B4c / ti(c,n) ceramic material and preparation method thereof

By mixing B4C and Ti3AlC2 powders and performing pressureless high-temperature sintering, a B4C/Ti(C,N) ceramic material with high fracture toughness was prepared. This solved the problems of high-temperature sintering and low toughness of boron carbide ceramics, achieved efficient densification and structural stability of the material, and reduced costs.

CN123062269APending Publication Date: 2026-11-10HUAQIAO UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611231905.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The high sintering temperature and low fracture toughness of boron carbide ceramics make it difficult to densify and prone to brittle failure in engineering applications. Furthermore, the synergistic sintering of titanium carbonitride and boron carbide is challenging, affecting the structural stability of the material.

Method used

B4C powder and Ti3AlC2 powder are mixed, ultrasonically dispersed, dried and ground, pressed into shape in a mold, and then subjected to pressureless high-temperature sintering and annealing in a nitrogen atmosphere. Ti(C,N) is generated in situ using Ti3AlC2, achieving dense sintering while maintaining the integrity of the material structure.

Benefits of technology

High fracture toughness B4C/Ti(C,N) ceramic materials were easily prepared at low temperatures, with a fracture toughness increase of 2 to 3 times, reducing sintering costs and avoiding residual oxygen impurities, resulting in a significant improvement in material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062269A_ABST
    Figure CN123062269A_ABST
Patent Text Reader

Abstract

This application provides a B4C / Ti(C,N) ceramic material and its preparation method, comprising mixing B4C and Ti3AlC2 powders with an organic solvent in a certain proportion, ultrasonically dispersing, drying, and then thoroughly grinding to obtain a mixed powder; pressing the mixed powder into a mold, sintering it at high temperature in an inert atmosphere, and then subjecting it to a subsequent high-temperature annealing treatment to obtain the B4C / Ti(C,N) ceramic material. This invention utilizes the in-situ reaction of Ti3AlC2 to generate Ti(C,N) to prepare B4C / Ti(C,N) ceramic materials, effectively avoiding the defects of residual particulate oxygen impurities in directly added Ti(C,N); the method is simple to operate, and the prepared sample exhibits high fracture toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of ceramic materials technology, and in particular relates to a B4C / Ti(C,N) ceramic material and its preparation method. Background Technology

[0002] Boron carbide ceramics, due to their ultra-high hardness, low density, and excellent neutron absorption capacity, have significant application value in defense, nuclear energy, and aerospace fields. However, the high sintering temperature and low fracture toughness of pure boron carbide have become key issues restricting its engineering applications. This is because boron carbide is a typical strongly covalently bonded ceramic with a low atomic diffusion rate and insufficient sintering driving force. High densification is difficult to achieve under conventional pressureless sintering conditions, often requiring higher sintering temperatures or even external pressure or sintering aids to obtain a good microstructure. Simultaneously, boron carbide has poor plastic deformation capacity, and once cracks initiate, they propagate rapidly, leading to brittle failure under impact, thermal stress, and complex service environments. To address these issues, existing technologies typically employ the introduction of second-phase particles to toughen boron carbide.

[0003] Titanium carbonitride is a ceramic material that combines the properties of both carbides and nitrides. It possesses advantages such as high hardness, good wear resistance, excellent thermal and chemical stability, and low density, making it valuable for applications in wear-resistant components, protective materials, cutting tools, and composite ceramics. Introducing titanium carbonitride into the boron carbide system is expected to synergistically improve the material's hardness, strength, and fracture toughness, thereby enhancing the overall performance of the composite material. However, the synergistic sintering of boron carbide and titanium carbonitride presents challenges. Titanium carbonitride is prone to nitrogen loss and grain growth under high temperature and low nitrogen partial pressure conditions, affecting structural stability; boron carbide is prone to nitridation under a nitrogen atmosphere, leading to the destruction of its original phase structure. Therefore, how to achieve dense sintering while suppressing interfacial reactions and maintaining the integrity of the boron carbide and titanium carbonitride structures remains a pressing technical problem to be solved in this field. Summary of the Invention

[0004] This application is made in view of the above-mentioned issues, and its purpose is to provide a B4C / Ti(C,N) ceramic material with high fracture toughness and a method for preparing the same.

[0005] The first aspect of this application provides a method for preparing B4C / Ti(C,N) ceramic materials, comprising the following steps: S1. Mix B4C powder, Ti3AlC2 powder and organic solvent, ultrasonically disperse for 0.5-2 h, dry at 65-85 ℃ for 6-24 h and then grind thoroughly to obtain mixed powder; S2. Weigh the mixed powder, put it into a mold and press it into shape. Take it out and sinter it under pressureless high temperature in a nitrogen atmosphere for 0.5 to 3 hours. Then, perform high temperature annealing treatment to obtain B4C / Ti(C,N) ceramic material.

[0006] In some embodiments, the die pressing force is 1.5–2.5 tf, the holding time is 7–15 min, and the thickness of the molded material is no greater than 2 mm. Preferably, the pressing force is 2 tf, the holding time is 10 min, and the thickness of the molded material is no greater than 2 mm.

[0007] In some embodiments, the particle size of the B4C powder is 5–15 μm, and the particle size of the Ti3AlC2 powder is 30–50 μm.

[0008] In some embodiments, the particle sizes of the B4C powder and Ti3AlC2 powder are 10 μm and 38 μm, respectively.

[0009] In some embodiments, the decomposition temperature of the Ti3AlC2 powder is 1150–1400 °C. Preferably, the decomposition temperature is 1200 °C.

[0010] In some embodiments, the mass ratio of B4C powder to Ti3AlC2 powder is 0.2–0.5: 0.2–0.8.

[0011] In some embodiments, the total mass ratio of the B4C powder and Ti3AlC2 powder to the volume ratio of the organic solvent is 1 g:10 mL, and the organic solvent is anhydrous ethanol or acetone.

[0012] In some embodiments, the high-temperature sintering temperature is 1100 ℃ to 1500 ℃, and the heating rate is 2 to 10 ℃ / min.

[0013] The high-temperature annealing temperature is 1100 ℃~1500 ℃, and the cooling rate is 2~10 ℃ / min.

[0014] The second aspect of this application provides a B4C / Ti(C,N) ceramic material obtained by the above preparation method.

[0015] The beneficial effects of this application are: This invention involves mixing B4C and Ti3AlC2 powders with an organic solvent, ultrasonically dispersing, drying, and then thoroughly grinding to obtain a mixed powder. This powder is then pressed into shape in a mold and subjected to pressureless high-temperature sintering and annealing in an inert atmosphere. This process achieves dense sintering while suppressing interfacial reactions and maintaining the complete structure of boron carbide and titanium carbonitride, thus obtaining B4C / Ti(C,N) ceramic materials.

[0016] This invention utilizes the in-situ reaction of Ti3AlC2 to generate Ti(C,N) to prepare B4C / Ti(C,N) ceramic materials, effectively avoiding the defects of residual particulate oxygen impurities in directly added Ti(C,N). The method is simple to operate, and the prepared samples have high fracture toughness.

[0017] The ceramic material prepared by this invention is easy to operate, can be sintered at a relatively low temperature, and has a high fracture toughness of 6–12 MPa·m. 1 / 2 Compared to pure boron carbide ceramics, the fracture toughness is increased by 2 to 3 times; and the sintering cost of boron carbide composite materials is reduced. Attached Figure Description

[0018] Figure 1 This is a powder diffraction pattern of the B4C / Ti(C,N) ceramic material prepared in Example 1 of the present invention; Figure 2 This is a micro Vickers hardness indentation image of the B4C / Ti(C,N) ceramic material prepared in Example 2 of the present invention; Figure 3 The image shows the powder diffraction pattern of the ceramic material in Comparative Example 1. Detailed Implementation

[0019] The following detailed description, with appropriate reference to the accompanying drawings, discloses an embodiment of a B4C / Ti(C,N) ceramic material and its preparation method. However, unnecessary details may be omitted. For example, detailed descriptions of well-known facts and repetitive descriptions of essentially identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0020] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0021] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0022] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0023] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0024] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0025] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0026] In one embodiment of this application, a method for preparing B4C / Ti(C,N) ceramic material is proposed, comprising the following steps: S1. Mix B4C powder, Ti3AlC2 powder and organic solvent, ultrasonically disperse for 0.5-2 h, dry at 65-85 ℃ for 6-24 h and then grind thoroughly to obtain mixed powder; S2. Weigh the mixed powder and place it into a mold to press it into shape. Take out the shaped sample and sinter it under pressureless high temperature in a nitrogen atmosphere for 0.5 to 3 hours. Then, perform high temperature annealing treatment to obtain B4C / Ti(C,N) ceramic material.

[0027] This application uses Ti3AlC2 powder as raw material. Compared to Ti3AlC2 raw material, which requires a series of chemical reactions during sintering of Ti, Al, and C precursors, the amount of Ti3AlC2 generated, the impurity phase composition, aluminum loss, and densification behavior all need to be re-optimized. Therefore, this solution is not simply a replacement of a raw material, but rather a separate material composition and reaction sintering process.

[0028] The pressureless method of this application refers to the sintering of the molded mixed powder in an atmospheric pressure atmosphere, i.e., nitrogen atmosphere replacing the original atmospheric pressure, and without the application of external mechanical pressure to the molded mixed powder.

[0029] In some embodiments, the die pressing force is 1.5–2.5 tf, the holding time is 7–15 min, and the thickness of the molded material is no greater than 2 mm. Preferably, the pressing force is 2 tf, the holding time is 10 min, and the thickness of the molded material is no greater than 2 mm.

[0030] The unit tf for compressive force represents "ton-force".

[0031] In some embodiments, the particle size of the B4C powder is 5–15 μm, and the particle size of the Ti3AlC2 powder is 30–50 μm.

[0032] In some embodiments, the particle sizes of the B4C powder and Ti3AlC2 powder are 10 μm and 38 μm, respectively.

[0033] In some embodiments, the decomposition temperature of the Ti3AlC2 powder is 1150–1400 °C. Preferably, the decomposition temperature is 1200 °C.

[0034] The purpose of setting the sintering temperature in this application is not simply to perform conventional sintering of B4C powder, but to decompose Ti3AlC2 under a nitrogen atmosphere and without external mechanical pressure, and to allow the titanium- and carbon-containing structures formed after decomposition to further react with nitrogen to generate Ti(C,N) in situ. Therefore, the sintering temperature needs to reach a temperature at which the Ti3AlC2 powder used can undergo significant decomposition and form Ti(C,N).

[0035] The formation mechanism of B4C / Ti(C,N) ceramic materials: The raw materials are B4C and Ti3AlC2. When Ti3AlC2 is heated, aluminum migrates or escapes from the original structure, leaving a structure mainly composed of titanium and carbon. Nitrogen then enters the structure, and some of the nitrogen replaces the carbon positions, forming Ti(C,N) containing titanium, carbon and nitrogen, and finally producing B4C / Ti(C,N) ceramic materials.

[0036] A high size ratio is used to control the reactivity of B4C and Ti3AlC2, thereby increasing the sintering rate of ceramics or the rate of solid-state reactions.

[0037] In some embodiments, the mass ratio of B4C powder to Ti3AlC2 powder is 0.2 g to 0.5 g : 0.2 g to 0.8 g.

[0038] An excessively high or low ratio can lead to a decrease in relative density, resulting in a decrease in fracture toughness and hardness.

[0039] In some embodiments, the total mass ratio of B4C powder and Ti3AlC2 powder to the volume ratio of organic solvent is 1 g: 6–15 mL, and the organic solvent is anhydrous ethanol or acetone. Preferably, the total mass ratio of B4C powder and Ti3AlC2 powder to the volume ratio of organic solvent is 1 g: 10 mL.

[0040] Ethanol and acetone evaporate quickly, dry quickly, and leave little residue.

[0041] When the amount of anhydrous ethanol added is too high, the liquid phase remains for a longer period during the drying process. Because ceramic particles of different sizes and densities settle at different rates in ethanol, larger, denser particles settle faster and accumulate at the bottom, while smaller, less dense particles settle more slowly and thus accumulate at the top, ultimately causing particle stratification and ineffective mixing. When the amount of anhydrous ethanol added is insufficient, the ceramic powder cannot be adequately wetted to form a suspension with good flowability. Excessive solids content may weaken ultrasonic cavitation and sound energy propagation, preventing the particle agglomerates from fully deagglomerating, resulting in localized enrichment and uneven mixing of different ceramic components.

[0042] In some embodiments, the high-temperature sintering temperature is 1100 ℃~1500 ℃, and the heating rate is 2~10 ℃ / min.

[0043] The high-temperature annealing temperature is 1100 ℃~1500 ℃, and the cooling rate is 2~10 ℃ / min.

[0044] Too low a temperature results in no reaction, while too high a temperature leads to excessive reaction, making it impossible to obtain B4C / Ti(C,N) ceramics. Heating too quickly can easily cause cracking, bulging, and deformation, while heating too slowly can easily lead to grain growth. Cooling too quickly can easily cause thermal shock cracking, while cooling too slowly can lead to coarsening of the microstructure and affect performance.

[0045] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0046] Example 1 The preparation method of the B4C / Ti(C,N) ceramic material in this embodiment includes the following steps: (1) Mix and disperse 0.40 g B4C powder (10 μm), 0.60 g Ti3AlC2 powder (38 μm) and 10 mL ethanol in a beaker to obtain a mixed solution. Place the beaker containing the mixed solution in an ultrasonic cleaner for ultrasonic dispersion for 2 h; place it in an oven and dry it at 80 ℃ for 12 h; after drying, take it out and grind it for 10 min for later use.

[0047] (2) Weigh 0.05g of the mixed powder and press it into shape in a 6×6 mm mold. Sinter it at 1400 ℃ for 1 h in a nitrogen atmosphere and then anneal it at 10 ℃ / min to obtain B4C / Ti(C,N) ceramic material.

[0048] The phase composition of the samples was determined using a MiniFlex600 X-ray diffractometer. The instrument used a Cu target, and the results showed that the main phases of the B4C / Ti(C,N) ceramic material were B4C and Ti(C,N).

[0049] Example 2 The preparation method of the B4C / Ti(C,N) ceramic material in this embodiment includes the following steps: (1) Mix and disperse 0.22 g B4C powder (10 μm), 0.78 g Ti3AlC2 powder (38 μm) and 10 mL ethanol in a beaker to obtain a mixed solution. Place the beaker containing the mixed solution in an ultrasonic cleaner for ultrasonic dispersion for 2 h; place it in an oven and dry it at 80 ℃ for 12 h; after drying, take it out and grind it for 10 min for later use.

[0050] (2) Weigh 0.05 g of the mixed powder and press it into shape using a 6×6 mm mold. Then, sinter it at 1400 °C for 1 h in a nitrogen atmosphere and anneal it at 10 °C / min to obtain B4C / Ti(C,N) ceramic material.

[0051] The microhardness of the samples was measured using a ZHV-1MDXS advanced semi-automatic micro Vickers hardness tester. The testing instrument used a diamond indenter in the shape of a square pyramid, which was pressed into the sample surface under a test force of 1.96 N. After a holding time of 10 s, the maximum microhardness of the sample reached 2843 HV, and the fracture toughness, measured using the indentation method, was up to 10.4 MPa·m. 1 / 2 .

[0052] Comparative Example 1 Compared to Example 2, the temperature was 1000 °C, and the other steps were the same as in Example 2.

[0053] The maximum fracture toughness of the obtained B4C / Ti(C,N) ceramic material is 3.34 MPa·m. 1 / 2 Due to the low temperature, B4C and Ti3AlC2 did not react to form B4C / Ti(C,N) ceramics.

[0054] Comparative Example 2 Compared with Example 2, the heat preservation time is 0 min, and the other steps are the same as in Example 2.

[0055] The maximum fracture toughness of the obtained B4C / Ti(C,N) ceramic material is 3.64 MPa·m. 1 / 2 Due to the short heat preservation time, the B4C / Ti(C,N) ceramic material has not yet been densified, with a relative density of only 72.23%.

[0056] This application achieves fracture toughness significantly higher than that of common literature at a low temperature of 1400℃, without external pressure, and with simple process equipment; it solves the problem of low-temperature sintering difficulty and low fracture toughness of boron carbide ceramics.

[0057] Figure 1 At 1400℃, Ti3AlC2 decomposes and produces Ti(C,N), with the main components being B4C and Ti(C,N). Figure 3At 1000℃, Ti3AlC2 did not decompose completely, and the main components of the ceramic were B4C and Ti3AlC2; the formation of Ti(C,N) improved the fracture toughness of B4C.

[0058] This application describes the decomposition behavior and product formation mechanism of Ti3AlC2 powder directly added under specific composition, specific heating regime, specific atmospheric pressure, and no external mechanical pressure conditions. For example, under static pressure of 2–5 GPa, Ti3AlC2 decomposes at 700–800 °C, with the main products being Al3Ti and TiC; while under SPS conditions of 30–40 MPa, high temperature or matrix reaction can also decompose Ti3AlC2 into TiC and Al-containing reaction products.

[0059] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A method for preparing B4C / Ti(C,N) ceramic material, characterized in that, Includes the following steps: S1. Mix B4C powder, Ti3AlC2 powder and organic solvent, ultrasonically disperse for 0.5-2 h, dry at 65-85℃ for 6-24 h and then grind thoroughly to obtain mixed powder; S2. Weigh the mixed powder, put it into a mold and press it into shape. Take it out and sinter it under pressureless high temperature in a nitrogen atmosphere for 0.5 to 3 hours. Then, perform high temperature annealing treatment to obtain B4C / Ti(C,N) ceramic material.

2. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, characterized in that, The pressing force of the mold is 1.5 to 2.5 tf, the holding time is 7 to 15 min, and the thickness of the molded material is no more than 2 mm.

3. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, characterized in that, The particle size of the B4C powder is 5–15 μm, and the particle size of the Ti3AlC2 powder is 30–50 μm.

4. The method for preparing B4C / Ti(C,N) ceramic material according to claim 3, characterized in that, The particle sizes of the B4C powder and Ti3AlC2 powder are 10 μm and 38 μm, respectively.

5. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, 3 or 4, characterized in that, The decomposition temperature of the Ti3AlC2 powder is 1150–1400℃.

6. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, 3 or 4, characterized in that, The mass ratio of B4C powder to Ti3AlC2 powder is 0.2–0.5: 0.2–0.

8.

7. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, characterized in that, The total mass ratio of B4C powder and Ti3AlC2 powder to the volume ratio of organic solvent is 1g:6-15mL, and the organic solvent is anhydrous ethanol or acetone.

8. The method for preparing B4C / Ti(C,N) ceramic material according to claim 1, characterized in that, The high-temperature sintering temperature is 1100 ℃~1500 ℃, and the heating rate is 2~10 ℃ / min.

9. A B4C / Ti(C,N) ceramic material, characterized in that, The B4C / Ti(C,N) ceramic material is obtained by the preparation method described in any one of claims 1 to 8.