A method for preparing weathered crack ceramic tiles based on granular through-body cloth
By applying a mixture of hard sand particles and dry glaze particles to the surface of the tile, combined with vacuum suction and mechanical polishing, the problem of imitating natural weathering cracks in rocks in existing technologies has been solved, and realistic weathering crack tiles have been produced efficiently.
Patent Information
- Application Number
- CN202611286359.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technology cannot simulate the sharp, three-dimensional cracks formed by natural weathering in a single firing process. It requires subsequent mechanical polishing or carving processes, which affects production efficiency.
A mixture of hard abrasive particles and dry glaze particles is used to create cracks during the firing and cooling process by taking advantage of the difference in thermal expansion coefficients. The hard abrasive particles are selectively retained by vacuum suction, and the crack effect is adjusted by mechanical polishing.
It achieves the formation of continuous network-like weathering grooves on the surface of ceramic tiles, providing a three-dimensional tactile experience and a realistic weathering and cracking texture with sharp edges, while also improving production efficiency and appearance controllability.
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic tile preparation technology, and in particular to a method for preparing weathered crack ceramic tiles based on granular through-body fabric. Background Technology
[0002] With the continuous upgrading of building ceramic manufacturing technology and the booming development of the high-end customized home decoration market, through-body ceramic tiles have gradually become one of the mainstream products in the market due to their excellent secondary processing performance, ultra-long wear resistance and lifespan and extremely high realism to natural stone.
[0003] In the existing manufacturing of imitation stone tiles, in order to reproduce the mottled texture and fault texture of weathered rocks such as natural marble or sandstone, the industry mainly relies on digital inkjet printing of the same color base and digital fine carving glaze to simulate the superposition of color and micro-concave and convex texture, in order to visually and tactilely approximate the rough effect of natural rocks after natural weathering.
[0004] However, the textures formed during the firing and melting process using existing technology are too smooth, making it difficult to simulate the sharp, three-dimensional cracks formed by natural weathering through a single tile firing process. A similar appearance can only be obtained by combining it with subsequent strong mechanical polishing or carving processes, which limits the efficiency of the final product. Summary of the Invention
[0005] To address the aforementioned shortcomings, the present invention aims to propose a method for preparing weathered crack ceramic tiles based on granular through-body fabric, thereby solving the problem that conventional crack ceramic tiles cannot imitate the sharp edge appearance effect formed by the natural weathering and cracking of rocks.
[0006] To achieve this objective, the present invention adopts the following technical solution: A method for preparing weathered crack ceramic tiles based on granular through-body fabric includes the following steps: S1. Apply a base glaze to the surface of the brick blank; S2. Apply a mixture of hard sand particles and dry glaze particles onto the base glaze to obtain the body to be treated. S3. Selectively suction the surface of the blank to be processed using vacuum suction, remove some of the dry glaze particles from the surface and retain the hard sand particles, so that the hard sand particles are partially exposed in the dry glaze particles, and obtain the brick blank with the glaze applied. S4. The finished brick blanks are sent into the kiln for firing and then cooled to produce ceramic tiles with weathering cracks. In the mixed dry particles, the mass fraction of hard sand particles is 1% to 30%, the melting point of the hard sand particles is higher than the firing temperature in step S4, the thermal expansion coefficient of the hard sand particles is greater than the thermal expansion coefficient of the surface glaze dry particles, the average particle size of the hard sand particles is 20 mesh to 80 mesh, and the average particle size of the surface glaze dry particles is 80 mesh to 160 mesh.
[0007] Preferably, in step S2, multiple groups of dry glaze particles mixed with different mass fractions of hard sand particles are applied according to a preset pattern by a positioning application method.
[0008] Preferably, the hard sand particles are at least one of corundum sand or quartz sand.
[0009] Preferably, in step S3, the vacuum suction pressure is -2 kPa to -10 kPa.
[0010] Preferably, in step S3, after covering the surface of the blank to be treated with a wire mesh, selective air is drawn from the surface of the blank to be treated through the mesh openings in the wire mesh. In the mixed dry granules, the average particle size of the hard sand particles is greater than the average particle size of the surface glaze dry granules, and the aperture of the wire mesh is smaller than the average particle size of the hard sand particles but larger than the average particle size of the surface glaze dry granules.
[0011] Preferably, in step S2, the application method is pipe-drop fabric, roller fabric, or digital powder spraying fabric.
[0012] Preferably, the coefficient of thermal expansion of the dry glaze particles is 5.5 × 10⁻⁶. -6 ~6.8×10 -6 / ℃.
[0013] Preferably, the chemical composition of the dry glaze particles includes, by mass percentage: 65%~70% SiO2, 9%~13% Al2O3, 2%~8% B2O3, and <2.5% Na2O+K2O.
[0014] Preferably, the method further includes step S5, which involves mechanically polishing the surface of the tile to remove some of the hard sand particles that are easily detached from the tile surface.
[0015] The technical solution provided by this invention may include the following beneficial effects: 1. By limiting the thermal expansion coefficient of hard sand particles to be greater than that of dry glaze particles, and utilizing the difference in thermal expansion coefficients between hard sand particles and dry glaze particles, during the cooling process after firing, some hard sand particles shrink significantly in volume, causing stress on the glaze surface and forming cracks. The stress superimposed on each other induces micro-cracks to connect and extend between the hard sand particles, ultimately forming a continuous network of natural weathering grooves on a macroscopic scale. This gives the weathered cracked tile a strong three-dimensional tactile feel and a realistic weathered and fractured texture.
[0016] 2. After the glaze hardens, it cracks during the cooling stage. Meanwhile, the hard sand particles, due to their high melting point, do not melt during the firing stage. Both the cracks and the exposed hard sand particles have relatively sharp edges. This solves the problem that conventional crackle glazes form cracks during the melting stage, and the appearance of grains formed by crystallization during the melting stage can only form relatively smooth edges, making it difficult to imitate the sharp edge appearance of natural weathering and cracking of rocks.
[0017] 3. Different mass fractions and average particle sizes of hard sand particles create weathering cracks of varying widths, depths, and overall appearances. By manually adjusting the amount and size of the hard sand particles, the overall appearance of the tile can be adjusted and controlled. Furthermore, the hard sand particles are only distributed within the dry glaze particles, preventing cracks from extending into the base glaze or even the tile body, thus avoiding impact on the tile's overall mechanical properties. Simultaneously, the selective nature of vacuum suction allows smaller dry glaze particles to be stripped and removed by the airflow, while larger hard sand particles remain exposed on the surface, enabling the glaze to better mimic the weathered surface morphology after firing.
[0018] 4. By positioning and applying the glaze dry granules mixed with hard sand particles, the glaze is applied to specific areas pre-set by humans according to different mass fractions. This allows the ceramic tile to produce cracks of different sizes in different areas after firing. Subsequent inkjet printing can also create richer surface effects.
[0019] 5. During vacuum suction, the use of wire mesh to intercept large-sized hard sand particles further reduces the loss of these particles and virtually eliminates the risk of large-scale accidental suction of hard sand particles caused by high negative pressure or localized turbulence on the billet surface, significantly improving the efficiency and stability of vacuum suction. Simultaneously, by covering the entire surface of the billet with wire mesh, hard sand particles are intercepted in situ, resolving the issue of significant displacement caused by airflow, which affects the distribution of hard sand particles.
[0020] 6. The coefficient of thermal expansion of corundum sand is approximately 8.0 × 10⁻⁶. -6 ~8.6×10 -6 At ℃, quartz sand not only has a higher coefficient of thermal expansion, but also a greater volume change rate due to crystal transformation. Meanwhile, the dry glaze particles maintain a relatively low coefficient of thermal expansion similar to that of conventional tile blanks and base glazes. This ensures a sufficient difference in coefficient of thermal expansion between the glaze and hard sand particles, allowing localized tensile stress to exceed the fracture threshold and form cracks. It also guarantees that the glaze layer as a whole maintains excellent thermal expansion adaptability with the underlying tile blank, preventing overall warping or glaze peeling.
[0021] 7. The surface glaze dry granules adopt a high-silicon, low-aluminum, and low-alkali metal formula, which not only ensures a low coefficient of thermal expansion but also significantly improves the high-temperature melt viscosity of the surface glaze. The high viscosity can effectively reduce the fluidity of the surface glaze dry granules with small average particle size at high temperatures, thereby avoiding affecting the distribution effect of hard sand particles. At the same time, strictly limiting Na2O+K2O<2.5% widens the preheating and degassing temperature range of the glaze layer, effectively solving the problem of pinholes and bubbles on the glaze surface caused by the small average particle size, high surface energy, and excessively fast melting of the surface glaze dry granules.
[0022] 8. The synergistic combination of corundum sand, quartz sand, and surface glaze granules: Although corundum sand and quartz sand do not melt at high temperatures, they are partially eroded by the molten surface glaze granules, resulting in good bonding between them. However, excessive erosion can cause the sharp edges of corundum sand and quartz sand to become rounded, affecting their simulated weathering appearance. The surface glaze granules, with a formula containing high silicon content and moderate aluminum content, can effectively control the erosion effect of quartz sand and corundum sand, allowing corundum sand and quartz sand to achieve a good balance between bonding and appearance during firing.
[0023] 9. This solution can also be combined with mechanical polishing to further refine the surface of the tile. Unlike conventional methods that require grinding the glaze layer with high polishing intensity to form texture, this solution only requires light polishing. Through the mechanical force of the polishing process, while removing some of the hard sand particles that are easy to fall off the surface of the tile, the glaze is caused to crack and pit a second time, forming a richer weathered appearance effect. Detailed Implementation
[0024] To facilitate understanding of the present invention, a more complete description is provided below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention.
[0025] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0027] A method for preparing weathered crack ceramic tiles based on granular through-body fabric includes the following steps: S1. Apply a base glaze to the surface of the brick blank; S2. Apply a mixture of hard sand particles and dry glaze particles onto the base glaze to obtain the body to be treated. S3. Selectively suction the surface of the blank to be processed using vacuum suction, remove some of the dry glaze particles from the surface and retain the hard sand particles, so that the hard sand particles are partially exposed in the dry glaze particles, and obtain the brick blank with the glaze applied. S4. The finished brick blanks are sent into the kiln for firing and then cooled to produce ceramic tiles with weathering cracks. In the mixed dry particles, the mass fraction of hard sand particles is 1% to 30%, the melting point of the hard sand particles is higher than the firing temperature in step S4, the thermal expansion coefficient of the hard sand particles is greater than the thermal expansion coefficient of the surface glaze dry particles, the average particle size of the hard sand particles is 20 mesh to 80 mesh, and the average particle size of the surface glaze dry particles is 80 mesh to 160 mesh.
[0028] By limiting the thermal expansion coefficient of hard sand particles to be greater than that of dry glaze particles, and utilizing the difference in thermal expansion coefficients between the hard sand particles and the dry glaze particles, during the cooling process after firing, some hard sand particles shrink significantly in volume, causing stress on the glaze surface and forming cracks. The stress superimposed on each other induces micro-cracks to connect and extend between the hard sand particles, ultimately forming a continuous network of natural weathering grooves on a macroscopic scale. This gives the weathered cracked tile a strong three-dimensional tactile feel and a realistic weathered and fractured texture.
[0029] After the glaze hardens, it cracks during the cooling stage. Meanwhile, the hard sand particles, due to their high melting point, do not melt during the firing stage. Both the cracks and the exposed hard sand particles have relatively sharp edges. This solves the problem that conventional crackle glazes form cracks during the melting stage, and the appearance of grains formed by crystallization during the melting stage can only form relatively smooth edges, making it difficult to imitate the sharp edge appearance of natural weathering and cracking of rocks.
[0030] Different mass fractions and average particle sizes of hard sand particles create weathering cracks of varying widths, depths, and overall appearances. By manually adjusting the amount and size of the hard sand particles, the overall appearance of the tile can be adjusted and controlled. Furthermore, the hard sand particles are only distributed within the dry glaze particles, preventing cracks from extending into the base glaze or even the tile body, thus avoiding impact on the tile's overall mechanical properties. Simultaneously, the selective nature of vacuum suction allows smaller dry glaze particles to be stripped and removed by the airflow, while larger hard sand particles remain exposed on the surface, enabling the glaze to better mimic the weathered surface morphology after firing.
[0031] Preferably, in step S2, multiple groups of dry glaze particles mixed with different mass fractions of hard sand particles are applied according to a preset pattern by a positioning application method.
[0032] By using targeted application, dry glaze particles mixed with hard sand are applied to specific areas pre-designed by humans according to different mass fractions. This allows the ceramic tile to develop cracks of varying sizes in different areas after firing. Subsequent inkjet printing can also create richer surface effects.
[0033] In one embodiment, 25% by mass of hard sand particles are used to form dense, deep cracks on the surface of the fired ceramic tile. Digital inkjet printing ink is then used to penetrate and develop color in the cracks, mimicking the appearance of severe weathering and cracking.
[0034] Preferably, the hard sand particles are at least one of corundum sand or quartz sand.
[0035] Both corundum sand and quartz sand have high coefficients of thermal expansion, and corundum sand has a density as high as 3.95-4.05 g / cm³. 3 This can further improve the separation efficiency of vacuum suction; while quartz sand can synergistically utilize its reversible crystal transformation at about 573°C to bring about a greater volume change rate, further improving the efficiency of stress fracture during the cooling process.
[0036] Preferably, in step S3, the vacuum suction pressure is -2 kPa to -10 kPa.
[0037] This negative pressure range ensures efficient extraction of dry glaze particles while preventing hard sand particles from being carried out and lost.
[0038] Preferably, in step S3, after covering the surface of the blank to be treated with a wire mesh, selective air is drawn from the surface of the blank to be treated through the mesh openings in the wire mesh. In the mixed dry granules, the average particle size of the hard sand particles is greater than the average particle size of the surface glaze dry granules, and the aperture of the wire mesh is smaller than the average particle size of the hard sand particles but larger than the average particle size of the surface glaze dry granules.
[0039] During vacuum suction, the use of wire mesh to intercept large-sized hard sand particles further reduces the loss of these particles and virtually eliminates the risk of large-scale accidental suction of hard sand particles caused by high negative pressure or localized turbulence on the billet surface, significantly improving the efficiency and stability of vacuum suction. Simultaneously, by covering the entire surface of the billet with wire mesh, hard sand particles are intercepted in situ, resolving the issue of significant displacement caused by airflow, which affects the distribution of hard sand particles.
[0040] It should be noted that regardless of the material separation method using vacuum suction, a very small amount of hard sand particles cannot be avoided from being carried out. The dry glaze particles containing a small amount of hard sand particles after vacuum suction can be mixed with mixed dry particles of similar mass fraction and put back into production. However, the mixing ratio needs to be controlled according to the specific situation to avoid too many small-sized hard sand particles affecting the average particle size of the hard sand particles, thereby affecting the appearance quality of the fired tiles.
[0041] Preferably, in step S2, the application method is pipe-drop fabric, roller fabric, or digital powder spraying fabric.
[0042] The above application method is more suitable for applying mixed dry particles with different particle sizes or specific gravities. It avoids the problem of uneven application of dry particles in the vertical direction caused by the difference in particle size or specific gravity between hard sand particles and surface glaze dry particles when using vibrating screen, screen printing, or centrifugal disc application methods.
[0043] In one embodiment, digital powder spraying is used to apply dry glaze particles mixed with 25% hard sand particles in a linear pattern. After firing, continuous cracks are formed, giving the ceramic tile surface a fractured effect similar to weathered sandstone.
[0044] Preferably, the coefficient of thermal expansion of the dry glaze particles is 5.5 × 10⁻⁶. -6 ~6.8×10 -6 / ℃.
[0045] The coefficient of thermal expansion of corundum sand is approximately 8.0 × 10⁻⁶. -6 ~8.6×10 -6 At ℃, quartz sand not only has a higher coefficient of thermal expansion, but also a greater volume change rate due to crystal transformation. Meanwhile, the dry glaze particles maintain a relatively low coefficient of thermal expansion similar to that of conventional tile blanks and base glazes. This ensures a sufficient difference in coefficient of thermal expansion between the glaze and hard sand particles, allowing localized tensile stress to exceed the fracture threshold and form cracks. It also guarantees that the glaze layer as a whole maintains excellent thermal expansion adaptability with the underlying tile blank, preventing overall warping or glaze peeling.
[0046] Preferably, the chemical composition of the dry glaze particles includes, by mass percentage: 65%~70% SiO2, 9%~13% Al2O3, 2%~8% B2O3, and <2.5% Na2O+K2O.
[0047] The surface glaze dry granules adopt a high-silicon, low-aluminum, and low-alkali metal formula, which not only ensures a low coefficient of thermal expansion but also significantly improves the high-temperature melt viscosity of the surface glaze melt. The high viscosity can effectively reduce the fluidity of the surface glaze dry granules with small average particle size at high temperatures, thereby avoiding affecting the distribution effect of hard sand particles. At the same time, strictly limiting Na2O+K2O<2.5% widens the preheating and degassing temperature range of the glaze layer, effectively solving the problem of pinholes and bubbles on the glaze surface caused by the small average particle size, high surface energy, and excessively fast melting of the surface glaze dry granules.
[0048] It is worth noting that although corundum sand and quartz sand do not melt at high temperatures, they are partially eroded by the molten glaze particles, resulting in better bonding between them. However, excessive erosion can cause the sharp edges of corundum sand and quartz sand to become rounded, affecting their simulated weathering appearance. The glaze particles, formulated with high silicon content and moderate aluminum content, can effectively control the erosion effect of quartz sand and corundum sand, allowing them to achieve a good balance between bonding and appearance during firing.
[0049] The boron content is adjusted as needed. A high boron content of 4% to 8% can reduce the high-temperature viscosity of the melt, and the high transparency of the glaze brought by high boron can better expose the three-dimensional visual effect brought by hard sand grains and cracks. When a relatively low boron content of 2% to 4% is used, the milky and hazy feeling of the glaze is used to simulate the appearance of weathered sandstone.
[0050] Preferably, the method further includes step S5, which involves mechanically polishing the surface of the tile to remove some of the hard sand particles that are easily detached from the tile surface.
[0051] This solution can also be combined with mechanical polishing to further refine the surface of the tile. Unlike conventional methods that require grinding the glaze layer with high polishing intensity to form texture, this solution only requires light polishing. Through the mechanical force of the polishing process, while removing some of the hard sand particles that are easy to fall off the surface of the tile, the glaze is caused to crack and pit a second time, forming a richer weathered appearance effect.
[0052] Example 1 Using conventional brick blanks and base glaze, the dry granules contain 10% hard sand particles with an average particle size of 40 mesh, and are composed of corundum sand and quartz sand in a mass ratio of 1:1. The dry glaze particles have a mesh size of 80 mesh, and their chemical composition by mass percentage includes: 65% SiO2, 9% Al2O3, 8% B2O3, and 2% Na2O + K2O. The preparation method is as follows: S1. Apply a base glaze to the surface of the brick blank; S2. The mixed dry granules are applied to the base glaze using a pipe drop method to obtain the body to be treated; S3. Selectively suction the surface of the blank to be processed using a -4kPa vacuum suction to remove some of the dry glaze particles from the surface and retain the hard sand particles, so that the hard sand particles are partially exposed in the dry glaze particles, and the brick blank with the glaze is obtained. S4. The finished brick blanks are sent into the kiln for firing and then cooled to obtain ceramic tiles with weathering cracks evenly distributed all over the surface.
[0053] Example 2 Using conventional brick blanks and base glaze, two groups were prepared. The first group contained 3% hard sand particles by mass, with an average particle size of 80 mesh, and a composition of corundum sand:quartz sand in a mass ratio of 2:1. The second group contained 25% hard sand particles by mass, with an average particle size of 20 mesh, and a composition of corundum sand:quartz sand in a mass ratio of 1:2. The surface glaze particles had a mesh size of 160 mesh. The chemical composition of the surface glaze particles, by mass percentage, included: 70% SiO2, 13% Al2O3, 3% B2O3, and 2% Na2O + K2O. The preparation method is as follows: S1. Apply a base glaze to the surface of the brick blank; S2. Using digital powder spraying, two sets of mixed dry particles are applied to the base glaze. The second set of mixed dry particles is applied according to the lines that form a block pattern as preset by the human, while the first set of mixed dry particles fills the other parts of the base glaze to obtain the body to be treated. S3. After covering the surface of the blank to be treated with a 120-mesh wire mesh, use -8kPa vacuum suction to selectively suction the surface of the blank through the mesh of the wire mesh to remove some of the dry glaze particles on the surface and retain the hard sand particles, so that the hard sand particles are partially exposed in the dry glaze particles, and the brick blank with the glaze is obtained. S4. The finished brick blanks are sent into the kiln for firing and then cooled to produce ceramic tiles with blocky weathering cracks.
[0054] Comparative Example 1 The preparation method of Comparative Example 1 is the same as that of Example 1, except that the average particle size of the hard sand particles is replaced with 100 mesh.
[0055] Because the average particle size of the hard sand is too fine, the sand particles and the dry glaze particles cannot form a suspension velocity difference during vacuum suction. Coarse and fine materials are sucked away and lost together, and the hard sand particle skeleton cannot be retained and exposed on the surface. At the same time, it is over-melted at the high temperature of firing, and cannot effectively form continuous cracks and retain sharp edges.
[0056] Comparative Example 2 The preparation method of Comparative Example 2 is the same as that of Example 1, except that the average particle size of the hard sand particles is replaced with 10 mesh.
[0057] Due to the excessively large average particle size of the hard sand, severe longitudinal sedimentation and stratification occur during the material spreading process. After firing, the excessively large particles in some areas touch the base glaze layer, affecting the overall mechanical strength of the tile.
[0058] Comparative Example 3 The preparation method of Comparative Example 3 is the same as that of Example 1, except that the average particle size of the dry glaze particles is replaced with 40 mesh.
[0059] Because the average particle size of the dry glaze particles is too large, and the particle size of the dry glaze particles is similar to that of the hard sand particles, although the dry glaze particles can be barely separated during vacuum suction due to the difference in specific gravity, the large size of the dry glaze particles requires an increased firing time during high-temperature firing to allow the dry glaze particles to completely melt, while the hard sand particles are excessively eroded and dissolved, making it impossible to effectively form continuous cracks and retain sharp edges.
[0060] Comparative Example 4 The preparation method of Comparative Example 4 is the same as that of Example 1, except that the average particle size of the dry glaze particles is replaced with 200 mesh.
[0061] Because the average particle size of the dry glaze particles is too small, the surface energy is too high. This causes the glaze to melt prematurely and close the pores in the high-temperature firing section of the kiln, blocking the normal release of decomposition gases from the base. This results in large areas of pinholes, pits, and severe foaming defects on the glaze surface of the fired ceramic tile.
[0062] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0063] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for preparing weathered crack ceramic tiles based on granular through-body fabric, characterized in that, Includes the following steps: S1. Apply a base glaze to the surface of the brick blank; S2. Apply a mixture of hard sand particles and dry glaze particles onto the base glaze to obtain the body to be treated. S3. Selectively suction the surface of the blank to be processed using vacuum suction, remove some of the dry glaze particles from the surface and retain the hard sand particles, so that the hard sand particles are partially exposed in the dry glaze particles, and obtain the brick blank with the glaze applied. S4. The finished brick blanks are sent into the kiln for firing and then cooled to produce ceramic tiles with weathering cracks. In the mixed dry particles, the mass fraction of hard sand particles is 1% to 30%, the melting point of the hard sand particles is higher than the firing temperature in step S4, the thermal expansion coefficient of the hard sand particles is greater than the thermal expansion coefficient of the surface glaze dry particles, the average particle size of the hard sand particles is 20 mesh to 80 mesh, and the average particle size of the surface glaze dry particles is 80 mesh to 160 mesh.
2. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: In step S2, multiple sets of dry glaze particles mixed with different mass fractions of hard sand particles are applied according to a preset pattern by a positioning application method.
3. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: The hard sand particles are at least one of corundum sand or quartz sand.
4. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: In step S3, the vacuum suction pressure is -2 kPa to -10 kPa.
5. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: In step S3, after covering the surface of the blank to be treated with a wire mesh, selective air is drawn from the surface of the blank through the mesh openings. In the mixed dry granules, the average particle size of the hard sand particles is greater than the average particle size of the surface glaze dry granules, and the aperture of the wire mesh is smaller than the average particle size of the hard sand particles but larger than the average particle size of the surface glaze dry granules.
6. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: In step S2, the application method is to use pipe-drop fabric, roller fabric, or digital powder spraying fabric.
7. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: The coefficient of thermal expansion of the dry glaze particles is 5.5 × 10⁻⁶. -6 ~6.8×10 -6 / ℃.
8. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that, The chemical composition of the dry glaze particles, by mass percentage, includes: 65%~70% SiO2, 9%~13% Al2O3, 2%~8% B2O3, and <2.5% Na2O+K2O.
9. The method for preparing weathered crack ceramic tiles based on granular through-body fabric according to claim 1, characterized in that: It also includes step S5, which involves mechanically polishing the surface of the tile to remove some of the hard sand particles that are easy to detach from the tile surface.