A method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder

Rare earth-doped bismuth oxide/zinc oxide powder was prepared by combining bismuth oxide and zinc oxide and doping with rare earth yttrium using a high-temperature mechanochemical method. This solved the problems of oxidation and emissivity reduction of bismuth oxide materials at high temperatures, achieving high infrared emissivity and high-temperature stability, which is suitable for radiation protection coatings.

CN123062004APending Publication Date: 2026-11-10WUHAN RES INST OF MATERIALS PROTECTION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611185608.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing bismuth oxide materials are easily oxidized at high temperatures and their infrared emissivity decreases. Single-component materials have insufficient infrared emissivity in specific wavelength bands, making it difficult to maintain the integrity of the crystal structure while improving infrared emissivity.

Method used

Bismuth oxide and zinc oxide were combined using a high-temperature mechanochemical method and doped with the rare earth element yttrium. The rare earth-doped bismuth oxide/zinc oxide high-emissivity powder was prepared by high-temperature ball milling reaction, avoiding the formation of impurity phases and optimizing infrared emission performance.

Benefits of technology

It achieves a high emissivity of 0.95 at room temperature and 0.96 at 500℃, significantly improving the infrared emissivity and high-temperature thermal stability of bismuth oxide materials, making it suitable for high-temperature thermal protection coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062004A_ABST
    Figure CN123062004A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder, belonging to the field of functional materials and their preparation technology. Based on a high-temperature ball milling process using a high-temperature mechanochemical method, this invention composites bismuth oxide and zinc oxide, and incorporates yttrium doping into the composite powder, achieving high-emissivity powder preparation in a short process and on a large scale. This invention improves the emissivity of bismuth oxide materials, providing excellent high-emissivity materials for fields such as high-emissivity coatings, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional materials and their preparation technology, and in particular to a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder. Background Technology

[0002] With the continuous development of aerospace technology, the interaction between aircraft and air during high-speed flight generates a large amount of heat, which causes aerodynamic heating effect on the surface of the aircraft. Radiation-type protective coatings can quickly radiate heat to the outside to reduce the heat conduction from the surface of the aircraft to the cabin, thus avoiding damage to the internal structure, electronic equipment and other critical components of the aircraft.

[0003] Since the 1960s and 70s, single-component compounds were first explored in the field of high-emissivity materials, with in-depth studies conducted on silicon carbide (SiC) and iron oxide (Fe2O3) as two single-component materials. However, silicon carbide is prone to oxidation under high-temperature or oxygen-rich conditions, making it unstable and easily leading to a decrease in emissivity. The infrared emissivity of iron oxide alone is insufficient. The functional properties of single materials are limited, and high-emissivity materials are no exception. To compensate for the shortcomings of single-component materials in specific infrared emissivity bands, materials with different high infrared emission characteristics are combined to achieve complementary enhancement of emissivity in various bands.

[0004] Bismuth oxide (Bi2O3) is a typical polycrystalline bismuth-based metal oxide infrared functional material. Its emissivity in the near-infrared band of 1.0–2.5 μm is 0.35–0.55, indicating strong near-infrared reflectivity. Its emissivity in the mid-infrared band of 3–5 μm is in the middle range of 0.60–0.70. It exhibits significantly high emissivity in the long-wave infrared atmospheric window of 8–14 μm. The emissivity of room-temperature stable α-phase bismuth oxide is 0.70–0.75, while the emissivity of defect-enriched β and δ crystal forms can be increased to 0.78–0.85.

[0005] Integrating dopant atoms into the matrix lattice to form substitutional or interstitial solid solutions, and utilizing heterovalent substitution to generate oxygen vacancies and lattice distortion, thereby enhancing lattice polarization, is a feasible path to improve the infrared emission performance of oxides. However, the crystal structure characteristics of different oxides vary significantly, and conventional doping modification often sacrifices lattice integrity for the improvement of the target performance. In the case of bismuth oxide, its infrared emission performance strongly depends on the ordered lattice vibrations maintained by the Bi-O bonds; once the crystallization behavior or lattice order of the matrix decreases, the vibrational response in the long-wave infrared region weakens, thus impairing emissivity. The technical contradiction in optimizing the emissivity of bismuth oxide lies in the fact that introducing defects through doping to improve emissivity must ensure that the crystal properties of bismuth oxide are not destroyed; however, maintaining the integrity of the matrix crystal structure and avoiding lattice distortion and grain refinement is also difficult to achieve effective doping modification. Therefore, the core challenge of doping modification is how to improve infrared emissivity while completely preserving the crystallinity of the bismuth oxide matrix, achieving both the modification effect and the integrity of the crystal structure.

[0006] In summary, providing a high infrared emissivity modification scheme for bismuth oxide composite systems, while simultaneously addressing multiple technical challenges such as interface impurity phase suppression, precise lattice doping, and high-temperature performance stability, and designing a short-process, mass-producible preparation process, is crucial for developing a bismuth oxide-based composite infrared emitting material that combines high infrared emissivity across the entire wavelength band, excellent high-temperature thermal stability, and suitability for large-scale production. This is a technical obstacle that urgently needs to be overcome in this field. Summary of the Invention

[0007] In view of the above-mentioned deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, further improving the infrared emissivity of bismuth oxide materials, and achieving short process and batch preparation.

[0008] To achieve the above objectives, the technical solution provided by the present invention is as follows: In a first aspect of the present invention, a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder is provided, comprising the following steps: (1) Prepare powdered raw materials according to a certain ratio, mix zinc oxide and bismuth oxide, then add yttrium oxide, and mix to obtain a mixture; (2) The mixture is combined with grinding aid and grinding beads to obtain ball milling material; (3) Under an inert atmosphere, the ball milling material is heated to a certain temperature and subjected to a high-temperature ball milling reaction. After the reaction is completed, the product is collected after cooling to obtain rare earth-doped bismuth oxide / zinc oxide high emissivity powder.

[0009] Preferably, in step (1), by mass ratio, 0.1 ≤ bismuth oxide : zinc oxide ≤ 10, 0 < yttrium oxide : zinc oxide ≤ 0.2.

[0010] Preferably, in step (1), the purity of bismuth oxide is ≥99.99%, the purity of zinc oxide is ≥99.99%, and the purity of yttrium oxide is ≥99.99%.

[0011] Preferably, in step (2), the grinding aid includes N,N-dimethylformamide (DMF) or ethanol, and the amount of grinding aid added is 2 wt.% to 5 wt.% of the mixture.

[0012] Preferably, in step (2), the ratio of the mixture to the grinding balls is (10~40):1.

[0013] Preferably, in step (2), the size distribution of the grinding beads is (1~10) mm: (1~5) mm: 1 mm, and the mass ratio of the grinding beads is (1~10): (1~10): (1~10).

[0014] Preferably, in step (3), the inert atmosphere is created by one or both of argon and nitrogen.

[0015] Preferably, in step (3), the temperature of the high-temperature ball milling reaction is 50~1200 ℃, the reaction time is 0.5~48 h, and the ball milling speed is 10~100 rpm.

[0016] In a second aspect of the present invention, a rare earth-doped bismuth oxide / zinc oxide high emissivity powder is provided, which is prepared by the preparation method provided in the first aspect of the present invention.

[0017] In a third aspect of the invention, an application of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder of the second aspect of the invention is provided, including: as an infrared radiation material for radiation-protective coatings.

[0018] Based on the above technical solutions, the design concept and principle of this invention are as follows: To further improve the infrared emissivity of bismuth oxide, this invention combines it with zinc oxide and simultaneously dops it with rare earth elements, preparing rare earth-doped bismuth oxide / zinc oxide (ZnO / Bi2O3:Y2O3) high infrared emissivity powder via a high-temperature mechanochemical method. Due to the unique advantages of the high-temperature mechanochemical method, the reaction temperature can be reduced, energy consumption saved, and it can be mass-produced in a single step, achieving the goal of short-process, large-scale production.

[0019] Specifically, bismuth oxide and zinc oxide readily form low-emissivity impurity phases at high temperatures. This invention utilizes a high-temperature mechanochemical method, employing mechanical activation to lower the reaction energy barrier, achieving uniform composite formation and element diffusion between the two phases. This ensures composite uniformity while completely avoiding impurity phase formation. Mechanical crushing and grain refinement constructs a nanoscale porous microstructure, optimizing infrared emission performance. High temperature promotes element diffusion, enabling the diffusion of yttrium ions (Y). 3+ The uniform solid solution in the bismuth oxide lattice allows for doping modification without subsequent heat treatment. Furthermore, the two phases are uniformly bonded at the interface under mechanical and thermal action, avoiding interfacial impurities caused by sintering.

[0020] As the characterization results in one or more embodiments of the present invention show, X-ray diffraction results indicate that the product contains standard characteristic diffraction peaks of bismuth oxide and zinc oxide, while yttrium ions selectively dissolve into the bismuth oxide lattice without forming an independent yttrium oxide phase, indicating that the process successfully solved the problem of impurity phases in multi-component composite doping. Furthermore, yttrium ions and bismuth ions (Bi... 3+ The difference in ionic radius induces lattice distortion and simultaneously generates a large number of oxygen vacancies. These lattice defects enhance phonon vibrations and infrared absorption transitions, thereby increasing the emissivity of the material. The aforementioned selective solid solution behavior and target are specific results for the zinc oxide / bismuth oxide system.

[0021] It is important to note that existing technologies include methods for forming composite materials from bismuth oxide and zinc oxide, or methods based on rare earth oxide doping. For example, Chinese invention patent (CN120664870A) discloses a method for preparing polycrystalline ceramics using zinc oxide as the main component and bismuth oxide as a necessary additive phase, doped with various rare earth oxides, via a solid-state method. The technical principle is to utilize rare earth ions to replace lattice sites and form a bismuth-rich second phase at grain boundaries, thereby inhibiting grain growth and regulating the microstructure. However, this method belongs to the field of electronic functional ceramics, aiming to regulate varistor voltage and nonlinear electrical characteristics, and should not be categorized with the infrared functional materials of this invention. Mechanistically, in existing methods, the core role of rare earth oxides is grain boundary segregation and the formation of a bismuth-rich second phase, which optimizes electrical performance by inhibiting zinc oxide grain growth; the doping target is the grain boundary. In contrast, in this method, yttrium enters the bismuth oxide lattice in ionic form through solid solution, enhancing infrared radiation transitions through oxygen vacancies and lattice distortion; the doping target is the matrix lattice. These two methods belong to different mechanisms and have different regulatory targets. In terms of process, existing processes employ a multi-step solid-state method involving room-temperature ball milling, molding, and high-temperature sintering, producing dense bulk ceramics. This solution, however, uses a one-step high-temperature ball milling method to prepare functional powders, resulting in a shorter process and avoiding grain coarsening and impurity phase formation caused by high-temperature sintering. Similarly, Chinese invention patent (CN116835973A) discloses the structural features of a two-phase composite of bismuth oxide and zinc oxide. However, in the field of infrared emission, bismuth oxide and zinc oxide readily react during conventional high-temperature treatment to form impurities such as bismuth-zinc spinel and low-melting-point bismuth-zinc glass. The infrared emissivity of these phases is far lower than that of the pure matrix phase, degrading overall emission performance. In terms of performance, relying solely on the physical mixing of two phases lacks precise control over lattice defects and microstructure, making a step-wise increase in emissivity impossible. Furthermore, this existing process has not been optimized for the emissivity and thermal stability of materials at high temperatures, lacking adaptability for high-temperature thermal protection scenarios.

[0022] Based on this process, the present invention ultimately achieves high emissivity performance optimization, which is the result of the synergistic effect of multiple mechanisms, including zinc oxide / bismuth oxide band complementarity, interface defect absorption, yttrium doping lattice distortion, and scattering by the porous structure of the product. As demonstrated by the actual performance advantages of this invention, the average emissivity reaches 0.95 at room temperature (2–16 μm) and 0.96 at 500 °C, overcoming the emissivity decay of existing materials such as silicon carbide at high temperatures, and achieving emission performance far exceeding that of single-component bismuth oxide and single zinc oxide.

[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention provides a method for preparing rare-earth-doped bismuth oxide / zinc oxide high-emissivity powders. Based on a high-temperature ball milling process using a high-temperature mechanochemical method, bismuth oxide and zinc oxide are composited, and yttrium is doped into the composite powder. This method enables the large-scale preparation of high-emissivity powders in a short process. This invention improves the emissivity of bismuth oxide materials, providing excellent high-emissivity materials for fields such as high-emissivity coatings, and has broad application prospects. Attached Figure Description

[0024] Figure 1 The X-ray diffraction (XRD) pattern of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1; Figure 2 The images show scanning electron microscope (SEM) images of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1 and energy dispersive X-ray spectroscopy (EDS) spectra of each sampling area. Figure 3 Thermogravimetric (TG) curves of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1. Figure 4 The results are obtained by differential scanning calorimetry (DSC) of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1. Figure 5 The infrared transmittance test results of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1 at room temperature; Figure 6 The results of infrared reflectance test at room temperature for the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1; Figure 7 The infrared transmittance test results of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1 at high temperature (500 °C); Figure 8 The infrared reflectance test results of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in Example 1 at high temperature (500 °C). Detailed Implementation

[0025] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.

[0026] Example 1 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 10 g of zinc oxide powder into a sealed bag, then add 10 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 4 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 200 g: 100 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 10 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus to obtain rare earth doped bismuth oxide / zinc oxide high emissivity powder (ZnO / Bi2O3:Y2O3).

[0027] Example 2 This embodiment provides a rare earth-doped bismuth oxide / zinc oxide high emissivity powder, which is prepared using the preparation method of Example 1.

[0028] XRD analysis was performed on the rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder of this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The results are as follows: Figure 1 As shown, XRD results indicate that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material can be precisely matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF98-005-3797), respectively, with no extra impurity diffraction peaks, indicating high product purity. No diffraction signal of the Y2O3 phase alone was observed in the spectrum, proving that rare earth Y element is dissolved into the Bi2O3 lattice via ion doping, inducing lattice distortion and introducing oxygen vacancies. The synergistic regulation of lattice vibration characteristics by polycrystalline phase composite and rare earth doping can effectively enhance the infrared absorption efficiency of the system in the 8–14 μm long-wave infrared window, thereby improving infrared emissivity and simultaneously enhancing the stability of phase and radiation properties during high-temperature service.

[0029] The powder in this embodiment was subjected to SEM testing with an accelerating voltage of 15 kV. The sample morphology is as follows. Figure 2As shown, the corresponding EDS results are shown in Tables 1-3.

[0030] Table 1: EDS spectra of rare earth-doped bismuth oxide / zinc oxide high emissivity powder samples from Example 2 (18 Results)

[0031] Table 2: EDS spectra of rare earth-doped bismuth oxide / zinc oxide high emissivity powder samples from Example 2 (19 Results)

[0032] Table 3: EDS spectra of rare earth-doped bismuth oxide / zinc oxide high emissivity powder samples from Example 2 (20 Results)

[0033] The SEM results showed that the sample consisted of nanoscale particle agglomerations with abundant porous structures between the particles, which enhanced the infrared light scattering absorption effect. EDS elemental analysis was performed at three characteristic sites in different regions of the powder. The energy dispersive spectroscopy results detected four target elements: Zn, Bi, Y, and O, with no impurity element signals. Quantitative analysis indicated that Zn was the main constituent phase, while Bi and Y were stably present at all sites, proving that the zinc oxide and yttrium-doped bismuth oxide phases were uniformly composited at the microscopic level, and that rare earth yttrium was successfully dispersed and doped into the system without forming an independent phase. Combined with XRD results, this further confirms that Y... 3+ The ionic solid solution enters the Bi2O3 lattice and induces lattice defects. The porous microstructure and lattice distortion work together to improve the material's absorption efficiency of infrared radiation, ultimately optimizing the infrared emission performance.

[0034] The rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder of this embodiment was subjected to TG testing at a heating rate of 5°C / min in an air atmosphere. The results are as follows. Figure 3As shown in the figure. The TG curve shows that the sample did not lose weight throughout the heating range of 40~720 ℃, and showed a gradual weight increase trend. The initial sample mass was 11.0600 mg, and the final residual mass was 104.7103% of the initial mass. A significant mass increase occurred in the range of 260~380 ℃, corresponding to a strong exothermic peak at 275.53 ℃ in the derivative thermogravimetric curve (DTG). This process is attributed to the oxidation reaction of oxygen adsorbed at low-valence metal sites by lattice defects in the powder. When the temperature rises to 733.44 ℃, a sharp exothermic peak appears in the DTG curve, representing the phase transformation of Bi2O3 from the monoclinic α phase to the cubic δ phase. The absence of decomposition, volatilization, or other deterioration behaviors in the sample within the test temperature range indicates that the composite material possesses excellent thermal stability and resistance to high-temperature oxidation. The sample composition and phase can be stably maintained under infrared testing conditions at 500 ℃. As the temperature increases, the degree of material oxidation increases, the crystal structure is regulated, the infrared absorption capacity is continuously enhanced, and the infrared emissivity gradually increases with the temperature, making it suitable for infrared radiation thermal control under high-temperature conditions.

[0035] The powder in this embodiment was subjected to DSC testing, and the results are as follows: Figure 4 As shown, the sample exhibits significant exothermic behavior starting at 268.2 °C, reaching a peak exothermic temperature at 271.7 °C, and ending at 277.2 °C. The total enthalpy change of this oxidation-exothermic process reaches 44.9 J / g. This exothermic peak corresponds to the oxidation reaction between oxygen vacancies in the powder lattice and low-valence metal ions adsorbing oxygen from the air, filling the oxygen vacancies and regulating the lattice microstructure. In the range of 277.2 °C to 750 °C, the sample only exhibits weak and continuous exothermic behavior, without significant endothermic or sharp phase transition characteristic peaks, proving that the material will not undergo crystal transformation or thermal decomposition below 750 °C. Combined with the thermogravimetric test results above, it can be seen that the powder only undergoes slow oxidation modification at a high temperature of 500 °C, with stable phase and composition structure. Optimization of lattice defects can enhance the infrared radiation absorption effect. Therefore, the infrared emissivity is improved at high temperature compared to room temperature, and the material has good high-temperature thermal stability and potential for regulating infrared radiation performance.

[0036] Example 3 This embodiment tests the infrared emissivity at room temperature of the rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder from Example 2 to study its application performance. This embodiment can also be considered an application example of the rare-earth-doped bismuth oxide high-emissivity powder material.

[0037] Infrared transmittance and absorptivity at room temperature, such as Figure 5 and Figure 6As shown in the figure, the infrared emissivity at room temperature was calculated based on the law of conservation of energy and Kirchhoff's law of thermal radiation. Test results show that the infrared transmittance of the composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 1.5%–7.8%, especially in the 8–14 μm long-wave infrared atmospheric detection window where the reflectivity is lowest. Calculations show that the infrared emissivity of the sample in the 2–16 μm range can reach 0.92–0.98, with an average of 0.95, demonstrating excellent high infrared emission performance. The porous microstructure, rare-earth doping-induced lattice distortion, and the synergistic absorption effect of the ZnO / Bi2O3 dual-phase structure collectively weaken infrared reflection loss, allowing most of the incident infrared radiation to be absorbed by the material and released as thermal radiation, thus endowing the material with extremely strong infrared radiation heat dissipation capabilities.

[0038] Example 4 This embodiment tests the infrared emissivity at high temperature of the rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder from Example 2 to study its application performance. This embodiment can also be regarded as an application embodiment of the rare-earth-doped bismuth oxide high-emissivity powder material.

[0039] The rare earth-doped bismuth oxide / zinc oxide high emissivity powder sample from Example 2 was subjected to infrared emissivity testing at 500 °C. The infrared transmittance and absorptivity of the sample at 500 °C are as follows: Figure 7 and Figure 8 As shown in the figure, the infrared transmittance of the sample at this temperature fluctuates slightly around 0%, indicating that infrared light has difficulty penetrating the coating and the energy loss during transmission is negligible. The infrared reflectance of the sample ranges from 0% to 7%, which is slightly lower than the results at room temperature. Calculations based on energy conservation and Kirchhoff's law of thermal radiation show that the infrared emissivity of the sample at 500 °C can reach 0.93–0.99, with an average infrared emissivity as high as 0.96, a slight increase compared to room temperature conditions. This phenomenon stems from the intensified thermal vibration of the material's lattice during heating, coupled with the continuous adsorption of oxygen at lattice defect sites, leading to oxidation modification and further enhancing the absorption capacity of the ZnO and Y-doped Bi₂O₃ dual system for infrared radiation.

[0040] In summary, this invention uses a high-temperature mechanochemical method to prepare ZnO / Bi2O3:Y2O3. The prepared material can effectively improve the infrared emissivity of Bi2O3 and ZnO, and has an average emissivity of 95 at room temperature and an average emissivity of 96 at high temperature, making it an excellent high-temperature thermal protective coating.

[0041] Example 5 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 10 g of zinc oxide powder into a sealed bag, then add 5 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 4 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 200 g: 100 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 10 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus to obtain rare earth doped bismuth oxide / zinc oxide high emissivity powder.

[0042] The rare earth-doped bismuth oxide / zinc oxide high emissivity powder prepared in this embodiment was tested using the characterization methods described above.

[0043] XRD analysis was performed on the rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder of this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The XRD test results showed that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material could be accurately matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF 98-005-3797), respectively. There were no extra impurity diffraction peaks, and the product purity was high. However, compared with Example 2, the peak value of Bi2O3 decreased, which indirectly reflects that the content was reduced. No diffraction signal of Y2O3 alone was observed in the spectrum, which proved that the rare earth Y element was dissolved into the Bi2O3 lattice in the form of ion doping, causing lattice distortion and introducing oxygen vacancies. The polycrystalline phase composite and rare earth doping synergistically regulate the lattice vibration characteristics of the material.

[0044] The infrared emissivity of rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder was tested, and the infrared emissivity was calculated at room temperature based on the law of conservation of energy and Kirchhoff's law of thermal radiation. The test results show that the infrared transmittance of this composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 2.6%–8.4%, especially in the 8–14 μm long-wave infrared atmospheric detection window where the reflectivity is lowest. Calculations show that the infrared emissivity of the sample can reach 0.90–0.96 in the 2–16 μm range, with an average infrared emissivity of 0.93. Although the emissivity decreases, it still exhibits excellent high infrared emission performance.

[0045] To investigate the sample performance at high temperatures, the sample in this embodiment was tested at 500 °C. The sample transmittance was almost 0%, and the overall infrared reflectance ranged from 3% to 9%, which was slightly lower than the results at room temperature. At 500 °C, the infrared emissivity of the sample reached 0.91 to 0.97, with an average infrared emissivity as high as 0.94, showing a slight increase compared to room temperature conditions.

[0046] Example 6 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 5 g of zinc oxide powder into a sealed bag, then add 10 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 4 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 200 g: 100 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 10 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus to obtain rare earth doped bismuth oxide / zinc oxide high emissivity powder.

[0047] XRD analysis was performed on the rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder of this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The XRD test results showed that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material could be accurately matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF 98-005-3797), respectively. There were no extra impurity diffraction peaks, and the product purity was high. However, compared with Example 7, the peak value of ZnO decreased, which indirectly reflects that the content was reduced. No diffraction signal of Y2O3 alone was observed in the spectrum, which proved that the rare earth Y element was dissolved into the Bi2O3 lattice in the form of ion doping, causing lattice distortion and introducing oxygen vacancies. The polycrystalline phase composite and rare earth doping synergistically regulate the lattice vibration characteristics of the material.

[0048] The infrared emissivity of rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder was tested. The infrared emissivity was calculated at room temperature based on the law of conservation of energy and Kirchhoff's law of thermal radiation. Test results show that the infrared transmittance of this composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 2.7%–8.5%, especially in the 8–14 μm long-wave infrared atmospheric detection window where the reflectivity is lowest. Calculations show that the infrared emissivity of the sample reaches 0.91–0.97 in the 2–16 μm range, with an average infrared emissivity of 0.94. Although the emissivity decreases, it still exhibits excellent high infrared emission performance.

[0049] To investigate the performance of samples at high temperatures, rare-earth-doped bismuth oxide / zinc oxide high-emissivity powder samples were tested at 500℃. The transmittance of the samples was almost 0%, and the infrared reflectance ranged from 2% to 9%, which was slightly lower than the results at room temperature. At 500℃, the infrared emissivity of the samples reached 0.91 to 0.98, with an average infrared emissivity as high as 0.945, showing a slight increase compared to room temperature conditions.

[0050] Example 7 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 10 g of zinc oxide powder into a sealed bag, then add 10 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 4 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 100 g: 200 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 10 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus and then taken out for tissue structure and performance testing.

[0051] XRD analysis was performed on the samples in this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The XRD test results showed that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material could be precisely matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF 98-005-3797), respectively. There were no extra impurity diffraction peaks, indicating high product purity. No diffraction signal of Y2O3 alone was observed in the spectrum, proving that rare earth Y element was dissolved into the Bi2O3 lattice in the form of ion doping, inducing lattice distortion and introducing oxygen vacancies. The polycrystalline phase composite and rare earth doping synergistically regulate the lattice vibration characteristics of the material.

[0052] The infrared emissivity of the sample was tested, and calculated at room temperature based on the law of conservation of energy and Kirchhoff's law of thermal radiation. The test results show that the infrared transmittance of the composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 2.1%–8.1%, especially in the 8–14 μm long-wave infrared atmospheric detection window where the reflectivity is lowest. Calculations show that the infrared emissivity of the sample reaches 0.93–0.96 in the 2–16 μm range, with an average infrared emissivity of 0.945. Although the emissivity decreases, it still exhibits excellent high infrared emission performance.

[0053] To investigate the sample performance at high temperatures, the samples were tested at 500 °C. The sample transmittance was almost 0%, and the infrared reflectance ranged from 3% to 7%, which was slightly lower than the results at room temperature. At 500 °C, the infrared emissivity of the samples reached 0.93 to 0.97, with an average infrared emissivity as high as 0.95, showing a slight increase compared to room temperature conditions.

[0054] Example 8 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 10 g of zinc oxide powder into a sealed bag, then add 10 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 2 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 200 g: 100 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 10 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus and then taken out for tissue structure and performance testing.

[0055] XRD analysis was performed on the samples in this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The XRD test results showed that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material could be precisely matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF 98-005-3797), respectively. There were no extra impurity diffraction peaks, indicating high product purity. No diffraction signal of Y2O3 alone was observed in the spectrum, proving that rare earth Y element was dissolved into the Bi2O3 lattice in the form of ion doping, inducing lattice distortion and introducing oxygen vacancies. The polycrystalline phase composite and rare earth doping synergistically regulate the lattice vibration characteristics of the material.

[0056] The infrared emissivity of the sample was tested, and calculated at room temperature based on the law of conservation of energy and Kirchhoff's law of thermal radiation. The test results show that the infrared transmittance of the composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 2.8%–8.7%, with the lowest reflectivity observed in the 8–14 μm long-wave infrared atmospheric detection window. Calculations show that the infrared emissivity of the sample reaches 0.91–0.97 in the 2–16 μm range, with an average infrared emissivity of 0.94. While the emissivity decreases, it still exhibits excellent high infrared emission performance.

[0057] To investigate the sample performance at high temperatures, the samples were tested at 500 °C. The sample transmittance was almost 0%, and the infrared reflectance ranged from 2% to 9%, which was slightly lower than the results at room temperature. At 500 °C, the infrared emissivity of the samples reached 0.91 to 0.98, with an average infrared emissivity as high as 0.945, showing a slight increase compared to room temperature conditions.

[0058] Example 9 This embodiment provides a method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, the steps of which are as follows: (1) After polishing the grinding jar, it is cleaned with deionized water, ethanol and acetone in sequence, and then dried at 80 °C to obtain a grinding jar without impurities. Place 10 g of zinc oxide powder into a sealed bag, then add 10 g of bismuth oxide into the sealed bag, shake well, then add 0.5 g of yttrium oxide into the sealed bag, shake the sealed bag to mix the three powders evenly. (2) Add the well-mixed powder into the ball mill jar, then add 4 wt.% DMF as a grinding aid, and then put the grinding beads with a size of 12 mm: 8 mm: 4 mm into the grinding jar at a mass ratio of 200 g: 100 g: 100 g and mix them evenly. (3) Place the prepared grinding jar into the inner cavity of the high-temperature mechanochemical apparatus and react at 500 °C and 60 r / min for 5 h, with argon atmosphere throughout. After the reaction is completed, the sample is cooled to room temperature with the apparatus and then taken out for tissue structure and performance testing.

[0059] XRD analysis was performed on the samples in this embodiment. The test conditions were: Cu Kα target, scanning range 2θ of 10°~90°, and scanning step size of 0.02°. The XRD test results showed that the diffraction characteristic peaks of the prepared ZnO / Bi2O3:Y2O3 composite material could be precisely matched with the standard cards of ZnO (PDF 98-006-7848) and Bi2O3 (PDF 98-005-3797), respectively. There were no extra impurity diffraction peaks, and the product purity was high. However, compared with Example 7, the peak value of ZnO decreased due to the shorter time, which indirectly reflects the reduced content. No diffraction signal of Y2O3 alone was observed in the spectrum, proving that rare earth Y element was dissolved into the Bi2O3 lattice in the form of ion doping, causing lattice distortion and introducing oxygen vacancies. The polycrystalline phase composite and rare earth doping synergistically regulate the lattice vibration characteristics of the material.

[0060] The infrared emissivity of the sample was tested, and calculated at room temperature based on the law of conservation of energy and Kirchhoff's law of thermal radiation. The test results show that the infrared transmittance of the composite sample is essentially close to zero across the entire infrared spectrum, indicating that infrared light has difficulty penetrating the coating material. The infrared reflectivity of the sample remains at a low level of 4.5%–10.5%, with the lowest reflectivity observed in the 8–14 μm long-wave infrared atmospheric detection window. Calculations show that the infrared emissivity of the sample reaches 0.89–0.95 in the 2–16 μm range, with an average infrared emissivity of 0.92. While the emissivity decreases, it still exhibits excellent high infrared emission performance.

[0061] To investigate the sample performance at high temperatures, the sample was tested at 500 °C. The sample transmittance was almost 0%, and the infrared reflectance ranged from 2% to 10%, which was slightly lower than the results at room temperature. At 500 °C, the infrared emissivity of the sample reached 0.90–0.98, with an average infrared emissivity as high as 0.94, showing a slight increase compared to room temperature conditions.

[0062] Those skilled in the art can select other parameter combinations based on the optimal parameter range of this invention, according to actual production conditions or needs, and can also achieve the basic purpose of this invention.

[0063] In summary, this process, based on high-temperature ball milling using a high-temperature mechanochemical method, combines bismuth oxide and zinc oxide, and incorporates yttrium doping into the composite powder. This allows for the rapid, large-scale preparation of high-emissivity powders in a short process. This invention improves the emissivity of bismuth oxide materials, providing excellent high-emissivity materials for fields such as high-emissivity coatings, and possesses broad application prospects.

[0064] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder, characterized in that, Includes the following steps: (1) Prepare powdered raw materials according to a certain ratio, mix zinc oxide and bismuth oxide, then add yttrium oxide, and mix to obtain a mixture; (2) The mixture is combined with grinding aid and grinding beads to obtain ball milling material; (3) Under an inert atmosphere, the ball milling material is heated to a certain temperature and subjected to a high-temperature ball milling reaction. After the reaction is completed, the product is collected after cooling to obtain rare earth-doped bismuth oxide / zinc oxide high emissivity powder.

2. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (1), by mass ratio, 0.1 ≤ bismuth oxide : zinc oxide ≤ 10, 0 < yttrium oxide : zinc oxide ≤ 0.

2.

3. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (1), the purity of bismuth oxide is ≥99.99%, the purity of zinc oxide is ≥99.99%, and the purity of yttrium oxide is ≥99.99%.

4. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (2), the grinding aid includes N,N-dimethylformamide or ethanol, and the amount of the grinding aid added is 2 wt.% to 5 wt.% of the mixture.

5. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (2), the ratio of the mixture to the grinding balls is (10~40):

1.

6. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: The size distribution of the grinding beads is (1~10) mm: (1~5) mm: 1 mm, and the mass ratio of the grinding beads is (1~10): (1~10): (1~10).

7. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (3), the inert atmosphere is created by one or both of argon and nitrogen.

8. The method for preparing rare earth-doped bismuth oxide / zinc oxide high emissivity powder according to claim 1, characterized in that: In step (3), the temperature of the high-temperature ball milling reaction is 50~1200 ℃, the reaction time is 0.5~48 h, and the ball milling speed is 10~100 rpm.

9. A rare earth-doped bismuth oxide / zinc oxide high emissivity powder, characterized in that: It is prepared by any one of the preparation methods described in claims 1 to 8.

10. An application of the rare earth-doped bismuth oxide / zinc oxide high emissivity powder as described in claim 9, characterized in that, include: It is used as an infrared radiation material in radiation-protective coatings.

Citation Information

Patent Citations

  • Bismuth oxide coated zinc oxide powder as well as preparation method and application thereof

    CN116835973A

  • Luminous multifunctional ZnO-Bi2O3-based voltage-sensitive ceramic as well as preparation method and application thereof

    CN120664870A