A foaming method for graphene oxide-based porous materials
By inserting a foaming agent between graphene oxide layers using dry foaming technology and then heat-treating it, the problems of complex preparation process and uneven pore size of graphene oxide-based porous materials have been solved, enabling large-scale industrial production and performance improvement of the materials.
Patent Information
- Application Number
- CN202611261319.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-06-26
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-10
Smart Images

Figure CN123062285A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nano-carbon material preparation technology, and more specifically, to a foaming method for graphene oxide-based porous materials. Background Technology
[0002] Graphene and its derivatives possess excellent electrical and thermal conductivity, mechanical properties, and high specific surface area, making them promising candidates for applications in energy storage, electromagnetic shielding, adsorption separation, catalyst supports, and composite material reinforcement. In particular, graphene aerogels, with their ultralight weight, three-dimensional interconnected network, porous structure, and compressibility, have become a crucial area of research and development in carbon materials.
[0003] Graphene oxide-based porous materials generally include aerogel powders, aerogel fibers, or aerogel membranes. Currently, the mainstream methods for preparing graphene oxide-based porous materials mainly include hydrothermal methods and sol-gel methods combined with freeze-drying technology. However, these traditional methods typically require liquid-phase systems, resulting in high solvent consumption. Furthermore, freeze-drying equipment is expensive, time-consuming, and energy-intensive, leading to high production costs and significantly limiting its large-scale industrial production.
[0004] Furthermore, for graphene oxide aerogel fibers, aerogel powders, and aerogel membranes, pore size uniformity is a key structural parameter determining their stability and product consistency in industrial applications. A uniform pore structure facilitates the uniform transport of gases, liquids, and ions within the material, preventing rapid penetration due to large local pores or mass transfer blockage caused by excessively small pores. This improves the efficiency and reliability of the material in adsorption separation, filtration purification, catalyst carriers, energy storage electrodes, thermal insulation, and sensing. Simultaneously, uniform pore size distribution reduces local stress concentration and structural defects, improving fiber continuity and mechanical strength, powder adsorption and dispersion consistency, and membrane material flux selectivity and durability. For large-scale production, stable and controllable pore size also helps reduce performance fluctuations between different locations and batches, improving processing adaptability, quality control, and service life. This is a crucial foundation for the transition of graphene oxide aerogel materials from laboratory preparation to standardized, continuous, and highly reliable industrial applications. Summary of the Invention
[0005] To address the shortcomings of existing technologies in preparing graphene oxide-based porous materials, such as complex processes, reliance on liquid-phase systems, and unfavorable conditions for large-scale preparation, this invention provides a method for preparing graphene oxide-based porous materials and their applications.
[0006] This invention employs dry foaming technology to directly prepare graphene oxide-based porous materials using a dry graphene oxide-foaming agent composite precursor as a raw material. The dry graphene oxide-foaming agent composite precursor is an assembly of graphene oxide with foaming agents intercalated between its layers. Specifically, the dry graphene oxide-foaming agent composite precursor is heat-treated at 100℃~1500℃ for 0.5h~6h to obtain the graphene oxide-based porous material. Due to the large number of oxygen-containing functional groups present between the graphene oxide layers, the foaming agent can be directly intercalated into the single-layer to 1nm graphene oxide interlayers. By controlling the foaming agent content and foaming conditions between atomic layers, the prepared graphene oxide-based porous material powder can achieve uniform and precisely adjustable pore size, possessing a well-developed pore structure, and a density ranging from 10-1500 mg / cm³. 3 Effective control within the range; in addition, since the dry foaming agent used will undergo a melting stage during the heat treatment process, the molten state can provide a homogeneous interface for bubble nucleation and reduce the nucleation energy barrier. The flow characteristics of the melt can promptly transfer and uniformly disperse the thermal stress and expansion force between the layers, prompting the bubbles to grow in a two-dimensional confined manner along the interlayer channels of graphene oxide, ensuring that the prepared porous material has a highly consistent pore size distribution and a globally uniform pore structure, significantly improving the overall uniformity of the material and reliably ensuring the pore size uniformity.
[0007] In this invention, the heat treatment temperature is selected based on the gas-generating characteristics of the foaming agent used, ensuring that the foaming agent undergoes decomposition, volatilization, and / or other gas-generating processes, producing enough gas to drive the exfoliation, expansion, and rearrangement of graphene oxide sheets. In this invention, the heat treatment temperature can be between 100℃ and 1500℃, and the heat treatment time can be between 0.5h and 6h. It should be noted that the above heat treatment temperature range represents the overall process window applicable to different types of foaming agents and different graphene oxide assemblies, and does not require that any foaming agent can achieve foaming at any temperature within this range. Those skilled in the art can select a heat treatment temperature and treatment time matching the selected foaming agent within the above range based on the decomposition temperature, volatilization temperature, or effective gas-generating temperature of the selected foaming agent, as well as factors such as the morphology, size, and density of the graphene oxide assembly.
[0008] In this invention, the mass fraction of the foaming agent in the dry graphene oxide-foaming agent composite precursor is 1%–90%. Those skilled in the art can adjust the adsorption and intercalation amount of the foaming agent based on the morphology, thickness, pore structure, and interlayer accessibility of the graphene oxide assembly, combined with the type of foaming agent, solution concentration, and impregnation conditions, thereby obtaining dry composite precursors with different foaming agent contents. Within the scope of this invention, the mass fraction of the foaming agent in the dry graphene oxide-foaming agent composite precursor can be 1%–90%, and the specific content can be selected according to the target degree of foaming, pore structure, and material density. Specifically, it can be obtained through at least the following two methods: Method 1: Impregnate graphene oxide assemblies (powder, film, and fiber) in a foaming agent solution to allow the foaming agent to enter the interlayer of graphene oxide, and obtain the dry graphene oxide-foaming agent composite precursor after drying.
[0009] The foaming agent used to implement method 1 can be an inorganic foaming agent and / or an organic foaming agent. Specifically, the inorganic foaming agent is selected from at least one of sodium bicarbonate, ammonium bicarbonate, ammonium carbonate, sodium carbonate, and potassium bicarbonate; the organic foaming agent is selected from at least one of azo foaming agents, nitroso foaming agents, sulfonyl hydrazides, and acyl hydrazides.
[0010] In the case of preparing the dry graphene oxide-foaming agent composite precursor using Method 1, the foaming agent mainly enters the interior of the graphene oxide assembly and the interlayer of graphene oxide sheets through the impregnation process. Therefore, the content of foaming agent in the obtained composite precursor can be controlled by adjusting the concentration of the foaming agent solution, impregnation time, impregnation temperature, the ratio of graphene oxide assembly to foaming agent solution, and the impregnation method. For denser graphene oxide assemblies, reduced pressure impregnation, cyclic reduced pressure-restored atmospheric pressure, and / or ultrasonic-assisted impregnation can also be used to promote the diffusion of the foaming agent into the interior of the assembly and the interlayer of graphene oxide, thereby increasing the loading of the foaming agent. After impregnation, the amount of foaming agent that has not entered the interlayer or has not been effectively retained by the assembly can be adjusted by controlling the amount of leaching, surface rinsing, or washing. Subsequently, the solvent is removed by drying to obtain the dry graphene oxide-foaming agent composite precursor with the predetermined foaming agent content. The actual mass fraction of the foaming agent in the dry composite precursor can be determined based on the mass change before and after drying, combined with the mass of the blank graphene oxide assembly. Alternatively, it can be determined using thermogravimetric analysis or other conventional quantitative analysis methods in the field. By adjusting the above parameters, the mass fraction of the foaming agent in the dry composite precursor can be continuously controlled within a certain range.
[0011] Method 2: Mix graphene oxide and a foaming agent in a solution to allow the foaming agent to enter the interlayer of graphene oxide. After processing and molding, graphene oxide assemblies are formed, and after drying, the dry graphene oxide-foaming agent composite precursor is obtained.
[0012] In the case of method 2, after mixing graphene oxide and the foaming agent, no further filtration, washing, centrifugation, or other treatments to separate the foaming agent from the graphene oxide are performed. Therefore, if the foaming agent does not undergo significant volatilization, decomposition, or loss during the drying process, the graphene oxide and the foaming agent, as non-volatile solid components, are essentially retained in the molded composite precursor. Thus, the dry-basis mass ratio of the foaming agent to graphene oxide in the obtained dry graphene oxide-foaming agent composite precursor is basically consistent with the mass ratio of the raw materials during mixing. The mass fraction of the foaming agent in the dry composite precursor can be determined based on the dry-basis feed amounts of graphene oxide and the foaming agent. For example, when the dry-basis mass ratio of graphene oxide to the foaming agent is 1:x, without considering trace losses during processing and drying, the theoretical mass fraction of the foaming agent in the obtained dry composite precursor is x / (1+x)×100%.
[0013] The foaming agent used to implement method 2 can be any organic biodegradable substance with a melting temperature lower than its decomposition temperature. Specifically, it can be selected from: water-soluble acids, polyols, and low molecular weight polymers. Those skilled in the art can select substances such as glycerol, ethylene glycol, propylene glycol, xylitol, erythritol, mannitol, salicylic acid, malic acid, citric acid, polyethylene glycol, polypropylene glycol, and polyvinyl alcohol as foaming agents as needed.
[0014] The graphene oxide assembly used as the initial raw material in Method 1 or the graphene oxide assembly formed by processing in Method 2 can be a powder, fiber or membrane formed from graphene oxide assembly; after foaming, aerogel powder, aerogel fiber or aerogel membrane is obtained.
[0015] In some embodiments of the present invention, the aerogel powder can be prepared using method 1, using graphene oxide powder (powdered graphene oxide assembly) as raw material, specifically as follows: (1) Preparation of graphene oxide powder. It is known that graphene oxide powder can be obtained by direct drying and grinding, spray drying, freeze drying and other methods.
[0016] Graphene oxide powder (powdered graphene oxide assemblies) was mixed with an aqueous solution of a foaming agent and dried to obtain a dry graphene oxide-foaming agent composite precursor. This precursor was then homogenized to prevent graphene oxide agglomeration and precisely control its particle size distribution. This uniform dispersion promoted the effective intercalation of the foaming agent between the graphene oxide sheets. During subsequent heat treatment, the foaming agent caused the graphene oxide to exfoliate, ultimately constructing a uniform three-dimensional porous network.
[0017] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, graphene aerogel powder is obtained.
[0018] Preferably, the heat treatment temperature is 400-600℃ and the heat treatment time is 1-3h.
[0019] Furthermore, the mass ratio of graphene oxide powder to foaming agent is 1:0.1 to 1:20, preferably 1:0.3 or higher.
[0020] Furthermore, the mass concentration of the aqueous solution of the foaming agent is 1% to 50%, preferably 5% to 30%.
[0021] Optionally, in some embodiments of the present invention, the aerogel powder can also be prepared using method 2, using graphene oxide powder (powdered graphene oxide assembly) as raw material, specifically as follows: (1) The graphene oxide solution is mixed with an aqueous solution of a foaming agent. The composite powder can be obtained by direct drying and grinding, spray drying, freeze drying, etc. After drying, a dry graphene oxide-foaming agent composite precursor powder is obtained; then it is homogenized to prevent the agglomeration of graphene oxide and to precisely control its particle size distribution. This uniform dispersion promotes the effective intercalation of the foaming agent between the graphene oxide sheets. In the subsequent heat treatment process, the foaming agent causes the graphene oxide to be exfoliated, and finally a three-dimensional porous network with a uniform structure is constructed.
[0022] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, graphene aerogel powder is obtained.
[0023] Preferably, the heat treatment temperature is 400-600℃ and the heat treatment time is 1-3h.
[0024] Furthermore, the mass ratio of graphene oxide powder to foaming agent is 1:0.1 to 1:20, preferably 1:0.3 or higher.
[0025] Furthermore, the mass concentration of the aqueous solution of the foaming agent is 1% to 50%, preferably 5% to 30%.
[0026] In some embodiments of the present invention, the aerogel fibers can be prepared using method 1, using graphene oxide fibers (fibrous graphene oxide assemblies) as raw materials, specifically as follows: (1) Preparation of graphene oxide fibers. It is known that graphene oxide fibers can be obtained by wet spinning, dry-jet wet spinning, dry spinning, gel-assisted spinning or blow spinning.
[0027] (2) The graphene oxide fibers are impregnated in a foaming agent solution to allow the foaming agent to enter the interlayer of the graphene oxide. The impregnation time is generally 0.1h to 24h, preferably 0.5h to 6h. For graphene oxide fibers with larger diameter, denser structure or poor wettability, the impregnation can be carried out under reduced pressure of 10kPa to 80kPa for 1min to 30min and then restored to normal pressure. This cycle can be repeated 1 to 5 times. Alternatively, ultrasonic-assisted impregnation can be used to promote the diffusion of the foaming agent into the fiber interior and the interlayer of the graphene oxide. Negative pressure treatment is not necessary and can be omitted if the foaming agent can be fully intercalated under normal pressure. After drying, the dry graphene oxide-foaming agent composite precursor is obtained.
[0028] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, graphene oxide aerogel fiber is obtained.
[0029] Optionally, in some embodiments of the present invention, the aerogel fibers can also be prepared using method 2, specifically as follows: (1) Mix the graphene oxide aqueous dispersion or polar organic solvent dispersion with a foaming agent so that the foaming agent enters the interlayer of the graphene oxide; the graphene oxide is preferably a single-layer or few-layer graphene oxide sheet with a transverse dimension of 0.1μm to 100μm, preferably 1μm to 50μm, and can form a stable dispersion system or liquid crystal phase in the solvent used.
[0030] (2) The process is carried out by wet spinning, dry-jet wet spinning, dry spinning or gel-assisted spinning; when wet spinning or dry-jet wet spinning is used, the mixed dispersion obtained in step (1) is extruded into the coagulation bath through the spinneret hole, and graphene oxide fibers are formed by coagulation, stretching, washing and collection, and the dry graphene oxide-foaming agent composite precursor is obtained after drying.
[0031] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, graphene oxide-based aerogel fibers are obtained.
[0032] In step (1) of this method, the graphene oxide is preferably a single-layer or few-layer graphene oxide sheet that can form a stable spinning solution or liquid crystal phase, and its transverse size can be 0.1μm to 100μm, preferably 1μm to 50μm; the concentration of graphene oxide in the mixed solution can be 1mg / mL to 100mg / mL, preferably 5mg / mL to 50mg / mL.
[0033] The mass ratio of graphene oxide to foaming agent can be 1:0.01 to 1:20, preferably 1:0.1 to 1:5; the mass fraction of foaming agent in the mixed solution can be 0.1% to 50%, preferably 1% to 30%. The mixing time in step (1) can be 0.1h to 24h, preferably 0.5h to 6h; during the mixing process, mechanical stirring, shear dispersion or low-power ultrasound can be used to fully disperse the foaming agent and allow it to enter the interlayer of graphene oxide. At the same time, vacuum degassing is performed before spinning to avoid bubbles affecting the continuous forming of fibers.
[0034] The foaming temperature in step (3) can be adjusted adaptively according to the fiber diameter, the density of the precursor, and the decomposition temperature of the foaming agent. Generally, it can still be selected within the range of 100℃ to 1500℃. It is preferable to adopt a segmented heating method, first preheating at 80℃ to 200℃ for 0.1h to 2h to allow residual solvent and low-boiling-point components to slowly escape, and then heating to 200℃ to 1500℃ and holding for 0.5h to 6h to complete the foaming. For fibers with larger diameter or denser structure, the heating rate can be controlled at 0.5℃ / min to 10℃ / min and the holding time can be appropriately extended to avoid surface cracking or insufficient internal foaming caused by rapid gas generation in the outer layer.
[0035] In some embodiments of the present invention, the aerogel membrane can be prepared using method 1, using graphene oxide membrane (film-like graphene oxide assembly) as raw material, specifically as follows: (1) Preparation of graphene oxide film. It is known that graphene oxide film can be processed and formed by methods such as blade coating, casting, vacuum filtration, spin coating, spraying, dip coating, roller coating, inkjet printing or layer-by-layer assembly to form graphene oxide film, and after drying, the dry graphene oxide-foaming agent composite precursor is obtained.
[0036] 2) The graphene oxide film is immersed in a foaming agent solution to allow the foaming agent to penetrate into the interlayer of the graphene oxide. The immersion time is generally 0.1h to 48h, preferably 0.5h to 12h. For graphene oxide films with a large thickness or dense interlayer stacking, the film can be immersed under reduced pressure of 10kPa to 80kPa for 1min to 30min, and then restored to normal pressure. This cycle can be repeated 1 to 5 times. Alternatively, ultrasonic-assisted immersion can be used to promote the diffusion of the foaming agent from the film surface to the film interior and between the layers. Negative pressure treatment is not necessary and can be omitted if the foaming agent can be fully intercalated under normal pressure. After drying, the dry graphene oxide-foaming agent composite precursor is obtained.
[0037] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0038] Optionally, in some embodiments of the present invention, the aerogel membrane can also be prepared using method 2, specifically as follows: (1) Mix the graphene oxide solution with the foaming agent in the solution so that the foaming agent enters the interlayer of the graphene oxide.
[0039] (2) The graphene oxide film is formed by means of scraping, casting, vacuum filtration, spin coating, spraying, dip coating, roller coating, inkjet printing or layer-by-layer assembly, and the dry graphene oxide-foaming agent composite precursor is obtained after drying.
[0040] (3) Heat treatment at 100℃~1500℃ for 0.5h~6h to decompose the foaming agent and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0041] In step (1) of this method, the graphene oxide is preferably a single-layer or few-layer graphene oxide sheet with a lateral size of 0.1 μm to 100 μm, preferably 1 μm to 50 μm; the concentration of graphene oxide in the mixed solution is 0.1 mg / mL to 50 mg / mL, preferably 1 mg / mL to 20 mg / mL, so as to balance the uniformity of film formation and the integrity of the film.
[0042] The mass ratio of graphene oxide to foaming agent can be 1:0.01 to 1:20, preferably 1:0.1 to 1:5; the mass fraction of foaming agent in the mixed solution can be 0.1% to 50%, preferably 1% to 30%. The mixing time in step (1) can be 0.1h to 24h, preferably 0.5h to 6h; mechanical stirring, shear dispersion or low-power ultrasound can be used during the mixing process, and static or vacuum degassing can be performed before film formation to ensure that the foaming agent is evenly distributed and enters the interlayer of graphene oxide.
[0043] The foaming temperature in step (3) can be adjusted adaptively according to the film thickness, the density of interlayer stacking, and the decomposition temperature of the foaming agent. Generally, it can still be selected within the range of 100℃ to 1500℃. It is preferable to adopt a segmented heating method, first preheating at 80℃ to 200℃ for 0.1h to 2h, and then heating to 200℃ to 1500℃ and holding for 0.5h to 6h. For thick films or high-density films, the heating rate can be controlled at 0.2℃ / min to 5℃ / min and the holding time can be appropriately extended to make the gas generation and expansion process in the film thickness direction more uniform and reduce the risk of local bubbling, cracking or delamination.
[0044] Based on method 1 or method 2 above, the mass fraction of the foaming agent in the dry graphene oxide-foaming agent composite precursor can be adjusted within the range of 1% to 90%, which can achieve precise control of the internal pores, wall thickness, and pore curvature of the graphene oxide-based aerogel macromaterial.
[0045] The heat treatment atmosphere is not, in principle, a necessary limiting condition for achieving in-situ gas-generating foaming in this invention. As long as the selected heat treatment environment allows the foaming agent to generate gas normally at the corresponding temperature, and causes the graphene oxide assembly to undergo lamellar peeling, expansion, rearrangement, and overlapping under the action of gas generation, the foaming process of this invention can be achieved. Depending on the composition, degree of reduction, conductivity, pore wall integrity, and other performance requirements of the obtained porous material, an air atmosphere, an inert gas atmosphere, a reducing gas atmosphere, or a vacuum environment can be further selected for heat treatment. The specific heat treatment atmosphere, along with the corresponding temperature, time, and heating rate, can be adaptively adjusted by those skilled in the art based on the gas generation characteristics of the selected foaming agent and the properties of the target material. For example, heat treatment in an inert gas atmosphere can reduce oxidative ablation and help maintain the carbon skeleton structure; heat treatment in a reducing atmosphere can further reduce the oxygen content of the material during or after foaming; heat treatment in a vacuum environment can promote the escape of volatile products; and heat treatment in an air atmosphere can utilize oxidation under suitable conditions to adjust the material composition or pore structure. For heat treatment in an air atmosphere, those skilled in the art can routinely adjust the heat treatment temperature and time according to the thermal stability and target performance of the graphene oxide material to avoid undesirable over-oxidation of the carbon skeleton due to excessively strong treatment conditions.
[0046] The present invention also relates to graphene oxide-based porous materials with well-developed pores and adjustable density obtained by the aforementioned method, which will be used in the fields of battery buffer protection, battery thermal runaway protection, high temperature thermal sealing, high temperature thermal buffering, and high temperature thermal management.
[0047] The advantages of this invention are: the dry foaming method provided by this invention has lower production costs compared to existing liquid-phase foaming methods, making it suitable for large-scale industrial production. The prepared graphene oxide-based porous material powder has a uniform and tunable pore size and a well-developed pore structure, with a density ranging from 10 to 1500 mg / cm³. 3 Effective regulation within the specified range.
[0048] Furthermore, this invention pre-places the foaming agent within the interlayer of graphene oxide, enabling gas nucleation, release, and decoupling of the layers to occur coupled within the confined space between the layers. This transforms the pore structure construction method, which is controlled by solvent mass transfer and drying processes in traditional liquid systems, into an in-situ gas-generating process within the solid composite precursor, shortening the gas diffusion path and improving gas generation utilization efficiency. Based on the morphological inheritance of graphene oxide assemblies and the interlayer confinement effect, this invention can achieve the construction and control of multi-scale pore structures while preserving the macroscopic morphology of powders, fibers, or films. By matching the melting, diffusion, and thermal decomposition windows of the foaming agent with the deoxidation, softening, and rearrangement windows of graphene oxide, the degree of layer peeling, pore wall integrity, and framework continuity can be synergistically adjusted in situ, thereby ensuring pore size uniformity. Attached Figure Description
[0049] Figure 1 This is a scanning electron microscope image of the aerogel membrane sample from Example 2; Figure 2 The compression mechanical curve of the aerogel membrane sample in Example 1; Figure 3 This is a scanning electron microscope image of the aerogel powder sample from Example 6; Figure 4 The compression mechanical curve of the aerogel powder sample in Example 9; Figure 5 This is a morphology diagram of the aerogel fibers in Example 11; Figure 6 The compression resilience diagram of aerogel fiber in Example 12 is shown. Figure 7 Here is a scanning electron microscope image of the aerogel membrane in Comparative Example 1; Figure 8 Here is a scanning electron microscope image of the aerogel fibers in Comparative Example 2; Figure 9 The image shows the X-ray diffraction pattern of the dry graphene oxide-foaming agent composite precursor film in Example 1. Detailed Implementation
[0050] The following examples are provided to further illustrate the present invention and are intended to explain the invention, not to limit its scope. Unless otherwise specified, all figures are expressed in parts by weight and weight percentages.
[0051] Unless otherwise specified, the raw materials used in this invention are all conventional commercially available products; unless otherwise specified, the methods used in this invention are all conventional methods in the field.
[0052] The graphene oxide described in this invention refers to a two-dimensional material in which oxygen-containing functional groups are bonded to the surface and boundaries of single-layer, double-layer, or multi-layer graphene. Any material that introduces oxygen atoms into the graphene structure, regardless of the oxygen content or whether it is distributed on the surface, at the edge, or inside the lattice, is considered to be the graphene oxide described in this invention.
[0053] The graphene oxide assembly described in this invention refers to a microscopic or macroscopic material with interlayer channels or gaps that allow foaming agent molecules to enter, formed by stacking or assembling graphene oxide sheets through interlayer forces. This includes, but is not limited to, graphene oxide powder, graphene oxide fibers, and graphene oxide films.
[0054] The "dry graphene oxide-foaming agent composite precursor" described in this invention refers to a precursor in which there is essentially no free solvent serving as a dispersion medium or continuous phase. The content of residual solvent in the composite precursor can be determined by weighing. Specifically, a certain amount of the dry graphene oxide-foaming agent composite precursor to be tested is taken, and its mass before treatment is recorded as m0. The sample is then subjected to constant temperature treatment at 60°C for 12 h to further remove residual water or organic solvents. After cooling to room temperature, the mass after treatment is recorded as m1. The mass fraction of residual solvent can be calculated as (m0-m1) / m0 × 100%. If the foaming agent and graphene oxide assembly used do not undergo significant decomposition, volatilization, or other weight loss under the above test conditions, and the measured mass loss does not exceed 5 wt%, the composite precursor can be considered to meet the dry state described in this invention. If necessary, the constant temperature treatment and weighing process can be repeated until the sample mass is substantially constant.
[0055] The graphene oxide-based porous material described in this invention refers to a porous three-dimensional carbon network material formed by heat treatment of the dry graphene oxide-foaming agent composite precursor, with thermally reduced graphene oxide sheets as the framework. Its interior contains uniformly distributed closed or open pores formed by the expansion of the foaming agent, with uniform and controllable pore size. Unless otherwise specified, the graphene oxide used in the following examples is few-layer graphene oxide (n=1~5) with a lateral dimension of 10~30μm and a carbon-oxygen ratio of approximately 1.5.
[0056] The embodiments of the present invention will be further described below with reference to several examples.
[0057] It should be understood that the described embodiments are merely some, not all, of the embodiments in this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.
[0058] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.
[0059] In the following embodiments, scanning electron microscopy was used to characterize the pore structure of the samples, and image analysis software was used to identify and count the pores in the microscopic images. Multiple different locations were selected for testing on each sample, and several random fields of view were selected at each location. The equivalent circle diameter of the pore was used as the pore diameter, and the average or median pore diameter, pore diameter standard deviation, and pore diameter coefficient of variation of the samples were finally obtained. and pore size distribution Value. Among them, The ratio of the standard deviation of pore size to the average pore size; pore size distribution. Value according to calculate, and These represent the pore sizes corresponding to cumulative pore size distribution reaching 10%, 50%, and 90%, respectively. Simultaneously, the average pore size at each test location is calculated, and the spatial pore size uniformity of the sample is evaluated based on the relative standard deviation (RSD) of the average pore size at different locations. , Value and The smaller the value, the more concentrated the pore size distribution of the sample and the better the consistency of pore size between different locations.
[0060] Specifically, CV, Span value, and RSD are calculated using the following methods: All holes identified in the test field are treated as a statistical population, and the equivalent circle diameter of each hole is used as the hole diameter value to calculate the overall average hole diameter. And the population standard deviation σ, then Sort all pore size data in ascending order, plot the cumulative pore size distribution curve, and read the pore size values corresponding to the cumulative distribution reaching 10%, 50%, and 90% respectively. and ,but For each test location, first calculate the average aperture of all holes within that location to obtain the average aperture for each location. Then calculate the mean of the average aperture at these locations. and standard deviation ,but .
[0061] In this application, the density of the aerogel is the apparent density. The test is performed by weighing the sample with a solid volume V to obtain m, and the surface density ρ of the aerogel is calculated based on m / V.
[0062] Example 1 A method for preparing a graphene oxide-based aerogel membrane includes the following steps: (1) The concentration of graphene oxide aqueous dispersion was 5 mg / mL. It was processed into graphene oxide membrane by vacuum filtration and dried under vacuum at 40℃ for 12 h to obtain graphene oxide membrane.
[0063] (2) Dissolve ammonium bicarbonate in deionized water to prepare a 15% (w / w) foaming agent solution. Immerse the graphene oxide membrane in the above foaming agent solution, and after immersion under reduced pressure of 50 kPa for 10 min, restore normal pressure. Repeat this cycle 3 times, and then continue immersion under normal pressure for 2 h to allow the foaming agent to penetrate into the interlayer of graphene oxide. After removal, gently rinse the surface with deionized water to remove any remaining droplets, and vacuum dry at 50 °C for 6 h to obtain a dry graphene oxide-foaming agent composite precursor membrane. The X-ray diffraction patterns of the precursor membrane before and after composite formation are shown below. Figure 9 The diffraction peaks of the graphene oxide and precursor composite film are all single peaks, and the 2theta angle shifts from ~11° to about ~4.5°, which proves that the foaming agent inside the precursor film has entered the nanolayers of graphene oxide and exhibits uniform intercalation behavior, laying the foundation for subsequent uniform foaming and pore formation.
[0064] (3) The composite precursor membrane is placed in a tube furnace and heated to 500°C at 3°C / min under a nitrogen atmosphere. The temperature is maintained for 2 hours to decompose ammonium bicarbonate and generate gas. Under the in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0065] The graphene oxide-based aerogel membrane prepared in this embodiment has an average pore size of 1.13 μm, a density of 81 mg / cm³, and a compression rebound curve as shown in the figure. Figure 2 The compression cycle curves at 90% strain for 10 cycles confirmed that the prepared aerogel membrane has good compression resilience and its mechanical properties are basically unaffected.
[0066] Example 2 A method for preparing a graphene oxide-based aerogel membrane includes the following steps: (1) The concentration of graphene oxide aqueous dispersion is 8 mg / mL. It is processed into a graphene oxide wet film on a PET substrate by a blade coating method. After drying at 60°C for 6 hours, the film is peeled off to obtain a graphene oxide film.
[0067] (2) Azodicarbonamide was dissolved in N,N-dimethylformamide to prepare a 10% (w / w) foaming agent solution. The graphene oxide membrane was immersed in the above foaming agent solution and ultrasonically assisted for 4 hours to allow the foaming agent to diffuse from the membrane surface to the membrane interior and between the layers. After removal, it was vacuum dried at 60°C for 8 hours to obtain a dry graphene oxide-foaming agent composite precursor membrane.
[0068] (3) The composite precursor membrane is placed in a tube furnace and heated in a segmented manner under an air atmosphere. First, the temperature is raised to 120°C at 2°C / min and preheated for 1 hour. Then, the temperature is raised to 210°C at 2°C / min and kept for 3 hours to decompose azodicarbonamide and generate gas. Under the in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0069] The graphene oxide-based aerogel membrane prepared in this embodiment has an average pore size of 751 nm (e.g., Figure 1 ), with a density of 122 mg / cm³.
[0070] Example 3 A method for preparing a graphene oxide-based aerogel membrane includes the following steps: (1) Disperse single-layer graphene oxide sheets with a transverse dimension of 20~50μm in deionized water to prepare a graphene oxide solution with a concentration of 8mg / mL. In this embodiment, polyethylene glycol is used as a foaming agent. Polyethylene glycol solution is added to the graphene oxide solution to make the mass ratio of graphene oxide to foaming agent 1:1.5. Mechanical stirring is performed for 4 hours to make the foaming agent evenly distributed and enter the interlayer of graphene oxide, and then allowed to stand for 2 hours to degas.
[0071] (2) The above mixed dispersion was processed and formed on a glass plate by a scraping method. The wet film thickness was controlled to be 800 μm. It was dried at 50°C for 12 h to obtain a dry graphene oxide-foaming agent composite precursor film.
[0072] (3) The composite precursor membrane is placed in a tube furnace and heated in stages under an argon atmosphere: first, the temperature is raised to 120°C at 1°C / min and preheated for 1 hour, then the temperature is raised to 600°C at 2°C / min and held for 2.5 hours to decompose polyethylene glycol and generate gas. Under the in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0073] The graphene oxide-based aerogel membrane prepared in this embodiment has an average pore size of 5.56 μm and a density of 10 mg / cm³. 3 .
[0074] Example 4 A method for preparing a graphene oxide-based aerogel membrane includes the following steps: (1) A single-layer graphene oxide sheet with a transverse dimension of 10-30 μm was dispersed in deionized water to prepare a graphene oxide solution with a concentration of 2 mg / mL. In this embodiment, citric acid was used as a foaming agent. Citric acid solution was added to the graphene oxide solution to make the mass ratio of graphene oxide to foaming agent 1:0.8. After low-power ultrasonic dispersion for 30 min, magnetic stirring was performed for 6 h to make the foaming agent uniformly dispersed and enter the interlayer of graphene oxide. The solution was then allowed to stand to degas.
[0075] (2) Take 200 mL of the above mixed dispersion and process it into a graphene oxide membrane by vacuum filtration. Dry it in vacuum at 60°C for 10 h to obtain a dry graphene oxide-foaming agent composite precursor membrane.
[0076] (3) The composite precursor membrane is placed in a tube furnace and heated in stages under a hydrogen / argon mixed atmosphere with a volume fraction of 5% H2. First, the temperature is increased to 120°C at 1°C / min and preheated for 0.5 h. Then, the temperature is increased to 800°C at 1.5°C / min and held for 3 h to decompose citric acid and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are promoted to peel, expand, rearrange and overlap, and the thermal reduction of graphene oxide is achieved at the same time. After cooling, a reduced graphene oxide-based aerogel membrane is obtained.
[0077] The reduced graphene oxide-based aerogel membrane prepared in this embodiment has an average pore size of 200 nm and a density of 270 mg / cm³. 3 .
[0078] Example 5 A method for preparing a graphene oxide-based aerogel membrane includes the following steps: (1) A graphene oxide aqueous dispersion with a concentration of 70 mg / mL was processed into a graphene oxide wet film on a stainless steel substrate by roller coating. After drying at 80°C for 4 hours, the film was peeled off to obtain a graphene oxide film.
[0079] (2) Sodium bicarbonate and ammonium bicarbonate were mixed at a mass ratio of 1:2 and dissolved in deionized water to prepare a mixed foaming agent solution with a total mass fraction of 20%. The graphene oxide membrane was immersed in the above foaming agent solution for 8 hours at room temperature, with intermittent ultrasonic assisted immersion to promote the diffusion of the foaming agent from the membrane surface to the membrane interior and between the layers. After removal, it was vacuum dried at 40°C for 12 hours to obtain a dry graphene oxide-foaming agent composite precursor membrane.
[0080] (3) The composite precursor membrane is placed in a tube furnace and heated in stages under a nitrogen atmosphere. First, the temperature is increased to 120°C at 1°C / min and preheated for 1 hour. Then, the temperature is increased to 300°C at 0.5°C / min and held for 4 hours to allow the mixed foaming agent to decompose and generate gas. Under the action of in-situ gas generation, the graphene oxide sheets are peeled, expanded, rearranged and overlapped. After cooling, a graphene oxide-based aerogel membrane is obtained.
[0081] The graphene oxide-based aerogel membrane prepared in this embodiment has an average pore size of 100 nm and a density of 1500 mg / cm³. 3 .
[0082] Example 6 (1) Graphene oxide slurry was synthesized using the modified Hummers method. The obtained slurry was diluted with deionized water to a concentration of 5 mg / mL and dried and shaped using a spray drying device. The inlet temperature was set to 200℃, the outlet temperature to 100℃, and the feed rate to 8 ml / min. Powdered graphene oxide assemblies were collected with a particle size of about 20 μm.
[0083] (2) Weigh out solid ammonium bicarbonate, dissolve it in deionized water, stir mechanically until completely dissolved, and prepare an ammonium bicarbonate aqueous solution with a mass concentration of 1% for later use.
[0084] (3) Weigh 10 g of the graphene oxide powder obtained in step (1) and add it to 100 ml of the above ammonium bicarbonate solution (so that the mass of the foaming agent is 1 g, i.e. GO: foaming agent = 1:0.1). Impregnate at room temperature (25℃) under normal pressure for 2 h. During the impregnation process, stir intermittently with a glass rod every 30 min to promote full contact between the solution and the powder, so that the ammonium bicarbonate molecules enter the interlayer of graphene oxide.
[0085] (4) The suspension obtained in step (3) is separated into solid and liquid by vacuum filtration device. A filter membrane with a pore size of 0.45 μm is used to filter until there is no obvious liquid film on the surface of the filter cake. The surface of the filter cake is slowly rinsed with a small amount of deionized water (about 20 mL) to remove excess foaming agent that has not been intercalated and adsorbed on the surface.
[0086] (5) Transfer the filter cake from step (4) to a vacuum drying oven, set the drying temperature to 50℃ and the vacuum degree to -0.095MPa, and dry at a constant temperature for 12 h to obtain dry graphene oxide-ammonium bicarbonate composite precursor powder.
[0087] (6) Place the dried composite precursor powder from step (5) into a grinding mortar and grind for 5 min. Then, sieve it through a 100-mesh standard sieve and collect the powder that passes through the sieve to break up the agglomerates and regulate the uniformity of the particle size distribution.
[0088] (7) The homogenized composite precursor powder from step (6) is evenly spread in a graphite box and placed in a muffle furnace. The temperature is raised from room temperature to 150 ℃ at a rate of 5 ℃ / min under air atmosphere and held at this temperature for 0.5 h. This allows ammonium bicarbonate to rapidly decompose and produce ammonia, carbon dioxide, and water vapor. The in-situ gas generation drives the exfoliation, expansion, rearrangement, and overlapping of the graphene oxide sheets. After the holding period, heating is stopped, and the powder is allowed to cool naturally to room temperature with the furnace, thus obtaining graphene oxide aerogel powder. Its microstructure is as follows: Figure 3 Its density is approximately 45 mg / cm³. 3 .
[0089] Example 7 (1) The aqueous dispersion of graphene oxide (concentration 8 mg / ml) was placed in a freeze dryer, and the freezing temperature was set to -50 ℃ and the freezing time was 24 h. The first drying temperature was -10 ℃ and the pressure was 20 Pa. The second drying temperature was 20 ℃ and the pressure was 5 Pa. The total drying time was 48 h. A sponge-like graphene oxide assembly was obtained and coarsely crushed into powder using a mortar and pestle.
[0090] (2) Weigh out sodium bicarbonate solid, dissolve it in deionized water, stir it in a 35 ℃ water bath for 30 min to prepare a sodium bicarbonate solution with a mass concentration of 5%, and keep it warm for later use to prevent precipitation.
[0091] (3) Weigh 5 g of the graphene oxide powder obtained in step (1) and add it to 30 ml of sodium bicarbonate solution preheated to 35 °C (the mass of the foaming agent is 1.5 g, i.e. GO: foaming agent = 1:0.3). Place it in a vacuum dryer, evacuate to an absolute pressure of 40 kPa and maintain for 5 min, then slowly restore to normal pressure. Repeat this operation 3 times, with a total impregnation time of 4 h (including decompression treatment time) to promote the full diffusion of the foaming agent into the interlayer and interior of the graphene oxide particles.
[0092] (4) The mixture obtained in step (3) is filtered using a Buchner funnel and qualitative filter paper. When the liquid level drops to the surface of the filter cake, the filter cake is gently pressed with a rubber stopper to squeeze out the excess liquid, so as to minimize the amount of free solution remaining in the filter cake.
[0093] (5) Transfer the filter cake obtained in step (4) to a forced-air drying oven, set the temperature to 50℃, and dry at a constant temperature for 8 h to obtain dry graphene oxide-sodium bicarbonate composite precursor powder.
[0094] (6) Place the dried composite precursor in a ceramic mortar and grind for 10 min. Then, use a vibrating sieve to pass it through a 200-mesh standard sieve and collect the uniform powder under the sieve to accurately control the particle size distribution of the precursor and avoid uneven local gas generation during subsequent heat treatment.
[0095] (7) The homogenized powder from step (6) is spread evenly in a graphite box and placed in a muffle furnace. The temperature is raised to 400 °C at a rate of 5 °C / min under air atmosphere and held at this temperature for 1.0 h to decompose sodium bicarbonate and generate gas. Simultaneously, the gentle oxidation of air removes some unstable oxygen-containing groups. The powder is then naturally cooled to room temperature to obtain graphene oxide aerogel powder. Its density is approximately 62 mg / cm³. 3 .
[0096] Example 8 (1) Take a single-layer graphene oxide aqueous dispersion with a solid content of 10 mg / ml and a transverse dimension of 5-20 μm for the graphene oxide sheets. Use a magnetic stirrer to stir at a low speed of 300 rpm for 30 min to restore it to a good uniform dispersion state.
[0097] (2) Weigh azodicarbonamide powder and dissolve it in a small amount of N,N-dimethylformamide (DMF) (AC to DMF mass ratio is 1:2). Then dilute with deionized water to a azodicarbonamide mass concentration of 20% to obtain a foaming agent diluent. Mix the graphene oxide dispersion and the foaming agent diluent at a graphene oxide to azodicarbonamide mass ratio of 1:5, and add deionized water to make the total volume suitable for spraying.
[0098] (3) Place the mixture obtained in step (2) under a high-speed shear emulsifier, set the speed to 800 rpm, and mechanically stir for 1 h; then switch to a low-power ultrasonic processor (power 200 W, frequency 40 kHz) and ultrasonically treat for 15 min to fully disperse the azodicarbonamide molecules and enter the interlayer of graphene oxide, while preventing the sheets from being excessively broken.
[0099] (4) Place the suspension from step (3) in a vacuum dryer and let it stand for 20 minutes under an absolute pressure of 30 kPa to remove bubbles carried in during the mixing process, so as to ensure that the droplets are uniform and no hollow defects are generated during subsequent spray drying molding.
[0100] (5) The mixture after defoaming in step (4) is dried and shaped using a centrifugal spray dryer. The inlet air temperature is set to 180 ℃, the outlet air temperature is set to 80 ℃, the atomizing disc speed is set to 25000 rpm, and the feed rate is set to 5 ml / min. The dried product is collected to obtain the dry graphene oxide-azodicarbonamide composite precursor powder.
[0101] (6) Place the powder collected in step (5) in a vacuum oven at 50 ℃ (vacuum degree -0.09 MPa) and continue drying for 4 hours to completely remove residual DMF and moisture; then grind it slightly with a mortar and pestle and pass it through a 150-mesh sieve to obtain a composite precursor powder with uniform particle size.
[0102] (7) The composite precursor powder from step (6) is placed in a tube furnace and heated from room temperature to 1500 ℃ at a rate of 3 ℃ / min under an argon atmosphere (flow rate 300 ml / min). The temperature is then held constant for 2.0 h to allow the azodicarbonamide to decompose and generate nitrogen and other gases, which in situ drive the expansion and exfoliation of the graphene oxide sheets. After the holding period, the furnace is cooled to room temperature to obtain graphene oxide aerogel powder. Its density is approximately 38 mg / cm³. 3 .
[0103] Example 9 (1) Disperse single-layer graphene oxide sheets (lateral dimensions 10-30 μm) in deionized water to prepare a stable dispersion with a concentration of 15 mg / ml. Stir at 400 rpm for 1 h using a magnetic stirrer to fully hydrate and peel off the sheets.
[0104] (2) Weigh out hydrated citric acid solid, dissolve it in deionized water, and prepare a citric acid aqueous solution with a mass concentration of 40%. Mix the graphene oxide dispersion obtained in step (1) with the citric acid solution at a dry basis mass ratio of graphene oxide to citric acid of 1:10, and add deionized water to adjust the total solid content of the mixture to about 10 mg / ml.
[0105] (3) The mixture obtained in step (2) is sheared at 10,000 rpm for 30 min using a high-speed shear emulsifier. During the shearing process, the mixture is cooled in an ice water bath to prevent local temperature rise from causing premature decomposition of citric acid. After shearing, the mixture is allowed to stand naturally for 30 min to defoam.
[0106] (4) Pour the defoamed mixture from step (3) into a stainless steel flat pan with a liquid layer thickness of about 5 mm. Place it in a freeze dryer and pre-freeze it at -60 ℃ for 24 h. Then dry it once at a pressure of 5 Pa and a temperature of -5 ℃ for 48 h, and then dry it again at 25 ℃ for 12 h to obtain a sponge-like graphene oxide-citric acid composite precursor solid.
[0107] (5) The sponge-like solid in step (4) is coarsely crushed using a high-speed pulverizer (10,000 rpm, 30s), and then passed through a 200-mesh standard sieve using a vibrating screen. The powder passing through the sieve is collected to obtain a dry composite precursor powder with uniform particle size distribution.
[0108] (6) Spread the sieved powder from step (5) evenly in a graphite box, place it in a tube furnace, and introduce a hydrogen / nitrogen mixture (5% H2 + 95% N2, total flow rate of 400 ml / min) as a protective gas and reducing gas. Raise the temperature from room temperature to 900 ℃ at a rate of 2 ℃ / min, and hold at the temperature for 4.0 h to allow citric acid to decompose and generate gas and foam. At the same time, hydrogen reduces the graphene oxide and lowers the oxygen content.
[0109] (7) After the heat preservation is completed, continue to maintain the flow of mixed gas and cool the furnace to below 60 °C. Then switch to pure nitrogen gas for purging for 20 min for passivation treatment. Remove the product to obtain reduced graphene oxide aerogel powder. Its density is approximately 28 mg / cm³. 3 .
[0110] The above powder was compacted to a density of 670 mg / cm³. 3 Its mechanical rebound curve is as follows Figure 4 The compression cycle curves at 20% strain (pressure exceeding 15MPa) for 5 cycles confirmed that the prepared aerogel powder block has good compression resilience and basically no decrease in mechanical properties.
[0111] Example 10 (1) 8 g of commercially available graphene oxide powder (particle size about 30 μm) prepared by freeze drying was placed in a vacuum drying oven and vacuum dried at 80 °C and -0.1 MPa for 4 h to remove physically adsorbed moisture and initially widen the interlayer spacing of graphene oxide, providing favorable conditions for subsequent impregnation.
[0112] (2) Weigh out potassium bicarbonate and ammonium bicarbonate solids respectively, dissolve them in deionized water, and prepare a mixed aqueous solution with a mass concentration of 25% for each component (i.e., 25 wt% potassium bicarbonate and 25 wt% ammonium bicarbonate). Stir magnetically for 30 min at room temperature until completely dissolved to obtain a composite foaming agent solution.
[0113] (3) Add 8 g of the pretreated graphene oxide powder in step (1) to 320 ml of composite foaming agent solution (the mass of the foaming agent is 160 g, i.e. GO: foaming agent = 1:20). Place the beaker in a vacuum desiccator, evacuate to an absolute pressure of 30 kPa and maintain for 5 min. Then slowly open the vent valve to restore normal pressure. Repeat this cycle 5 times. Then continue to impregnate under normal pressure for a total time of 3 h to allow the two foaming agents to fully enter the interlayer of graphene oxide.
[0114] (4) Transfer the suspension after soaking in step (3) to a centrifuge tube, centrifuge at 8000 rpm for 10 min, carefully pour off the supernatant, and collect the bottom precipitate; wash the precipitate with a small amount of deionized water once and centrifuge again to remove the foaming agent residue that has not been intercalated on the surface.
[0115] (5) Spread the precipitate obtained by centrifugation in step (4) evenly in a glass dish, place it in a vacuum drying oven, set the temperature to 60 ℃ and the vacuum degree to -0.095 MPa, and dry at a constant temperature for 10 h to obtain dry graphene oxide-composite foaming agent precursor powder.
[0116] (6) Place the dried composite precursor from step (5) in an agate mortar and grind for 8 min. Then, pass it through a 140-mesh standard sieve and collect the uniform powder that passes through the sieve to ensure that the heating and gas generation behavior of each particle is consistent during the subsequent heat treatment process.
[0117] (7) The homogenized powder obtained in step (6) is spread evenly in a graphite box and placed in a tube furnace. The furnace is heated in stages under a nitrogen atmosphere (flow rate 250 ml / min): First, the temperature is raised from room temperature to 120 ℃ at a rate of 3 ℃ / min, and preheated at this constant temperature for 0.5 h to allow residual water of crystallization and low-boiling-point components to slowly escape; then, the temperature is further raised to 1200 ℃ at a rate of 5 ℃ / min, and held at this constant temperature for 6.0 h to allow the composite foaming agent to fully decompose and generate gas, driving the in-situ peeling and expansion of the graphene oxide sheets; after the holding period, the furnace is cooled to room temperature, and the powder is removed and gently passed through a 200-mesh sieve to obtain graphene oxide aerogel powder. Its density is approximately 52 mg / cm³. 3 .
[0118] Example 11 A method for preparing graphene oxide aerogel fibers includes the following steps: (1) Preparation of water-based graphene oxide dispersion: Select single-layer or few-layer graphene oxide sheets with a transverse dimension of about 5 μm. Use deionized water as the dispersion medium to prepare a water-based graphene oxide dispersion with a concentration of 30 mg / mL.
[0119] (2) The graphene oxide spinning solution was extruded through a needle into a coagulation bath for solidification and fixation. The resulting fiber was dried in an oven at 50 °C for 18 h to obtain a dry precursor.
[0120] (3) Preparation of sodium bicarbonate aqueous solution: Add ethylene glycol to deionized water to prepare a sodium bicarbonate aqueous solution with a mass concentration of 15%.
[0121] (4) The dry precursor of graphene oxide fiber was soaked in sodium bicarbonate aqueous solution at room temperature for 30 min and dried at 60℃ for 30 min to obtain the dry precursor of graphene oxide fiber-foaming agent.
[0122] (5) Preparation of graphene oxide aerogel fibers: The precursor was placed in a tube furnace and heated to 1500 ℃ at a rate of 1 ℃ / min, and held at that temperature for 5 h. The thermal decomposition of sodium bicarbonate produced gas, causing the sheets to peel and expand. After cooling, aerogel fibers were obtained, with the following microstructure: Figure 5 .
[0123] Example 12 A method for preparing graphene oxide aerogel fibers includes the following steps: (1) Preparation of graphene oxide spinning solution: Select monolayer or few-layer graphene oxide with a transverse dimension of about 10 μm, and use DMF as the dispersion medium to prepare a dispersion with a concentration of 25 mg / mL.
[0124] (2) Preparation of glycerol-DMF solution: Add glycerol to DMF and stir at 30 °C to dissolve, so as to prepare a glycerol-DMF solution with a mass concentration of 25%.
[0125] (3) Preparation of spinning solution containing foaming agent: The above dispersion and glycerol solution were mixed under magnetic stirring for 2 h to obtain a uniform spinning solution, wherein the final concentration of graphene oxide was 12 mg / mL and the mass ratio of foaming agent to graphene oxide was 1:2.
[0126] (4) Preparation of graphene oxide-glycerol composite precursor: The dry-jet wet spinning process was adopted. The spinning solution was extruded through the needle and then entered the coagulation bath through the air section for solidification and fixation. The resulting fiber was dried at 70 °C for 8 h to obtain the dry precursor.
[0127] (5) Preparation of graphene oxide aerogel fibers: The precursor was placed in a tube furnace and heated to 1300 ℃ at a rate of 3 ℃ / min, and held at that temperature for 3 h. The gas produced by the volatilization / decomposition of glycerol caused the sheets to peel and expand. After cooling, aerogel fibers were obtained, and their compression-resilience curves are shown below. Figure 6 The compression cycle curves at 90% strain for 100 cycles confirmed that the prepared aerogel fiber had good compression resilience and no significant decrease in mechanical properties.
[0128] Example 13 A method for preparing graphene oxide aerogel fibers includes the following steps: (1) Preparation of graphene oxide fiber precursor: Select monolayer or few-layer graphene oxide with a transverse dimension of about 30 μm, prepare a dispersion with a concentration of 20 mg / mL using DMF as the dispersion medium, spin the fiber using dry-jet wet spinning process, and dry it at 60 ℃ for 12 h after solidification to obtain graphene oxide fiber.
[0129] (2) Preparation of dry graphene oxide-ammonium carbonate composite precursor: Ammonium carbonate was dissolved in deionized water to prepare a 20% (w / w) ammonium carbonate aqueous solution. The dried graphene oxide fibers were placed in this solution and impregnated under reduced pressure of 50 kPa for 15 min. After restoring to normal pressure, the fibers were removed and the cycle was repeated 3 times, with a total impregnation time (including the cycle) of 6 h. After removal, the fibers were dried at 60 ℃ to obtain the composite precursor.
[0130] (3) Preparation of graphene oxide aerogel fibers: The composite precursor was placed in a tube furnace and heated to 450 °C at a rate of 5 °C / min, and held at that temperature for 1.5 h. The decomposition of ammonium carbonate produced gas, causing the sheets to peel off and expand. After cooling, aerogel fibers were obtained.
[0131] Example 14 A method for preparing graphene oxide aerogel fibers includes the following steps: (1) Preparation of graphene oxide spinning solution: Select monolayer or few-layer graphene oxide with a transverse dimension of about 20 μm, and use DMF as the dispersion medium to prepare a dispersion with a concentration of 35 mg / mL.
[0132] (2) Preparation of polyethylene glycol 400-DMF solution: Add polyethylene glycol 400 to DMF and stir to dissolve at 40 °C to prepare a polyethylene glycol-DMF solution with a mass concentration of 30%.
[0133] (3) Preparation of spinning solution containing foaming agent: The above dispersion was magnetically stirred and mixed with polyethylene glycol solution for 4 h to obtain a uniform spinning solution, wherein the final concentration of graphene oxide was 18 mg / mL and the mass ratio of foaming agent to graphene oxide was 1:1.
[0134] (4) Preparation of graphene oxide-polyethylene glycol composite precursor: wet spinning was used, followed by coagulation, stretching, washing and drying at 60 °C for 12 h to obtain dry precursor.
[0135] (5) Preparation of graphene oxide aerogel fibers: The precursor was placed in a tube furnace and heated to 600 °C at a rate of 8 °C / min, and held at that temperature for 1 h. The gas produced by the volatilization / decomposition of polyethylene glycol caused the sheets to peel off and expand. After cooling, aerogel fibers were obtained.
[0136] Example 15 A method for preparing graphene oxide aerogel fibers includes the following steps: (1) Preparation of graphene oxide aqueous dispersion: Select monolayer or few-layer graphene oxide with a transverse dimension of about 50 μm, and use deionized water as the dispersion medium to prepare a graphene oxide aqueous dispersion with a concentration of 10 mg / mL.
[0137] (2) Preparation of xylitol aqueous solution: Add xylitol to deionized water and stir at 40 °C to dissolve it, and prepare a xylitol aqueous solution with a mass concentration of 10%.
[0138] (3) Preparation of xylitol-containing spinning solution: The above dispersion was magnetically stirred and mixed with xylitol solution for 6 h to obtain a uniform spinning solution, wherein the final concentration of graphene oxide was 5 mg / mL and the mass ratio of foaming agent to graphene oxide was 1:3.
[0139] (4) Preparation of graphene oxide-xylitol composite precursor: wet spinning was used, followed by coagulation, stretching, washing and drying at 50 °C for 16 h to obtain dry precursor.
[0140] (5) Preparation of graphene oxide aerogel fibers: The precursor was placed in a tube furnace and heated to 800 ℃ at a rate of 10 ℃ / min, and held at that temperature for 0.5 h. The xylitol thermal decomposition produced gas, causing the sheets to peel off and expand. After cooling, aerogel fibers were obtained.
[0141] Comparative Example 1 Same as Example 5, except that the solution is heated during soaking to achieve liquid-phase foaming, as detailed below: (1) A graphene oxide aqueous dispersion with a concentration of 12 mg / mL was processed into a graphene oxide wet film on a stainless steel substrate by roller coating. After drying at 80°C for 4 hours, the film was peeled off to obtain a graphene oxide film.
[0142] (2) Sodium bicarbonate and ammonium bicarbonate are mixed in a mass ratio of 1:2 and dissolved in deionized water to prepare a mixed foaming agent solution with a total mass fraction of 20%.
[0143] The graphene oxide membrane was immersed in the above-mentioned foaming agent solution. In order to ensure the liquid phase foaming of the sodium bicarbonate and ammonium bicarbonate system, the temperature of the solution system should be at least 80°C to ensure the mildest solution foaming, with the smallest pore size and the highest density. After being taken out, it was vacuum dried at 40°C for 12 hours and then cooled to obtain a graphene oxide-based aerogel membrane.
[0144] The graphene oxide-based aerogel membrane prepared in this comparative example has an extremely wide pore size distribution and no uniform characteristic pore size value (e.g., Figure 8The density is 315 mg / cm³. 3 .
[0145] Comparative Example 2 Same as Example 11, except that liquid phase foaming is achieved in a high-temperature coagulation bath, as detailed below: (1) Preparation of water-based graphene oxide dispersion: Select single-layer or few-layer graphene oxide sheets with a transverse dimension of about 5 μm. Use deionized water as the dispersion medium to prepare a water-based graphene oxide dispersion with a concentration of 30 mg / mL.
[0146] (2) The graphene oxide spinning solution was extruded through a needle into a coagulation bath for solidification and fixation. The resulting fiber was dried in an oven at 50 °C for 18 h to obtain a dry precursor.
[0147] (3) Preparation of sodium bicarbonate aqueous solution: Add ethylene glycol to deionized water to prepare a sodium bicarbonate aqueous solution with a mass concentration of 15%.
[0148] (4) The dry precursor of graphene oxide fiber was immersed in sodium bicarbonate aqueous solution at 100°C for 30 min to decompose and foam the sodium bicarbonate in the aqueous solution. Finally, it was dried at 60°C for 30 min to obtain graphene oxide fiber aerogel fiber.
[0149] The aerogel fibers prepared in this comparative example, due to the foaming process occurring in the liquid phase, have large and highly unevenly distributed pore structures. After drying, the pore walls collapse significantly, making it impossible to maintain a uniform pore size distribution (e.g., ...). Figure 9 ).
Claims
1. A method for foaming a graphene oxide-based porous material, characterized in that, At least including: The dry graphene oxide-foaming agent composite precursor was heat-treated at 100℃~1500℃ for 0.5h~6h to obtain a graphene oxide-based porous material; the dry graphene oxide-foaming agent composite precursor is a graphene oxide assembly with foaming agents intercalated between the layers.
2. The foaming method according to claim 1, characterized in that, The dry graphene oxide-foaming agent composite precursor was obtained by the following method: The graphene oxide assembly was immersed in a foaming agent solution to allow the foaming agent to enter the interlayer of the graphene oxide. After drying, the dry graphene oxide-foaming agent composite precursor was obtained.
3. The foaming method according to claim 2, characterized in that, The foaming agent is an inorganic foaming agent and / or an organic foaming agent; The inorganic foaming agent is selected from at least one of sodium bicarbonate, ammonium bicarbonate, ammonium carbonate, sodium carbonate, and potassium bicarbonate. The organic foaming agent is selected from at least one of azo foaming agents, nitroso foaming agents, sulfonyl hydrazides, and acyl hydrazides.
4. The foaming method according to claim 1, characterized in that, The dry graphene oxide-foaming agent composite precursor was obtained by the following method: Graphene oxide and a foaming agent are mixed in a solution, allowing the foaming agent to penetrate the interlayer of the graphene oxide. After processing and molding, a graphene oxide assembly is formed, and after drying, the dry graphene oxide-foaming agent composite precursor is obtained.
5. The foaming method according to claim 4, characterized in that, The foaming agent is an organic biodegradable substance with a melting temperature lower than its decomposition temperature.
6. The foaming method according to any one of claims 1-5, characterized in that, The graphene oxide assembly is a powder, fiber, or membrane formed by assembling graphene oxide; after foaming, it yields aerogel powder, aerogel fiber, or aerogel membrane.
7. The foaming method according to any one of claims 1-5, characterized in that, The mass fraction of the foaming agent in the dry graphene oxide-foaming agent composite precursor is 1%–90%.
8. The foaming method according to claim 1, characterized in that, Heat treatment is carried out in an air atmosphere, an inert gas atmosphere, a reducing gas atmosphere, or a vacuum environment.
9. The foaming method according to claim 1, characterized in that, The density of the graphene oxide-based porous material is 10–1500 mg / cm³. 3 .
10. The application of the graphene oxide / reduced graphene oxide / graphene aerogel material according to any one of claims 1 to 9 in the fields of battery buffering and protection, battery thermal runaway protection, high-temperature heat sealing, high-temperature heat buffering, high-temperature thermal management, and catalysis.