–10 min, allowing the molten metal to enter the interconnected pores of the carbide porous ceramic preform under the action of the high gravity field and form a continuous metal phase. Here, g0 is the standard gravitational acceleration. After centrifugation, the material is cooled to obtain a carbide ceramic-metal interpenetrating phase composite material composed of a continuous carbide ceramic framework phase and a continuous metal phase.
[0048] The technical effects achieved by the present invention will be further illustrated below through specific embodiments and comparative examples. Unless otherwise stated, sample number "S-Cu-(CrW" is used. x "Cy" indicates a copper / chromium carbide-tungsten interpenetrating phase composite material prepared by gravity-assisted copper melting and infiltration; where x represents the mass percentage of W powder added relative to Cr2O3 raw material, and y represents the centrifugal acceleration in g. Numbers in sample names are not used as stoichiometric subscripts for crystals.
[0049] Example 1: Preparation of porous preforms containing tungsten chromium carbide
[0050] Cr2O3 powder and W powder were ball-milled in a zirconia ball mill jar without adding a copper source. After ball milling, the mixture was dried and molded to obtain a disc-shaped blank. Under the example conditions, the ball milling speed was 150 r / min, the ball milling time was 12 h, and the molding pressure was approximately 100 MPa. The blank was placed in a tube furnace and subjected to gas-phase carbothermic reduction at approximately 1150 °C for 12–20 h in a mixed atmosphere of CH4:H2:Ar = 40:180:180 sccm. Subsequently, the atmosphere was switched to a wet H2 atmosphere containing trace amounts of water vapor, and decarburization / wet hydrogen reduction was performed at approximately 1150 °C in H2 + approximately 150 ppm H2O for 3–5 h to reduce the influence of free carbon on subsequent melting and infiltration.
[0051] This step yields porous preforms of (CrW10)C, (CrW25)C, and (CrW50)C with a three-dimensional continuous open-pore structure. To illustrate the effect of W addition on the topology of the framework, a control preform of (CrW0)C without W was also prepared. Typical topological parameters of the preforms are shown in Table 1.
[0052] In this invention, "topological parameters" refers to a set of structural parameters used to characterize the three-dimensional open-pore network structure of carbide porous ceramic preforms, including but not limited to open porosity, average pore size, skeleton ligament thickness, W enrichment characteristics, and connectivity index C. i And tortuosity τ. These parameters collectively reflect the size, number, continuity, flow resistance, and spatial constraint of the ceramic skeleton on the metallic phase within the preform. Among them, open porosity primarily affects the volume fraction that can be filled by the molten metal; average pore size affects the capillary and viscous resistance encountered by the melt entering the channels; skeleton ligament thickness reflects the load-bearing capacity of the continuous ceramic skeleton; W enrichment characteristics are used to characterize the distribution of W-containing carbide phases within the skeleton; C i τ is used to characterize the relative connectivity of a channel or skeleton network; τ is used to characterize the tortuosity of a channel or skeleton network relative to a straight path.
[0053] Table 1 Typical topological parameters of porous chromium carbide tungsten carbide preforms with different W addition amounts
[0054]
[0055] Note: C i τ represents connectivity and tortuosity; both are dimensionless relative parameters used to describe the structural features of typical embodiments. Specific values can be obtained through image analysis, 3D reconstruction, or equivalent network analysis, and are mainly used for relative comparisons between different prefabricated bodies.
[0056] The parameters listed in Table 1 are representative topological parameters of typical samples, used to illustrate the regulatory effect of W addition on the network structure of carbide porous ceramic preforms, and should not be construed as the sole limitation on the scope of protection of this invention. With increasing W addition, the average pore size and porosity of the preform slightly decrease, and the W enrichment characteristics gradually evolve from discrete micro-regions to a network distribution, indicating that W can mediate the local reconstruction of the ceramic skeleton. This type of topological change alters the flow resistance and filling path of molten metal in micron-level interconnected channels. Furthermore, it enhances the spatial constraint of the continuous ceramic skeleton on the metallic phase after the composite material is formed, and improves the strength, hardness, and large strain load-bearing capacity of the interpenetrating phase composite material through crack deflection, path extension, and local load sharing.
[0057] Example 2: Copper centrifugal melting and infiltration based on chromium carbide tungsten carbide ceramic preforms under high gravity
[0058] A porous preform of (CrW10)C, (CrW25)C, or (CrW50)C, a copper block, a tungsten block, and graphite paper are sequentially placed into a boron nitride crucible, which is then sealed with a boron nitride crucible lid. In a separate boron nitride crucible, copper granules approximately 1 mm in diameter are added as balancing weights to ensure that the total mass of the balancing crucible is the same as or within the centrifuge's allowable balancing error range.
[0059] Preheat the pit furnace to 1300℃, then place the crucible to be melted into the pit furnace. After the furnace temperature returns to 1300℃, hold for 30 minutes to allow the copper source to fully melt. After holding, quickly remove the crucible and place it in a movable titanium alloy centrifuge sleeve, immediately installing it into a centrifuge. Before starting centrifugation, the titanium alloy centrifuge sleeve can be in a vertical position; after starting centrifugation and accelerating with the rotor, the titanium alloy centrifuge sleeve rotates tangentially by approximately 90° to a horizontal position under centrifugal force, allowing the crucible to be melted to be centrifuged in a horizontal position at 1250g for 5 minutes. After centrifugation, remove the crucible and cool to room temperature to obtain S-Cu-(CrW10)C-1250, S-Cu-(CrW25)C-1250, and S-Cu-(CrW50)C-1250 composite materials. See also Figure 3 The obtained chromium carbide tungsten ceramic-copper interpenetrating phase composite material showed good bonding between copper and the preform under hypergravity assistance, with no interfacial delamination.
[0060] See Figure 4 and Figure 5 Surface and cross-sectional SEM results show that preforms with different W contents all formed composite structures after copper hypergravity infiltration. The copper phase entered the internal channels of the preforms and formed a continuous interpenetrating phase structure with the chromium carbide tungsten ceramic framework. With the increase of W content, the bright white W-containing characteristic phase gradually increased in the microstructure, indicating that the W-mediated topological features of the preform stage were inherited after hypergravity infiltration.
[0061] To verify the effect of centrifugal acceleration due to centrifugation on the continuity of copper phase filling, copper infiltration was performed under conditions of 750 g⁻¹, 1000 g⁻¹, and 1250 g⁻¹, using (CrW₀)₃ preforms as a control. (See also...) Figure 6 SEM observations showed that as centrifugation acceleration increased, the integrity of the sample tissue improved; the corresponding conductivity, Brinell hardness, and density also increased simultaneously, indicating that centrifugation acceleration under high gravity has a direct technical effect on the continuity of copper phase filling, the formation of conductive networks, and the hardness-conductivity synergy.
[0062] Example 3: Centrifugal melting and infiltration of aluminum based on chromium carbide tungsten ceramic preforms under high gravity
[0063] Porous chromium carbide or tungsten-containing chromium carbide preforms, AlSi10 alloy, W briquettes, and graphite paper are placed into a boron nitride crucible. The pit furnace is preset to 850–950°C, preferably about 900°C. After the furnace temperature returns to the preset temperature, it is held for 30 min to melt the AlSi10 alloy, and then centrifuged under 1000g of hypergravity for 5 min.
[0064] Comparative Example 1: Pressureless Copper Infiltration Based on Chromium Carbide Tungsten Ceramic Preform
[0065] This comparative example provides copper pressureless melting infiltration based on chromium carbide tungsten ceramic preforms. The implementation process is similar to that of Example 2, except that centrifugal treatment is not performed and the melting infiltration time is 5 hours.
[0066] Comparative Example 2: Pressureless melting infiltration of aluminum based on chromium carbide tungsten ceramic preforms
[0067] This comparative example provides pressureless melting and infiltration of aluminum based on chromium carbide tungsten ceramic preforms. The implementation process is similar to that of Example 3, except that centrifugation treatment is not performed and the melting and infiltration time is 5 hours.
[0068] The inventors conducted high strain rate dynamic compression response, hardness, electrical conductivity, density, and quasi-static compression response tests on the samples obtained in Examples 2 and 3, as well as Comparative Examples 1 and 2.
[0069] See Figure 7 And Table 2, at approximately 0.9 × 10 3 ~1.35×10 3 s -1 At relatively low dynamic strain rates, the engineering strength of the sample is approximately 800–950 MPa; at approximately 4.89 × 10⁻⁶ MPa... 3 ~5.06×10 3 s -1At higher dynamic strain rates, the engineering strength of the sample increased to approximately 1050–1250 MPa, and the load-bearing termination strain increased to approximately 0.38–0.42. These results demonstrate that the chromium carbide-tungsten carbide-copper interpenetrating phase composite material obtained in this invention exhibits significant high strain rate strengthening response and large deformation load-bearing capacity.
[0070] Table 2 S-Cu-(CrW) x Dynamic compression response of C-1250 composite material
[0071]
[0072] The electrical conductivity, Brinell hardness, and density of the S-Cu-(CrW0)C, S-Cu-(CrW10)C, S-Cu-(CrW25)C, and S-Cu-(CrW50)C samples were tested and compared with typical values of commercial tungsten copper materials CuW70~CuW90. The results are shown in Table 3.
[0073] Table 3. Comparison of electrical conductivity, Brinell hardness, density, and EC×HBW between the material of this invention and commercial tungsten copper materials.
[0074]
[0075] Note: EC is electrical conductivity, HBW is Brinell hardness; CuW70~CuW90 are reference data for commercial tungsten copper. EC×HBW is a comprehensive synergistic index expressed as the product of electrical conductivity and Brinell hardness.
[0076] As shown in Table 3, the chromium carbide-tungsten carbide-copper interpenetrating phase composite materials prepared in this invention all exhibit high density, ranging from 98.83% to 99.59%, indicating that rapid high-gravity melting and infiltration can fully fill the pores of the framework and obtain a dense, continuous metallic phase. In traditional tungsten-copper materials, the Brinell hardness gradually increases with increasing W content, but the electrical conductivity decreases significantly. In contrast, the S-Cu-(CrW50)C-1250 sample of this invention achieves a Brinell hardness of 262.1 ± 5.2 HBW while maintaining an electrical conductivity of 37.56 ± 0.31 % IACS, exhibiting conductivity close to that of CuW75 and Brinell hardness close to or exceeding that of CuW90.
[0077] Furthermore, using EC×HBW as the comprehensive performance index, the S-Cu-(CrW25)C-1250 and S-Cu-(CrW50)C-1250 of this invention are approximately 9651 and 9844, respectively, which are higher than the approximately 7020 to 7480 of typical CuW70 to CuW90 materials, indicating that this invention has significant advantages in the comprehensive synergy of conductivity and hardness. This advantage stems from the continuous copper phase conductive network, the constraint of the chromium carbide tungsten skeleton, and the preservation of the continuity and integrity of the interpenetrating structure by rapid melting and infiltration under high gravity.
[0078] Quasi-static compression tests were performed on the S-Cu-(CrW0)C-1250, S-Cu-(CrW10)C-1250, S-Cu-(CrW25)C-1250, and S-Cu-(CrW50)C-1250 samples obtained in Example 2. See [link / reference] Figure 8 The results show that at 0.001 s -1 Under compression, all samples exhibited significant high-strain densification bearing characteristics. The maximum engineering compressive stresses during the high-strain densification stage, when compressed to approximately 80% of the engineering strain, were approximately 3335.7–3376.0 MPa, 3029.2–3374.3 MPa, 3145.0–3253.0 MPa, and 3507.2–3549.6 MPa, respectively; the average values for each group were approximately 3355.9 MPa, 3201.8 MPa, 3199.0 MPa, and 3528.4 MPa, with S-Cu-(CrW50)C-1250 exhibiting the highest values. Furthermore, at 0.1 s⁻¹... -1 Under quasi-static compression conditions, the maximum engineering compressive stress of the sample at approximately 65–70% engineering strain is approximately 1845.9–2399.2 MPa, indicating that the material of the present invention not only possesses a high strain rate strengthening response but also has excellent quasi-static large strain compression bearing capacity.
[0079] Table 4 shows a comparison of the performance and preparation efficiency of the representative copper-based sample obtained by centrifugal melting in Example 2 and the representative copper-based sample obtained by pressureless melting in Comparative Example 1. Centrifugal melting intensifies the melting stage of the representative copper system from approximately 5 hours in the previous pressureless melting process to approximately 5 minutes, significantly increasing the melting rate. Simultaneously, the obtained samples maintain an electrical conductivity of 37.19–37.56 %IACS and a Brinell hardness of 254.3–262.1 HBW, placing them within the same high conductivity and high hardness application range as the applicant's previous pressureless melting samples (39.28–39.94 %IACS and 289.87–304.13 HBW). This demonstrates that the present invention can significantly improve melting efficiency while maintaining relatively high overall performance, and further achieve high strain rate and quasi-static large strain bearing capacity.
[0080] Table 4 Comparison of performance and preparation efficiency of representative copper-based samples in Example 2 (high gravity centrifugal melting infiltration) and Comparative Example 1 (pressureless melting infiltration).
[0081]
[0082] See Figure 9The pressureless AlSi10 melting sample prepared in Comparative Example 2 exhibited significant structural defects, unfilled areas, and residual pores. An alumina film or powder was observed at the preform / AlSi10 interface, hindering wetting and interfacial contact. In contrast, the 1000g high-gravity melting sample prepared in Example 3 maintained a relatively intact overall structure. Along the high-gravity assisted melting direction, the interfacial oxide film was broken or weakened, and the AlSi10 interface with the preform showed good bonding. (Schematic diagram of the bonding mechanism follows.) Figure 10 As can be seen, the oxide film on the surface of aluminum alloy melt and the non-ideal wetting angle will result in greater resistance to entry under normal pressureless melting, making it difficult for the melt to fully enter the micron-level interconnected channels; the supergravity field provides additional physical force to drive the melt to overcome or reduce the resistance of the oxide film, wetting angle and channels, thereby achieving effective entry that is difficult to achieve under conventional pressureless melting conditions.
[0083] Those skilled in the art should understand that variations can be implemented by combining existing technology with the above embodiments, which will not be elaborated here. Such variations do not affect the essence of the present invention, and will not be elaborated here either.
[0084] The preferred embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above. Systems and structures not described in detail should be understood as being implemented in a conventional manner in the art. Any person skilled in the art can make many possible variations and modifications to the technical solutions of the present invention using the methods and techniques disclosed above, or modify them into equivalent embodiments with equivalent changes, without departing from the scope of the present invention. This does not affect the essential content of the present invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing carbide ceramic-metal interpenetrating phase composite materials using centrifugal melting and infiltration under high gravity, characterized in that, Includes the following steps: S1. Obtain a carbide porous ceramic preform with a three-dimensional continuous open-pore structure; the carbide porous ceramic preform can maintain a continuous ceramic skeleton structure at the subsequent metal infiltration temperature; S2. The carbide porous ceramic preform, metal source, high-temperature resistant press block and oxygen barrier layer are sequentially loaded into a metal melt crucible and sealed to obtain a crucible to be melted and infiltrated. S3. Balance the mass and center of gravity of the crucible to be melted and infiltrated with the balancing crucible. S4. Place the crucible to be melted in a heating furnace at a preset temperature and keep it in an inert atmosphere, reducing atmosphere, vacuum environment or a local low oxygen environment formed by the oxygen barrier layer to keep the metal source in a molten state. S5. While the metal source remains in a molten state, the crucible to be melted is quickly installed into a centrifugal device and centrifuged at a centrifugal acceleration of 750–1500 g0 (g0 is the standard gravitational acceleration) for 1–10 minutes, so that the molten metal enters the interconnected pores of the carbide porous ceramic preform under the action of the hypergravity field and forms a continuous metal phase; after centrifugation, it is cooled to obtain a carbide ceramic-metal interpenetrating phase composite material composed of a continuous carbide ceramic framework phase and a continuous metal phase.
2. The method according to claim 1, characterized in that, The carbide porous ceramic preform is a single carbide ceramic preform or a multiphase carbide ceramic preform; the open porosity of the carbide porous ceramic preform is 40-75%, the average pore size is 0.2-50 μm, and the skeleton ligament thickness is 0.2-20 μm.
3. The method according to claim 2, characterized in that, The carbide porous ceramic preform is a porous ceramic preform of chromium carbide and its doped system.
4. The method according to claim 1, characterized in that, Before being loaded into the molten metal crucible, the carbide porous ceramic preform undergoes a pretreatment process to remove pore residues, reduce oxide film, or improve the pore interface state.
5. The method according to claim 1, characterized in that, The metal source is one or more of copper, copper alloy, aluminum, or aluminum alloy; the metal melt resistant crucible prevents molten metal leakage under hypergravity melting conditions and reduces the risk of molten metal contamination and metal reaction with the crucible; the oxygen barrier layer is one of graphite paper, graphite sheet, carbon paper, or carbon felt; the high-temperature resistant press maintains the relative position of the metal source and the carbide porous ceramic preform during crucible heating, transfer, and centrifugation, and promotes the molten metal to penetrate into the carbide porous ceramic preform along the hypergravity centrifugal force driving direction.
6. The method according to claim 5, characterized in that, The metal melt resistant crucible is a boron nitride crucible; the high-temperature resistant briquette is a W briquette, a Mo briquette, a graphite briquette, an alumina briquette, or other briquette that remains solid at the melting temperature of the metal source.
7. The method according to claim 1, characterized in that, In step S5, the heat-insulated crucible to be melted is quickly transferred to the movable titanium alloy centrifugal sleeve and immediately installed in the centrifugal device. The movable titanium alloy centrifugal sleeve can be in a vertical state before centrifugal start-up. After centrifugal start-up and acceleration with the rotor, the movable titanium alloy centrifugal sleeve swings about 90° tangentially along the rotor to a horizontal state under the action of centrifugal force, so that the crucible to be melted changes from a vertical state to a horizontal state with the sleeve and completes the rapid melting and infiltration under gravity.
8. A carbide ceramic-metal interpenetrating phase composite material prepared by the method according to any one of claims 1 to 7, characterized in that, The composite material comprises a three-dimensional continuous carbide ceramic framework phase and a continuous metallic phase filling the interconnected pores of the carbide ceramic framework phase, wherein the carbide ceramic framework phase and the continuous metallic phase form an interpenetrating phase structure.
9. The carbide ceramic-metal interpenetrating phase composite material according to claim 8, characterized in that, When the continuous metallic phase is a copper phase or a copper alloy phase, the electrical conductivity EC of the composite material is not less than 35% IACS, the Brinell hardness is not less than 220 HBW, the density is not less than 98.5%, and the electrical conductivity-hardness composite index expressed as EC×HBW is not less than 9000; when the carbide ceramic framework phase is a chromium carbide-based ceramic framework phase and the continuous metallic phase is a copper phase or a copper alloy phase, at 0.001 s -1 Under quasi-static compression conditions, when compressed to approximately 80% of the engineering strain, the maximum engineering compressive stress of the composite material during the large-strain densification stage is 3000–3550 MPa; at 0.1 s⁻¹ -1 Under quasi-static compression conditions, when compressed to approximately 65–70% of the engineering strain, the maximum engineering compressive stress of the composite material is 1850–2400 MPa; at 0.8 × 10⁻⁶ MPa... 3 ~1.35×10 3 s -1 Under dynamic compressive strain rate, the peak dynamic compressive engineering strength of the composite material is 800–950 MPa; at 4.5 × 10⁻⁶ MPa... 3 ~5.5×10 3 s -1 Under dynamic compressive strain rate, the dynamic compressive peak engineering strength of the composite material is 1000-1250 MPa, and the load-bearing termination engineering strain is 0.30-0.
45. The load-bearing termination engineering strain refers to the engineering strain corresponding to the first drop of the dynamic compressive stress to 90% of the peak engineering stress after the peak.
10. The application of the carbide ceramic-metal interpenetrating phase composite material of claim 8 or 9 in high-voltage electrical contacts, arc-erosion resistant components, high-hardness conductive structural components, high-strain-rate impact-bearing components, high-speed load-transfer components, rail transit electrical contact components, aerospace impact-resistant conductive structural components, high-temperature conductive wear-resistant components, or metal / ceramic interpenetrating phase structural components.
Citation Information
Patent Citations
Preparation method of cermet
CN103074534A
Method for preparing three-dimensional continuous network Cr3C2-Cu composites by utilizing infiltration process
CN104451237A