A method for preparing high-performance tungsten alloy high-energy penetrating materials by injection molding

By combining nano-boride core-shell powder with micron-sized powder and employing powder metallurgy injection molding technology, the problem of poor machinability of high-performance tungsten alloy materials has been solved, enabling the preparation of tungsten alloy materials with high density, high precision, and excellent mechanical properties, while reducing costs.

CN123060100APending Publication Date: 2026-11-10UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611167769.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-03
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing processes for preparing high-performance tungsten alloy high-energy penetrating materials suffer from poor machinability, making it difficult to achieve miniaturization, complex three-dimensional structural design, and mass production with consistent results.

Method used

By constructing a bimodal particle size distribution using nano-boron core-shell powder and micron powder, and combining it with powder metallurgy injection molding technology, high-performance tungsten alloy high-energy penetrating materials can be directly prepared by controlling the appropriate ratio of nano-powder to micron powder, binder, and sintering methods, thus avoiding subsequent machining.

Benefits of technology

It has enabled the preparation of high-density, high-performance tungsten alloy materials with high dimensional accuracy and excellent mechanical properties, while reducing raw material consumption and processing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060100A_ABST
    Figure CN123060100A_ABST
Patent Text Reader

Abstract

A method for preparing high-performance tungsten alloy high-energy penetrating materials by injection molding. The method involves solution combustion synthesis to prepare Ni, Fe, Co, and Cu metal-coated boride core-shell structured nanopowders. The alloy composition by mass percentage is: 50–90% W, 0–40% Zr, 0–40% Ti, 0–5% Ni, 0–5% Fe, 0–5% Co, 0–5% Cu, and 0.1–1% nano-borides. This invention utilizes the low-temperature liquid phase formed during sintering by introducing low-melting-point alloying elements, while simultaneously adding a small amount of Ni, Fe, Co, and Cu-coated boride nanopowders to promote sintering densification and produce dispersion strengthening. This significantly improves the relative density and mechanical properties of the tungsten alloy injection-molded parts. Furthermore, the process is simple, easily controlled, and suitable for the field of metal injection molding. The high-performance tungsten alloy high-energy penetrating material prepared by this invention has a relative density ≥98.5%, a product dimensional accuracy of less than ±0.3%, a quasi-static compressive strength ≥1700MPa, a quasi-static compressive strain ≥40%, a dynamic compressive strength ≥2200MPa, and a dynamic compressive strain ≥50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-performance tungsten alloy preparation, and a method for preparing high-performance tungsten alloy high-energy penetrating materials by injection molding. Background Technology

[0002] High-performance tungsten alloy high-energy penetrating materials combine the high density and strength of tungsten with the high energy release characteristics of active metals such as zirconium and titanium. When used as fragmentation materials for warheads, they possess the strength, hardness, and toughness of traditional structural materials, while also responding promptly to high-speed impact stimuli, rapidly releasing a large amount of energy to inflict combined penetration, deflagration, and combustion damage on the target, significantly enhancing their destructive power.

[0003] Currently, the mainstream preparation process for high-performance tungsten alloy high-energy penetrating materials is powder metallurgy. This process involves uniformly mixing tungsten powder, zirconium powder, titanium powder, and other metal powders, pressing them into molds, and then sintering them at high temperatures to complete the shaping. However, the presence of high-density tungsten and the active metals zirconium and titanium in the alloy limits the poor machinability of this material, resulting in significant limitations in miniaturization, three-dimensional complex structure design, and mass production with consistent quality.

[0004] Powder injection molding (PIM) technology combines the advantages of powder metallurgy and polymer injection molding. By uniformly mixing micron / submicron tungsten alloy powder with thermoplastic / thermosetting binders, and then performing injection molding, catalytic / solvent debinding, and controlled atmosphere sintering, it can achieve near-net-shape forming, high geometrical freedom, and excellent dimensional repeatability. It has become a key process route for preparing high-performance tungsten alloy high-energy penetrating materials. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing high-performance tungsten alloy high-energy penetrating materials by injection molding, based on a bimodal particle size distribution constructed from nano-boron core-shell powder and micron-sized powder. This invention directly prepares the final shape of the high-performance tungsten alloy high-energy penetrating material using metal powder injection molding, eliminating the need for subsequent machining and reducing raw material consumption and processing costs. By controlling the appropriate ratio of nano-powder to micron-sized powder, using suitable binders, and employing matching sintering methods, a method for preparing high-density and high-performance tungsten alloy high-energy penetrating materials is achieved.

[0006] The present invention adopts the following technical solution: On one hand, the present invention provides a method for preparing a high-performance tungsten alloy high-energy penetrating material by injection molding, comprising: S1. Weigh micron- and nano-sized metal powder raw materials of high-performance tungsten alloy high-energy penetrating material according to the composition ratio, mix them evenly by ball milling, then mix them with binder in an argon environment in a mixer, then crush them and screen them with a 0.5mm sieve to obtain particles of appropriate size, and continue to crush and screen the larger particles to prepare a uniformly mixed injection molding feed with good rheological properties. S2. The feed material prepared in the previous step is used to prepare a tungsten alloy penetrating material preform on an injection molding machine using injection molding technology; S3. The preform prepared in the previous step is subjected to a degreasing process to obtain a degreased preform with a porous structure; S4. Sinter the degreased blank from the previous step to obtain a high-performance tungsten alloy high-energy penetrating material.

[0007] Furthermore, in step S1, the high-performance tungsten alloy high-energy penetrating material is mainly composed of 50-90% W, 0-40% Zr, 0-40% Ti, 0-5% Ni, 0-5% Fe, 0-5% Co, 0-5% Cu, and 0.1-1% nano boride by mass fraction.

[0008] Further, in step S1, the micron-sized metal powder is W powder with a diameter of 1-3 μm, Zr element is introduced through ZrH2 with a diameter of 10-30 μm, and Ti element is introduced through TiH2 with a diameter of 10-30 μm.

[0009] Further, in step S1, the nanoscale metal powder is a core-shell structured nanopowder prepared by solution combustion synthesis, consisting of nano-borides coated with at least one element, Ni, Fe, Co, and Cu, with an average particle size of 40–100 nm. The preparation process involves preparing an aqueous solution of nitrates of the aforementioned alloying elements and glycine at a molar ratio of 1:0.5–2, and then continuously heating 20–50 nm nano-borides (mainly including any one of nano-HfB2, ZrB2, TiB2, LaB6, WB2, and MoB2) to prepare metal oxide-coated nano-borides. Subsequently, hydrogen reduction is performed to prepare Ni, Fe, Co, and Cu metal-coated nano-boride core-shell structured nanopowder.

[0010] Furthermore, in step S1, the nanoscale metal powder accounts for 1 to 10% of the total weight of the metal powder raw materials.

[0011] Further, in step S1, the volume ratio of the micron- and nano-sized metal powder raw materials to the binder is 1:0.5 to 1, and the metal powder and binder are mixed evenly and then kneaded at a temperature of 150 to 190°C for 1 to 3 hours.

[0012] Furthermore, in step S2, a high-performance tungsten alloy high-energy penetrating material preform is prepared on an injection molding machine using injection molding technology. The injection temperature is 150–180°C, the injection pressure is 90–120 Bar, the injection speed is 70–90%, and the holding time is 0.5–2 s.

[0013] Further, in step S4, the sintering is first held at 600-750°C for 2-4 hours. This stage is the dehydrogenation reaction of ZrH2 or TiH2 to pure metallic Zr or Ti. A suitable thermal decomposition process is used to control the dehydrogenation reaction rate to prevent deformation or cracking of the green body. Then, the temperature is raised to 1300-1700°C to start densification sintering. The sintering holding time is 1-3 hours, the heating rate is 2-5°C / min, and the sintering condition is vacuum sintering.

[0014] The high-performance tungsten alloy high-energy penetrating material produced by injection molding after sintering of this invention has a relative density ≥98.5%, a product dimensional accuracy of less than ±0.3%, a quasi-static compressive strength ≥1700MPa, a quasi-static compressive strain ≥40%, a dynamic compressive strength ≥2200MPa, and a dynamic compressive strain ≥50%.

[0015] The key technical point of this invention is: In-situ synthesized Ni, Fe, Co, and Cu coated nano-borides were prepared by solution combustion synthesis. This nanopowder can promote activated sintering and significantly improve mechanical properties through nano-boride dispersion strengthening.

[0016] By introducing trace amounts of low-melting-point alloying elements and combining them with pressureless sintering, the relative density of the material is increased, the sintering temperature is reduced, energy is saved, and grain refinement is facilitated, thereby improving mechanical properties.

[0017] The injection-molded high-performance tungsten alloy high-energy penetrating material prepared by this invention has a relative density ≥98.5%, a product dimensional accuracy of less than ±0.3%, a quasi-static compressive strength ≥1700MPa, a quasi-static compressive strain ≥40%, a dynamic compressive strength ≥2200MPa, and a dynamic compressive strain ≥50%.

[0018] The beneficial effects of this invention are as follows: 1. This invention enables the preparation of complex-shaped, high-precision, high-performance tungsten alloy high-energy penetrating materials using injection molding technology.

[0019] 2. This invention uses solution combustion synthesis to prepare Ni, Fe, Co and Cu metal-coated nano-borides with core-shell structured nanopowders. On the one hand, adding a small amount of nanopowder promotes activation sintering, and on the other hand, the nano-borides can significantly improve the mechanical properties of tungsten alloys.

[0020] 3. Compared with methods such as hot pressing sintering and hot isostatic pressing sintering to improve the relative density of injection molded parts, the pressureless sintering process of this invention can achieve a relative density of ≥98.5%, without the need to introduce expensive and complex additional equipment or process steps. The process is simple and cost-effective.

[0021] 4. In this invention, Zr is introduced through ZrH2, and Ti is introduced through TiH2. This effectively reduces the surface oxidation caused by improper storage of the high-energy reactivity of Zr and Ti, which leads to the deterioration of the alloy's mechanical properties after sintering. Compared to pure metallic Zr and Ti, the storage cost and risk of their hydrides are relatively lower.

[0022] 5. The injection-molded high-performance tungsten alloy high-energy penetrating material prepared by this invention has a relative density ≥98.5%, a product dimensional accuracy of less than ±0.3%, a quasi-static compressive strength ≥1700MPa, a quasi-static compressive strain ≥40%, a dynamic compressive strength ≥2200MPa, and a dynamic compressive strain ≥50%. Attached Figure Description

[0023] Figure 1 The diagram shown is a schematic flow chart of the preparation process of a high-performance tungsten alloy high-energy penetrating material by powder injection molding according to an embodiment of the present invention.

[0024] Figure 2 The image shown is a scanning electron microscope (SEM) image of the fracture surface of a high-performance tungsten alloy high-energy penetrating material prepared by powder injection molding in Example 1.

[0025] Figure 3 The image shows a quasi-static compressive true stress-strain curve of a high-performance tungsten alloy high-energy penetrating material prepared by powder injection molding in Example 1.

[0026] Figure 4 The image shows a dynamic compression true stress-strain curve of a powder injection molded high-performance tungsten alloy high-energy penetrating material prepared in Example 1. Detailed Implementation

[0027] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be noted that the technical features or combinations of technical features described in the following embodiments should not be considered in isolation, but can be combined with each other to achieve better technical effects.

[0028] Example 1

[0029] Internal mixing: 1μm W powder, 10μm ZrH2, 10μm TiH2, Ni, Fe, and 25nm HfB2 were weighed in a weight ratio of 74:10.22:10.42:3.5:1.5:1. Ni, Fe, and 25nm HfB2 were synthesized into 40nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.57. The metal powders and binder were mixed in an internal mixer at 180°C under argon atmosphere for 2 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0030] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 160°C, the injection pressure is 100 Bar, the injection speed is 90%, and the holding time is 1 second. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0031] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0032] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 650℃ at a heating rate of 5℃ / min and held for 2.5h. Then the temperature is raised to 1000℃ at a heating rate of 4℃ / min and then raised to 1480℃ at a heating rate of 3℃ / min and held for 2h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0033] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 99.25% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0034] Comparative Example 1

[0035] Internal mixing: 1μm W powder, 10μm ZrH2, 10μm TiH2, Ni, and Fe were weighed in a weight ratio of 75:10.22:10.42:3.5:1.5. Ni and Fe were synthesized into 40nm nanoparticles through solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.57. The metal powders and binder were mixed in an internal mixer at 180°C under argon atmosphere for 2 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0036] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 160°C, the injection pressure is 100 Bar, the injection speed is 90%, and the holding time is 1 second. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0037] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0038] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 650℃ at a heating rate of 5℃ / min and held for 2.5h. Then the temperature is raised to 1000℃ at a heating rate of 4℃ / min and then raised to 1480℃ at a heating rate of 3℃ / min and held for 2h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0039] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 99.37% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of <1700MPa, a quasi-static compressive strain of <40%, a dynamic compressive strength of <2200MPa, and a dynamic compressive strain of <50%.

[0040] Comparative Example 2

[0041] Internal mixing: 1μm W powder, 10μm ZrH2, 10μm TiH2, 2μm Ni, 2μm Fe, and 25nm HfB2 were weighed in a weight ratio of 74:10.22:10.42:3.5:1.5:1. All metal powders were ball-milled and mixed uniformly. The volume ratio of all metal powders to binder was 1:0.57. The metal powders and binder were mixed in an internal mixer at 180°C under argon atmosphere for 2 hours. Afterward, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a uniformly mixed injection molding feedstock with good rheological properties.

[0042] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 160°C, the injection pressure is 100 Bar, the injection speed is 90%, and the holding time is 1 second. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0043] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0044] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 650℃ at a heating rate of 5℃ / min and held for 2.5h. Then the temperature is raised to 1000℃ at a heating rate of 4℃ / min and then raised to 1500℃ at a heating rate of 3℃ / min and held for 2h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0045] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 98.35% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of <1700MPa, a quasi-static compressive strain of <40%, a dynamic compressive strength of <2200MPa, and a dynamic compressive strain of <50%.

[0046] In Example 1, nano-borides were added to the alloy, while in Comparative Example 1, they were not added; all other preparation processes were the same. The absence of nano-borides resulted in a slight increase in the alloy's relative density, but the lack of the dispersion strengthening effect of the nano-borides significantly reduced the mechanical properties of the alloy, all falling below the specified values.

[0047] In Comparative Example 2, instead of using Ni and Fe coated boride nanopowder, micron-sized Ni and Fe powder were directly mixed with nano-borides. Compared to Example 1, the sintering temperature was higher and the holding time was longer. However, the relative density of the alloy in Comparative Example 2 was <99%, and the mechanical properties of the alloy decreased significantly, all of which were below the specifications.

[0048] Example 2

[0049] Internal mixing: 1.5μm W powder, 15μm ZrH2, Ni, Co, and 30nm TiB2 were weighed in a weight ratio of 69.2:20.44:7:3:0.8. Ni, Fe, and 30nm TiB2 were synthesized into 45nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.63. The metal powders and binder were mixed in an internal mixer at 155°C under argon atmosphere for 3 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0050] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 155°C, the injection pressure is 120 Bar, the injection speed is 75%, and the holding time is 2s. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0051] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0052] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 700℃ at a heating rate of 5℃ / min and held for 2 hours. Then the temperature is raised to 1100℃ at a heating rate of 5℃ / min and then raised to 1350℃ at a heating rate of 2.5℃ / min and held for 1.5 hours. Subsequently, the blank is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0053] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 99.32% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0054] Example 3

[0055] Internal mixing: 2μm W powder, 20μm TiH2, Co, and 50nm ZrB2 were weighed in a weight ratio of 63:31.26:6.5:0.5. Ni, Fe, and 50nm ZrB2 were synthesized into 90nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.59. The metal powders and binder were mixed in an internal mixer at 185°C under argon atmosphere for 2.5 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0056] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 170°C, the injection pressure is 110 Bar, the injection speed is 85%, and the holding time is 1.5s. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0057] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0058] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 750℃ at a heating rate of 4℃ / min and held for 1.5h. Then the temperature is raised to 1200℃ at a heating rate of 3℃ / min and then raised to 1350℃ at a heating rate of 3℃ / min and held for 3h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0059] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 98.87% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0060] Example 4

[0061] Internal mixing: 1μm W powder, 12μm ZrH2, 15μm TiH2, Ni, Fe, Co, Cu, and 35nm LaB6 were weighed in the following weight ratio: 59.7:20.44:10.42:2.48:2.35:2.49:2.68:0.3. Ni, Fe, and 35nm LaB6 were synthesized into 40nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.58. The metal powders and binder were mixed in an internal mixer at 175°C under argon atmosphere for 2.5 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0062] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 165°C, the injection pressure is 120 Bar, the injection speed is 70%, and the holding time is 1.5 s. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0063] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0064] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 700℃ at a heating rate of 3.5℃ / min and held for 4 hours. Then the temperature is raised to 1150℃ at a heating rate of 3.5℃ / min and then raised to 1400℃ at a heating rate of 3℃ / min and held for 2.5 hours. Subsequently, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0065] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 98.91% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0066] Example 5

[0067] Internal mixing: 1μm W powder, 20μm ZrH2, 10μm TiH2, Ni, Cu, and 30nm HfB2 were weighed in a weight ratio of 74:20.44:5.21:1.5:1.5:0.5. Ni, Fe, and 30nm MoB2 were synthesized into 36nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.54. The metal powders and binder were mixed in an internal mixer at 180°C under argon atmosphere for 3.5 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0068] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 165°C, the injection pressure is 115 Bar, the injection speed is 80%, and the holding time is 0.5 s. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0069] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0070] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 750℃ at a heating rate of 5℃ / min and held for 2.5h. Then the temperature is raised to 1050℃ at a heating rate of 5℃ / min and then raised to 1500℃ at a heating rate of 2.5℃ / min and held for 3h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0071] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 99.52% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0072] Example 6

[0073] Internal mixing: 3μm W powder, 30μm ZrH2, Ni, Co, and 25nm WB2 were weighed in a weight ratio of 54.8:40.88:2.5:2.5:0.2. Ni, Fe, and 25nm WB2 were synthesized into 32nm core-shell structured nanoparticles via solution thermal combustion. All metal powders were then ball-milled until homogeneous. The volume ratio of all metal powders to binder was 1:0.55. The metal powders and binder were mixed in an internal mixer at 180°C under argon atmosphere for 3 hours. Subsequently, the mixture was crushed and sieved through a 0.5mm sieve to obtain appropriately sized particles. Larger particles were further crushed and sieved to prepare a homogeneous injection molding feedstock with good rheological properties.

[0074] Injection: The feed material prepared in the previous step is loaded into the injection molding machine. The injection temperature is 170°C, the injection pressure is 95 Bar, the injection speed is 80%, and the holding time is 2s. The high-performance tungsten alloy high-energy penetrating material billet is obtained by injection molding.

[0075] Degreasing: The high-performance tungsten alloy high-energy penetrating material blank is placed in an oxalic acid degreasing furnace for degreasing treatment, and finally a porous degreased blank is obtained.

[0076] Sintering: The degreased blank obtained in the previous step is placed in a sintering furnace for vacuum sintering. The temperature is raised to 700℃ at a heating rate of 4℃ / min and held for 3.5h. Then the temperature is raised to 1200℃ at a heating rate of 3.5℃ / min and then raised to 1700℃ at a heating rate of 3℃ / min and held for 2h. After that, it is cooled with the furnace to obtain a high-performance tungsten alloy high-energy penetrating material injection molded part.

[0077] The final product is a high-performance tungsten alloy high-energy penetrating material with a relative density of 99.25% obtained by powder injection molding. The product has a dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.

[0078] While embodiments of the present invention have been provided herein, those skilled in the art should understand that modifications can be made to the embodiments without departing from the spirit of the invention. The above embodiments are merely exemplary and should not be construed as limiting the scope of the invention.

Claims

1. A method for preparing a high-performance tungsten alloy high-energy penetrating material by injection molding, characterized in that, The method includes: S1. Weigh micron- and nano-sized metal powder raw materials of high-performance tungsten alloy high-energy penetrating material according to the composition ratio, mix them evenly by ball milling, then mix them with binder in an argon environment in a mixer, then crush them and screen them with a 0.5mm sieve to obtain particles of appropriate size, and continue to crush and screen the larger particles to prepare a uniformly mixed injection molding feed with good rheological properties. S2. The feed material prepared in the previous step is used to prepare a tungsten alloy penetrating material preform on an injection molding machine using injection molding technology; S3. The preform prepared in the previous step is subjected to a degreasing process to obtain a degreased preform with a porous structure; S4. Sinter the degreased blank from the previous step to obtain a high-performance tungsten alloy high-energy penetrating material.

2. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S1, the high-performance tungsten alloy high-energy penetrating material is mainly composed of 50-90% W, 0-40% Zr, 0-40% Ti, 0-5% Ni, 0-5% Fe, 0-5% Co, 0-5% Cu, and 0.1-1% nano boride by mass fraction.

3. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S1, the micron-sized metal powder is W powder with a diameter of 1-3 μm, Zr element is introduced through ZrH2 with a diameter of 10-30 μm, and Ti element is introduced through TiH2 with a diameter of 10-30 μm.

4. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S1, the nanoscale metal powder is a core-shell structured nanoparticle of at least one element, Ni, Fe, Co, and Cu, prepared by solution combustion synthesis, with an average particle size of 40-100 nm. The preparation process involves preparing an aqueous solution of nitrates of the above alloying elements and glycine at a molar ratio of 1:0.5-2, and then continuously heating 20-50 nm nano-borides to prepare metal oxide-coated nano-borides. Subsequently, hydrogen reduction is performed to prepare Ni, Fe, Co, and Cu metal-coated nano-boride core-shell structured nanoparticles. The borides include any one of nano-HfB2, ZrB2, TiB2, LaB6, WB2, and MoB2.

5. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S1, the nanoscale metal powder accounts for 1 to 10% of the total weight of the metal powder raw materials.

6. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S1, the volume ratio of the micron- and nano-sized metal powder raw materials to the binder is 1:0.5 to 1. After being mixed evenly, the metal powder and binder are kneaded at a temperature of 150 to 190°C for 1 to 3 hours.

7. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S2, a high-performance tungsten alloy high-energy penetrating material preform is prepared on an injection molding machine using injection molding technology. The injection temperature is 150-180°C, the injection pressure is 90-120 Bar, the injection speed is 70-90%, and the holding time is 0.5-2s.

8. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, In step S4, the sintering is first held at 600-750°C for 2-4 hours, and then the temperature is increased to 1300-1700°C. The sintering holding time is 1-3 hours, the heating rate is 2-5°C / min, and the sintering condition is vacuum sintering.

9. The method for preparing high-performance tungsten alloy high-energy penetrating material by injection molding as described in claim 1, characterized in that, The sintered injection-molded high-performance tungsten alloy high-energy penetrating material has a relative density of ≥98.5%, a product dimensional accuracy of less than ±0.3%, a quasi-static compressive strength of ≥1700MPa, a quasi-static compressive strain of ≥40%, a dynamic compressive strength of ≥2200MPa, and a dynamic compressive strain of ≥50%.