A method for preparing battery-grade lithium sulfate using waste battery black powder
By combining defluorinating agents and carbothermal reduction with multi-stage impurity removal and evaporation crystallization, the problem of removing impurities from waste battery black powder was solved, and high-purity lithium sulfate was prepared, thus solving the problems of high impurity load and substandard purity in existing technologies.
Patent Information
- Application Number
- CN202611523629.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies cannot completely remove fluorides and conductive carbon impurities from waste battery black powder, resulting in a high impurity load during lithium recycling. Fine iron phosphate colloids pollute the refining process, lithium sulfate purity does not meet standards, and mixing different types of batteries can easily cause transition metal co-dissolution and generate a large amount of waste acid.
A defluorinating agent is used to deeply remove fluorides and conductive carbon impurities. Lithium is then directionally converted into water-soluble lithium salts through carbothermic reduction. This process is combined with multi-stage deep impurity removal and evaporation crystallization. A dispersant is added to prevent crystal distortion, resulting in battery-grade lithium sulfate.
It significantly reduces the fluorine and carbon content in the material, improves the lithium selective water leaching rate, reduces the subsequent impurity removal load, realizes the preparation of high-purity lithium sulfate, avoids crystal distortion and impurity encapsulation, and meets battery-grade requirements.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application belongs to the field of resource recycling and reuse technology, and relates to a method for preparing battery-grade lithium sulfate using waste battery black powder. Background Technology
[0002] As one of the most critical components of new energy vehicles, power batteries generate a large number of waste batteries with the rapid development of the new energy field. Improper disposal of these waste batteries not only pollutes the environment but also wastes resources. Currently, the conventional recycling process for waste batteries mainly includes the following steps: First, meticulous classification according to battery type; next, physical disassembly to separate the different battery components; then, high-temperature calcination and crushing / sorting to extract valuable materials; and finally, recovery and extraction of the electrolyte.
[0003] However, fluorides (such as PVDF), conductive carbon, and ferric phosphate colloids in waste battery black powder are difficult to completely remove, resulting in a high impurity load in the leachate after carbothermic lithium extraction. Fine ferric phosphate colloids also contaminate the refining process, and conventional impurity removal methods are insufficient to reduce the total impurity content to battery-grade requirements. Furthermore, during lithium recovery, the high supersaturation and residual fluorine and carbon during lithium sulfate evaporation and crystallization easily trigger secondary nucleation, microcrystal agglomeration, and impurity encapsulation, leading to crystal distortion and substandard product purity. In addition, direct wet acid leaching of mixed battery black powders of different types can easily cause transition metal co-dissolution and generate large amounts of waste acid.
[0004] Based on the above research, there is a need to provide a method for preparing battery-grade lithium sulfate using waste battery black powder, which can produce high-purity lithium sulfate products. Summary of the Invention
[0005] The purpose of this application is to provide a method for preparing battery-grade lithium sulfate using waste battery black powder. The method significantly reduces the fluorine and carbon content through decarbonization and defluorination, and then uses carbothermal reduction to directionally convert lithium into water-soluble lithium salt, while the transition metal remains as an insoluble phase. After four stages of deep impurity removal and the addition of a dispersant for evaporation and crystallization, battery-grade lithium sulfate can be obtained.
[0006] To achieve the purpose of this application, the following technical solution is adopted:
[0007] This application provides a method for preparing battery-grade lithium sulfate using waste battery black powder, the method comprising the following steps:
[0008] (1) Mix the mixed battery black powder with the defluorinated carbon agent and heat and burn it to obtain defluorinated carbon black powder;
[0009] (2) The defluorinated carbon black powder, reducing agent and phosphorus phase regulator described in step (1) are mixed and calcined to obtain calcined material. The calcined material is then subjected to water immersion, solid-liquid separation and filtration purification to obtain lithium-containing leachate.
[0010] (3) The lithium-containing leachate obtained in step (2) is subjected to dephosphorization treatment, and then sulfuric acid is added to the dephosphorized lithium-containing solution to obtain crude lithium sulfate solution;
[0011] The crude lithium sulfate solution was subjected to sequential removal of iron and aluminum, calcium and magnesium, metal residues and organic impurities to obtain a refined lithium sulfate stock solution.
[0012] (4) The refined lithium sulfate stock solution described in step (3) is mixed with a dispersant and then evaporated and crystallized. Then, solid-liquid separation, washing, drying and sieving are performed to obtain battery-grade lithium sulfate.
[0013] This application first employs a defluorinating agent to deeply remove carbon and fluorine from the mixed battery black powder, thoroughly removing fluorides (such as PVDF) and conductive carbon impurities, significantly reducing the fluorine and carbon content in the material, and minimizing LiF formation and lithium loss. Then, the defluorinated black powder, reducing agent, and phosphorus phase regulator are mixed and calcined to complete phase reconstruction, reducing nickel, cobalt, manganese, iron, and other metal oxides in the black powder to elemental solid phases, while lithium is directionally converted into water-soluble lithium salts. Therefore, carbothermic reduction calcination results in a high lithium selective water leaching rate, enabling the directional conversion of lithium into water-soluble lithium salts while transition metals remain as insoluble phases. Finally, the calcined material is leached with water to achieve selective preferential dissolution of lithium, while heavy metals, phosphorus, and graphite residues are retained. After solid-liquid separation... A low-impurity crude lithium solution is obtained. The crude lithium solution is then filtered and purified to obtain a high-purity lithium-ion stock solution with low impurities, which significantly reduces the subsequent impurity removal load. Next, dephosphorization treatment is performed to reduce the content of soluble phosphate in the solution. Then, sulfuric acid is added to the lithium-containing solution after dephosphorization to convert lithium carbonate, lithium hydroxide, lithium oxide and / or other alkaline lithium-containing components into lithium sulfate. Then, multi-stage coupled deep impurity removal and refining are performed to remove iron and aluminum, calcium and magnesium, metal residues and organic impurities, to obtain a refined lithium sulfate stock solution. Finally, a dispersant is added to the refined lithium sulfate stock solution to avoid crystal distortion and microcrystal agglomeration that encapsulates impurities. Therefore, this application obtains battery-grade lithium sulfate product through the cooperation of multiple steps.
[0014] In some embodiments, the defluorinating agent in step (1) includes sodium p-toluenesulfonate.
[0015] This application uses sodium p-toluenesulfonate as a defluorinating agent, which can promote the complete removal of PVDF and carbon impurities.
[0016] In some embodiments, the mass of the defluorinated carbon agent in step (1) is 0.2wt% to 1wt% of the mass of the mixed battery black powder, for example, it can be 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1.0wt%, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0017] In some embodiments, the heating and combustion temperature in step (1) is 550°C to 650°C, for example, 550°C, 570°C, 600°C, 620°C or 650°C; the time is 0.5h to 1.5h, for example, 0.5h, 0.75h, 1h, 1.25h or 1.5h, but not limited to the listed values, other unlisted values within the range are also applicable.
[0018] The heating and combustion described in this application takes place in a fluidized bed combustion chamber. The fluidized bed heating system and air pump are started to heat the air at a constant temperature and pump hot air for continuous combustion.
[0019] In some embodiments, the mixed battery black powder in step (1) includes lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder.
[0020] This application obtains primary pre-treated black powder by fully discharging waste batteries, then shearing, crushing, peeling off the electrodes, ultra-fine grinding, and demagnetizing them. Different types of primary pre-treated black powder are then mixed to obtain mixed battery black powder.
[0021] This application does not specify a particular mass ratio for the lithium iron phosphate battery black powder, ternary lithium battery black powder, and lithium cobalt oxide battery black powder; those skilled in the art can make a reasonable selection based on their needs. Preferably, the mass ratio of the lithium iron phosphate battery black powder, ternary lithium battery black powder, and lithium cobalt oxide battery black powder is 1:(0.5~2):(0.5~2), for example, it can be 1:1:1, 1:0.5:2, 1:2:0.5, or 1:2:2, but is not limited to the listed values; other unlisted values within the range are also applicable.
[0022] In some embodiments, the calcination in step (2) is carried out under an inert atmosphere, and the calcination temperature is 750℃~850℃, for example, it can be 750℃, 760℃, 770℃, 780℃, 790℃, 800℃, 810℃, 820℃, 830℃, 840℃ or 850℃; the time is 2.5h~3h, for example, it can be 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3.0h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0023] In some embodiments, the reducing agent in step (2) includes any one or a combination of at least two of graphite powder, carbon black, coke powder or biochar.
[0024] In some embodiments, the amount of reducing agent added in step (2) is 5wt% to 15wt% of the mass of the defluorinated carbon black powder, for example, it can be 5wt%, 7.5wt%, 10wt%, 12.5wt% or 15wt%, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0025] In some embodiments, the phosphorus phase regulator in step (2) includes sodium carbonate.
[0026] In some embodiments, the molar ratio of the phosphorus phase regulator to the total phosphorus in the mixed battery black powder in step (2) is (0.8~1.5):1 (preferably (0.8~1.1):1), for example, 0.8:1, 1:1, 1.2:1, 1.4:1 or 1.5:1, but not limited to the listed values. Other unlisted values within the range are also applicable.
[0027] In some embodiments, the water immersion temperature in step (2) is 60°C to 70°C, for example, 60°C, 62°C, 64°C, 65°C, 66°C, 68°C, or 70°C; the time is 1.5h to 2h, for example, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, or 2.0h, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0028] In some embodiments, the solid-liquid mass ratio of the water immersion in step (2) is (3~5):1, for example, it can be 3:1, 3.5:1, 4:1, 4.5:1 or 5:1, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0029] In some embodiments, the filter membrane used for filtration and purification in step (2) is a modified polyether ether ketone-polyarylsulfone composite membrane.
[0030] The modified polyetheretherketone-polyarylsulfone composite membrane described in this application is prepared by polyetheretherketone sulfonation modification, imidazole functionalization grafting, polyarylsulfone quaternization modification, and zinc acetate inorganic doping composite. It has the characteristics of accurately retaining metal colloids and iron phosphate microparticles, anti-fouling, and high lithium permeability. It can accurately retain copper and aluminum microparticles and iron phosphate fine colloids, significantly reducing the subsequent impurity removal load and avoiding crystal encapsulation caused by iron phosphate passing through the filter.
[0031] In some embodiments, the dephosphorization treatment in step (3) includes adding lime milk to adjust the pH of the system to 9-10, for example, 9, 9.2, 9.4, 9.6, 9.8 or 10, but not limited to the listed values. Other unlisted values within the range are also applicable.
[0032] In some embodiments, in step (3), sulfuric acid is added to bring the pH of the solution to 4.5-5.5, for example, 4.5, 4.7, 4.9, 5.1, 5.3 or 5.5, and then a flocculant is used to further remove iron and aluminum.
[0033] In some embodiments, a sodium-free organic flocculant is used for the removal of iron and aluminum in step (3), wherein the sodium-free organic flocculant includes nonionic polyacrylamide and / or polydimethyldiallyl ammonium chloride.
[0034] In some embodiments, ammonium fluoride is used to remove calcium and magnesium in step (3).
[0035] In some embodiments, a chelating resin is used for the removal of metal residues in step (3), wherein the chelating resin includes any one or a combination of at least two of HP4010, HP705, HP4030, Lewatit TP207, Lewatit TP220 or AmberSep IRC748.
[0036] This application uses lithium-specific chelating resin to deeply remove trace amounts of metal residues such as nickel, cobalt, manganese, and copper.
[0037] In some embodiments, activated carbon adsorption is used to remove organic impurities in step (3).
[0038] In some embodiments, after removing organic impurities, the lithium sulfate stock solution obtained in step (3) is filtered to obtain a total impurity content of ≤0.5ppm. For example, it can be 0.5ppm, 0.4ppm, 0.3ppm, 0.2ppm or 0.1ppm, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0039] In some embodiments, the dispersant in step (4) is a polymeric dispersant, which includes any one or a combination of at least two of polyethylene glycol, polyether, polyacrylic acid or carboxymethyl cellulose.
[0040] The dispersant described in this application is a water-soluble polymeric dispersant. The polymeric dispersant is adsorbed on the surface of the crystal nucleus, inhibiting secondary nucleation and microcrystal aggregation in the lithium sulfate solution under high supersaturation, inducing steady-state crystal directional growth, and completely avoiding defects such as crystal nucleus distortion and impurity encapsulation caused by fluorine and carbon residues.
[0041] In some embodiments, the concentration of the dispersant in the mixture obtained by mixing the lithium sulfate stock solution in step (3) with the dispersant is 5 mg / L to 30 mg / L, for example, it can be 5 mg / L, 8 mg / L, 10 mg / L, 15 mg / L, 20 mg / L, 25 mg / L or 30 mg / L, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0042] In some embodiments, the vacuum degree of the evaporation crystallization in step (4) is -0.08MPa to -0.09MPa, for example, it can be -0.09MPa, -0.085MPa or -0.08MPa; the temperature is 75℃ to 85℃, for example, it can be 75℃, 78℃, 80℃, 82℃ or 85℃, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0043] In some embodiments, the purity of the battery-grade lithium sulfate in step (4) is ≥99.99%, for example, it can be 99.99%, 99.992%, 99.994%, 99.996%, 99.998% or 99.999%, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0044] Compared with the prior art, this application has the following advantages:
[0045] This application first employs a defluorinating agent to deeply remove carbon and fluorine from the mixed battery black powder, thoroughly removing fluorides (such as PVDF) and conductive carbon impurities, significantly reducing the fluorine and carbon content in the material, and decreasing LiF formation and lithium loss. Then, the defluorinated black powder is mixed with a reducing agent and calcined to complete phase reconstruction, reducing metal oxides such as nickel, cobalt, manganese, and iron in the black powder to elemental solid phases, while lithium is directionally converted into water-soluble lithium salts. Therefore, the carbothermic reduction calcination results in a high lithium selective water leaching rate, enabling the directional conversion of lithium into water-soluble lithium salts while transition metals remain as insoluble phases. Then... The roasted material is leached in water to achieve selective and preferential leaching of lithium, while heavy metals, phosphorus, and graphite residues are retained. After solid-liquid separation, a low-impurity crude lithium solution is obtained. The crude lithium solution is then filtered and purified to obtain a low-impurity high-purity lithium-ion stock solution, which significantly reduces the subsequent impurity removal load. Next, a multi-stage coupled deep impurity removal and refining process is carried out to remove iron and aluminum, calcium and magnesium, metal residues, and organic impurities, resulting in a lithium sulfate stock solution. Finally, a dispersant is added to the lithium sulfate stock solution to avoid crystal distortion and microcrystal agglomeration that encapsulates impurities. Therefore, this application obtains a battery-grade lithium sulfate product through the cooperation of multiple steps. Detailed Implementation
[0046] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.
[0047] Example 1
[0048] This embodiment provides a method for preparing battery-grade lithium sulfate using waste battery black powder, the method comprising the following steps:
[0049] (1) After fully discharging lithium iron phosphate batteries, nickel cobalt manganese ternary batteries and lithium cobalt oxide batteries respectively, they are sheared and crushed, electrode stripped, ultra-fine ground and demagnetized to obtain lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder respectively. The lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder are mixed in a mass ratio of 1:1:1 to obtain mixed battery black powder;
[0050] The mixed battery black powder and sodium p-toluenesulfonate were uniformly mixed to obtain a mixed powder, wherein the mass of sodium p-toluenesulfonate was 0.5 wt% of the mass of the mixed battery black powder; the mixed powder was fed into a fluidized bed combustion chamber, the fluidized bed heating system and the air pump were started, the temperature was kept constant to 600℃ and hot air was pumped to continue combustion for 1 hour, and after natural cooling, defluorinated carbon black powder was obtained.
[0051] (2) The defluorinated carbon black powder, reducing agent (specifically carbon black) and phosphorus phase regulator (specifically sodium carbonate) mentioned in step (1) are mixed. The amount of reducing agent added is 10 wt% of the mass of the defluorinated carbon black powder, and the molar ratio of phosphorus phase regulator to total phosphorus in the mixed battery black powder is 1:1. Then, the mixture is calcined at 800°C for 2.5 h in an argon atmosphere to obtain calcined material. The calcined material is then water-immersed at a liquid-solid mass ratio of 4:1, with the water immersion temperature controlled at 70°C and the water immersion time at 1.5 h. After filtration, crude lithium liquid is obtained. The crude lithium liquid is then filtered and purified using a modified polyetheretherketone-polyarylsulfone composite membrane to obtain lithium-containing leachate.
[0052] (3) Lime milk was added to the lithium-containing leachate obtained in step (2) to adjust the pH to 9.5 for dephosphorization treatment; then dilute sulfuric acid was added to the lithium-containing solution after dephosphorization to adjust the pH to 5, and then sodium-free organic flocculant (specifically non-ionic polyacrylamide) was added to remove iron and aluminum impurities; then battery-grade ammonium fluoride was added to precipitate and remove calcium and magnesium impurities; then lithium-specific chelating resin (specifically HP705) was used to remove impurities, and finally activated carbon adsorption was used to remove trace organic impurities. After precision filtration, lithium sulfate stock solution was obtained.
[0053] (4) After the lithium sulfate stock solution in step (3) is precisely filtered through a polyethersulfone filter membrane with a pore size of 0.22 μm, it is sent to the MVR evaporation system and evaporated and crystallized at a vacuum of -0.09 MPa and a temperature of 80°C. During the evaporation feeding stage, a dispersant (specifically polyethylene glycol) is continuously added to control the concentration of the dispersant in the system to 20 mg / L, so as to obtain the crystallization liquid.
[0054] (5) The crystallization liquid obtained in step (4) is centrifuged, washed with ultrapure water, vacuum dried and sieved to obtain battery-grade lithium sulfate.
[0055] Example 2
[0056] This embodiment provides a method for preparing battery-grade lithium sulfate using waste battery black powder, the method comprising the following steps:
[0057] (1) After fully discharging lithium iron phosphate batteries, nickel cobalt manganese ternary batteries and lithium cobalt oxide batteries respectively, they are sheared and crushed, electrode stripped, ultra-fine ground and demagnetized to obtain lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder respectively. The lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder are mixed in a mass ratio of 1:0.5:0.5 to obtain mixed battery black powder;
[0058] The mixed battery black powder and sodium p-toluenesulfonate were uniformly mixed to obtain a mixed powder, wherein the mass of sodium p-toluenesulfonate was 1 wt% of the mass of the mixed battery black powder; the mixed powder was fed into a fluidized bed combustion chamber, the fluidized bed heating system and the air pump were started, the temperature was kept constant to 550°C and hot air was pumped to continue combustion for 0.5 h, and after natural cooling, defluorinated carbon black powder was obtained.
[0059] (2) The defluorinated carbon black powder, reducing agent (specifically graphite powder) and phosphorus phase regulator (specifically sodium carbonate) mentioned in step (1) are mixed. The amount of reducing agent added is 5 wt% of the mass of the defluorinated carbon black powder, and the molar ratio of phosphorus phase regulator to total phosphorus in the mixed battery black powder is 0.8:1. Then, the mixture is calcined at 780°C for 2.5 h in an argon atmosphere to obtain calcined material. The calcined material is then water-immersed at a liquid-solid mass ratio of 5:1, with the water immersion temperature controlled at 60°C and the water immersion time at 2 h. After filtration, crude lithium liquid is obtained. The crude lithium liquid is then filtered and purified using a modified polyetheretherketone-polyarylsulfone composite membrane to obtain lithium-containing leachate.
[0060] (3) Lime milk was added to the lithium-containing leachate obtained in step (2) to adjust the pH to 9 and perform dephosphorization treatment; then dilute sulfuric acid was added to the lithium-containing solution after dephosphorization to adjust the pH to 4.5, and then sodium-free organic flocculant (specifically non-ionic polyacrylamide) was added to remove iron and aluminum impurities; then battery-grade ammonium fluoride was added to precipitate and remove calcium and magnesium impurities; then lithium-specific chelating resin (specifically HP705) was used to remove impurities, and finally activated carbon adsorption was used to remove trace organic impurities. After precision filtration, lithium sulfate stock solution was obtained.
[0061] (4) After the lithium sulfate stock solution described in step (3) is precisely filtered through a polyethersulfone filter membrane with a pore size of 0.22 μm, it is sent to the MVR evaporation system and evaporated and crystallized at a vacuum of -0.09 MPa and a temperature of 85°C. During the evaporation feeding stage, a dispersant (specifically polyethylene glycol) is continuously added to control the concentration of the dispersant in the system to 30 mg / L, so as to obtain the crystallization liquid.
[0062] (5) The crystallization liquid obtained in step (4) is centrifuged, washed with ultrapure water, vacuum dried and sieved to obtain battery-grade lithium sulfate.
[0063] Example 3
[0064] This embodiment provides a method for preparing battery-grade lithium sulfate using waste battery black powder, the method comprising the following steps:
[0065] (1) After fully discharging lithium iron phosphate batteries, nickel cobalt manganese ternary batteries and lithium cobalt oxide batteries respectively, they are sheared and crushed, electrode stripped, ultra-fine ground and demagnetized to obtain lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder respectively. The lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder are mixed in a mass ratio of 1:2:2 to obtain mixed battery black powder;
[0066] The mixed battery black powder and sodium p-toluenesulfonate were uniformly mixed to obtain a mixed powder, wherein the mass of sodium p-toluenesulfonate was 0.2 wt% of the mass of the mixed battery black powder; the mixed powder was fed into a fluidized bed combustion chamber, the fluidized bed heating system and the air pump were started, the temperature was kept constant to 650°C and hot air was pumped to continue combustion for 1.5 hours, and after natural cooling, defluorinated carbon black powder was obtained.
[0067] (2) The defluorinated carbon black powder / reducing agent (specifically carbon black) and phosphorus phase regulator (specifically sodium carbonate) mentioned in step (1) are mixed. The amount of reducing agent added is 15 wt% of the mass of the defluorinated carbon black powder, and the molar ratio of phosphorus phase regulator to total phosphorus in the mixed battery black powder is 1.5:1. Then, the mixture is calcined at 850°C for 3 hours in an argon atmosphere to obtain calcined material. The calcined material is then soaked in water at a liquid-solid mass ratio of 3:1, with the water soaking temperature controlled at 70°C and the water soaking time at 1.5 hours. After filtration, crude lithium liquid is obtained. The crude lithium liquid is then filtered and purified using a modified polyetheretherketone-polyarylsulfone composite membrane to obtain lithium-containing leachate.
[0068] (3) Lime milk was added to the lithium-containing leachate obtained in step (2) to adjust the pH to 10 for dephosphorization treatment; then dilute sulfuric acid was added to the lithium-containing solution after dephosphorization to adjust the pH to 5.5, and then sodium-free organic flocculant (specifically non-ionic polyacrylamide) was added to remove iron and aluminum impurities; then battery-grade ammonium fluoride was added to precipitate and remove calcium and magnesium impurities; then lithium-specific chelating resin (specifically HP705) was used to remove impurities, and finally activated carbon adsorption was used to remove trace organic impurities. After precision filtration, lithium sulfate stock solution was obtained.
[0069] (4) After the lithium sulfate stock solution in step (3) is precisely filtered through a polyethersulfone filter membrane with a pore size of 0.22 μm, it is sent to the MVR evaporation system and evaporated and crystallized at a vacuum of -0.08 MPa and a temperature of 75°C. During the evaporation feeding stage, a dispersant (specifically sodium carboxymethyl cellulose) is continuously added to control the concentration of the dispersant in the system to 5 mg / L, so as to obtain the crystallization liquid.
[0070] (5) The crystallization liquid obtained in step (4) is centrifuged, washed with ultrapure water, vacuum dried and sieved to obtain battery-grade lithium sulfate.
[0071] Example 4
[0072] This embodiment provides a method for preparing battery-grade lithium sulfate using waste battery black powder. The method is the same as in Example 1 except that the modified polyether ether ketone-polyarylsulfone composite membrane in step (2) is replaced with a polyether sulfone filter membrane.
[0073] Example 5
[0074] This embodiment provides a method for preparing battery-grade lithium sulfate using waste battery black powder. The method is the same as in Example 1 except that the dispersant in step (4) is sodium dodecyl sulfate.
[0075] Comparative Example 1
[0076] This comparative example provides a method for preparing lithium sulfate using waste battery black powder. The method is the same as in Example 1, except that the mixed battery black powder in step (1) is not mixed with sodium p-toluenesulfonate and burned, and the mixed battery black powder in step (1) is directly processed in step (2).
[0077] Comparative Example 2
[0078] This comparative example provides a method for preparing lithium sulfate using waste battery black powder. Except for step (1), in which the defluorinated carbon black powder is not mixed with a reducing agent and calcined, but directly leached in water, the method is the same as in Example 1.
[0079] Comparative Example 3
[0080] This comparative example provides a method for preparing lithium sulfate using waste battery black powder. The method is the same as that in Example 1 except that step (3) is not performed.
[0081] Comparative Example 4
[0082] This comparative example provides a method for preparing lithium sulfate using waste battery black powder. Except for step (4) when evaporation and crystallization is carried out without the addition of a dispersant, the method is the same as that in Example 1.
[0083] The purity of lithium sulfate obtained by the preparation methods described in the above examples and comparative examples is shown in Table 1:
[0084] Table 1
[0085]
[0086] As can be seen from Table 1 above:
[0087] As shown in Examples 1-3 and Comparative Example 1, this application significantly reduces the fluorine and carbon content in the material and improves the purity of lithium sulfate by using a defluorinating agent for combustion. As shown in Examples 1-3 and Comparative Example 2, this application uses carbothermal reduction, which allows the calcined material obtained by carbothermal reduction to remove transition metals through water leaching, resulting in crude lithium liquid, which greatly reduces metal impurities in the product and improves the purity of lithium sulfate. As shown in Examples 1-3 and Comparative Example 3, this application achieves deep impurity removal through multi-stage impurity removal treatment, resulting in high-purity lithium sulfate products. As shown in Examples 1-3 and Comparative Example 4, this application adds a dispersant during evaporation and crystallization to prevent crystal agglomeration and encapsulation of impurities, thereby further improving the purity of lithium sulfate. As shown in Examples 1 and 4, this application preferably uses a modified polyetheretherketone-polyarylsulfone composite membrane as a filter membrane, which can further improve the impurity removal effect. As shown in Examples 1 and 5, this application preferably adds a polymeric dispersant during evaporation and crystallization, which can induce the directional growth of stable crystals and further improve the purity of the product.
[0088] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. A method for preparing battery-grade lithium sulfate using waste battery black powder, characterized in that, The method includes the following steps: (1) Mix the mixed battery black powder with the defluorinated carbon agent and heat and burn it to obtain defluorinated carbon black powder; (2) The defluorinated carbon black powder, reducing agent and phosphorus phase regulator described in step (1) are mixed and calcined to obtain calcined material. The calcined material is then subjected to water immersion, solid-liquid separation and filtration purification to obtain lithium-containing leachate. (3) The lithium-containing leachate obtained in step (2) is subjected to dephosphorization treatment, and then sulfuric acid is added to the dephosphorized lithium-containing solution to obtain crude lithium sulfate solution; The crude lithium sulfate solution was subjected to sequential removal of iron and aluminum, calcium and magnesium, metal residues and organic impurities to obtain a refined lithium sulfate stock solution. (4) The refined lithium sulfate stock solution described in step (3) is mixed with a dispersant and then evaporated and crystallized. Then, solid-liquid separation, washing, drying and sieving are performed to obtain battery-grade lithium sulfate.
2. The method according to claim 1, characterized in that, The defluorinating agent in step (1) includes sodium p-toluenesulfonate; And / or, the mass of the defluorinated carbon agent in step (1) is 0.2wt% to 1wt% of the mass of the mixed battery black powder.
3. The method according to claim 1 or 2, characterized in that, The heating and combustion temperature in step (1) is 550℃~650℃, and the time is 0.5h~1.5h; And / or, the mixed battery black powder in step (1) includes lithium iron phosphate battery black powder, ternary battery black powder and lithium cobalt oxide battery black powder.
4. The method according to claim 1 or 2, characterized in that, The calcination in step (2) is carried out under an inert atmosphere, and the calcination temperature is 750~850℃, and the time is 2.5h~3h; And / or, the reducing agent in step (2) includes any one or a combination of at least two of graphite powder, carbon black, coke powder, and biochar; And / or, the amount of reducing agent added in step (2) is 5wt%~15wt% of the mass of the defluorinated carbon black powder; And / or, the phosphorus phase modifier in step (2) includes sodium carbonate; And / or, the molar ratio of the phosphorus phase regulator in step (2) to the total phosphorus in the mixed battery black powder is (0.8~1.5):
1.
5. The method according to claim 1 or 2, characterized in that, The water immersion temperature in step (2) is 60℃~70℃, and the time is 1.5h~2h; And / or, the solid-liquid mass ratio of the water immersion in step (2) is (3~5):1; And / or, the filter membrane used for filtration and purification in step (2) is a modified polyether ether ketone-polyarylsulfone composite membrane.
6. The method according to claim 1 or 2, characterized in that, The dephosphorization treatment in step (3) includes adding lime slurry to adjust the pH of the system to 9-10; And / or, in step (3), sulfuric acid is added until the pH of the solution is 4.5 to 5.5; And / or, sodium-free organic flocculants are used for the removal of iron and aluminum in step (3), wherein the sodium-free organic flocculants include nonionic polyacrylamide and / or polydimethyldiallyl ammonium chloride; And / or, ammonium fluoride is used for the removal of calcium and magnesium in step (3).
7. The method according to claim 1 or 2, characterized in that, The removal of metal residues in step (3) is performed using a chelating resin, wherein the chelating resin includes any one or a combination of at least two of HP4010, HP705, HP4030, Lewatit TP207, Lewatit TP220 or AmberSep IRC748. And / or, activated carbon adsorption is used to remove organic impurities as described in step (3); And / or, after removing organic impurities as described in step (3), the lithium sulfate stock solution with a total impurity content ≤0.5ppm is obtained by filtration.
8. The method according to claim 1 or 2, characterized in that, The dispersant in step (4) is a polymeric dispersant, which includes any one or a combination of at least two of polyethylene glycol, polyether, polyacrylic acid or carboxymethyl cellulose; And / or, in the mixture obtained by mixing the lithium sulfate stock solution described in step (3) with the dispersant, the concentration of the dispersant is 5 mg / L to 30 mg / L.
9. The method according to claim 1 or 2, characterized in that, The vacuum degree of the evaporation crystallization in step (4) is -0.08MPa to -0.09MPa, and the temperature is 75℃ to 85℃.
10. The method according to claim 1 or 2, characterized in that, The purity of the battery-grade lithium sulfate in step (4) is ≥99.99%.