Preparation method and application of one-pot simultaneous polymerization of micro-crosslinked polyesteramide
The one-pot simultaneous polymerization method for preparing micro-crosslinked polyesteramide utilizes a protonic acid-metal composite catalytic system and the addition of appropriate crosslinking agents to solve the problems of cumbersome procedures, long cycles, and improper crosslinking in existing processes. This method achieves efficient and uniform synthesis of polyesteramide, which is suitable for engineering plastics, fibers, and hot melt adhesives.
Patent Information
- Application Number
- CN202611475448.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-10
AI Technical Summary
Existing polyesteramide synthesis processes suffer from problems such as cumbersome procedures, long production cycles, high energy consumption, uneven chain sequence distribution, low equipment utilization, and improper timing of crosslinking agent addition.
A one-pot simultaneous polymerization method for preparing micro-crosslinked polyesteramides was developed. This method utilizes a protic acid-metal composite catalytic system to simultaneously carry out the ring-opening polymerization of lactams and the esterification reaction of aliphatic dicarboxylic acids-aliphatic diols. By combining this with the appropriate timing of the addition of crosslinking agents, micro-crosslinked polyesteramides with narrow molecular weight distribution and uniform structure were prepared.
It shortens the reaction cycle, reduces energy consumption, achieves uniform molecular weight distribution and thermoplasticity of the material, avoids the formation of macroscopic gels, and is suitable for a variety of application scenarios.
Smart Images

Figure CN123062707A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer synthesis chemistry technology, specifically relating to the preparation method and application of one-pot simultaneous polymerization of micro-crosslinked polyesteramide. Background Technology
[0002] Polyesteramides contain both ester and amide bonds in their main chain, combining the processability of polyester with the high strength and wear resistance of polyamides. They are a class of high-performance polymer materials with excellent comprehensive properties and are widely used in fiber, engineering plastics, hot melt adhesives and other fields.
[0003] The synthesis of polyesteramides currently generally employs a stepwise polymerization process: first, the lactam is hydrolyzed and ring-opened to prepare a polyamide prepolymer, and then a diacid and diol are introduced for esterification and polycondensation reactions; or a polyester oligomer is prepared first, and then amide monomers are introduced for copolymerization. This stepwise polymerization process has the following inherent drawbacks: 1) The process is complicated, requiring a separate high-pressure prepolymerization section, resulting in a long production cycle and high energy consumption; 2) The ring-opening polymerization and esterification reaction of lactams are carried out in stages, which easily generates long-chain polyamide blocks or long polyester blocks. The chain sequence distribution is uneven, the molecular weight distribution of the product is wide, and the batch performance fluctuates greatly. 3) Multiple feeding operations and switching of pressure and temperature conditions are required, resulting in low equipment utilization.
[0004] There is a limited amount of research on one-pot polyesteramide, but the inability to balance the ring-opening rate of lactams with the esterification rate of dicarboxylic acids and diols leads to a disconnect between the two reaction processes, making it difficult to achieve simultaneous generation of amide and ester units. Furthermore, the existing one-pot technology has not solved the problem of the timing of crosslinking agent addition, making it impossible to achieve mild and controllable molecular-scale micro-crosslinking. Summary of the Invention
[0005] Existing stepwise polyesteramide preparation processes suffer from long cycles and uneven chain sequence distribution; existing one-pot methods struggle to achieve balanced ring-opening. To address the shortcomings of improper esterification reaction rate and timing of crosslinking agent addition, the first objective of this invention is to provide a one-pot method for the simultaneous polymerization of micro-crosslinked polyesteramides.
[0006] The second objective of this invention is to provide micro-crosslinked polyesteramide prepared by the above method; the third objective is to provide its applications.
[0007] To achieve the first objective mentioned above, the technical solution adopted by the present invention includes: This invention discloses a one-pot simultaneous polymerization method for preparing micro-crosslinked polyesteramide, comprising the following steps: S1. Under the protection of an inert gas, the lactam monomer, aliphatic diacid, aliphatic diol, and composite catalyst are added to the reactor and heated to carry out the reaction. Under the action of the composite catalyst, the lactam ring-opening polymerization and the aliphatic diacid-aliphatic diol esterification reaction occur simultaneously, so that the amide structural unit and the ester structural unit are generated simultaneously until the acid value of the system drops below the preset value. S2. Add a crosslinking agent to the system and maintain the temperature for the reaction; S3. Continue heating to carry out a staged vacuum polycondensation reaction. The reaction endpoint is controlled by the melt stirring torque. Micro-crosslinked polyesteramide is then discharged. The crosslinking agent is selected from polyhydroxy compounds or polycarboxylic acid compounds; The composite catalyst is obtained by combining a protic acid catalyst and a metal catalyst. The polyhydroxy compound is selected from one or more of glycerol, trimethylolpropane, and pentaerythritol; The polycarboxylic acid compound is selected from pyromellitic acid and / or citric acid.
[0008] This invention uses protic acids In this metal-composite catalytic system, the lactam monomer, aliphatic diacid, aliphatic diol, and composite catalyst are added to the reactor in a single step, eliminating the need for pre-synthesization of the polyamide prepolymer. Simultaneously, the ring-opening hydrolysis polymerization of the lactam and the reaction of the diacid occur within the same reaction system. In the diol esterification reaction, amide and ester structural units are generated simultaneously, inhibiting the formation of long blocks and resulting in a low-dispersion matrix with uniform sequence distribution. After the acid value of the system decreases to the threshold and the carboxyl active sites are moderately consumed, a crosslinking agent is added. The crosslinking agent is only added to the molecular chain in the later stage, gently constructing a molecular-scale micro-crosslinked network without macroscopic gelation. Subsequent stepwise vacuum polycondensation yields the target product.
[0009] In the composite catalyst, the protic acid mainly catalyzes the hydrolysis and ring-opening of lactams; the metal catalyst mainly catalyzes esterification and subsequent polycondensation. The reasonable combination of the two catalysts controls the ratio of protic acid and metal catalyst to match the two types of reaction rates and achieve the synchronous growth of amide and ester units. If the catalyst ratio is out of balance, one type of reaction will proceed preferentially, generating a large number of long blocks and widening the molecular weight distribution.
[0010] The present invention chooses to add the crosslinking agent later because the concentration of carboxyl and hydroxyl groups in the system is very high in the early stage of the reaction. Adding the crosslinking agent early will cause violent crosslinking and directly produce macroscopic gel. After esterification, when the acid value drops to 25 mg KOH / g, the active sites are partially consumed. At this time, the crosslinking agent is added to achieve mild and controllable micro-crosslinking, forming only molecular-scale local crosslinking and maintaining the thermoplasticity of the material.
[0011] Furthermore, the lactam monomer is selected from autolactam and / or dodecalactam.
[0012] Furthermore, the aliphatic dicarboxylic acid is selected from one or more of the following: succinic acid, octanoic acid, sebacic acid, dodecanoic acid, terephthalic acid, and isophthalic acid. Furthermore, the aliphatic diol is selected from ethylene glycol, 1,3-diol, etc. Propylene glycol, 1,4 Butylene glycol, 1,5 Pentylene glycol, 1,8 Octanediol, 1,10 One or more of decanediol.
[0013] Furthermore, the protic acid catalyst is selected from one or more of p-toluenesulfonic acid, methanesulfonic acid, and benzenesulfonic acid; The metal catalyst is selected from one or more of tetrabutyl titanate, tetraethyl titanate, antimony trioxide, and zinc acetate.
[0014] Furthermore, the molar ratio of the lactam monomer to the aliphatic diacid is (6:4) to (8.5:1.5). For example, the molar ratio of the lactam monomer to the aliphatic diacid can be 6:4, 6.5:3.5, 7:3, 7.5:2.5, 8:2, 8.5:1.5, etc.
[0015] Furthermore, the molar ratio of the aliphatic diol to the aliphatic diacid is (1.3~2.2):1. For example, the molar ratio of the aliphatic diol to the aliphatic diacid can be 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, etc.
[0016] Furthermore, the amount of crosslinking agent added is 0.2 to 6 wt% of the sum of the mass of the lactam monomer and the aliphatic diacid monomer. For example, the amount of crosslinking agent added is 0.2 wt%, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, etc., of the sum of the mass of the lactam monomer and the aliphatic diacid monomer.
[0017] Furthermore, the composite catalyst is a mixture of a protic acid catalyst and a metal catalyst in a mass ratio of (0.5~3):1. For example, the composite catalyst is a mixture of a protic acid catalyst and a metal catalyst in a mass ratio of 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, or 3:1.
[0018] Furthermore, the total amount of the composite catalyst added is 0.05~0.8 wt% of the sum of the mass of the lactam and aliphatic diacid monomers. For example, the total amount of the composite catalyst added is 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, etc., of the sum of the mass of the lactam and aliphatic diacid monomers.
[0019] Furthermore, the reaction temperature in step S1 is 190~230℃, the reaction time is 2~6 h, and the reaction endpoint of the esterification reaction is when the acid value of the system drops below 25mgKOH / g.
[0020] Furthermore, the heat preservation reaction time after adding the crosslinking agent in step S2 is 10~60 min.
[0021] Furthermore, the staged vacuum polycondensation reaction includes a pre-polycondensation stage and a final polycondensation stage; The polycondensation temperature of the pre-polymerization stage is 230~235℃, the vacuum degree is 1000~5000 Pa, and the duration of the pre-polymerization stage is 0.5~4 h. The final polycondensation stage has a polycondensation temperature of 235~245℃ and a vacuum degree of 50~500 Pa.
[0022] Furthermore, the melt stirring torque at the endpoint of the staged vacuum polycondensation reaction is controlled at 20~25N. m; if the torque is less than 20N If the degree of polymerization is insufficient, the mechanical properties will not meet the standards; if the torque is too high, excessive cross-linking is likely to occur, resulting in macroscopic gelation.
[0023] To achieve the second objective mentioned above, the technical solution adopted by the present invention includes: This invention discloses a micro-crosslinked polyesteramide prepared using the method described above. The micro-crosslinked polyesteramide exhibits molecular-scale micro-crosslinking, is thermoplastic and melt-processable, and does not contain macroscopic gel.
[0024] Furthermore, the structural units derived from lactam monomers account for 60-85% of the total molar proportion of the micro-crosslinked polyester amide structural units.
[0025] Furthermore, the micro-crosslinked polyesteramide has a melting point higher than 155℃, a glass transition temperature greater than 48℃, an initial decomposition temperature ≥390℃, a tensile strength ≥55 MPa, and a molecular weight distribution index ≤2.2. A high molecular weight distribution index indicates a large variation in molecular chain length, resulting in a mixture of long and short chains within the polymer. This can cause fluctuations in the material's melting point, unstable flowability during injection molding and extrusion, and inconsistent mechanical properties and batch-to-batch uniformity in the finished product.
[0026] To achieve the third objective mentioned above, the technical solution adopted by the present invention includes: This invention discloses the application of micro-crosslinked polyesteramide as described above in the preparation of engineering plastics, industrial fibers, hot melt adhesives, and general packaging materials.
[0027] Beneficial effects of the invention This invention provides a one-pot simultaneous polymerization method for preparing micro-crosslinked polyesteramide. With the participation of a protonic acid-metal complex catalytic system and appropriate timing of crosslinking agent addition, a novel material with narrow molecular weight distribution and good structural uniformity is ultimately prepared. Compared with existing technologies, this method has the following advantages: 1. Process innovation eliminates the need for a separate high-pressure prepolymerization process: all basic monomers are fed in one go, eliminating the need for pre-high-pressure hydrolysis to prepare polyamide prepolymers, shortening the reaction cycle by more than 30%, reducing energy consumption, simplifying operation, and adapting to existing high-pressure reactors in the polyester amide industry, making it easy to industrialize.
[0028] 2. Uniform chain sequence and narrow molecular weight distribution: protic acid Metal-based catalysis simultaneously regulates the ring-opening polymerization and esterification reactions of lactams, resulting in the synchronous generation of amide and ester units. This suppresses long block structures, leading to a product molecular weight distribution index ≤2.2 and significantly better batch stability than traditional stepwise processes.
[0029] 3. Controllable crosslinking timing to avoid early gelation: Crosslinking agent is not added at the initial stage of feeding; crosslinking agent is added after the acid value of the system drops below the preset value and the active sites are moderately consumed, so as to achieve mild molecular-scale micro-crosslinking, maintain the thermoplasticity of the material, avoid macroscopic gelation, and take into account both thermal and mechanical properties.
[0030] 4. High versatility: The crosslinking agent can be either polyhydroxy or polycarboxylic acid such as trimesic acid and citric acid; the process parameters are adjustable, the product performance window is wide, and it is suitable for various applications such as engineering plastics, fibers, hot melt adhesives, and packaging. Attached Figure Description
[0031] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.
[0032] Figure 1 The NMR spectrum of the polyesteramide prepared in Example 1 is shown. Detailed Implementation
[0033] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0034] Performance testing methods 1) Thermal stability: Thermogravimetric analysis was used to test the initial decomposition temperature at a nitrogen atmosphere with a heating rate of 20℃ / min. The initial decomposition temperature at which the weight loss was 5wt% was recorded.
[0035] 2) Thermal properties: Differential scanning calorimeter test, nitrogen atmosphere, heating rate 10℃ / min, and melting point recorded.
[0036] 3) Mechanical properties: Tensile strength and modulus were determined in accordance with GB / T 1040.1-2006.
[0037] 4) Molecular weight distribution: Number-average molecular weight and molecular weight distribution index were determined by gel permeation chromatography (GPC).
[0038] 5) GB / T 2895-2008 Determination of partial and total acid values of polyester resins in plastics.
[0039] Example 1 1 mol caprolactam, 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 0.1 g p-toluenesulfonic acid, and 0.1 g tetrabutyl titanate were added to a 5 L high-pressure reactor in one step; nitrogen was purged three times; the temperature was raised to 215 °C and held for 4 h to carry out the esterification reaction; the acid value of the system was tested and found to be 19 mg KOH / g, indicating that the esterification reaction endpoint had been reached.
[0040] Maintain the temperature inside the vessel, add 1.42g of glycerin, and keep warm for 30 minutes.
[0041] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 230℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 240℃, and the vacuum at 200Pa; the reaction continues until the torque reaches 25N. The reaction was stopped at m; the material was discharged under nitrogen pressure and pelletized. (See NMR image.) Figure 1 .
[0042] The prepared polyesteramide has the following properties after testing: melting point 168℃; Tg 51℃; initial thermal decomposition temperature 398℃; tensile strength 54.2MPa; molecular weight distribution index PDI 1.98; no macroscopic gel, and can be injection molded and extruded.
[0043] Example 2 1 mol caprolactam, 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 0.1 g p-toluenesulfonic acid, and 0.1 g tetrabutyl titanate were added to a 5 L high-pressure reactor in one step; nitrogen was purged three times; the temperature was raised to 215 °C and held for 4 h for esterification reaction. The acid value of the system was tested and found to be 18.6 mg KOH / g, indicating that the esterification reaction endpoint had been reached.
[0044] Maintain the temperature inside the vessel, add 3.45g of glycerin, and keep warm for 30 minutes.
[0045] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 230℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 240℃, and the vacuum at 200Pa; the reaction continues until the torque reaches 24N. The reaction is stopped. Nitrogen gas is applied to pressurize the material before pelletizing.
[0046] The prepared polyesteramide was tested and found to have the following properties: melting point 169℃; Tg 53℃; initial thermal decomposition temperature 400℃; tensile strength 57.5MPa; PDI 2.05; no macroscopic gelation.
[0047] Example 3 1 mol caprolactam, 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 0.08 g p-toluenesulfonic acid, and 0.08 g tetrabutyl titanate were added to a 5 L high-pressure reactor in one step; nitrogen was purged three times; the temperature was raised to 215 °C and held for 4 h for esterification reaction; the acid value of the system was tested and found to be 19.2 mg KOH / g, indicating that the esterification reaction endpoint had been reached.
[0048] Maintain the temperature inside the vessel, add 2.10g of trimesic acid, and keep warm for 30 minutes.
[0049] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 235℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 242℃, and the vacuum at 200Pa; the reaction continues until the torque reaches 24N. m-reaction; nitrogen pressurization for discharge and pelletizing.
[0050] The prepared polyesteramide was tested and found to have the following properties: melting point 170℃; Tg 54℃; initial thermal decomposition temperature 401℃; tensile strength 58.1MPa; molecular weight distribution index PDI 2.01; no macroscopic gel.
[0051] Comparative Example 1 1 mol caprolactam and 10 g water were added to a 5 L high-pressure reactor and purged with nitrogen three times. The reaction was carried out at 1.2 MPa and 190 °C for 1 h to obtain a polyamide prepolymer. The pressure was released, and 0.3 mol sebacic acid, 0.5 mol 1,4-butanediol and 0.16 g tetrabutyl titanate were added. The reaction was carried out at 215 °C for 4 h. Then 1.42 g glycerol was added and the mixture was kept at this temperature for 30 min.
[0052] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 230℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 240℃, and the vacuum at 200Pa; the reaction continues until the torque reaches 25N. The reaction is stopped; nitrogen gas is applied to pressurize and pelletize the material.
[0053] The prepared polyesteramide has the following properties after testing: melting point 162℃; Tg 46℃; initial thermal decomposition temperature 392℃; tensile strength 52.8MPa; molecular weight distribution index (PDI) 2.57. The product has a wide molecular weight distribution, large differences between long and short chain components, and significant fluctuations in processing fluidity.
[0054] Comparative Example 2 1 mol caprolactam, 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 0.02 g p-toluenesulfonic acid, and 0.18 g tetrabutyl titanate were added to a 5 L high-pressure reactor in one step; nitrogen was purged three times; the temperature was raised to 215 °C and held for 4 h to carry out the esterification reaction; the acid value of the system was tested and found to be 21 mg KOH / g, indicating that the esterification reaction endpoint had been reached.
[0055] Maintain the temperature inside the vessel, add 1.42g of glycerin, and keep warm for 30 minutes.
[0056] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 230℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 240℃, and the vacuum at 200Pa; the reaction continues until the torque reaches 25N. The reaction is stopped; nitrogen gas is applied to pressurize and pelletize the material.
[0057] Due to the hysteresis of caprolactam ring opening, a large number of long polyamide blocks are generated. After testing, the properties of the prepared polyesteramide are as follows: melting point 174℃; Tg 56℃; tensile strength 53.3MPa; PDI 2.61; the molecular chain length distribution is wide, the melt flow is unstable during melt processing, the mechanical properties of the product have large dispersion, and the batch consistency is poor.
[0058] Comparative Example 3 1 mol caprolactam, 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 0.18 g p-toluenesulfonic acid, and 0.02 g tetrabutyl titanate were added to a 5 L high-pressure reactor in one step; nitrogen was purged three times; the temperature was raised to 215 °C and held for 4 h to carry out the esterification reaction; the acid value of the system was tested and found to be 21 mg KOH / g, indicating that the esterification reaction endpoint had been reached.
[0059] Maintain the temperature inside the vessel, add 1.42g of glycerin, and keep warm for 30 minutes.
[0060] Staged vacuum polycondensation: The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The pre-polymerization temperature is set at 230℃, the vacuum at 3000Pa, and the pre-polymerization time is 2 hours; the final polymerization temperature is set at 240℃, the vacuum at 200Pa, and the torque is 4N. After m, the reaction stops and growth ceases, failing to yield a polyesteramide with sufficient strength. This is because there is too little tetrabutyl titanate catalyst, resulting in insufficient catalytic activity during the polyester polycondensation stage.
[0061] Comparative Example 4 70g caprolactam, 30g sebacic acid, 45.6g 1,4-butanediol, 1.42g glycerol, 0.08g p-toluenesulfonic acid, and 0.08g tetrabutyl titanate were added to a 5L high-pressure reactor in one go; nitrogen was purged three times; the temperature was raised to 215℃, and a large number of gel particles appeared in the reactor after 120 minutes of reaction, so the experiment was terminated and no processable product could be obtained.
[0062] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing micro-crosslinked polyesteramide by one-pot simultaneous polymerization, characterized in that, Includes the following steps: S1. Under the protection of an inert gas, the lactam monomer, aliphatic diacid, aliphatic diol, and composite catalyst are added to the reactor and heated to carry out the reaction. Under the action of the composite catalyst, the lactam ring-opening polymerization and the aliphatic diacid-aliphatic diol esterification reaction occur simultaneously, so that the amide structural unit and the ester structural unit are generated simultaneously until the acid value of the system drops below the preset value. S2. Add a crosslinking agent to the system and maintain the temperature for the reaction; S3. Continue heating to carry out a staged vacuum polycondensation reaction. The reaction endpoint is controlled by the melt stirring torque. Micro-crosslinked polyesteramide is then discharged. The crosslinking agent is selected from polyhydroxy compounds or polycarboxylic acid compounds; The composite catalyst is obtained by combining a protic acid catalyst and a metal catalyst. The polyhydroxy compound is selected from one or more of glycerol, trimethylolpropane, and pentaerythritol; The polycarboxylic acid compound is selected from pyromellitic acid and / or citric acid.
2. The preparation method according to claim 1, characterized in that, The lactam monomer is selected from autolactam and / or dodelactam; The aliphatic dicarboxylic acid is selected from one or more of succinic acid, adipic acid, octanoic acid, sebacic acid, and dodecanoic acid; The aliphatic diol is selected from one or more of ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,8-octanediol, and 1,10-decanediol; The protic acid catalyst is selected from one or more of p-toluenesulfonic acid, methanesulfonic acid, and benzenesulfonic acid; The metal catalyst is selected from one or more of tetrabutyl titanate, tetraethyl titanate, antimony trioxide, and zinc acetate.
3. The preparation method according to claim 1, characterized in that, The molar ratio of the lactam monomer to the aliphatic dicarboxylic acid is (6:4) to (8.5:1.5). The molar ratio of the aliphatic diol to the aliphatic diacid is (1.3~2.2):1; The amount of the crosslinking agent added is 0.2~6 wt% of the sum of the mass of the lactam monomer and the aliphatic dicarboxylic acid monomer; The composite catalyst is a mixture of a protic acid catalyst and a metal catalyst in a mass ratio of (0.5~3):1; Preferably, the amount of the composite catalyst added is 0.05 to 0.8 wt% of the sum of the masses of the lactam monomer and the aliphatic dicarboxylic acid monomer.
4. The preparation method according to claim 1, characterized in that, The reaction temperature in step S1 is 190~230℃, the reaction time is 2~6 h, and the reaction endpoint is when the acid value of the system drops below 25 mgKOH / g.
5. The preparation method according to claim 1, characterized in that, The heat preservation reaction time in step S2 is 10~60 min.
6. The preparation method according to claim 1, characterized in that, The staged vacuum polycondensation reaction includes two stages: pre-polycondensation and final polycondensation. The polycondensation temperature of the pre-polycondensation stage is 230~235℃, the vacuum degree is 1000~5000 Pa, and the duration of the pre-polycondensation stage is 0.5~4 h. The polycondensation temperature of the final polycondensation stage is 235~245℃, and the vacuum degree is 50~500 Pa.
7. The preparation method according to claim 1, characterized in that, In step S3, the controlled torque reaches 20~25N. m is the endpoint of the staged vacuum polycondensation reaction.
8. A microcrosslinked polyesteramide, characterized in that, It is prepared by the preparation method according to any one of claims 1-7.
9. The microcrosslinked polyesteramide according to claim 8, characterized in that, In the micro-crosslinked polyester amide, the structural units derived from lactam monomers account for 60-85% of the total molar proportion of the micro-crosslinked polyester amide structural units; The micro-crosslinked polyesteramide has a melting point higher than 155℃, a glass transition temperature greater than 48℃, an initial decomposition temperature ≥390℃, a tensile strength ≥55 MPa, and a molecular weight distribution index ≤2.
2.
10. The application of the microcrosslinked polyesteramide as described in claim 8 or 9 in the preparation of engineering plastics, industrial fibers, hot melt adhesives, and general packaging materials.