A wear-resistant and scratch-resistant alloy nameplate and its preparation method

By using matrix injection molding and surface multilayer composite technology, high-hardness, corrosion-resistant, wear-resistant and scratch-resistant alloy nameplates are constructed, solving the problem of insufficient surface hardness of traditional alloy nameplates and achieving a significant improvement in high durability and scratch resistance.

CN123060101APending Publication Date: 2026-11-10KUNSHAN DIANFU PRECISION COMPONENTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611357188.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional alloy nameplates have limited surface hardness, insufficient wear and scratch resistance, weak coating adhesion, and limited corrosion resistance, making them difficult to withstand scratches from sharp objects and wear in humid environments.

Method used

By employing matrix injection molding and surface multilayer composite technology, a gradient composite structure consisting of a titanium transition layer, a titanium nitride layer, a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer, and a nitriding modified layer is constructed. Combined with magnetron sputtering and low-temperature plasma nitriding technology, a high-hardness, corrosion-resistant, wear-resistant, and scratch-resistant alloy nameplate is created.

Benefits of technology

Significantly improves the durability of alloy nameplates, increases hardness and scratch resistance, enhances the adhesion between the coating and the substrate, and improves wear resistance and corrosion resistance in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of alloy technology, specifically to a wear-resistant and scratch-resistant alloy nameplate and its preparation method. The finished product is prepared by matrix injection molding and multi-layer surface composite. 420W is selected as the metal powder. By controlling the feed ratio of the binder system and the injection molding process parameters, the rheological uniformity of the feed is improved, while the green strength is enhanced. By sequentially constructing a gradient composite structure on the pretreated part, consisting of a titanium transition layer, a titanium nitride layer, a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer, and a nitriding modified layer, an alloy nameplate with high hardness, corrosion resistance, wear resistance, and scratch resistance is synergistically constructed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy nameplate technology, specifically to a wear-resistant and scratch-resistant alloy nameplate and its preparation method. Background Technology

[0002] Signage, serving as a medium for information display, product certification, and brand identification, is widely used in various fields such as instruments, equipment, and decoration. Traditional alloy signs are mostly made of stainless steel, copper alloy, or aluminum alloy, and manufactured through processes such as stamping and etching. However, these traditional signs have limited surface hardness and insufficient wear and scratch resistance. During transportation and daily use, they are easily scratched by friction and impacts, resulting in fading of luster and blurring of patterns.

[0003] To improve the durability of alloy nameplates, the current market often uses processes such as electroplating and spraying to prepare coatings. However, the resulting coatings suffer from weak adhesion to the substrate and limited hardness improvement. Furthermore, single hard coatings lack self-lubricating properties, making them unsuitable for scratching by sharp objects, and their corrosion resistance is limited, significantly impacting the product's aesthetics and lifespan. Summary of the Invention

[0004] The purpose of this invention is to provide a wear-resistant and scratch-resistant alloy nameplate and its preparation method, so as to solve the problems in the prior art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: A method for preparing a wear-resistant and scratch-resistant alloy nameplate includes the following steps: S1: Mix metal powder and binder and feed them into the mixture, then injection mold to obtain a green body; S2: The green blank is subjected to pre-rinsing, degreasing, and post-rinsing treatments in sequence to obtain a degreased part; S3: The degreased parts are subjected to hot degreasing, vacuum sintering, partial pressure sintering and cooling treatment in sequence to obtain sintered parts; S4: The sintered parts are subjected to dry sandblasting and washing treatment in sequence to obtain pretreated parts; S5: A titanium transition layer, a titanium nitride layer, a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer, and a nitriding modification layer are sequentially formed on the surface of the pretreated part. After washing and quality inspection, a wear-resistant and scratch-resistant alloy nameplate is obtained.

[0006] Furthermore, in the preparation of the green body, the mass ratio of the metal powder to the binder is (90-93):(7-10).

[0007] Furthermore, by mass percentage, the adhesive composition is: 2-4% zinc stearate, 2-4% ethylene-vinyl acetate copolymer, 4-7% polyethylene, 28-31% paraffin wax, and the balance being polyoxymethylene.

[0008] Furthermore, the working conditions for injection molding are as follows: mold temperature is 100-105℃, injection pressure is 25MPa, injection speed is 40mm / s, and cooling time is 5-7s; the working conditions for pre-rinsing are: temperature is 120-125℃, and time is 90-100min; the working conditions for degreasing are: oxalic acid solution is used as the degreasing solvent, temperature is 125-130℃, and time is 350-400min; the working conditions for post-rinsing are: temperature is 125-130℃, and time is 30-40min.

[0009] Furthermore, the working conditions for thermal debonding are: heating from 18°C ​​to 850°C at a rate of 3°C / min; the working conditions for vacuum sintering are: heating from 850°C to 1050°C at a rate of 3°C / min; the working conditions for partial pressure sintering are: pressure of 20-30 kPa, gas atmosphere of argon, temperature of 1050°C to 1340°C at a rate of 3°C / min, and then cooling down to 900°C at a rate of 3°C / min; the working conditions for cooling are: cooling down from 900°C to 20°C at a rate of 4°C / min.

[0010] Furthermore, the working conditions for dry sandblasting are as follows: the abrasive is 170-mesh zircon sand, and the abrasive velocity in the sand delivery pipe is 50-120 m / s.

[0011] Furthermore, step S5 includes the following preparation steps: 1) Evacuate the vacuum, introduce argon gas, heat to 295-305℃, use titanium as the target material to form a titanium transition layer on the surface of the pretreated part, and then introduce nitrogen gas for 15-20 minutes to obtain a titanium nitride layer. 2) In an argon atmosphere, (AlTiZrNiMo) 1-x Z x The composite target and the boron-doped molybdenum disulfide target are energized and pre-sputtered for 15-20 minutes. Then, by controlling the target baffle switch, the titanium nitride layer is alternately oriented towards (AlTiZrNiMo). 1-x Z x A composite target and a boron-doped molybdenum disulfide target are used to alternately form a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer on a titanium nitride layer. 3) Then nitrogen gas is introduced, and the flow ratio of nitrogen gas to argon gas is controlled at 3:4. The temperature is maintained for 60-90 minutes to form a nitriding modified layer on the high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer.

[0012] Furthermore, (AlTiZrNiMo) 1-x Z x In the composite target, the molar ratio of Al, Ti, Zr, Ni and Mo is 1:1:1:1:1, x is 0.01-0.03, and Z is one or a combination of La, Ce and Y.

[0013] Furthermore, Z is a mixture of La and Ce in a mass ratio of 1:1.

[0014] Furthermore, the preparation of the boron-doped molybdenum disulfide target includes the following steps: (1) Weigh out nano molybdenum disulfide, ferric chloride, boric acid and anhydrous ethanol, mix them, sonicate for 10-15 min, dry, grind, keep at 595-605ºC for 110-130 min under nitrogen atmosphere, wash with hydrochloric acid, dry, and obtain boron-doped molybdenum disulfide. (2) After ball milling and drying, the boron-doped molybdenum disulfide powder is loaded into a graphite mold treated with boron nitride, and then hot-pressed and sintered in a vacuum environment. After cooling and processing, a boron-doped molybdenum disulfide target is obtained.

[0015] Furthermore, the working conditions for hot pressing sintering are: temperature of 1000-1050℃, pressure of 36MPa, and time of 3-4h.

[0016] Compared with the prior art, the beneficial effects of the present invention are: This invention provides a wear-resistant and scratch-resistant alloy nameplate and its preparation method. By injection molding of the substrate and multi-layer composite of the surface, an alloy nameplate with high hardness, corrosion resistance, wear resistance and scratch resistance is prepared, which greatly improves the durability of the alloy nameplate.

[0017] 420W metal powder was selected, and zinc stearate was used as a lubricant in the binder system. Ethylene-vinyl acetate copolymer was used as a compatibilizer and plasticizer. By controlling the feed ratio of the binder system and limiting the injection molding process parameters, the rheological uniformity and green strength of the feed were improved. This enabled the one-time molding of alloy nameplates with three-dimensional structures. Compared with traditional processes, this reduced material loss and subsequent processing, and has the potential for large-scale application.

[0018] By combining oxalic acid degreasing with stepped controlled temperature sintering, the binder is safely and thoroughly removed from the green blank, and the metal powder is densified and sintered to obtain sintered parts with high density, few internal defects and good strength, which provides a solid support for the surface coating. The combination of dry grinding and washing ensures that the surface of the pretreated parts is clean and uniformly rough, providing a good base for subsequent coating. By sequentially constructing a gradient composite structure on the pretreated part, consisting of a titanium transition layer, a titanium nitride layer, a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer, and a nitriding modification layer, an alloy nameplate with high hardness, corrosion resistance, wear resistance, and scratch resistance was synergistically constructed.

[0019] A titanium transition layer is deposited on the pretreated part using vacuum coating technology, followed by the introduction of nitrogen gas to generate a titanium nitride layer in situ. This not only improves the hardness but also serves as a solid substrate for subsequent multilayer structures, avoiding the problem of overall peeling failure of the multilayer film due to stress concentration during use.

[0020] To further improve the wear and scratch resistance of alloy nameplates, a high-entropy alloy layer that is corrosion-resistant and wear-resistant is introduced. In order to achieve both high hardness and low friction and wear resistance, existing technologies usually introduce solid lubricants such as molybdenum disulfide as a second phase into the high-entropy alloy to form a composite layer. However, the addition often leads to the deterioration of hardness / strength, and there are also problems such as the failure of wear resistance of molybdenum disulfide in humid environments.

[0021] This invention employs magnetron sputtering on a titanium nitride layer to construct a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer through alternating deposition, thereby improving its toughness. When external loads or cracks propagate to this structure, the hard high-entropy alloy layer bears the main mechanical stress, providing high hardness and load-bearing capacity; while the intermediate soft boron-doped molybdenum disulfide layer effectively dissipates energy by inducing microcrack deflection and bifurcation, preventing crack penetration and propagation. This sandwich-like design of alternating hard and soft layers allows the coating to maintain high hardness while improving impact resistance and scratch resistance. At the same time, the use of boron-doped molybdenum disulfide instead of commonly used molybdenum disulfide improves its oxidation resistance and structural density, enabling it to maintain stable wear resistance even in humid environments.

[0022] In the construction of the high-entropy alloy layer, the introduction of Ti provides chemical bonding continuity, continues the strong Ti-N covalent bond, and improves the bonding strength between the titanium nitride layer and the high-entropy alloy layer. Zr and Ti are in the same group and can be seamlessly integrated into the interface transition region constructed by Ti to form a solid solution-reinforced interface region. Al and Ni tend to form an ordered B2 phase, providing high strength and high modulus for the high-entropy alloy layer. The introduction of Mo plays a role in stress regulation and high-temperature stability, while the introduction of rare earth elements plays a role in grain refinement, effectively improving the bonding strength between the titanium nitride layer and the high-entropy alloy layer.

[0023] During the deposition of boron-doped molybdenum disulfide, Al and Ti atoms on the surface of the high-entropy alloy layer react with S to form a transition layer, transforming the weak van der Waals interface into a strong chemical bonding interface, effectively improving the bonding force. Zr and Mo can be strengthened through solid solution, enhancing strength and thermal stability. The introduction of rare earth elements plays a role in interface purification and sulfidation, refining surface grains, increasing the bonding area, and making it easier for boron-doped molybdenum disulfide to spread on the surface of the high-entropy alloy, achieving a denser and more uniform coverage and improving bonding strength.

[0024] By using low-temperature plasma nitriding to modify the high-entropy alloy layer on the surface, a nitride-reinforcing phase is formed on the surface without damaging the internal molybdenum disulfide lubricating layer, which greatly improves the surface hardness and scratch resistance. Detailed Implementation

[0025] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0026] Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.

[0027] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not intended to limit the present invention.

[0028] Example 1: A method for preparing a wear-resistant and scratch-resistant alloy nameplate, comprising the following steps: S1: By mass percentage, 2% zinc stearate, 2% ethylene-vinyl acetate copolymer, 4% polyethylene, 28% paraffin wax, and the balance polyoxymethylene are mixed as a binder; metal powder and binder are mixed and fed in a mass ratio of 91.76:8.24, and then injection molded at a temperature of 100℃, an injection pressure of 25MPa, an injection speed of 40mm / s, and a cooling time of 5s to obtain a green body; S2: The green blank is subjected to a pre-rinsing treatment at 120°C for 100 min, a degreasing treatment at 125°C for 350 min using oxalic acid solution, and a post-rinsing treatment at 125°C for 40 min to obtain a degreased part. S3: The degreased part is subjected to the following treatments in sequence: hot degreasing treatment from 18°C ​​to 850°C at a rate of 3°C / min and holding for 60 min; vacuum sintering treatment from 850°C to 1050°C at a rate of 3°C / min and holding for 60 min; pressure 25 kPa; gas atmosphere argon; temperature from 1050°C to 1340°C at a rate of 3°C / min and holding for 150 min; then partial pressure sintering treatment from 3°C / min to 900°C; and cooling treatment from 900°C to 20°C at a rate of 4°C / min to obtain the sintered part. S4: The sintered parts are subjected to dry sandblasting treatment with 170-mesh zircon sand and a sand velocity of 90m / s in the sand conveying pipe, followed by washing treatment, to obtain pre-treated parts; S5: Includes the following preparation steps: 1) Reduce the pressure to 10 by drawing a vacuum. -3 Pa, argon gas is introduced, the temperature is raised to 300℃, titanium is used as the target material to form a titanium transition layer on the surface of the pretreated part, and then nitrogen gas is introduced for 20 minutes to obtain a titanium nitride layer. 2)(1) Weigh 0.3g of nano molybdenum disulfide, 0.1g of ferric chloride, 1g of boric acid and 20mL of anhydrous ethanol, mix them, sonicate for 10min, dry, grind, keep warm at 595ºC for 130min under nitrogen atmosphere, wash with 3mol / L hydrochloric acid, dry, and obtain boron-doped molybdenum disulfide. (2) After ball milling and drying, the boron-doped molybdenum disulfide powder is placed into a graphite mold treated with boron nitride, and hot-pressed and sintered at 1000℃ and 36MPa for 4 hours in a vacuum environment. After cooling and processing, a boron-doped molybdenum disulfide target is obtained. (AlTiZrNiMo) 1-x Z x In the composite target, the molar ratio of Al, Ti, Zr, Ni, and Mo is 1:1:1:1:1, x is 0.01, and Z is a mixture of La and Ce in a mass ratio of 1:1. In an argon atmosphere, the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target are pre-sputtered for 15 minutes using a DC power supply with a current of 300 mA. Then, by controlling the target baffle switch, the titanium nitride layer is alternately directed toward the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target, and a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer is alternately formed on the titanium nitride layer. 3) Then nitrogen gas is introduced, and the flow ratio of nitrogen to argon gas is controlled at 3:4. The temperature is maintained for 60 minutes to form a nitriding modified layer on the high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer. After washing and quality inspection, a wear-resistant and scratch-resistant alloy nameplate is obtained.

[0029] Example 2: A method for preparing a wear-resistant and scratch-resistant alloy nameplate, comprising the following steps: S1: By mass percentage, 3% zinc stearate, 3% ethylene-vinyl acetate copolymer, 5% polyethylene, 29% paraffin wax, and the balance polyoxymethylene are mixed to obtain a binder; metal powder and binder are mixed and fed in a mass ratio of 91.76:8.24, and then injection molded at a temperature of 103℃, an injection pressure of 25MPa, an injection speed of 40mm / s, and a cooling time of 6s to obtain a green body; S2: The green blank is sequentially subjected to a pre-rinsing treatment at 123°C for 95 minutes, a degreasing treatment at 127°C for 350 minutes using oxalic acid solution, and a post-rinsing treatment at 127°C for 35 minutes to obtain a degreased part. S3: The degreased part is subjected to the following treatments in sequence: hot degreasing treatment from 18°C ​​to 850°C at a rate of 3°C / min and holding for 60 min; vacuum sintering treatment from 850°C to 1050°C at a rate of 3°C / min and holding for 60 min; pressure of 25 kPa; gas atmosphere of argon; temperature from 1050°C to 1340°C at a rate of 3°C / min and holding for 150 min; then partial pressure sintering from 900°C to 900°C at a rate of 3°C / min; and cooling treatment from 900°C to 20°C at a rate of 4°C / min to obtain the sintered part. S4: The sintered parts are subjected to dry sandblasting treatment with 170-mesh zircon sand and a sand velocity of 90m / s in the sand conveying pipe, followed by washing treatment, to obtain pre-treated parts; S5: The preparation includes the following steps: 1) Reduce the pressure to 10 by drawing a vacuum. -3 Pa, argon gas is introduced, and the temperature is raised to 300℃. Using titanium as the target material, a titanium transition layer is formed on the surface of the pretreated part. Then, nitrogen gas is introduced for 20 minutes to obtain a titanium nitride layer. 2)(1) Weigh 0.3g of nano molybdenum disulfide, 0.1g of ferric chloride, 1g of boric acid and 20mL of anhydrous ethanol, mix them, sonicate for 13min, dry, grind, keep warm at 600ºC for 120min under nitrogen atmosphere, wash with 3mol / L hydrochloric acid, dry, and obtain boron-doped molybdenum disulfide. (2) After ball milling and drying, the boron-doped molybdenum disulfide powder is placed into a graphite mold treated with boron nitride, and hot-pressed and sintered at 1025℃ and 36MPa for 3.5h under vacuum. After cooling and processing, a boron-doped molybdenum disulfide target is obtained. In an argon atmosphere, the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target were pre-sputtered for 18 minutes using a DC power supply with a current of 300 mA. Then, by controlling the target baffle switch, the titanium nitride layer was alternately directed toward the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target, and high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layers were alternately formed on the titanium nitride layer. (AlTiZrNiMo) 1-x Z x In the composite target, the molar ratio of Al, Ti, Zr, Ni, and Mo is 1:1:1:1:1, x is 0.02, and Z is a mixture of La and Ce in a mass ratio of 1:1. 3) Then nitrogen gas is introduced, and the flow ratio of nitrogen to argon gas is controlled at 3:4. The temperature is maintained for 80 minutes to form a nitriding modified layer on the high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer. After washing and quality inspection, a wear-resistant and scratch-resistant alloy nameplate is obtained.

[0030] Example 3: A method for preparing a wear-resistant and scratch-resistant alloy nameplate, comprising the following steps: S1: By mass percentage, 4% zinc stearate, 4% ethylene-vinyl acetate copolymer, 7% polyethylene, 31% paraffin wax, and the balance polyoxymethylene are mixed to obtain a binder; metal powder and binder are mixed and fed in a mass ratio of 91.76:8.24, and then injection molded at a temperature of 105℃, an injection pressure of 25MPa, an injection speed of 40mm / s, and a cooling time of 7s to obtain a green body; S2: The green blank is subjected to a pre-rinsing treatment at 125°C for 90 min, a degreasing treatment at 130°C for 350 min using oxalic acid solution, and a post-rinsing treatment at 130°C for 30 min to obtain a degreased part. S3: The degreased part is subjected to the following treatments in sequence: hot degreasing treatment from 18°C ​​to 850°C at a rate of 3°C / min and holding for 60 min; vacuum sintering treatment from 850°C to 1050°C at a rate of 3°C / min and holding for 60 min; pressure 25 kPa; gas atmosphere argon; temperature from 1050°C to 1340°C at a rate of 3°C / min and holding for 150 min; partial pressure sintering treatment from 900°C to 900°C at a rate of 3°C / min; and cooling treatment from 900°C to 20°C at a rate of 4°C / min to obtain the sintered part. S4: The sintered parts are subjected to dry sandblasting treatment with 170-mesh zircon sand and a sand velocity of 90m / s in the sand conveying pipe, followed by washing treatment, to obtain pre-treated parts; S5: The preparation includes the following steps: 1) Reduce the pressure to 10 by drawing a vacuum. -3 Pa, argon gas is introduced, the temperature is raised to 300℃, titanium is used as the target material to form a titanium transition layer on the surface of the pretreated part, and then nitrogen gas is introduced for 20 minutes to obtain a titanium nitride layer. 2)(1) Weigh 0.3g of nano molybdenum disulfide, 0.1g of ferric chloride, 1g of boric acid and 20mL of anhydrous ethanol, mix them, sonicate for 15min, dry, grind, keep warm at 605ºC for 110min under nitrogen atmosphere, wash with 3mol / L hydrochloric acid, dry, and obtain boron-doped molybdenum disulfide. (2) Mix boron-doped molybdenum disulfide powder, ball mill and dry it, then put it into a graphite mold treated with boron nitride, and hot press and sinter it at 1050℃ and 36MPa for 3h in a vacuum environment, cool it and process it to obtain a boron-doped molybdenum disulfide target. In an argon atmosphere, the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target were pre-sputtered for 20 minutes using a DC power supply with a current of 300 mA. Then, by controlling the target baffle switch, the titanium nitride layer was alternately directed toward the (AlTiZrNiMo)1-xZx composite target and the boron-doped molybdenum disulfide target, and high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layers were alternately formed on the titanium nitride layer. In the (AlTiZrNiMo)1-xZx composite target, the molar ratio of Al, Ti, Zr, Ni, and Mo is 1:1:1:1:1, x is 0.03, and Z is a mixture of La and Ce in a mass ratio of 1:1. 3) Then nitrogen gas is introduced, and the flow ratio of nitrogen to argon gas is controlled at 3:4. The temperature is maintained for 90 minutes to form a nitriding modified layer on the high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer. After washing and quality inspection, a wear-resistant and scratch-resistant alloy nameplate is obtained.

[0031] Comparative Example 1: Using Example 3 as the control group, the boron-doped molybdenum disulfide target was replaced with a molybdenum disulfide target (99.9%), while other processes were normal.

[0032] Comparative Example 2: Using Example 3 as the control group, the (AlTiZrNiMo)1-xZx composite target was replaced with an AlTiZrNiMo target, wherein the molar ratio of Al, Ti, Zr, Ni and Mo was 1:1:1:1:1, and other processes were normal.

[0033] Comparative Example 3: Using Example 3 as the control group, no nitriding modified layer was prepared, and other processes were normal.

[0034] In the examples and comparative examples, the thickness of the green blank is 2 mm, the thickness of the titanium transition layer is 50 nm, and the thickness of the high-entropy alloy layer and the boron-doped molybdenum disulfide layer are both 500 nm. A high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer is alternately formed on the titanium nitride layer.

[0035] Sources of raw materials used (for illustrative purposes only): Ethylene-vinyl acetate copolymer EV150: Mitsui, Japan; Polyethylene H5520: Basel; Polyoxymethylene granules M270-44: Polyplastics Engineering Plastics, Japan; 420W powder (MIM stainless steel powder): Yingtan Longding New Material Technology Co., Ltd.; Nano molybdenum disulfide (10nm, 99.9%), zinc stearate (99%), paraffin wax (99%, density 0.82g / cm³). 3 ), ferric chloride, boric acid, ethanol, boron nitride: analytical grade, commercially available.

[0036] Performance testing: The alloy nameplates prepared in the examples and comparative examples were tested. Hardness: The test was conducted using a hardness tester, referring to GB / T 230.1, with a loading time of 5 seconds. Wear resistance: The test was conducted using a universal friction and wear tester with GCr15 as the wear material. The turntable speed was 120 r / min, the load was 20 N, the wear time was 30 min, and the sample was kept at a relative humidity of 85% and a temperature of 25℃ for 24 h. Then the wear resistance test was carried out. The weight before and after wear was measured using a balance, and the wear resistance was expressed by the weight difference. Salt spray corrosion resistance: The surface was placed in a salt spray chamber and continuously sprayed with a 5% sodium chloride aqueous solution for 24 hours at a temperature of 35°C and a pH of 7. The surface was observed for signs of rust, pitting, etc. No signs were observed, which was considered acceptable; otherwise, it was considered unacceptable. The results are shown in Table 1. Table 1

[0037] This invention provides a wear-resistant and scratch-resistant alloy nameplate and its preparation method. By injection molding of the substrate and multi-layer composite of the surface, an alloy nameplate with high hardness, corrosion resistance, wear resistance and scratch resistance is prepared, which greatly improves the durability of the alloy nameplate. In Table 1, / indicates that the item was not tested.

[0038] Comparing Example 3 with Comparative Examples 1 and 2, it can be seen that the present invention uses magnetron sputtering on the titanium nitride layer to construct a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer through alternating deposition, thereby improving its toughness. When external loads or cracks extend to this structure, the hard high-entropy alloy layer bears the main mechanical stress, providing high hardness and load-bearing capacity; while the soft boron-doped molybdenum disulfide layer in the middle effectively dissipates energy by inducing microcrack deflection and bifurcation, preventing crack penetration and propagation. The sandwich design of alternating hard and soft layers enables the coating to achieve fracture toughness and impact resistance while maintaining high hardness. At the same time, the use of boron-doped molybdenum disulfide instead of common molybdenum disulfide improves its oxidation resistance and structural density, enabling it to maintain stable wear resistance even in humid environments.

[0039] In the construction of the high-entropy alloy layer, the introduction of Ti provides chemical bonding continuity, continues the strong covalent bond between Ti and N, and improves the bonding strength between the titanium nitride layer and the high-entropy alloy layer. Zr and Ti are in the same group and can be seamlessly integrated into the interface transition region constructed by Ti to form a solid solution-reinforced interface region. Although the direct chemical bonding between Al and Ni and TiN is relatively weak, Al and Ni tend to form an ordered B2 phase, which provides high strength and high modulus for the high-entropy alloy layer. The introduction of Mo plays a role in stress regulation and high-temperature stability, while the introduction of rare earth elements plays a role in grain refinement, effectively improving the bonding strength between the titanium nitride layer and the high-entropy alloy layer.

[0040] During the deposition of boron-doped molybdenum disulfide, Al and Ti atoms on the surface of the high-entropy alloy layer react with S to form a transition layer, transforming the weak van der Waals interface into a strong chemical bond interface, effectively improving the bonding force. Zr and Mo can be solid-solution to enhance strength and thermal stability. The introduction of rare earth elements plays a role in interface purification and sulfidation, refining surface grains, increasing bonding area, and making it easier for boron-doped molybdenum disulfide to spread across the entire surface, achieving a denser and more uniform coverage and reducing interface defects.

[0041] A comparison of Example 3 and Comparative Example 3 shows that by using low-temperature plasma nitriding to modify the outermost high-entropy alloy layer, a nitride-reinforcing phase is formed on the surface without damaging the internal molybdenum disulfide lubricating layer, which significantly improves the surface hardness and scratch resistance.

[0042] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the present invention's specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.

Claims

1. A method for preparing a wear-resistant and scratch-resistant alloy nameplate, characterized in that, Includes the following steps: S1: Mix metal powder and binder and feed them into the mixture, then injection mold to obtain a green body; S2: The green blank is subjected to pre-rinsing, degreasing, and post-rinsing treatments in sequence to obtain a degreased part; S3: The degreased parts are subjected to hot degreasing, vacuum sintering, partial pressure sintering and cooling treatment in sequence to obtain sintered parts; S4: The sintered parts are subjected to dry sandblasting and washing treatment in sequence to obtain pretreated parts; S5: A titanium transition layer, a titanium nitride layer, a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer, and a nitriding modification layer are sequentially formed on the surface of the pretreated part. After washing and quality inspection, a wear-resistant and scratch-resistant alloy nameplate is obtained.

2. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 1, characterized in that, The working conditions for injection molding are as follows: mold temperature is 100-105℃, injection pressure is 25MPa, injection speed is 40mm / s, and cooling time is 5-7s; the working conditions for pre-rinsing are: temperature is 120-125℃, and time is 90-100min; the working conditions for degreasing are: oxalic acid solution is used as the degreasing solvent, temperature is 125-130℃, and time is 350-400min; the working conditions for post-rinsing are: temperature is 125-130℃, and time is 30-40min.

3. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 1, characterized in that, The working conditions for thermal debonding are: heating from 18°C ​​to 850°C at a rate of 3°C / min; the working conditions for vacuum sintering are: heating from 850°C to 1050°C at a rate of 3°C / min; the working conditions for partial pressure sintering are: pressure of 20-30 kPa, gas atmosphere of argon, temperature of 1050°C to 1340°C at a rate of 3°C / min, and then cooling down to 900°C at a rate of 3°C / min; the working conditions for cooling are: cooling down from 900°C to 20°C at a rate of 4°C / min.

4. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 1, characterized in that, The working conditions for the dry sandblasting process are as follows: the abrasive is 170-mesh zircon sand, and the abrasive velocity in the sand conveying pipe is 50-120 m / s.

5. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 1, characterized in that, In the preparation of the green body, the mass ratio of the metal powder to the binder is (90-93):(7-10); the binder, by mass percentage, consists of: 2-4% zinc stearate, 2-4% ethylene-vinyl acetate copolymer, 4-7% polyethylene, 28-31% paraffin wax, and the balance is polyoxymethylene.

6. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 1, characterized in that, Step S5 includes the following preparation steps: 1) Evacuate the vacuum, introduce argon gas, heat to 295-305℃, use titanium as the target material to form a titanium transition layer on the surface of the pretreated part, and then introduce nitrogen gas for 15-20 minutes to obtain a titanium nitride layer. 2) In an argon atmosphere, (AlTiZrNiMo) 1-x Z x The composite target and the boron-doped molybdenum disulfide target are energized and pre-sputtered for 15-20 minutes. Then, by controlling the target baffle switch, the titanium nitride layer is alternately oriented towards (AlTiZrNiMo). 1-x Z x A composite target and a boron-doped molybdenum disulfide target are used to alternately form a high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer on a titanium nitride layer. 3) Then nitrogen gas is introduced, and the flow ratio of nitrogen gas to argon gas is controlled at 3:

4. The temperature is maintained for 60-90 minutes to form a nitriding modified layer on the high-entropy alloy-boron-doped molybdenum disulfide-high-entropy alloy layer.

7. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 6, characterized in that, (AlTiZrNiMo) 1-x Z x In the composite target, the molar ratio of Al, Ti, Zr, Ni and Mo is 1:1:1:1:1, x is 0.01-0.03, and Z is one or a combination of La, Ce and Y.

8. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 6, characterized in that, The preparation of a boron-doped molybdenum disulfide target includes the following steps: (1) Weigh out nano molybdenum disulfide, ferric chloride, boric acid and anhydrous ethanol, mix them, sonicate for 10-15 min, dry, grind, keep at 595-605ºC for 110-130 min under nitrogen atmosphere, wash with hydrochloric acid, dry, and obtain boron-doped molybdenum disulfide. (2) After ball milling and drying, the boron-doped molybdenum disulfide powder is loaded into a graphite mold treated with boron nitride, and then hot-pressed and sintered in a vacuum environment. After cooling and processing, a boron-doped molybdenum disulfide target is obtained.

9. The method for preparing a wear-resistant and scratch-resistant alloy nameplate according to claim 8, characterized in that, The working conditions for hot pressing sintering are: temperature 1000-1050℃, pressure 36MPa, and time 3-4h.

10. A wear-resistant and scratch-resistant alloy nameplate, characterized in that, It is prepared by the preparation method described in any one of claims 1-9.