High-purity cs2zncl4 raw material, preparation method and scintillation single crystal preparation method
The high-purity Cs2ZnCl4 raw material was prepared by a high-concentration hydrothermal method using hydrochloric acid, which solved the problem of controlling trace impurities in the growth of Cs2ZnCl4 single crystals, and enabled the growth of high-performance scintillation single crystals, thus improving optical quality and scintillation performance.
Patent Information
- Application Number
- CN202611409793.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to effectively control trace heavy metal impurities and water/oxygen-related impurities during the growth of Cs2ZnCl4 scintillation single crystals, leading to a decline in crystal optical quality and scintillation performance.
A chlorine-rich acidic reaction system was constructed using high-concentration hydrochloric acid. Under sealed hydrothermal conditions, CsCl and ZnCl2 reacted to form Cs2ZnCl4 components. Impurities were separated by crystallization, followed by filtration, washing, and drying to obtain high-purity raw materials, which were then subjected to molten crystal growth.
The content of impurities such as Tl and Pb was significantly reduced, which improved the optical transmittance and scintillation output of Cs2ZnCl4 single crystals while maintaining ultrafast time response performance.
Smart Images

Figure CN123061995A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of scintillator technology for radiation detection, specifically relating to a high-purity raw material for the growth of Cs2ZnCl4 scintillator single crystals, a hydrothermal preparation method of the high-purity raw material, and a method for preparing Cs2ZnCl4 scintillator single crystals using the high-purity raw material. Background Technology
[0002] With the development of high-energy physics experiments, medical imaging, and ultra-high count rate radiation detection technologies, the demand for ultrafast scintillators with decay times in the nanosecond or even sub-nanosecond range is becoming increasingly urgent (Z. Wang et al., Needs, Trends, and Advances in Scintillators for Radiographic Imaging and Tomography, IEEE Trans. Nucl. Sci., 70(2023):1244–1254). Cs2ZnCl4 single crystal is an inorganic scintillator with valence band-core band (CVL) luminescence and a decay time of 1.6–1.8 ns, possessing excellent potential for ultrafast timing radiation detection (D. Rutstrom et al., Improved light yield and growth of large-volume ultrafast single crystal scintillators Cs2ZnCl4 and Cs3ZnCl5, Optical Materials, 133(2022):112912).
[0003] However, the luminescence process of Cs₂ZnCl₄ scintillators is easily affected by trace impurities and structural defects, and trace amounts of heavy metal ions (such as Tl) can also affect it. + Pb 2+ (e.g.,) may introduce defect levels or carrier trapping centers into the single crystal, thereby reducing the scintillation output of the single crystal by competitively capturing migrating carriers and inducing nonradiative recombination processes (M. Nikl et al., Complex oxidescintillators: Material defects and scintillation performance, Physica Status Solidi B, 245(2008):1701–1722). Meanwhile, the CsCl and ZnCl2 raw materials used to grow Cs₂ZnCl₄ single crystals are both halides, which are highly susceptible to introducing OH groups during use and preparation. -Oxygen-containing impurities such as water may form oxyhalides, hydroxyl-related defects, or other competing impurities during subsequent single crystal growth, thereby damaging the crystallinity of the single crystal, inducing scattering defects or cracks, affecting the transmittance of the single crystal to its own scintillation light, and may reduce the scintillation efficiency of the single crystal by forming nonradiative recombination centers (S. Swider et al., Impurity segregation in zone-refined precursors for crystalline halide scintillators, Nuclear Instruments and Methods in Physics Research Section A, 784(2015):5–8).
[0004] There are various conventional methods for purifying raw materials, typically including aqueous solution crystallization utilizing differences in solubility and zone melting purification and single crystal growth purification utilizing differences in segregation coefficients. However, for halide raw materials used in the scintillation single crystal growth of Cs₂ZnCl₄, these methods still have certain limitations in controlling trace impurities. The impurity removal effect during aqueous solution crystallization is affected by impurity partitioning behavior, co-crystallization behavior, and the solution environment. For heavy metal impurities with similar coordination or crystallization behavior to matrix ions, separation is quite difficult (F. Rosenberger, HG Riveros, Segregation in alkalihalide crystallization from aqueous solutions, J. Chem. Phys., 60(1974):668–673); at the same time, the aqueous solution treatment process may also introduce or leave residual oxygen-containing impurities such as water and hydroxyl groups. Melt purification (zone melting or growth) mainly relies on the difference in segregation coefficients of impurities in the solid and melt. For impurities with segregation coefficients close to or much greater than 1, the removal efficiency is limited (WG Pfann, Zone Melting, Science, 135(1962):1101–1109). Melt purification requires long-term and multiple high-temperature processes, which may exacerbate the non-stoichiometric volatilization of CsCl and ZnCl2 halide components and induce macroscopic or microscopic structural defects such as component deviation and impurity equivalence.
[0005] There is an urgent need to develop high-purity Cs2ZnCl4 raw materials and their low-temperature preparation methods to effectively control trace heavy metal impurities and water / oxygen-related impurities, and to eliminate or reduce the probability of microscopic and macroscopic defects, thus laying the technological foundation for the preparation of high-purity raw materials for the growth of high-performance Cs2ZnCl4 scintillation single crystals. Summary of the Invention
[0006] This invention addresses the problem that when commercial CsCl and ZnCl2 raw materials are directly used to grow Cs2ZnCl4 scintillation single crystals, trace impurities such as Tl and Pb in the raw materials can easily enter the crystal and affect its optical quality and scintillation performance. The invention provides a high-purity raw material for growing Cs2ZnCl4 scintillation single crystals, a method for preparing the high-purity raw material, and a method for preparing Cs2ZnCl4 scintillation single crystals. This invention involves preparing a mixed raw material according to the stoichiometric ratio of CsCl and ZnCl2, constructing a chlorine-rich acidic reaction system using high-concentration hydrochloric acid, and fully dissolving CsCl and ZnCl2 in the chlorine-rich acidic medium under sealed hydrothermal conditions to form a reaction system containing Cs2ZnCl4 components. Subsequently, controlled cooling is used to precipitate Cs2ZnCl4 in the form of crystalline crystals, allowing impurities such as Tl and Pb to be preferentially retained in the mother liquor. After separation, washing, and drying under normal pressure, a high-purity crystalline Cs2ZnCl4 raw material with low Tl and low Pb is obtained. This high-purity raw material is further melted and crystal grown to obtain a Cs2ZnCl4 scintillation single crystal with high optical transmittance, high scintillation light output, and nanosecond-level fast decay characteristics.
[0007] According to a first aspect of the present invention, a high-purity raw material for scintillation single crystal growth of Cs₂ZnCl₄ is provided. The high-purity raw material is a crystalline Cs₂ZnCl₄ compound raw material, and based on the total mass of the high-purity raw material, the content of Tl impurities in the high-purity raw material is ≤1.0 ppm, and the content of Pb impurities is ≤0.2 ppm. Preferably, the content of Tl impurities in the high-purity raw material is ≤0.4 ppm.
[0008] In some technical solutions, based on the total mass of the high-purity raw materials, the contents of Fe, Mn and Co impurities are ≤1.0 ppm, and the contents of Cr, Cu and V impurities are ≤0.1 ppm.
[0009] According to a second aspect of the present invention, a method for preparing the above-mentioned high-purity raw material for Cs₂ZnCl₄ scintillation single crystal growth is further provided, comprising the following steps: Weigh out CsCl and ZnCl2 raw materials according to a molar ratio of 2:1 and mix them to obtain a mixed raw material; The mixed raw materials are dispersed and dissolved in hydrochloric acid with a concentration of 5-12 mol / L to form a chlorine-rich acidic reaction system; The chlorine-rich acidic reaction system was placed in a sealed hydrothermal reactor resistant to hydrochloric acid corrosion and subjected to a hydrothermal reaction at 150–200°C for 12–24 h, so that CsCl and ZnCl2 formed a reaction system containing Cs2ZnCl4 components in the chlorine-rich acidic medium; after the hydrothermal reaction, the temperature was lowered to allow Cs2ZnCl4 to precipitate in the form of crystalline crystals; The precipitated crystalline Cs2ZnCl4 raw material was collected and then filtered, washed, and dried under normal pressure to obtain the high-purity raw material for Cs2ZnCl4 scintillation single crystal growth.
[0010] In some technical solutions, the concentration of the hydrochloric acid is 8–12 mol / L.
[0011] In some technical solutions, the concentration of hydrochloric acid is 10-12 mol / L; the hydrothermal reactor is equipped with a hydrochloric acid corrosion-resistant lining, and the material of the hydrochloric acid corrosion-resistant lining is polytetrafluoroethylene or para-polystyrene; the filling degree of the chlorine-rich acid reaction system in the hydrothermal reactor is 20%-40%.
[0012] In some technical solutions, the chlorine-rich acidic reaction system is heated to the reaction temperature of the hydrothermal reaction at a heating rate of 1 to 5 °C / min; after the hydrothermal reaction is completed, it is cooled to room temperature at a cooling rate of 0.01 to 0.5 °C / min.
[0013] In some technical solutions, the washing is carried out using anhydrous ethanol; the temperature of the atmospheric pressure drying is 60-100℃, and the time is 6-24h.
[0014] According to a third aspect of the present invention, a method for preparing a Cs₂ZnCl₄ scintillation single crystal is further provided, comprising the following steps: The high-purity raw material for the above-mentioned Cs2ZnCl4 scintillation single crystal growth is placed in a crucible or container resistant to halide melt corrosion. The high-purity raw material is heated to complete or partial melting under vacuum or inert gas protection conditions to form Cs2ZnCl4 melt; By controlling the movement of the crucible, seed crystal, or molten zone relative to the temperature field, the Cs2ZnCl4 melt can undergo crystal growth. After the crystal growth is completed, the temperature is lowered to obtain Cs2ZnCl4 scintillation single crystal.
[0015] In some technical solutions, the crystal growth is achieved using any one of the following methods: crucible lowering method, Czochralski method, zone melting method, mold guiding method, or micro-pulling method.
[0016] In some technical solutions, the crystal growth adopts the crucible descent method; the high-purity raw material is loaded into a quartz crucible, the quartz crucible is evacuated and sealed, and the sealed quartz crucible is placed in a crucible descent growth furnace; the melting zone temperature of the crucible descent growth furnace is 600-700℃, the low temperature zone temperature is 400-500℃, the temperature gradient at the solid-liquid interface is 10-30℃ / cm, and the descent rate of the quartz crucible is 0.1-2.0 mm / h.
[0017] The present invention, by employing the above technical solution, has at least the following beneficial effects: 1. This invention utilizes the synergistic effect of a high-concentration hydrochloric acid-rich system and a sealed hydrothermal crystallization process to crystallize and precipitate the main compound of Cs₂ZnCl₄, while reducing the degree of co-precipitation of trace impurities such as Tl and Pb with the main compound. The Tl and Pb contents in the obtained Cs₂ZnCl₄ raw material can be controlled to below 1 ppm and 0.2 ppm, respectively. Under preferred conditions, the Tl content can be further controlled to below 0.4 ppm, providing high-purity compound raw materials for high-performance scintillation single crystal growth.
[0018] 2. This invention directly converts CsCl and ZnCl2 into uniformly crystalline Cs2ZnCl4 compound raw materials. By filtering, washing with anhydrous ethanol and drying at normal pressure, the residual mother liquor, residual acid and adsorbed water are reduced, which helps to reduce impurities, cracks and light scattering defects caused by raw material impurities and local component inhomogeneity during the subsequent high-temperature melting process, thereby improving the quality of single crystal growth.
[0019] 3. The Cs2ZnCl4 scintillation single crystal grown using the high-purity raw materials of this invention can maintain a transmittance of over 60% at 230 nm and over 80% in the 300–800 nm wavelength range. The light output is increased from approximately 959 ph / MeV of the initial raw material-grown single crystal to approximately 1484 ph / MeV, while the scintillation decay time is maintained at approximately 1.76 ns. This demonstrates that the optical quality and scintillation light output can be improved while maintaining ultrafast time response performance. Attached Figure Description
[0020] Figure 1 The X-ray powder diffraction pattern of the high-purity Cs2ZnCl4 raw material prepared in the embodiment of the present invention and its comparison with standard diffraction data are shown. Figure 2 The image shows a comparison of physical specimens of single crystals grown using high-purity Cs2ZnCl4 raw materials according to embodiments of the present invention and single crystals grown directly using the initial raw materials. Figure 3 This is a comparison chart of the ultraviolet-visible light transmittance of single crystals grown using high-purity Cs2ZnCl4 raw materials from the embodiments of the present invention and single crystals grown directly using the initial raw materials. Figure 4 The image shows a comparison of the X-ray excitation emission spectra of single crystals grown using high-purity Cs2ZnCl4 raw materials from the embodiments of the present invention and single crystals grown directly using the initial raw materials. Figure 5 The comparison between single crystals grown using high-purity Cs₂ZnCl₄ feedstock in the embodiments of the present invention and single crystals grown directly using the initial feedstock is shown below. 137 Comparison of pulse height spectra under Cs gamma-ray excitation; Figure 6This is a comparison of the scintillation decay curves of single crystals grown using high-purity Cs2ZnCl4 raw materials according to embodiments of the present invention and single crystals grown directly using the initial raw materials under pulsed X-ray excitation. Detailed Implementation
[0021] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments. It should be understood that the embodiments described are only for illustrating the present invention and are not intended to limit the scope of protection of the present invention.
[0022] Unless otherwise stated, the raw materials, reagents, and equipment used in the embodiments of this invention are all available through conventional commercial channels, and the detection and operation methods used are conventional methods in the art. Operations without specific conditions can be performed according to conventional conditions in the art or conditions recommended by the equipment manufacturer.
[0023] General implementation method: Optional growth methods for Cs2ZnCl4 scintillation single crystals The crystalline Cs₂ZnCl₄ raw material obtained by this invention can be used for melt growth of Cs₂ZnCl₄ scintillation single crystals. In one specific embodiment of this invention, the crucible lowering method is used for single crystal growth; in addition to the crucible lowering method, melt crystal growth methods such as the Czochralski method, zone melting method, guided mold method, or micro-pull-down method can also be used when the corresponding equipment conditions are available.
[0024] When using the above-mentioned optional growth method, the Cs2ZnCl4 raw material can be loaded into a crucible or container resistant to halide melt corrosion, and heated under vacuum or inert atmosphere protection to form a melt; then, by controlling the movement of the crucible, seed crystal, guide mold component or molten zone relative to the temperature field, the melt is directionally solidified, and then slowly cooled to room temperature to obtain Cs2ZnCl4 crystal.
[0025] Among them, when using the Czochralski method, the crystal can grow along the seed crystal direction by controlling the contact between the seed crystal and the surface of the melt, the seed crystal pulling rate, the rotation rate, and the temperature gradient near the solid-liquid interface; when using the zone melting method, a melting zone can be formed by local heating, and the melting zone can be controlled to move along the charging direction, so that the melt solidifies directionally behind the melting zone; when using the guide mold method, the melt can form a stable meniscus through the guide mold component, and a crystal with a predetermined cross-sectional shape can be obtained by controlling the pulling rate, the melt temperature, and the interface temperature field; when using the micro-pull-down method, the melt can be continuously supplied through the micro-holes at the bottom of the crucible, and crystal growth can be achieved by controlling the seed crystal pull-down rate and the solid-liquid interface position.
[0026] The specific temperature, pulling rate, rotation rate, melting zone movement rate, mold structure, micropore size, crucible or container material, and cooling procedure of the above-mentioned melt growth method can be selected and adjusted according to the type of growth equipment used and the target crystal size requirements.
[0027] Example 1: Hydrothermal preparation of high-purity Cs2ZnCl4 raw material (1) Raw material synthesis: Commercial 4N grade CsCl powder and commercial 4.5N grade ZnCl2 powder were weighed according to a CsCl:ZnCl2 molar ratio of 2:1. The total mass of the mixed raw materials was placed in a 120 mL reactor, and 30 mL of 12 mol / L concentrated hydrochloric acid was added as an acidic reaction medium. The reactor filling degree was 25%.
[0028] (2) Hydrothermal reaction: The reactor is placed in a constant temperature oven and heated to 160 ℃ at a heating rate of 1 ℃ / min. It is then kept at 160 ℃ for 12 h to allow the raw materials to fully dissolve and react in a chlorine-rich acidic medium, forming a reaction system containing Cs2ZnCl4 components.
[0029] (3) Cooling crystallization and post-treatment: After the hydrothermal reaction was completed, the temperature was lowered to room temperature at a rate of 0.1 °C / min. During the cooling process, as the supersaturation of the system increased, Cs2ZnCl4 gradually precipitated in the form of crystalline material. After cooling to room temperature, the reaction system was filtered, and the obtained crystalline Cs2ZnCl4 material was collected and washed five times with anhydrous ethanol to remove residual acid and mother liquor impurities from the surface of the material. Subsequently, it was placed in an atmospheric pressure drying oven and dried at 60 °C for 24 h to remove residual solvent, adsorbed water and residual acid from the surface.
[0030] To evaluate the control effect of the hydrothermal preparation process of this invention on trace metal impurities, inductively coupled plasma mass spectrometry (ICP-MS) was performed on commercial CsCl powder, commercial ZnCl2 powder, and high-purity Cs2ZnCl4 raw material prepared by hydrothermal synthesis. Considering the problem of uneven microscopic sampling in mechanically mixed powders, the impurity content in the initial raw material was obtained by converting the measured impurity content of commercial CsCl powder and commercial ZnCl2 powder according to their mass fractions in the stoichiometric composition of Cs2ZnCl4. The mass fractions of CsCl and ZnCl2 in the mixed raw material were approximately 71.18% and 28.82%, respectively. Table 1 shows the ICP-MS test results of representative trace metal impurity contents in the initial raw material and the high-purity Cs2ZnCl4 raw material prepared by hydrothermal synthesis of this invention.
[0031]
[0032] Note: The conventional mixed raw material was calculated based on a CsCl:ZnCl2 molar ratio of 2:1; ND indicates that it is below the ICP-MS detection limit.
[0033] As shown in Table 1, compared with the initial raw materials, the Tl and Pb contents in the high-purity Cs₂ZnCl₄ raw materials purified by the hydrothermal process of this invention are significantly reduced. Specifically, the Tl content decreased from 7.959 ppm to 0.4 ppm, and the Pb content decreased from 2.590 ppm to <0.2 ppm. Simultaneously, the Fe content decreased from 0.949 ppm to 0.3 ppm, and the Mn and Co contents decreased below the detection limit. Other tested transition metal impurities such as Cr, Cu, and V also remained at low levels. These results demonstrate that the hydrothermal preparation process of this invention can effectively control key heavy metal impurities in Cs₂ZnCl₄ raw materials and keep common transition metal impurities such as Fe, Mn, and Co at low levels, thus providing a high-purity raw material basis for the subsequent growth of high-optical-quality Cs₂ZnCl₄ scintillation single crystals using the crucible lowering method.
[0034] Example 2: Single crystal growth using the crucible lowering method (1) Loading and sealing: The high-purity Cs2ZnCl4 raw material obtained in Example 1 was loaded into a quartz crucible. After the crucible was evacuated, it was sealed using an oxyhydrogen flame sealing machine to reduce the influence of moisture, oxygen-containing impurities and external atmosphere on the melt.
[0035] (2) Melting: Place the sealed quartz crucible in a vertical crucible descending growth furnace and gradually heat it until the raw material is completely melted.
[0036] (3) Single crystal growth: Set the melting zone temperature to 650 ℃ and the low temperature zone temperature to 450 ℃, and pass the crucible through the temperature gradient zone at a rate of 0.8 mm / h to allow the melt to gradually crystallize.
[0037] (4) Cooling and crystal removal: After the crystallization process is complete, stop the crucible descent and slowly cool it to room temperature according to the preset cooling program. Open the crucible and remove the Cs2ZnCl4 single crystal. The appearance, optical transmittance, X-ray excitation luminescence, and other properties of the obtained single crystal are then analyzed. 137 Cs gamma-ray pulse height spectrum and scintillation attenuation performance are shown in [reference]. Figures 2-6 .
[0038] Example 3: Preparation of Cs₂ZnCl₄ raw material under 8 mol / L hydrochloric acid conditions This embodiment was performed in accordance with Example 1, except that the hydrochloric acid concentration was adjusted to 8 mol / L, the hydrothermal reaction temperature was 160 ℃, and the isothermal time was 12 h. The mass of the dried product obtained was 4.1 g, and the apparent crystallization yield was 82%. The XRD phase identification results and Tl and Pb contents of the obtained sample are shown in Table 2.
[0039] Example 4: Preparation of Cs2ZnCl4 raw material under closed hydrothermal conditions at 180℃ This embodiment was performed in accordance with Example 1, except that the hydrothermal reaction temperature was adjusted to 180 °C and the isothermal time was 12 h. The mass of the dried product obtained was 4.4 g, and the apparent crystallization yield was 88%. The XRD phase identification results and Tl and Pb contents of the obtained sample are shown in Table 2.
[0040] Example 5: Preparation of Cs2ZnCl4 raw material under 24-hour closed hydrothermal conditions This embodiment was performed in accordance with Example 1, except that the isothermal time was adjusted to 24 h. The mass of the dried product obtained was 4.7 g, and the apparent crystallization yield was 94%. The XRD phase identification results and Tl and Pb contents of the obtained sample are shown in Table 2.
[0041] Comparative Example 1: Cs2ZnCl4 single crystals prepared by conventional processes The preparation process of Cs₂ZnCl₄ single crystals in this comparative example is the same as in Example 2, except that hydrothermal purification is not used. 4N-grade CsCl and 4.5N-grade ZnCl₂ raw materials are directly loaded into a quartz crucible, and growth is performed using the same crucible lowering growth parameters.
[0042] The results showed that the Tl content in the comparative single crystal remained at around 4 ppm. Its transmittance decreased significantly at 369 nm, and its absorption intensity at 227 nm was stronger than that of the hydrothermally prepared and purified single crystal. In the radiation emission spectrum, the intensity of its emission peak was reduced by about 40% compared with that of the hydrothermally prepared and purified single crystal.
[0043] Comparative Example 2: Preparation of Cs2ZnCl4 raw material under low concentration hydrochloric acid conditions This comparative example was conducted in accordance with Example 1, except that the hydrochloric acid concentration was adjusted to 2 mol / L, the hydrothermal reaction temperature was 160 ℃, and the isothermal time was 12 h. The mass of the dried product obtained was 3.2 g, and the apparent crystallization yield was 64%. The XRD phase identification results and Tl and Pb contents of the obtained samples are shown in Table 2.
[0044] Comparative Example 3: Preparation of Cs2ZnCl4 raw material under low-temperature closed reaction conditions This comparative example was conducted according to Example 1, with the only difference being that the hydrothermal reaction temperature was adjusted to 100 °C and the isothermal time was 12 h. The mass of the dried product obtained was 4.2 g, and the apparent crystallization yield was 84%. The XRD phase identification results and Tl and Pb contents of the obtained samples are shown in Table 2.
[0045] Comparative Example 4: Preparation of Cs₂ZnCl₄ raw material under atmospheric pressure heating conditions In this comparative example, the raw materials were weighed according to a CsCl to ZnCl2 molar ratio of 2:1, and 30 mL of 12 mol / L hydrochloric acid was added. The mixture was heated at 60°C for 12 h under normal pressure, and then cooled to room temperature. The remaining steps of filtration, washing with anhydrous ethanol, and drying under normal pressure were the same as in Example 1. The mass of the dried product obtained was 4.3 g, and the apparent crystallization yield was 86%. The XRD phase identification results and Tl and Pb contents of the obtained samples are shown in Table 2.
[0046] To facilitate comparison of the process parameters of Example 1, Examples 3-5 and Comparative Examples 2-4, the main hydrothermal reaction conditions and post-treatment conditions are summarized in Tables 2 and 3, respectively.
[0047]
[0048] Note: Apparent crystallization yield = mass of solid obtained after drying / total mass of CsCl and ZnCl2 fed × 100%. Tl and Pb were detected by ICP-MS, with units of μg / g equivalent to ppm; Pb < 0.2 μg / g indicates below the detection limit. XRD results were used for phase identification and cannot characterize the content of trace impurities such as Tl and Pb.
[0049] As shown in Table 2, under the same raw material ratio and post-treatment conditions, Example 1, using 12 mol / L hydrochloric acid and a closed hydrothermal reaction at 160 °C for 12 h, yielded an apparent crystallization yield of 88% for the Cs₂ZnCl₄ raw material. XRD phase identification showed it to be Cs₂ZnCl₄ phase, with no detectable impurities. The Tl content was 0.4 μg / g, and the Pb content was below 0.2 μg / g. Compared to Example 1, Comparative Example 2, using a low-concentration hydrochloric acid (2 mol / L), under closed hydrothermal reaction conditions, while still predominantly Cs₂ZnCl₄ phase, showed a lower apparent crystallization yield (64%) and a higher Tl content (2.6 μg / g). This indicates that the low-concentration hydrochloric acid system is not conducive to inhibiting the co-precipitation of Tl impurities and the main Cs₂ZnCl₄ compound.
[0050] Comparative Example 3 used 12 mol / L hydrochloric acid but lowered the reaction temperature to 100 °C. The resulting product had a Tl content of 1.4 μg / g, which was higher than that of Example 1. This indicates that using only high-concentration hydrochloric acid without the closed hydrothermal reaction conditions within the range of 150–200 °C is still insufficient for controlling Tl impurities. Comparative Example 4 used 12 mol / L hydrochloric acid and heated at 60 °C under normal pressure. The resulting product had a Tl content of 1.7 μg / g, which was also significantly higher than that of Example 1. This shows that atmospheric pressure heating crystallization cannot achieve the impurity control effect under the closed hydrothermal conditions of this invention.
[0051] The above results indicate that the chlorine-rich acidic system constructed with high-concentration hydrochloric acid and the closed hydrothermal reaction conditions at 150–200 °C have a synergistic effect on reducing the Tl impurity content in the Cs2ZnCl4 raw material. Under the optimized conditions, a high-purity raw material for Cs2ZnCl4 scintillation single crystal growth with a well-defined Cs2ZnCl4 phase, a high apparent crystallization yield, and low Tl and Pb contents can be obtained.
[0052]
[0053] Figure 1 The X-ray diffraction (XRD) pattern of high-purity Cs₂ZnCl₄ raw material powder obtained by the hydrothermal preparation process in an embodiment of the present invention is given. From... Figure 1 As can be seen intuitively, all the characteristic diffraction peaks of the raw material obtained by hydrothermal preparation are consistent with the standard powder diffraction card (PDF#04-010-5876) of Cs2ZnCl4. The diffraction peaks are sharp and the baseline is stable. No impurity phase characteristic peaks belonging to free CsCl, ZnCl2 or other water-containing by-products (such as hydrate complex ions) were observed.
[0054] Figure 2 The paper presents photographs of Cs₂ZnCl₄ single crystals grown using the high-purity raw materials of this invention via the crucible lowering method (top) and comparative single crystals obtained directly from raw materials without hydrothermal preparation via the crucible lowering method (bottom). Figure 2 It can be seen that the Cs2ZnCl4 single crystal grown using the high-purity raw materials of this invention has a smoother surface, while the surface of the comparative single crystal has more cracks.
[0055] Figure 3 Optical transmittance spectra of a 2 mm thick Cs₂ZnCl₄ single crystal grown using the high-purity raw materials of this invention and a comparative single crystal grown using the initial raw materials are presented. As shown in Table 1, after hydrothermal preparation with high-concentration hydrochloric acid according to this invention, key trace metal impurities in the obtained Cs₂ZnCl₄ raw material are effectively controlled. Combined with... Figure 3 It can be seen that reducing impurities decreases the background absorption of the single crystal in the ultraviolet and deep ultraviolet bands. The single crystal grown from the initial raw materials has an impurity absorption band around 230 nm, while the absorption of the single crystal grown using the high-purity raw materials of this invention is significantly reduced in this band. Its transmittance at 230 nm remains above 60%, and its optical transmittance in the wide band of 300–800 nm reaches above 80%, thus improving optical transparency.
[0056] Figure 4 X-ray excitation emission spectra of a comparative single crystal grown directly from the initial raw materials and a single crystal grown using the high-purity raw materials of this invention are presented. Figure 4It can be seen that the main emission peaks of the single crystals grown from the initial raw materials and those grown using the high-purity raw materials of this invention are located between 270 and 280 nm. Furthermore, the single crystals grown using the high-purity raw materials of this invention exhibit enhanced intrinsic ultraviolet emission under X-ray excitation. This result is consistent with the lower Tl content and better optical quality of the hydrothermally treated samples; however, the specific microscopic mechanism still requires further investigation.
[0057] Figure 5 The growth of single crystals using the initial raw materials and the growth of single crystals using the high-purity raw materials of this invention are given. 137 Pulse height spectrum excited by a Cs gamma-ray source. Figure 5 The energy spectrum distribution shows that, compared with the single crystal grown using the high-purity raw materials of this invention, the full-energy peak of the single crystal shifts to higher channel addresses, indicating an improvement in its light output. The light yield of the single crystal increases from approximately 959 ph / MeV before purification to approximately 1484 ph / MeV of the high-purity single crystal.
[0058] To verify the effect of the purification process on the ultrafast time response characteristics of Cs₂ZnCl₄ single crystals, this invention obtained the scintillation decay curves of the single crystals under pulsed X-ray excitation, as shown in the figure. Figure 6 The single-exponential fitting results show that the decay times of the single crystal grown using the high-purity raw materials of this invention and the single crystal grown using the initial raw materials are 1.76 ns and 1.74 ns, respectively. The results indicate that the Cs₂ZnCl₄ single crystal grown using the high-purity raw materials of this invention maintains a fast decay response while improving optical quality and increasing light output, and no obvious slow decay tail was observed.
[0059] In this invention, by constructing an acidic hydrothermal system with suitable concentration, the content of trace impurities such as Tl and Pb in the Cs₂ZnCl₄ raw material is reduced. The scintillation single crystal obtained by growing this raw material using the crucible-lowering method exhibits higher optical transmittance and stronger X-ray excitation luminescence. While maintaining the nanosecond-level fast decay characteristics of Cs₂ZnCl₄ single crystal, its scintillation light output is improved, making it suitable for applications such as high-count-rate radiation detection.
[0060] Finally, it is necessary to state that the above embodiments are only used to further illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-creative improvements and adjustments made by those skilled in the art based on the above content of the present invention shall fall within the scope of protection of the present invention.
Claims
1. A high-purity raw material for the scintillation single crystal growth of Cs₂ZnCl₄, characterized in that, The high-purity raw material is a crystalline Cs2ZnCl4 compound raw material. Based on the total mass of the high-purity raw material, the content of Tl impurities in the high-purity raw material is ≤1.0 ppm and the content of Pb impurities is ≤0.2 ppm.
2. The high-purity raw material for Cs₂ZnCl₄ scintillation single crystal growth according to claim 1, characterized in that, Based on the total mass of the high-purity raw materials, the content of Tl impurities in the high-purity raw materials is ≤0.4 ppm, the content of Fe, Mn and Co impurities is ≤1.0 ppm, and the content of Cr, Cu and V impurities is ≤0.1 ppm.
3. A method for preparing the high-purity raw material for Cs₂ZnCl₄ scintillation single crystal growth as described in claim 1 or 2, characterized in that, Includes the following steps: Weigh out CsCl and ZnCl2 raw materials according to a molar ratio of 2:1 and mix them to obtain a mixed raw material; The mixed raw materials are dispersed and dissolved in hydrochloric acid with a concentration of 5-12 mol / L to form a chlorine-rich acidic reaction system; The chlorine-rich acidic reaction system was placed in a sealed hydrothermal reactor resistant to hydrochloric acid corrosion and subjected to a hydrothermal reaction at 150–200°C for 12–24 h, so that CsCl and ZnCl2 formed a reaction system containing Cs2ZnCl4 components in the chlorine-rich acidic medium; after the hydrothermal reaction, the temperature was lowered to allow Cs2ZnCl4 to precipitate in the form of crystalline crystals; The precipitated crystalline Cs2ZnCl4 raw material was collected and then filtered, washed, and dried under normal pressure to obtain the high-purity raw material for Cs2ZnCl4 scintillation single crystal growth.
4. The preparation method according to claim 3, characterized in that, The concentration of the hydrochloric acid is 8–12 mol / L.
5. The preparation method according to claim 4, characterized in that, The concentration of the hydrochloric acid is 10-12 mol / L; the hydrothermal reactor is equipped with a hydrochloric acid corrosion resistant lining, and the material of the hydrochloric acid corrosion resistant lining is polytetrafluoroethylene or para-polystyrene; the filling degree of the chlorine-rich acid reaction system in the hydrothermal reactor is 20%-40%.
6. The preparation method according to claim 3, characterized in that, The chlorine-rich acidic reaction system is heated to the hydrothermal reaction temperature at a heating rate of 1–5 °C / min; after the hydrothermal reaction is completed, it is cooled to room temperature at a cooling rate of 0.01–0.5 °C / min.
7. The preparation method according to claim 3, characterized in that, The washing is performed using anhydrous ethanol; the atmospheric pressure drying is carried out at a temperature of 60–100°C for 6–24 hours.
8. A method for preparing a Cs₂ZnCl₄ scintillation single crystal, characterized in that, Includes the following steps: The high-purity raw material for Cs2ZnCl4 scintillation single crystal growth as described in claim 1 or 2, or the high-purity raw material for Cs2ZnCl4 scintillation single crystal growth obtained by the preparation method described in any one of claims 3 to 7, is placed into a crucible or container resistant to halide melt corrosion. The high-purity raw material is heated to complete or partial melting under vacuum or inert gas protection conditions to form Cs2ZnCl4 melt; By controlling the movement of the crucible, seed crystal, or molten zone relative to the temperature field, the Cs2ZnCl4 melt can undergo crystal growth. After the crystal growth is completed, the temperature is lowered to obtain Cs2ZnCl4 scintillation single crystal.
9. The method for preparing Cs₂ZnCl₄ scintillation single crystal according to claim 8, characterized in that, The crystal growth is performed using any one of the following methods: crucible lowering method, Czochralski method, zone melting method, mold guiding method, or micro-pulling method.
10. The method for preparing Cs₂ZnCl₄ scintillation single crystal according to claim 9, characterized in that, The crystal growth is performed using a crucible descent method. The high-purity raw material is loaded into a quartz crucible, which is then evacuated and sealed. The sealed quartz crucible is placed in a crucible descent growth furnace. The melting zone temperature of the crucible descent growth furnace is 600–700°C, the low-temperature zone temperature is 400–500°C, the temperature gradient at the solid-liquid interface is 10–30°C / cm, and the descent rate of the quartz crucible is 0.1–2.0 mm / h.