A low-dielectric borosilicate glass, its preparation method and application

By precisely controlling the chemical composition and preparation process of borosilicate glass, the problems of easy phase separation and high viscosity at high temperatures in high-frequency signal transmission have been solved, achieving the effects of low dielectric constant and low dielectric loss, making it suitable for high-frequency electronic device packaging.

CN123062162APending Publication Date: 2026-11-10IRICO +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610951720.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing borosilicate glass is prone to phase separation and has unstable dielectric properties in high-frequency signal transmission, making it difficult to simultaneously meet the requirements of low dielectric constant and low dielectric loss. Furthermore, it has high viscosity at high temperatures, making it difficult to melt.

Method used

By precisely controlling the molar percentages of SiO2, B2O3, Al2O3, La2O3, and alkali metal oxides, the dielectric and process properties are optimized. The glass is formed using a pull-down or melt-forming method, combined with annealing treatment, to control the viscosity and dielectric properties of the glass.

Benefits of technology

It achieves a dielectric constant of less than 6 and a dielectric loss of less than 100×10-4 at a frequency of 10GHz, meeting the packaging requirements of high-frequency electronic devices. Moreover, the process is simple and efficient, and suitable for mass production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a low-dielectric borosilicate glass, its preparation method, and its applications, relating to the field of electronic materials technology. The chemical composition, by molar percentage, includes: 70-85.5% SiO2, 0.5-4% Al2O3, 10-16.5% B2O3, 0-2.5% Li2O, 0.1-5% Na2O, 0-2.5% K2O, 0.1-1% CaO+SrO, 0.1-0.5% La2O3, 0-0.5% Y2O3, and 0.1-1% F2+Cl2, with the molar ratio of Al2O3 to Li2O+Na2O+K2O greater than 0.2. This material exhibits a dielectric constant of less than 6 and a dielectric loss of less than 100 × 10⁻⁶ at a frequency of 10 GHz. ‑4 At a viscosity of 10000P, the viscosity temperature is less than 1250℃. Through component synergistic design, phase separation is suppressed and dielectric properties are reduced, making it suitable for high-frequency electronic device packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic materials technology, specifically relating to a low-dielectric borosilicate glass, its preparation method, and its application. Background Technology

[0002] With the rapid development of 5G mobile communication, millimeter-wave radar, high-speed integrated circuits, and artificial intelligence computing clusters, the operating frequencies of electronic components are constantly increasing, placing unprecedentedly stringent requirements on the dielectric properties of packaging materials. In high-frequency signal transmission, the dielectric constant (Dk) of the packaging material directly determines the signal transmission delay in the medium, while the dielectric loss (Df) directly affects signal integrity and energy attenuation. Therefore, developing packaging materials with ultra-low dielectric constants and ultra-low dielectric losses has become a key technical challenge in the field of electronic materials.

[0003] Glass materials, due to their excellent electrical insulation, thermal stability, and chemical stability, are gradually becoming an important alternative to traditional organic packaging materials. Among them, borosilicate glass, with its excellent thermal and chemical stability, has broad application prospects in the field of electronic packaging. However, traditional borosilicate glass is prone to liquid-phase separation (phase separation) within a certain composition range, forming boron-rich and silicon-rich phases, resulting in inhomogeneous microstructure, which in turn causes fluctuations in dielectric properties, decreased mechanical strength, and deterioration in chemical stability, seriously affecting the long-term reliability of packaged devices. Secondly, the high SiO2 content in the borosilicate glass system leads to high viscosity at high temperatures and difficulty in melting; although B2O3 can be used as a flux to reduce viscosity, simply increasing B2O3 will exacerbate the phase separation tendency. Thirdly, the effect of boron on dielectric loss is closely related to its structure: when boron exists in the form of [BO4] tetrahedra, it helps to reduce dielectric loss, while when it exists in the form of [BO3] trigonal prisms, it increases dielectric loss; although the introduction of alkali metal oxides can reduce viscosity, it will significantly increase dielectric loss. Existing technologies lack a systematic design that considers the synergistic effects of the components, especially at high frequencies (such as 10 GHz) to simultaneously achieve a dielectric constant of less than 6 and a dielectric loss of less than 100 × 10⁻⁶. -4 Difficulties still exist. Summary of the Invention

[0004] In order to overcome the shortcomings of the prior art, the present invention aims to provide a low-dielectric borosilicate glass, its preparation method and application, so as to solve the technical problems of easy phase separation, excessively high viscosity at high temperature and difficulty in meeting the requirements of high frequency packaging for both dielectric constant and dielectric loss in the prior art.

[0005] To achieve the above objectives, the present invention employs the following technical solution: In a first aspect, the present invention provides a low-dielectric borosilicate glass, the chemical composition of which, in molar percentage, comprises: 70%~85.5% SiO2, 0.5%~4% Al2O3, 10%~16.5% B2O3, 0%~2.5% Li2O, 0.1%~5% Na2O, 0%~2.5% K2O, 0.1%~1% CaO+SrO, 0.1%~0.5% La2O3, 0%~0.5% Y2O3, and 0.1%~1% F2+Cl2.

[0006] A further improvement of the present invention is that the ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O and K2O is greater than 0.2.

[0007] A further improvement of the present invention is that, in mole percentage, its chemical composition includes: 75%~82% SiO2, 1%~3% Al2O3, 12%~15% B2O3, 0.5%~2% Li2O, 1%~4% Na2O, 0.5%~2% K2O, 0.3%~0.8% CaO+SrO, 0.2%~0.4% La2O3, 0.1%~0.5% Y2O3, and 0.3%~0.8% F2+Cl2.

[0008] A further improvement of the present invention is that the temperature of the low-dielectric borosilicate glass at a viscosity of 10,000 poise is below 1250°C.

[0009] A further improvement of this invention is that the low-dielectric borosilicate glass has a dielectric constant of less than 6 and a dielectric loss of less than 100 × 10⁻⁶ at a frequency of 10 GHz. -4 .

[0010] Secondly, the present invention also provides a method for preparing low-dielectric borosilicate glass, comprising the following steps: S1. Mix the raw materials weighed according to the design ratio evenly to obtain the batch material; S2, the batch material is melted, clarified and homogenized to obtain molten glass; S3, the molten glass is shaped to obtain a glass sample block; S4. The formed glass sample is annealed and then cooled to room temperature to obtain the low-dielectric borosilicate glass.

[0011] A further improvement of the present invention is that the melting temperature in S2 is less than 1700°C.

[0012] A further improvement of the present invention is that the molding described in S3 is performed using a pull-down method or a melt-forming method.

[0013] A further improvement of the present invention is that the annealing temperature in S4 is 500~600℃, the holding time is 2~4 hours, and the cooling rate is 0.5~2℃ / minute.

[0014] Thirdly, the present invention also provides the application of low-dielectric borosilicate glass in the preparation of electronic chip packaging materials.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a low-dielectric borosilicate glass that achieves synergistic optimization of dielectric properties and processing performance by precisely controlling the molar percentage range of key components such as SiO2, B2O3, Al2O3, La2O3 and alkali metal oxides. The SiO2 content is controlled between 70% and 85.5% to ensure the mechanical strength and chemical stability of the glass; the B2O3 content is limited to 10% to 16.5%, which can effectively reduce the dielectric constant and high-temperature viscosity, while avoiding phase separation tendency caused by excessive content; the Al2O3 content is in the range of 0.5% to 4%, and the molar ratio of Al2O3 to Li2O, Na2O, and K2O is ensured to be greater than 0.2, thereby effectively suppressing the common liquid phase separation phenomenon in borosilicate glasses and improving material consistency and reliability. The trace introduction of La2O3 at 0.1% to 0.5% helps to further reduce dielectric loss without significantly increasing polarization loss; in addition, through a reasonable ratio of alkali metals and alkaline earth metals and the introduction of Y2O3, the temperature of the glass at a viscosity of 10,000 poise can be controlled below 1250°C. Through the synergistic design of the above components, the glass material of the present invention can achieve a dielectric constant of less than 6 and a dielectric loss of less than 100 × 10⁻⁶ at a frequency of 10 GHz. -4 Its superior performance effectively reduces signal transmission delay and loss, meeting the dual requirements of high-frequency electronic device packaging for material dielectric properties and molding processes.

[0016] This invention also provides a method for preparing low-dielectric borosilicate glass, comprising four steps: raw material mixing, melting, clarification and homogenization, forming, and annealing and cooling. This method is simple and continuous; the raw materials are directly melted, clarified, and homogenized at high temperature after mixing, eliminating the need for intermediate pretreatment or step-by-step melting, effectively shortening the overall process cycle and improving production efficiency. The forming step is flexibly adaptable to industrial production methods such as the pull-down method or the melting method, enabling continuous and stable preparation of large-size glass substrates to meet the needs of large-scale production. The annealing step is specifically designed for the glass properties of this component system. By controlling the annealing temperature range, it can effectively eliminate internal thermal stress in the glass, prevent cracks or deformation during cooling, and improve product yield and dimensional stability. The entire process parameters can be flexibly adjusted according to the actual composition, eliminating the need for complex and expensive specialized equipment, and facilitating easy transfer and scale-up between laboratory pilot tests and large-scale industrial production. Therefore, the preparation method of this invention solves the technical problem of balancing low dielectric properties and efficient forming in existing processes, and has good prospects for industrial application.

[0017] Furthermore, the borosilicate glass prepared by this invention is particularly suitable for electronic chip packaging and can meet the stringent requirements of high-frequency electronic devices for packaging materials. Detailed Implementation

[0018] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0019] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0020] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0021] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0022] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0023] This invention provides a low-dielectric borosilicate glass, whose chemical composition, by mole percentage, comprises: 70%~85.5% SiO2, 0.5%~4% Al2O3, 10%~16.5% B2O3, 0%~2.5% Li2O, 0.1%~5% Na2O, 0%~2.5% K2O, 0.1%~1% CaO+SrO, 0.1%~0.5% La2O3, 0%~0.5% Y2O3, and 0.1%~1% F2+Cl2, wherein the molar ratio of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is greater than 0.2.

[0024] Preferably, its chemical composition, by mole percentage, includes: 75%~82% SiO2, 1%~3% Al2O3, 12%~15% B2O3, 0.5%~2% Li2O, 1%~4% Na2O, 0.5%~2% K2O, 0.3%~0.8% CaO+SrO, 0.2%~0.4% La2O3, 0.1%~0.5% Y2O3, and 0.3%~0.8% F2+Cl2. This low-dielectric borosilicate glass has a temperature below 1250℃ at a viscosity of 10000 poise, a dielectric constant of less than 6 at a frequency of 10 GHz, and a dielectric loss of less than 100 × 10⁻⁶. -4 .

[0025] This invention also provides a method for preparing low-dielectric borosilicate glass, comprising the following steps: S1. Mix the raw materials weighed according to the design ratio evenly to obtain the batch material; S2, the batch material is melted, clarified and homogenized at a temperature below 1700°C to obtain molten glass; S3, the molten glass is formed by the downward pulling method or the melting method to obtain a glass sample block; S4. The formed glass sample is annealed at 500~600℃ for 2~4 hours, and then cooled to room temperature at a cooling rate of 0.5~2℃ / min to obtain the low dielectric borosilicate glass.

[0026] This invention also provides the application of low-dielectric borosilicate glass in the preparation of electronic chip packaging materials.

[0027] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0028] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" represents weight percentage, "parts" represents parts by weight, and "ratio" represents weight proportion.

[0029] Example 1 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 80%, Al2O3: 1.5%, B2O3: 11%, Li2O: 2.4%, Na2O: 3.5%, K2O: 0.4%, CaO: 0.3%, SrO: 0.2%, La2O3: 0.3%, F2: 0.2%, Cl2: 0.2%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.24, which is greater than 0.2.

[0030] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0031] (2) The batch material is melted, clarified and homogenized at 1680℃, and then shaped to obtain a glass sample.

[0032] (3) The formed glass sample is annealed at a temperature of 570°C for 4 hours and then cooled to room temperature at a rate of 0.5°C / minute to obtain the low dielectric borosilicate glass.

[0033] Performance testing: The dielectric properties of the glass at 10 GHz were determined using the resonant cavity method. The results showed that its dielectric constant was 5.3 and its dielectric loss was 85 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1200℃.

[0034] Example 2 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 81%, Al2O3: 1%, B2O3: 12%, Li2O: 0.5%, Na2O: 3.3%, K2O: 0.4%, CaO: 0.5%, SrO: 0.3%, La2O3: 0.4%, F2: 0.3%, Cl2: 0.3%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.24, which is greater than 0.2.

[0035] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0036] (2) The batch material is melted, clarified and homogenized at 1680℃, and then shaped to obtain a glass sample.

[0037] (3) The formed glass sample is annealed at a temperature of 580°C for 2 hours and then cooled to room temperature at a rate of 2°C / minute to obtain the low dielectric borosilicate glass.

[0038] Performance testing: The dielectric properties of the glass at a frequency of 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 5.2 and its dielectric loss was 72 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1180℃.

[0039] Example 3 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 81.5%, Al2O3: 1%, B2O3: 11.5%, Li2O: 0.2%, Na2O: 3.5%, K2O: 0.3%, CaO+SrO: 0.6%, La2O3: 0.2%, Y2O3: 0.5%, F2+Cl2: 0.7%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.25, which is greater than 0.2.

[0040] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0041] (2) The batch material is melted, clarified and homogenized at 1680℃, and then formed by melting to obtain a glass sample.

[0042] (3) The formed glass sample is annealed at a temperature of 590°C for 3 hours and then cooled to room temperature at a rate of 1°C / minute to obtain the low dielectric borosilicate glass.

[0043] Performance testing: The dielectric properties of the glass at a frequency of 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 4.9 and its dielectric loss was 80 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1230℃.

[0044] Example 4 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 81%, Al2O3: 1.4%, B2O3: 12%, Li2O: 1.5%, Na2O: 3.2%, K2O: 0.4%, CaO+SrO: 0.2%, La2O3: 0.1%, F2+Cl2: 0.2%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.27, which is greater than 0.2.

[0045] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0046] (2) The batch material is melted, clarified and homogenized at 1680℃, and then formed by melting to obtain a glass sample.

[0047] (3) The formed glass sample is annealed at a temperature of 530°C for 3 hours and then cooled to room temperature at a rate of 2°C / minute to obtain the low dielectric borosilicate glass.

[0048] Performance testing: The dielectric properties of the glass at a frequency of 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 4.4 and its dielectric loss was 60 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1190℃.

[0049] Example 5 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition in molar percentage: SiO2: 77%, Al2O3: 1.8%, B2O3: 16.2%, Na2O: 3%, K2O: 1.2%, CaO+SrO: 0.5%, La2O3: 0.1%, F2+Cl2: 0.2%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.43, which is greater than 0.2 (Li2O is not present in this embodiment, therefore Li2O is counted as 0).

[0050] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0051] (2) The batch material is melted, clarified and homogenized at 1680℃, and then formed by melting to obtain a glass sample.

[0052] (3) The formed glass sample is annealed at a temperature of 520°C for 3 hours and then cooled to room temperature at a rate of 1°C / minute to obtain the low dielectric borosilicate glass.

[0053] Performance testing: The dielectric properties of the glass at 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 4.5 and its dielectric loss was 67 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1190℃.

[0054] Example 6 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 70%, Al2O3: 4%, B2O3: 13%, Li2O: 2.5%, Na2O: 5%, K2O: 2.5%, CaO+SrO: 1%, La2O3: 0.5%, Y2O3: 0.5%, F2+Cl2: 1%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.4, which is greater than 0.2.

[0055] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0056] (2) The batch material is melted, clarified and homogenized at 1680℃, and then shaped to obtain a glass sample.

[0057] (3) The formed glass sample is annealed at a temperature of 520°C for 3 hours and then cooled to room temperature at a rate of 1°C / minute to obtain the low dielectric borosilicate glass.

[0058] Performance testing: The dielectric properties of the glass at a frequency of 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 5.2 and its dielectric loss was 95 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1240℃.

[0059] Example 7 This embodiment provides a low-dielectric borosilicate glass with the following chemical composition by mole percentage: SiO2: 85.5%, Al2O3: 0.5%, B2O3: 10%, Li2O: 1%, Na2O: 0.1%, K2O: 0.8%, CaO+SrO: 1%, La2O3: 0.5%, Y2O3: 0.5%, F2+Cl2: 0.1%. The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O, and K2O is 0.26, which is greater than 0.2.

[0060] The preparation method of this low-dielectric borosilicate glass is as follows: (1) Weigh each raw material according to the molar percentage of the above chemical components, mix them evenly, and obtain the compound.

[0061] (2) The batch material is melted, clarified and homogenized at 1680℃, and then formed by melting to obtain a glass sample.

[0062] (3) The formed glass sample is annealed at a temperature of 580°C for 4 hours and then cooled to room temperature at a rate of 2°C / minute to obtain the low dielectric borosilicate glass.

[0063] Performance testing: The dielectric properties of the glass at a frequency of 10 GHz were measured using the resonant cavity method. The results showed that its dielectric constant was 4.2 and its dielectric loss was 55 × 10⁻⁶. -4 The viscosity of the glass was tested using a 1700℃ high-temperature viscometer, and the temperature at which the viscosity reached 10,000 poise was 1240℃.

[0064] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.

Claims

1. A low-dielectric borosilicate glass, characterized in that, Its chemical composition, by mole percentage, includes: 70%~85.5% SiO2, 0.5%~4% Al2O3, 10%~16.5% B2O3, 0%~2.5% Li2O, 0.1%~5% Na2O, 0%~2.5% K2O, 0.1%~1% CaO+SrO, 0.1%~0.5% La2O3, 0%~0.5% Y2O3, and 0.1%~1% F2+Cl2.

2. The low-dielectric borosilicate glass according to claim 1, characterized in that, The ratio of the molar amount of Al2O3 to the sum of the molar amounts of Li2O, Na2O and K2O is greater than 0.

2.

3. The low-dielectric borosilicate glass according to claim 1, characterized in that, Its chemical composition, by mole percentage, includes: 75%~82% SiO2, 1%~3% Al2O3, 12%~15% B2O3, 0.5%~2% Li2O, 1%~4% Na2O, 0.5%~2% K2O, 0.3%~0.8% CaO+SrO, 0.2%~0.4% La2O3, 0.1%~0.5% Y2O3, and 0.3%~0.8% F2+Cl2.

4. The low-dielectric borosilicate glass according to claim 1, characterized in that, The low-dielectric borosilicate glass has a temperature below 1250°C at a viscosity of 10,000 poise.

5. The low-dielectric borosilicate glass according to claim 1, characterized in that, The low-dielectric borosilicate glass has a dielectric constant of less than 6 and a dielectric loss of less than 100 × 10⁻⁶ at a frequency of 10 GHz. -4 .

6. A method for preparing low-dielectric borosilicate glass as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Mix the raw materials weighed according to the design ratio evenly to obtain the batch material; S2, the batch material is melted, clarified and homogenized to obtain molten glass; S3, the molten glass is shaped to obtain a glass sample block; S4. The formed glass sample is annealed and then cooled to room temperature to obtain the low-dielectric borosilicate glass.

7. The method for preparing low-dielectric borosilicate glass according to claim 6, characterized in that, The melting temperature described in S2 is less than 1700°C.

8. The method for preparing low-dielectric borosilicate glass according to claim 6, characterized in that, The molding described in S3 uses either the pull-down method or the melt-forming method.

9. The method for preparing low-dielectric borosilicate glass according to claim 6, characterized in that, The annealing temperature in S4 is 500~600℃, the holding time is 2~4 hours, and the cooling rate is 0.5~2℃ / minute.

10. The use of a low-dielectric borosilicate glass as described in any one of claims 1 to 5 in the preparation of electronic chip packaging materials.