A method for preparing a dual-core lithium manganese iron phosphate cathode material

By using a segmented heating rate control and gas release buffer step method, a dual-core lithium manganese iron phosphate cathode material was prepared, solving the problem of particle size control of lithium manganese iron phosphate cathode material, achieving simultaneous improvement of high-density and high-rate performance, and enhancing the stability and electrochemical performance of the material.

CN123061925APending Publication Date: 2026-11-10锂源(深圳)科学研究有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611124452.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing lithium manganese iron phosphate cathode materials suffer from problems such as the mutual constraint between compaction density and rate performance, and poor batch stability in particle size control. Current technologies cannot achieve precise and controllable bimodal particle size construction, resulting in uneven material performance and battery performance degradation.

Method used

By controlling the calcination of the amorphous precursor through segmented heating rates, large and small particle size nuclei are formed. Gas release buffer steps are set in a specific temperature range to prepare a dual-nucleus lithium manganese iron phosphate cathode material. The particle size distribution is regulated by gas release kinetics, and the electrochemical performance is improved by combining it with a carbon coating layer.

Benefits of technology

It achieved an increase in compaction density to 2.4-2.5 g/cm3, a 1C discharge specific capacity ≥140 mAh/g, a capacity retention rate ≥95% after 100 1C charge-discharge cycles, and improved the synergistic optimization of material batch stability and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061925A_ABST
    Figure CN123061925A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a dual-nucleus lithium manganese iron phosphate cathode material. The method involves mixing manganese and iron sources (which release gas during calcination) with lithium, phosphorus, and water, followed by grinding and drying to obtain an amorphous precursor. The amorphous precursor is then divided into amorphous precursor A and amorphous precursor B. Amorphous precursor A and amorphous precursor B are heated to their respective calcination temperatures at different heating rates, with the difference in heating rates ≥15℃ / min, to obtain large and small-sized nuclei. Finally, the large-sized and small-sized nuclei are mixed uniformly in a specific ratio, then mixed with a carbon source and water, and finally ground, dried, and calcined. The cathode material of this invention can achieve a compaction degree of 2.4-2.5 g / cm³. 3 Furthermore, the 1C discharge specific capacity is ≥140 mAh / g, the capacity retention rate after 100 1C charge-discharge cycles is ≥95%, and the retention rate from 0.1C to 1C can reach over 89.7%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium manganese iron phosphate cathode materials, and particularly relates to a method for preparing a bicrystalline lithium manganese iron phosphate cathode material. Background Technology

[0002] Lithium manganese iron phosphate, as a novel phosphate cathode material, combines the high safety of lithium iron phosphate with the high voltage advantage of lithium manganese phosphate. It has advantages such as high energy density, good thermal stability, and low cost, and is considered one of the ideal cathode materials for next-generation power lithium-ion batteries.

[0003] Currently, its commercial application faces two major challenges: low compaction density: LMFP with a single particle size distribution has large inter-particle voids during electrode rolling, limiting its volumetric energy density. A contradiction between rate capability and compaction: Small-diameter particles offer good rate capability but low compaction density; large-diameter particles have high compaction density but long lithium-ion diffusion paths and poor rate capability. Conventional processes produce lithium manganese iron phosphate materials with a single particle size distribution. Small-diameter cathode materials have a large specific surface area and many packing voids, resulting in low compaction density; while large-diameter cathode materials have significantly extended lithium-ion transport paths, leading to a significant decrease in rate capability and fast-charging performance. Therefore, existing single-particle-size systems cannot simultaneously achieve high compaction density and high-rate electrochemical performance.

[0004] Currently, to improve particle size distribution and balance material performance, the industry uses physical blending of two finished lithium manganese iron phosphate materials with different particle sizes, relying on external force doping to achieve a mix of coarse and fine particles. However, this post-physical gradation method has many inherent defects: poor powder mixing uniformity, coarse and fine particles are prone to agglomeration and segregation, resulting in poor batch consistency and stability of materials; at the same time, the loose bonding at the interface of heterogeneous particles will significantly increase the electrode interface impedance, hindering the rapid transport of lithium ions, ultimately causing the battery cycle stability and rate performance to degrade, failing to solve the performance balance problem at its root.

[0005] Some technologies have attempted to control the particle size of materials by adjusting a single calcination process parameter. However, this method has an unclear particle size control mechanism and a very narrow process window. Fine-tuning the parameters can easily lead to abnormal grain growth and poor particle size uniformity. It is difficult to accurately construct a bimodal particle size structure with significant differences in particle size and uniform distribution within the same reaction system, and it is impossible to achieve synergistic optimization of compaction density and electrochemical performance.

[0006] In summary, existing lithium manganese iron phosphate preparation technologies are all post-processed and passive particle size control methods, which cannot achieve precise and controllable bimodal particle size construction from the source of precursors. They always face the technical challenges of mutual constraints between compaction density and rate performance, as well as poor batch stability. Summary of the Invention

[0007] Purpose of the invention: This invention provides a method for preparing a dual-nucleation lithium manganese iron phosphate cathode material, which achieves precise and controllable dual-peak particle size construction from the perspective of crystal nucleation, effectively solving the technical problems of mutual restriction between compaction density and rate performance and poor batch stability.

[0008] Technical solution: The present invention provides a method for preparing a dual-core lithium manganese iron phosphate cathode material, characterized by comprising the following steps:

[0009] (1) Amorphous precursor is obtained by mixing manganese source, iron source, lithium source, phosphorus source and water, grinding and drying; the manganese source and iron source are both manganese source and iron source that can release gas during calcination.

[0010] (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined separately under an inert atmosphere, wherein:

[0011] The calcination conditions for amorphous precursor A are as follows: heat to 500-700℃ at a first heating rate of 1-5℃ / min and hold for 4-15 hours to obtain large-size crystal nuclei.

[0012] The calcination conditions for amorphous precursor B are as follows: heat to 500-700℃ at a second heating rate of 15-25℃ / min and hold for 4-15 hours to obtain small-diameter crystal nuclei.

[0013] Furthermore, the difference between the second heating rate and the first heating rate is ≥15℃ / min;

[0014] (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei evenly at a mass ratio of x:(1-x) to obtain a mixture, wherein 0.15<x<0.35;

[0015] (4) Mix the mixed materials, carbon source and water, grind, dry and calcine to obtain a double-core lithium manganese iron phosphate cathode material.

[0016] Furthermore, in step (1) of the preparation method of the present invention, the manganese source is at least selected from manganese carbonate, manganese oxalate, ferric manganese carbonate, and ferric manganese oxalate; the iron source is at least selected from ferrous carbonate, ferrous oxalate, ferric manganese carbonate, and ferric manganese oxalate. More preferably, the manganese source is selected from manganese oxalate and / or ferric manganese oxalate, and the iron source is selected from ferrous oxalate and / or ferric manganese oxalate.

[0017] Furthermore, in step (2) of the preparation method of the present invention, both the amorphous precursor A and the amorphous precursor B are provided with a buffer step for gas release during the heat preservation calcination process, and the buffer step is a heat preservation reaction at a temperature range of 280-380℃ for 0.5-2h.

[0018] Furthermore, in step (1) of the preparation method of the present invention, the lithium source is lithium carbonate or mixed lithium; wherein the mixed lithium is a mixture of lithium carbonate and lithium hydroxide, and the molar number of lithium hydroxide is 5-30% of the molar number of mixed lithium.

[0019] Furthermore, in step (1) of the preparation method of the present invention, the phosphorus source is at least selected from one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or phosphoric acid.

[0020] Furthermore, in step (1) of the preparation method of the present invention, the molar ratio of Li, Mn, Fe and P in the lithium source, manganese source, iron source and phosphorus source is (1-1.05):(0.5-0.8):(0.2-0.5):1.

[0021] Furthermore, in step (4) of the preparation method of the present invention, the carbon source is selected from at least one of glucose, sucrose, polyethylene glycol, and citric acid, and the mass of the carbon source added is 8-15% of the mass of the mixture.

[0022] Furthermore, in step (4) of the preparation method of the present invention, the calcination temperature is 700-800℃ and the calcination time is 10-25h.

[0023] Beneficial Effects: Compared with existing technologies, the significant advantage of this invention is that the core of the preparation method lies in the gas release-mediated "entropy-enthalpy competition" particle size control, that is, using gas release kinetics to mediate nucleation density, using slow heating to form large crystal nuclei and using rapid heating to form small crystal nuclei, thereby preparing a bicrystalline lithium manganese iron phosphate cathode material. Furthermore, by precisely controlling the gas release rate through buffer steps, the electrochemical performance is synergistically improved, achieving a simultaneous improvement in compaction density and rate performance. Specifically:

[0024] (1) Significantly improved compaction density: With the help of bimodal gradation (large particles form the skeleton and small particles fill the voids), the compaction density can be increased from the conventional single-peak density of 2.32 g / cm³. 3 Increased to 2.4-2.5 g / cm³ 3 .

[0025] (2) Synergistic optimization of electrochemical performance: Small particles provide high specific surface area and short lithium-ion diffusion path, ensuring excellent rate performance (1C discharge specific capacity ≥140 mAh / g); large particles and complete carbon coating reduce side reaction activity, and the retention rate from 0.1C to 1C can reach more than 89.7%, and the capacity retention rate after 100 charge-discharge cycles at 1C is ≥95%; the buffer step precisely controls the gas release rate, which can effectively adjust the concentration of defects inside the crystal nucleus (such as cation mixing and oxygen vacancies), providing a means for fine tuning of electrochemical performance.

[0026] (3) High stability between different batches: The large and small crystal nuclei originate from the same precursor. The particle size is controlled only by the heating rate, which fundamentally overcomes the surface chemical potential difference and interface polarization problem that exists in the mechanical mixing of the two materials.

[0027] Furthermore, the gas release step introduced by this preparation method significantly widens the process window of the rapid heating path, making it easy to scale up industrially; the method is based on gas release kinetics control and has high universality. Attached Figure Description

[0028] Figure 1 SEM image of the lithium manganese iron phosphate material prepared in Example 2;

[0029] Figure 2 The particle size distribution curve of the lithium manganese iron phosphate material prepared in Example 2 is shown.

[0030] Figure 3 SEM image of lithium manganese iron phosphate material prepared in Example 3;

[0031] Figure 4 The particle size distribution curve of the lithium manganese iron phosphate material prepared in Example 3 is shown.

[0032] Figure 5 SEM image of lithium manganese iron phosphate material prepared in Example 4;

[0033] Figure 6 The particle size distribution curve of the lithium manganese iron phosphate material prepared in Example 4 is shown.

[0034] Figure 7 SEM image of lithium manganese iron phosphate material prepared in Example 5;

[0035] Figure 8 The particle size distribution curve of the lithium manganese iron phosphate material prepared in Example 5 is shown.

[0036] Figure 9 SEM image of lithium manganese iron phosphate material prepared in Comparative Example 1;

[0037] Figure 10 The particle size distribution curve of the lithium manganese iron phosphate material prepared for Comparative Example 1 is shown. Detailed Implementation

[0038] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be noted that all raw materials used in the present invention are commercially available. It should also be noted that the amount of deionized water added in the following embodiments and comparative examples of the present invention is sufficient to prepare a slurry.

[0039] Example 1

[0040] Example 1 uses an oxalate system, and the preparation method of its bicrystalline lithium manganese iron phosphate cathode material includes the following steps:

[0041] (1) Weigh manganese oxalate, ferrous oxalate, lithium carbonate and ammonium dihydrogen phosphate according to the stoichiometric ratio Li:Mn:Fe:P=1.03:0.7:0.3:1, add deionized water, grind in a sand mill until the slurry D50=500nm, and spray dry to obtain amorphous precursor powder.

[0042] (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined under an inert atmosphere.

[0043] (2.1) Preparation of large-size crystal nuclei: Amorphous precursor A was placed in a tube furnace, nitrogen gas was introduced, and the temperature was slowly increased to 650℃ at the first heating rate of 3℃ / min and kept at the temperature for 10h. After cooling, large-size crystal nuclei were obtained.

[0044] (2.2) Preparation of small-size crystal nuclei: Amorphous precursor B was placed in a tube furnace, nitrogen was introduced, and the temperature was rapidly increased to 650℃ at a second heating rate of 20℃ / min and held for 10h. After cooling, small-size crystal nuclei were obtained.

[0045] (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei in a mass ratio of 3:7 (i.e., x=0.3) and add them to a mixing tank. Mix at low speed for 1 hour to obtain a mixture.

[0046] (4) Add glucose and deionized water at a mass of 12 wt% to the mixture, mix, grind and dry, and then heat to 750℃ at 5℃ / min under nitrogen atmosphere and keep it at the temperature for 10h. After natural cooling, crush and sieve, the double-crystal core particle size lithium manganese iron phosphate cathode material is obtained.

[0047] Example 2

[0048] Example 2 describes a method for preparing a bicrystalline lithium manganese iron phosphate cathode material using an oxalate system and a gas buffer step, comprising the following steps:

[0049] (1) Weigh manganese oxalate, ferrous oxalate, lithium carbonate and ammonium dihydrogen phosphate according to the stoichiometric ratio Li:Mn:Fe:P=1.03:0.7:0.3:1, add deionized water, grind in a sand mill until the slurry D50=500nm, and spray dry to obtain amorphous precursor powder.

[0050] (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined under an inert atmosphere.

[0051] (2.1) Preparation of large-size crystal nuclei: Amorphous precursor A was placed in a tube furnace, nitrogen was introduced, and the temperature was slowly increased to the buffer step at the first heating rate of 3℃ / min. The reaction was held at 320℃ for 1h. Then the temperature was increased to 650℃ at the first heating rate of 3℃ / min and held for 10h. The large-size crystal nuclei were obtained by cooling.

[0052] (2.2) Preparation of small-size crystal nuclei: Amorphous precursor B was placed in a tube furnace, nitrogen was introduced, and the temperature was rapidly increased to the buffer step at a second heating rate of 20℃ / min. The reaction was held at 320℃ for 1h. Then the temperature was increased to 650℃ at a second heating rate of 20℃ / min and held for 10h. The small-size crystal nuclei were obtained by cooling.

[0053] (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei in a mass ratio of 3:7 (i.e., x=0.3) and add them to a mixing tank. Mix at low speed for 1 hour to obtain a mixture.

[0054] (4) Add glucose and deionized water at a mass of 12 wt% to the mixture, mix, grind and dry, and then heat to 750℃ at 5℃ / min under nitrogen atmosphere and keep it at the temperature for 10h. After natural cooling, crush and sieve, the double-crystal core particle size lithium manganese iron phosphate cathode material is obtained.

[0055] Example 3

[0056] The preparation method of the dual-size nucleus lithium manganese iron phosphate cathode material in Example 3, step (1) uses a carbonate system + mixed lithium, specifically including the following steps:

[0057] (1) Manganese carbonate, ferrous carbonate, lithium carbonate, lithium hydroxide and ammonium dihydrogen phosphate were weighed according to the stoichiometric ratio Li:Mn:Fe:P=1.03:0.7:0.3:1, wherein the molar number of lithium hydroxide was 10% of the molar number of mixed lithium. Deionized water was added, and the mixture was ground in a sand mill until the slurry D50=500nm. The mixture was then spray-dried to obtain amorphous precursor powder.

[0058] (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined under an inert atmosphere.

[0059] (2.1) Preparation of large-size crystal nuclei: Amorphous precursor A was placed in a tube furnace, nitrogen gas was introduced, and the temperature was slowly increased to the buffer step at the first heating rate of 2℃ / min. The reaction was held at 300℃ for 1.5h. Then the temperature was increased to 650℃ at the first heating rate of 2℃ / min and held for 10h. The large-size crystal nuclei were obtained by cooling.

[0060] (2.2) Preparation of small-size crystal nuclei: Amorphous precursor B was placed in a tube furnace, nitrogen was introduced, and the temperature was rapidly increased to the buffer step at a second heating rate of 18℃ / min. The reaction was held at 300℃ for 1.5h. Then the temperature was increased to 650℃ at a second heating rate of 18℃ / min and held for 12h. The small-size crystal nuclei were obtained by cooling.

[0061] (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei in a mass ratio of 1:3 (i.e., x=0.25) and add them to a mixing tank. Mix at low speed for 1 hour to obtain a mixture.

[0062] (4) Add 10 wt% of sucrose and deionized water to the mixture, mix, grind and dry, and then heat to 750℃ at 5℃ / min under nitrogen atmosphere and keep it at that temperature for 20h. After natural cooling, crush and sieve, the double-crystal core particle size lithium manganese iron phosphate cathode material is obtained.

[0063] Example 4

[0064] The preparation method of the dual-size nucleus lithium manganese iron phosphate cathode material in Example 4 is basically the same as that in Example 3. The main difference is that in step (1), a raw material system of manganese carbonate + ferrous carbonate + lithium carbonate + ammonium dihydrogen phosphate is used to obtain the dual-size nucleus lithium manganese iron phosphate cathode material.

[0065] Example 5

[0066] Example 5 describes a method for preparing a bicrystalline lithium manganese iron phosphate cathode material using an oxalate system and a gas buffer step, comprising the following steps:

[0067] (1) Weigh manganese oxalate, ferrous oxalate, lithium carbonate and ammonium dihydrogen phosphate according to the stoichiometric ratio Li:Mn:Fe:P=1.03:0.7:0.3:1, add deionized water, grind in a sand mill until the slurry D50=500nm, and spray dry to obtain amorphous precursor powder.

[0068] (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined under an inert atmosphere.

[0069] (2.1) Preparation of large-size crystal nuclei: Amorphous precursor A was placed in a tube furnace, nitrogen gas was introduced, and the temperature was slowly increased to the buffer step at the first heating rate of 5℃ / min. The reaction was held at 350℃ for 0.5h. Then the temperature was increased to 700℃ at the first heating rate of 5℃ / min and held for 4h. The reaction was then cooled to obtain large-size crystal nuclei.

[0070] (2.2) Preparation of small-size crystal nuclei: Amorphous precursor B was placed in a tube furnace, nitrogen gas was introduced, and the temperature was rapidly increased to the buffer step at a second heating rate of 25℃ / min. The reaction was held at 350℃ for 0.5h. Then the temperature was increased to 700℃ at a second heating rate of 25℃ / min and held for 4h. The small-size crystal nuclei were obtained by cooling.

[0071] (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei at a mass ratio of 1:4 (i.e., x=0.2) in a mixing tank and mix at low speed for 1 hour to obtain a mixture.

[0072] (4) Add 8 wt% glucose and deionized water to the mixture, mix, grind and dry, and then heat to 800℃ at 5℃ / min and keep it for 20h under nitrogen atmosphere. After natural cooling, crush and sieve, the double-core lithium manganese iron phosphate cathode material is obtained.

[0073] Comparative Example 1

[0074] The preparation steps are the same as in Example 2, but step (2.1) uses a heating rate of 5℃ / min and step (2.2) uses 10℃ / min, with a difference of only 5℃ / min.

[0075] Comparative Example 2

[0076] The preparation steps are the same as in Example 2, but in step (3), the mixing mass ratio of large-diameter crystal nuclei and small-diameter crystal nuclei is changed to x=0.5, that is, large and small crystal nuclei are mixed in equal amounts to obtain LMFP.

[0077] Performance Testing - Electrochemical Performance

[0078] The compaction density of lithium manganese iron phosphate cathode material was tested according to GBT30835-2014 using a PRCD1100 powder compaction testing device; the results are shown in Table 1.

[0079] The lithium manganese iron phosphate cathode materials obtained in Examples 1 to 5 and Comparative Examples 1 and 2 were used to prepare coin cells and their electrochemical performance was evaluated. The lithium manganese iron phosphate cathode material, Super P (conductive carbon black), and PVDF were uniformly mixed in an NMP solution at a ratio of 90:5:5 to obtain a slurry. The slurry was applied to bright aluminum foil by hand and then dried at 100°C. After the NMP had completely evaporated, the electrode was cut into electrode sheets with a diameter of 13 mm. The electrode sheets were then dried overnight at 105°C in a vacuum oven. After weighing, the electrode sheets were quickly transferred to a glove box. Lithium metal was used as the counter electrode, Celgard 2400 as the separator, and the electrolyte was 1 mol / L. The assembled battery was prepared by dissolving LiPF6 in a mixed solvent of EC / DMC / EMC (volume ratio 1:1:1). Electrochemical performance was tested using the Xinwei testing system, employing constant current-constant voltage charging (CC-CV) and constant current discharging (DC) methods to analyze the charge and discharge behavior of the coin cell. The test voltage range was 2.0-4.35 V.

[0080] Table 1. Cathode Material Performance Data

[0081]

[0082] As shown in Table 1, the compaction density of the lithium manganese iron phosphate cathode material prepared in Examples 1 to 5 of this invention can be increased to 2.4-2.5 g / cc. As shown in Examples 2 to 5, the 1C discharge specific capacity is ≥140 mAh / g, and the capacity retention rate after 100 1C charge-discharge cycles is ≥95%.

[0083] Combining Examples 1 and 2, it can be seen that the compaction density of Example 1 is slightly lower than that of Example 2 (2.45 g / cm³). 3 vs. 2.47 g / cm 3 Example 1 lacked a gas buffer step at 280-380℃, resulting in a decrease in 1C discharge specific capacity and 0.1C to 1C retention rate. The reason for this is that the absence of the gas buffer step allows CO2 to burst and impact the crystal lattice during rapid heating, creating high-density defects such as closed pores and dislocations. These defects become ion transport traps at high rates, causing the 1C capacity to plummet to 135 mAh / g and the 0.1C to 1C retention rate to only 87.1%. In Example 2, the introduction of a buffer step during the cathode material preparation process allows for a stable release of gas before the critical nucleation period, significantly reducing the lattice defect density and achieving a 0.1C to 1C retention rate of 91.8%, demonstrating a significant rate advantage under the same compaction conditions.

[0084] Performance testing - structural characterization

[0085] The morphology and particle size distribution of the lithium manganese iron phosphate cathode materials prepared in Examples 2 to 5, Comparative Examples 1 and 2 were characterized, and the results are as follows: Figures 1 to 10 As shown in Table 2, the particle size distribution data of lithium manganese iron phosphate cathode material is as follows.

[0086] Table 2. Particle size distribution of lithium manganese iron phosphate cathode materials in Examples 2-5 and Comparative Example 1

[0087]

[0088] Note: The D50 value may fluctuate by ±50nm (this is due to differences in raw materials, process conditions and measurement, and is within the normal range of fluctuation).

[0089] Combination Figure 1 and Figure 2 It can be seen that during the preparation of the cathode material in Example 2 of the present invention, a temperature difference of 17℃ / min was used to obtain large crystal nucleus particle sizes (e.g., Figure 1 (as shown in the red box) and small crystal nucleus size (such as...) Figure 1 (Green box) to construct a bimodal gradation. Small particles fill the gaps between large particles in the skeleton, increasing the compaction density to 2.47 g / cm³. 3 Simultaneously, the filling particles themselves construct parallel short-range lithium-ion channels, allowing the dense electrode to maintain efficient mass transfer. Therefore, the 1C capacity of 145 mAh / g remains essentially the same, achieving lossless rate capability under high pressure. In contrast, the comparative example 1, with a heating rate difference of 5℃, yielded a cathode material exhibiting a single-peak distribution, such as... Figure 9-10 As shown, the particles follow the packing of equal-diameter spheres, resulting in high porosity and a compacted density of only 2.32 g / cm³. 3 .

[0090] Comparative analysis of the data from Example 2 and Comparative Example 2 shows that the proportion of large crystal nuclei in Comparative Example 2 exceeds the standard (x=0.5), although the small particles filling the interstitial spaces contribute 2.45 g / cm³. 3 High-pressure compaction is achieved, but solid-phase diffusion presents a problem where a large number of lithium ions cannot penetrate the large crystal grains of hundreds of nanometers. That is, during charging and discharging, the diffusion of lithium ions is hindered due to the excessive distance, increasing battery polarization and leading to a decrease in capacity; the 0.1C capacity is only 145 mAh / g, and the 1C capacity is even lower at only 128 mAh / g. Example 2 precisely controls the proportion of large crystal nuclei at 0.3 and creates a strong reducing atmosphere using CO generated from oxalate decomposition to suppress Mn. 2+ Oxidation and Fe antisite defects significantly improve lattice purity, achieving a purity of 2.47 g / cm³. 3 Compaction achieves a high reversible capacity of 158 mAh / g.

[0091] Based on the above data, further analysis of the mechanism reveals that when preparing the cathode materials of Examples 2 to 5 of this invention, different segmented heating rates were used, namely, slow heating at 1-5℃ / min and rapid heating at 15-25℃ / min, respectively, to carry out the calcination reaction, ensuring that the difference in heating rate between the two was ≥15℃ / min. This ensured that the particle size distribution of large and small crystal nuclei did not overlap, achieving an ideal bimodal gradation, and ultimately achieving a synergistic improvement in compaction density and rate performance. Specifically, as follows... Figure 1-8 As shown, the obtained cathode material exhibits a particle size distribution, and the particle size distribution curve clearly shows two peaks, one high and one low.

[0092] Specifically, under a slow heating rate of 1-5℃ / min, the decomposition reaction of carbonates / oxalates proceeds smoothly within a relatively wide low-temperature window. The system exhibits low gas partial pressure and low supersaturation, resulting in a high nucleation barrier and the formation of only a small number of stable nuclei. Upon reaching the subsequent reaction temperature, the dissociated Mn, Fe, P, Li, and other species tend to slowly deposit on the surface of existing nuclei via thermodynamic diffusion (i.e., enthalpy-driven epitaxial growth). The grains gradually grow larger with fewer internal defects, ultimately forming large-diameter nuclei.

[0093] Under rapid heating at 15-25℃ / min, the precursor is quickly pushed into the decomposition temperature zone. Carbonates / oxalates and ammonium salts decompose rapidly in a very short time, releasing gases such as CO2 explosively. This not only generates a strong micro-area stirring effect, promoting compositional homogenization, but more importantly, it instantly creates extremely high local supersaturation and a high-entropy state (ΔS increases sharply), leading to a significant reduction in the nucleation barrier and triggering exponential explosive nucleation. A massive number of tiny crystal nuclei are generated in a short time, and these nuclei compete for limited diffusing material, ensuring that each nucleus ultimately grows to a relatively small size.

[0094] Furthermore, a heat-insulating step is incorporated into the 280-380℃ temperature range where CO2 and NH3 are concentrated, which is crucial for addressing lattice defects caused by rapid heating. This temperature range precisely corresponds to the gas release from carbonate / oxalate and ammonium phosphate salts. The heat-insulating treatment allows some gas to escape smoothly, preserving the high supersaturation driving force required for subsequent entry into the high-temperature nucleation region while avoiding lattice pores, microcracks, and abnormal strain caused by instantaneous gas impact. By precisely controlling the gas release rate through the buffer step, the concentration of defects inside the crystal nucleus (such as cation mixing and oxygen vacancies) can be effectively adjusted, providing a means for fine-tuning electrochemical performance.

[0095] Finally, carbon coating and high-temperature calcination are performed. However, carbon coating does not only provide a conductive layer. The amorphous carbon layer can act as a physical barrier when sintered at 700-800℃, effectively inhibiting surface diffusion between large and small crystal nuclei and the fusion of sintering necks, thereby maintaining the bimodal distribution microstructure constructed in step (3). At the same time, the carbon reducing atmosphere can moderately induce Mn / Fe interdiffusion in the lattice, eliminating nanoscale chemical heterogeneity and obtaining a thermodynamically stable homogeneous solid solution.

[0096] In addition to the above embodiments, it should be noted that the process and parameter conditions defined by the present invention can achieve the technical effects claimed above, and therefore no further experimental verification is required.

Claims

1. A method for preparing a bicrystalline lithium manganese iron phosphate cathode material, characterized in that, Includes the following steps: (1) Amorphous precursor is obtained by mixing manganese source, iron source, lithium source, phosphorus source and water, grinding and drying; the manganese source and iron source are both manganese source and iron source that can release gas during calcination. (2) The amorphous precursor is divided into amorphous precursor A and amorphous precursor B, and calcined separately under an inert atmosphere, wherein: The calcination conditions for amorphous precursor A are as follows: heat to 500-700℃ at a first heating rate of 1-5℃ / min and hold for 4-15 hours to obtain large-size crystal nuclei. The calcination conditions for amorphous precursor B are as follows: heat to 500-700℃ at a second heating rate of 15-25℃ / min and hold for 4-15 hours to obtain small-diameter crystal nuclei. Furthermore, the difference between the second heating rate and the first heating rate is ≥15℃ / min; (3) Mix large-diameter crystal nuclei and small-diameter crystal nuclei evenly at a mass ratio of x:(1-x) to obtain a mixture, wherein 0.15<x<0.35; (4) Mix the mixed materials, carbon source and water, grind, dry and calcine to obtain a double-core lithium manganese iron phosphate cathode material.

2. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (1), the manganese source is selected from at least one of manganese carbonate, manganese oxalate, ferric manganese carbonate, and ferric manganese oxalate; the iron source is selected from at least one of ferrous carbonate, ferrous oxalate, ferric manganese carbonate, and ferric manganese oxalate.

3. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 2, characterized in that, The manganese source is selected from manganese oxalate and / or ferric manganese oxalate, and the iron source is selected from ferrous oxalate and / or ferric manganese oxalate.

4. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (2), both the amorphous precursor A and the amorphous precursor B are provided with a buffer step for gas release during the heat preservation calcination process, and the buffer step is a heat preservation reaction at a temperature range of 280-380℃ for 0.5-2h.

5. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (1), the lithium source is lithium carbonate or mixed lithium; wherein the mixed lithium is a mixture of lithium carbonate and lithium hydroxide, and the molar number of lithium hydroxide is 5-30% of the molar number of mixed lithium.

6. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (1), the phosphorus source is selected from at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or phosphoric acid.

7. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (1), the molar ratio of Li, Mn, Fe and P in the lithium source, manganese source, iron source and phosphorus source is (1-1.05):(0.5-0.8):(0.2-0.5):

1.

8. The method for preparing the bicrystalline core-size lithium manganese iron phosphate cathode material according to claim 1, characterized in that, In step (4), the carbon source is selected from at least one of glucose, sucrose, polyethylene glycol, and citric acid, and the mass of the carbon source added is 8-15% of the mass of the mixture.