A composite flame retardant for TPU, a TPU composite material and its preparation method

By using a composite flame retardant made of boron-nitrogen-doped carbon nanotubes with phosphorus modified on the surface and loaded with lanthanum, the problems of easy aggregation and insufficient interfacial compatibility of TPU flame retardants in the matrix are solved, and the synergistic improvement of flame retardancy, smoke suppression and mechanical properties is achieved.

CN123062791APending Publication Date: 2026-11-10TAIZHOU UNIV (ZHEJIANG)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611153198.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing TPU flame retardant systems, flame retardants are prone to agglomeration and have insufficient interfacial compatibility, making it difficult to achieve both smoke suppression and mechanical properties, and the preparation process is complex.

Method used

Using boron-nitrogen-doped carbon nanotubes as the substrate, phosphorus is modified on the surface and lanthanum is loaded to form a multi-element synergistic composite flame retardant. It is prepared through pyrolysis, acidification, modification and loading processes to improve dispersibility and interfacial compatibility.

Benefits of technology

It achieves a synergistic improvement in flame retardancy, smoke suppression, and mechanical properties, forming a continuous physical barrier network that reduces heat release rate and smoke release while maintaining good mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062791A_ABST
    Figure CN123062791A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of flame retardant materials, and relates to a composite flame retardant for TPU, a TPU composite material, and a method for preparing the same. The composite flame retardant for TPU includes boron-nitrogen-doped carbon nanotubes (BNiTVs), the surface of which is modified with phosphorus, and lanthanum is also loaded onto the BNiTVs. This invention uses BNiTVs as a substrate, modifying their surface with phosphorus and loading lanthanum to form a multi-element synergistic composite flame retardant system. The doping of boron and nitrogen atoms enhances the polarity of the carbon nanotube surface, providing abundant active sites for the subsequent loading of phosphorus and lanthanum. The phosphorus and lanthanum modified and loaded onto the carbon nanotube surface reduce the tendency for entanglement and aggregation between carbon nanotubes, enabling the composite flame retardant to achieve relatively uniform dispersion in the TPU matrix. This facilitates the construction of a continuous physical barrier network within the matrix, overcoming the defect of traditional carbon nanotubes that are prone to aggregation and failure due to poor dispersibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of flame retardant materials technology, specifically to a composite flame retardant for TPU, a TPU composite material, and a method for preparing the same. Background Technology

[0002] With the rapid development of the polymer materials industry, thermoplastic polyurethane elastomer (TPU) has been widely used in many fields such as wire and cable sheathing, automotive parts, electronic device protective materials, films, and footwear materials due to its excellent wear resistance, flexibility, oil resistance, and ease of processing and molding. However, TPU molecular chains contain a large number of flammable organic segments, making it highly flammable when exposed to fire. During combustion, it exhibits high heat release rates, large amounts of smoke, and severe molten dripping, posing significant fire safety hazards. These combustion characteristics not only accelerate flame spread but may also release large amounts of toxic fumes during a fire, causing greater loss of life and property. Therefore, effectively improving the flame retardant and smoke-suppressing properties of TPU has become a key issue that must be addressed to expand its application in electrical, transportation, construction, and electronic packaging sectors where fire safety requirements are high.

[0003] Researchers have developed various flame-retardant systems for the flame-retardant modification of TPU. Early studies focused on traditional flame retardants such as those containing phosphorus and nitrogen. For example, Chen et al. modified waste aramid fibers with phosphoric acid and used them in TPU. At an addition of only 1.00 wt%, the peak heat release rate (PHRR) of the composite material decreased by 48.1%, indicating that the phosphorus-containing component can promote char formation and play a role in condensed phase flame retardancy. However, the dispersion state and interfacial bonding strength of fiber-based flame retardants in the matrix still have a significant impact on the overall performance of the material. Kanbur et al. modified carbon nanotubes (CNTs) with acid and introduced them into TPU. They found that acidified CNTs had better dispersion uniformity than unmodified CNTs, and the thermal stability and combustion performance of the material were improved. However, when relying solely on carbon nanotubes, the flame-retardant effect is highly dependent on the dispersion state, and unmodified carbon nanotubes are prone to agglomeration and failure.

[0004] To achieve more efficient flame retardant and smoke suppression effects, two-dimensional nanomaterials are gradually being introduced into TPU flame retardant systems. For example, Yu et al. achieved flame retardant and smoke suppression of TPU through interface-modified ultrathin MXene nanosheets. Luo et al. further prepared phosphated chitosan-functionalized MXene (PCS-MXene), which reduced the PHRR, total heat release, and total smoke release of TPU by 66.7%, 21.0%, and 27.7%, respectively, at an addition of 3 wt%. These two-dimensional nanoflame retardants have high flame retardant efficiency, but sheet materials such as MXene often require complex exfoliation and surface functionalization processes to improve dispersibility, making the preparation process relatively cumbersome. Furthermore, the flame retardant effect is still limited by the stacking of the sheets and interfacial compatibility.

[0005] In recent years, research on introducing metal-organic frameworks (MOFs), layered inorganic nanomaterials, and rare earth elements into TPU flame-retardant systems has attracted much attention, aiming to further improve flame-retardant performance through catalytic char formation and synergistic smoke suppression. For example, Wan et al. constructed ZIF-67@MXene and added it to TPU. With an addition of only 0.5 wt%, the peak smoke release rate and total smoke release were reduced by 50% and 22%, respectively, showing a good smoke suppression effect, but its inhibition of heat release was still relatively limited. Han et al. synergistically used α-ZrP nanosheets with nitrogen-containing flame retardants in TPU, confirming that the organic-inorganic synergistic structure helps to balance flame retardancy and mechanical properties. Yu et al. reported the La-MOF@MXene system, which reduced the PHRR of TPU composites by 49.4% with an addition of 3 wt%, while the tensile strength and elongation at break reached 42.4 MPa and 686%, respectively, indicating that rare earth elements and two-dimensional nanosheets can produce good synergistic flame retardant and reinforcing effects. However, overall, although existing TPU flame retardant systems have gradually evolved from single phosphorus-based, nitrogen-based, or nanofiller-based systems to multi-element, multi-structure synergistic systems, they still generally suffer from problems such as easy agglomeration of flame retardants in the matrix, insufficient interfacial compatibility, difficulty in balancing smoke suppression and mechanical properties, and relatively complex preparation processes.

[0006] Therefore, there is a need for a novel composite flame retardant system that has excellent dispersibility and combines efficient flame retardancy, smoke suppression, and interface enhancement functions. Summary of the Invention

[0007] (a) Technical problems to be solved To address the problem in existing TPU flame retardant systems that suffer from difficulty in achieving both smoke suppression and mechanical properties due to the easy aggregation of flame retardants in the matrix and insufficient interfacial compatibility, this invention provides a composite flame retardant for TPU, a TPU composite material, and a method for preparing the same.

[0008] (II) Technical Solution To achieve the above objectives, the main technical solutions adopted by the present invention include: A composite flame retardant for TPU includes boron-nitrogen-doped carbon nanotubes, the surface of which is modified with phosphorus and lanthanum is loaded onto the surface of the boron-nitrogen-doped carbon nanotubes.

[0009] The present invention also provides a method for preparing the above-mentioned composite flame retardant for TPU, comprising the following steps: S1: Dissolve urea, boric acid and polyethylene glycol in water, dry them and then pyrolyze them under an inert atmosphere to obtain boron-nitrogen-doped carbon nanotubes. S2: Acidification treatment of boron-nitrogen-doped carbon nanotubes to obtain acidified boron-nitrogen-doped carbon nanotubes; S3: React acidified boron nitrogen-doped carbon nanotubes with a phosphorus source to obtain phosphorus-modified boron nitrogen-doped carbon nanotubes; S4: React phosphorus-modified boron-nitrogen-doped carbon nanotubes with lanthanum ions to obtain a composite flame retardant for TPU.

[0010] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S1, the mass ratio of urea to boric acid is 35:1-40:1, and the mass ratio of polyethylene glycol to urea is 1:10-1:12.

[0011] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S1, the pyrolysis treatment temperature is 850-950℃ and the time is 3-5h, and the inert atmosphere is a nitrogen atmosphere.

[0012] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S2, boron-nitrogen-doped carbon nanotubes are added to a nitric acid solution and acidified for 1.5-2.5 hours, with the concentration of the nitric acid solution being 20-30 wt%.

[0013] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S3, boron nitrogen-doped carbon nanotubes are dispersed in anhydrous ethanol, ultrasonically treated, and then a phosphorus source is added. After stirring, the mixture is heated to 55-65℃ and reacted for 3.5-4.5 hours to obtain phosphorus-modified boron nitrogen-doped carbon nanotubes. The phosphorus source is phosphorus oxychloride, and the mass ratio of the phosphorus source to the boron nitrogen-doped carbon nanotubes is 1:8-1:12.

[0014] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S4, phosphorus-modified boron-nitrogen-doped carbon nanotubes are dispersed in water, ultrasonically treated, and then lanthanum nitrate or lanthanum nitrate hexahydrate is added. After stirring, the mixture is heated to 75-85℃ and reacted for 3.5-4.5 hours. After drying, the composite flame retardant for TPU is obtained.

[0015] In the preparation method of the composite flame retardant for TPU as described above, preferably, in step S4, the mass ratio of phosphorus-modified boron-nitrogen-doped carbon nanotubes to lanthanum nitrate or lanthanum nitrate hexahydrate is 1:0.01-1:0.05.

[0016] The present invention also provides a TPU composite material, comprising a TPU matrix and the above-mentioned composite flame retardant for TPU or the composite flame retardant for TPU prepared by the above-mentioned preparation method; the mass of the composite flame retardant for TPU accounts for 0.1-15% of the mass of the TPU composite material.

[0017] The present invention also provides a method for preparing the above-mentioned TPU composite material, specifically by melt-blending TPU with the TPU using a composite flame retardant to prepare the TPU composite material.

[0018] (III) Beneficial Effects The composite flame retardant for TPU of this invention uses boron-nitrogen-doped carbon nanotubes as a substrate, with phosphorus and lanthanum loaded onto their surfaces to form a multi-element synergistic composite flame retardant system. The doping of boron and nitrogen atoms enhances the polarity of the carbon nanotube surface, providing abundant active sites for subsequent loading of phosphorus and lanthanum. The phosphorus and lanthanum elements modified and loaded onto the carbon nanotube surface reduce the tendency for entanglement and aggregation between carbon nanotubes, enabling the composite flame retardant to achieve relatively uniform dispersion in the TPU matrix. This facilitates the construction of a continuous physical barrier network within the matrix, overcoming the shortcomings of traditional carbon nanotubes that are prone to aggregation and failure due to poor dispersibility.

[0019] After introducing this composite flame retardant into the TPU matrix, during combustion, boron and nitrogen help improve the thermal stability of the char layer, phosphorus promotes TPU dehydration and char formation, and lanthanum catalyzes char formation and suppresses smoke. The synergistic effect of these components promotes the formation of a continuous and dense protective char layer, effectively blocking the transfer of heat, oxygen, and combustible volatiles, thus significantly reducing the heat release rate and smoke emission during TPU combustion. Simultaneously, the improved dispersibility of the composite flame retardant in the TPU matrix alleviates stress concentration caused by particle agglomeration, helping the TPU composite material maintain good mechanical properties while achieving flame retardant and smoke-suppressing performance, thus achieving a synergistic improvement in flame retardancy, smoke suppression, and mechanical properties. Attached Figure Description

[0020] Figure 1 The flowchart shows the preparation process of La@P-BCN-GNTs in Example 1; Figure 2 a represents the FTIR spectra of BCN, P-BCN, and LPBN0.03 in Example 1; Figure 2 b shows the XRD patterns of BCN, P-BCN, and LPBN0.03; Figure 3 XPS spectra of BCN, P-BCN, and LPBN0.03; Figure 4 SEM, TEM, STEM-HAADF images and EDS elemental distribution maps of BCN and LPBN 0.03; Figure 5 XRD patterns of TPU and its composites; Figure 6 TEM images of TPU / BCN10 and TPU / LPBN10 composite materials; Figure 7 Stress-strain curves of TPU composites with different LPBN ratios at a 1wt% addition amount; Figure 8 HRR and SPR curves for TPU composites with different LPBN ratios at 1 wt% addition. Figure 9 The TG curves (a) and DTG curves (b) of TPU and TPU / LPBN0.03 composite material in air atmosphere are shown. Figure 10 HRR and SPR curves for TPU and TPU / LPBN0.03 composite materials; Figure 11 Stress-strain curves of TPU and TPU / LPBN0.03 composite materials; Figure 12 Digital photographs of the carbon residue after combustion of TPU and TPU / LPBN0.03 composite materials; Figure 13 SEM images of carbon residue from TPU and TPU / LPBN0.03 composite materials; Figure 14 FTIR spectra (a) and Raman spectra (b) of the carbon residues of TPU and TPU / LPBN0.03 composite materials. Detailed Implementation

[0021] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0022] This invention provides a composite flame retardant for TPU, comprising boron-nitrogen-doped carbon nanotubes, wherein the surface of the boron-nitrogen-doped carbon nanotubes is modified with phosphorus. Furthermore, the boron-nitrogen-doped carbon nanotubes are also loaded with lanthanum. That is, the composite flame retardant for TPU of this invention is lanthanum-loaded phosphorus-modified boron-nitrogen-doped carbon nanotubes, La@P-BCN-GNTs, abbreviated as LPBN.

[0023] This invention addresses the problems of high heat release rate and large smoke emission during the combustion of TPU by providing a multi-element synergistic composite flame retardant system. This composite flame retardant uses boron-nitrogen-doped carbon nanotubes as the framework substrate. The one-dimensional tubular structure of the carbon nanotubes forms a continuous physical barrier network within the TPU matrix, delaying the transfer of heat, oxygen, and combustible volatiles. Furthermore, boron and nitrogen atoms are doped into the carbon nanotube framework, forming BN and BCN bonds, providing abundant active sites for subsequent loading of phosphorus and lanthanum elements. Simultaneously, boron and nitrogen themselves contribute to improving the thermal stability of the char layer during combustion. This invention further modifies the surface of the boron-nitrogen-doped carbon nanotubes with phosphorus. Phosphorus-containing functional groups such as PO, P=O, and POC can promote dehydration and char formation of the TPU matrix during combustion, exerting a condensed-phase flame retardant effect. Simultaneously, this invention also loads lanthanum onto the boron-nitrogen-doped carbon nanotubes. Lanthanum can catalyze char formation and suppress smoke during combustion, promoting the formation of a denser and more stable protective char layer. This composite flame retardant organically combines the physical barrier effect of one-dimensional carbon nanotubes with the synergistic flame retardant effect of multiple elements (B, N, P, and La), achieving a synergistic improvement in flame retardancy, smoke suppression, and mechanical properties in TPU.

[0024] The present invention also provides a method for preparing the above-mentioned composite flame retardant for TPU, comprising the following steps: S1: Urea, boric acid and polyethylene glycol are dissolved in water, dried and then pyrolyzed under an inert atmosphere to obtain boron-nitrogen-doped carbon nanotubes.

[0025] S2: Acidification treatment is performed on boron-nitrogen-doped carbon nanotubes to obtain acidified boron-nitrogen-doped carbon nanotubes.

[0026] S3: React acidified boron-nitrogen-doped carbon nanotubes with a phosphorus source to obtain phosphorus-modified boron-nitrogen-doped carbon nanotubes.

[0027] S4: React phosphorus-modified boron-nitrogen-doped carbon nanotubes with lanthanum ions to obtain a composite flame retardant for TPU.

[0028] Preferably, in step S1, the mass ratio of urea to boric acid is 35:1-40:1, and the mass ratio of polyethylene glycol to urea is 1:10-1:12. Under these ratios, urea serves as both a nitrogen and carbon source, boric acid as a boron source, and polyethylene glycol as a carbon source and structure directing agent. Optimizing the proportions of each raw material is beneficial for forming carbon nanotubes with complete tubular morphology and uniform boron and nitrogen doping during pyrolysis. If the ratio of urea to boric acid deviates from this range, for example, if boric acid is excessive, it may lead to excessive boron doping in the carbon nanotube wall, damaging the graphitized structure of the carbon nanotubes. If boric acid is insufficient, the boron doping is inadequate, failing to fully utilize the stabilizing effect of boron on the carbon layer in the subsequent flame-retardant process. The amount of polyethylene glycol added also affects the morphology and yield of the carbon nanotubes. The preferred molecular weight is polyethylene glycol 2000. A molecular weight that is too low results in shorter chain segments, which is not conducive to the directed growth of the tubular structure; a molecular weight that is too high increases the viscosity of the system, which is not conducive to the uniform mixing of the raw materials. The preferred drying temperature for the mixed aqueous solution of urea, boric acid, and polyethylene glycol is 90-110℃, and the drying time is 8-12 hours, in order to fully remove moisture and avoid water vapor from adversely affecting the product structure during pyrolysis.

[0029] Preferably, in step S1, the pyrolysis temperature is 850-950℃, the time is 3-5 hours, and the inert atmosphere is preferably nitrogen. Pyrolysis temperature and time are key parameters affecting the growth quality of carbon nanotubes. If the temperature is too low or the time is too short, urea and boric acid will not decompose sufficiently, resulting in incomplete carbon nanotube growth, numerous tube wall defects, and insufficient B and N doping. If the temperature is too high or the time is too long, it may lead to excessive graphitization of the carbon nanotube walls, reducing active sites, which is detrimental to subsequent phosphorus modification and lanthanum loading, while also increasing energy consumption. Within the range of 850-950℃, combined with nitrogen atmosphere protection, this invention can obtain boron-nitrogen-doped carbon nanotubes with complete tubular structures, moderate B and N doping amounts, and abundant surface active sites.

[0030] Preferably, in step S2, boron-nitrogen-doped carbon nanotubes are added to a nitric acid solution and acidified for 1.5-2.5 hours. The concentration of the nitric acid solution is preferably 20-30 wt%. The purpose of the acidification treatment is to increase the surface active sites and polarity, providing reaction anchors for subsequent phosphorus modification. If the nitric acid concentration is too low or the acidification time is too short, the surface oxidation degree will be insufficient, resulting in low efficiency of subsequent phosphorus modification. If the nitric acid concentration is too high or the acidification time is too long, the carbon nanotubes may be over-etched, damaging their tubular structure and reducing the skeletal stability of the flame retardant. Using a 20-30 wt% nitric acid solution at room temperature for 1.5-2.5 hours can effectively increase the content of surface active sites while maintaining the structural integrity of the carbon nanotubes.

[0031] Preferably, in step S3, boron-nitrogen-doped carbon nanotubes are dispersed in anhydrous ethanol, ultrasonically treated for 10-24 min, and then a phosphorus source is added. After stirring at room temperature for 1 h, the temperature is raised to 55-65℃ and reacted for 3.5-4.5 h to obtain phosphorus-modified boron-nitrogen-doped carbon nanotubes. The phosphorus source is preferably phosphorus oxychloride. The mass ratio of phosphorus source to boron-nitrogen-doped carbon nanotubes is preferably 1:8-1:12. Using POCl3 as the phosphorus source allows it to react with the oxygen-containing functional groups on the surface of the acidified carbon nanotubes, forming phosphorus-containing bonding structures such as PO, POC, and P=O, thus firmly modifying the carbon nanotube surface with phosphorus. Anhydrous ethanol, as the reaction medium, effectively disperses the carbon nanotubes without reacting violently with POCl3. Ultrasonic treatment helps break up the agglomerates of carbon nanotubes, ensuring uniform dispersion and improving the uniformity of phosphorus modification. After the reaction, the nanotubes are preferably vacuum-dried at 80℃ for 12 h to remove residual solvent and byproducts.

[0032] Preferably, in step S4, phosphorus-modified boron-nitrogen-doped carbon nanotubes are dispersed in water, ultrasonically treated for 20-25 min, and then lanthanum nitrate or lanthanum nitrate hexahydrate is added. The mixture is stirred at room temperature for 1 h, then heated to 75-85℃ and reacted for 3.5-4.5 h. After drying, a composite flame retardant for TPU is obtained. Lanthanum nitrate or lanthanum nitrate hexahydrate serves as the lanthanum source, providing La... 3+ Ions. The abundant phosphorus- and oxygen-containing functional groups on the surface of phosphorus-modified boron-nitrogen-doped carbon nanotubes can serve as La... 3+ The coordination or adsorption sites of lanthanum allow for effective loading of lanthanum onto the surface of carbon nanotubes. Ultrasonic treatment aids in the dispersion of carbon nanotubes in water, improving the uniformity of lanthanum loading. After the reaction, vacuum drying at 80°C for 12 hours is preferred to obtain the final product. If the reaction temperature is too low or the time is too short, the lanthanum loading will be insufficient, resulting in limited catalytic carbonization and smoke suppression effects. If the temperature is too high or the time is too long, some of the loaded lanthanum may detach, reducing the loading efficiency.

[0033] Preferably, in step S4, the mass ratio of phosphorus-modified boron-nitrogen-doped carbon nanotubes to lanthanum nitrate or lanthanum nitrate hexahydrate is 1:0.01-1:0.05. The lanthanum loading has a significant impact on the overall performance of the composite flame retardant. When the mass ratio is below 0.01, the lanthanum loading is too low, resulting in insufficient catalytic char formation and smoke suppression, and limited improvement in flame retardant effect. When the mass ratio is above 0.05, the lanthanum loading is too high, which may lead to local agglomeration of the composite flame retardant in the TPU matrix. On the one hand, this reduces dispersibility and affects the formation of the physical barrier network; on the other hand, the agglomerates may become stress concentration points, adversely affecting the mechanical properties of the composite material. Controlling the mass ratio within the range of 1:0.01-1:0.05, and more preferably 1:0.03, can achieve the best balance between flame retardant effect, smoke suppression effect, and mechanical properties.

[0034] The above-mentioned preparation method of the present invention uses readily available raw materials, has mild and controllable process conditions, does not require complex peeling or surface functionalization treatment, and is easy to scale up for production.

[0035] This invention also provides a TPU composite material, comprising a TPU matrix and the aforementioned composite flame retardant for TPU. Preferably, the mass of the composite flame retardant for TPU accounts for 0.1-15% of the mass of the TPU composite material, more preferably 0.1-10%. When the amount of flame retardant added is less than 0.1%, the distribution density in the TPU matrix is ​​too low, making it difficult to form an effective continuous physical barrier network and sufficient condensed phase flame retardant effect, resulting in insignificant flame retardant and smoke suppression effects. When the amount added is greater than 15%, the flame retardant is overfilled in the matrix, easily causing local agglomeration and stress concentration, leading to a significant decrease in the tensile strength and elongation at break of the composite material, while the processing fluidity of melt blending deteriorates. Within the addition range of 0.1-15%, as the addition amount increases, the flame retardant and smoke suppression properties of the composite material gradually improve, allowing for flexible adjustment between flame retardant performance and mechanical properties according to actual application requirements.

[0036] This invention also provides a method for preparing the above-mentioned TPU composite material. Specifically, TPU is melt-blended with a composite flame retardant to obtain the TPU composite material. Preferably, the melt-blending temperature is 170-180℃, the melting time is 8-12 min, and the rotor speed is 50-70 rpm. This temperature range is higher than the softening temperature of TPU, ensuring that the TPU is fully melted and the flame retardant is uniformly dispersed in the matrix, while preventing thermal degradation of TPU due to excessive temperature. If the melt-blending time is too short, the flame retardant will not be evenly dispersed. If the time is too long, it may cause oxidative degradation of TPU at high temperature, affecting the material properties. More preferably, after melt-blending, the composite material can be placed in a mold, preheated at 170-180℃ for 5-10 min, and hot-pressed at 10-15 MPa for 5-10 min to prepare a sample for subsequent testing.

[0037] Through the aforementioned melt blending process, the composite flame retardant can achieve relatively uniform dispersion in the TPU matrix. Compared to unmodified carbon nanotubes, the phosphorus and lanthanum elements modified on the surface of the composite flame retardant of this invention increase its surface polarity and interfacial interaction with the TPU molecular chains, effectively weakening the van der Waals forces and self-aggregation tendency between carbon nanotubes, resulting in a significant reduction in agglomerate size. This favorable dispersion not only facilitates the construction of a continuous physical barrier network in the TPU matrix, fully leveraging the barrier effect of one-dimensional carbon nanotubes, but also alleviates the stress concentration phenomenon caused by the agglomeration of traditional carbon nanotubes, enabling the composite material to maintain good mechanical properties while achieving flame retardant and smoke-suppressing performance.

[0038] During combustion, the synergistic flame-retardant mechanism of the composite flame retardant of this invention, involving multiple elements (B, N, P, and La), is manifested in the following ways: the tubular structure of boron-nitrogen-doped carbon nanotubes forms a physical barrier layer in the matrix, delaying the transfer of heat, oxygen, and combustible volatiles. Boron and nitrogen exist in the carbon nanotube framework in the form of BN and BCN, which helps to improve the thermal stability and structural integrity of the carbon layer. Phosphorus is modified on the surface of the carbon nanotubes in the form of phosphorus-containing functional groups, promoting the dehydration and char formation of TPU at high temperatures and accelerating the condensed phase carbonization reaction. Lanthanum plays a catalytic role in char formation, further promoting the formation of a continuous and dense composite carbon layer. Post-combustion char analysis shows that B, N, P, and La elements are all retained in the condensed phase and participate in the carbon layer construction. The carbon layer exhibits a significant expansion morphology, with more complete and continuous coverage, and a significant reduction in cracks and pores. At the same time, the graphitization degree and orderliness of the carbon layer are greatly improved. This continuous, expanded, dense, and highly graphitized protective carbon layer effectively blocks the transfer of heat, oxygen, and combustible volatiles, thus exhibiting a significantly reduced heat release rate and smoke release rate in cone calorimetry.

[0039] To further clarify the present invention and its technological advancements, the following description is provided in conjunction with specific embodiments and technical effects.

[0040] Example 1: like Figure 1 As shown, this embodiment provides a method for preparing a composite flame retardant for TPU, including the following steps: S1: Urea, boric acid, and polyethylene glycol 2000 were mixed in deionized water at a mass ratio of 110:3:10, with a mass-to-volume ratio of 1 g of polyethylene glycol 2000 to 50 mL of deionized water. The mixture was stirred at room temperature for 30 min. Then, it was dried at 100 °C for 10 h. The dried product was placed at the bottom of a quartz tube and pyrolyzed in a tube furnace at 900 °C for 4 h under a nitrogen atmosphere to obtain boron-nitrogen-doped carbon nanotubes, i.e., BCN-GNTs.

[0041] S2: Add BCN-GNTs to a 25wt% nitric acid solution, stir at room temperature for 2 hours, filter, wash, and dry to obtain acidified BCN-GNTs.

[0042] S3: Dissolve acidified BCN-GNTs in anhydrous ethanol at a mass-to-volume ratio of 1 g: 20 mL, sonicate for 10 min, then add POCl3 at a mass ratio of 1:10 to acidified BCN-GNTs, stir at room temperature for 1 h, heat to 60 °C and react for 4 h, then vacuum dry at 80 °C for 12 h to obtain phosphorus-modified boron-nitrogen-doped carbon nanotubes, namely P-BCN-GNTs, or P-BCN for short.

[0043] S4: P-BCN was dissolved in deionized water at a mass-to-volume ratio of 1 g:50 mL. The mixture was sonicated for 24 min, and then La(NO3)3•6H2O was added at a mass ratio of 1:0.03. The mixture was stirred at room temperature for 1 h, heated to 80 °C and reacted for 4 h. The mixture was then vacuum dried at 80 °C for 12 h to obtain a black powder product, namely the lanthanum-supported phosphorus-modified boron nitrogen-doped carbon nanotube La@P-BCN-GNTs (LPBN) composite flame retardant system.

[0044] Example 2: This embodiment provides a method for preparing a composite flame retardant for TPU. The difference from Embodiment 1 is that in step S4, the mass ratio of P-BCN to La(NO3)3•6H2O is 1:0.01.

[0045] Example 3: This embodiment provides a method for preparing a composite flame retardant for TPU. The difference from Embodiment 1 is that in step S4, the mass ratio of P-BCN to La(NO3)3•6H2O is 1:0.05.

[0046] Example 4: This embodiment provides a method for preparing a composite flame retardant for TPU, comprising the following steps: S1: Urea, boric acid, and polyethylene glycol 2000 were mixed in deionized water at a mass ratio of 35:1 (urea to boric acid), 1:10 (polyethylene glycol to urea), and 1 g:50 mL (polyethylene glycol 2000 to deionized water). The mixture was stirred at room temperature for 30 min. Then, it was dried at 90 °C for 8 h. The dried product was placed at the bottom of a quartz tube and pyrolyzed in a tube furnace at 850 °C for 3 h under a nitrogen atmosphere to obtain boron-nitrogen-doped carbon nanotubes, i.e., BCN-GNTs.

[0047] S2: Add BCN-GNTs to a 20wt% nitric acid solution, stir at room temperature for 1.5h, filter, wash, and dry to obtain acidified BCN-GNTs.

[0048] S3: Dissolve acidified BCN-GNTs in anhydrous ethanol at a mass-to-volume ratio of 1 g: 20 mL, sonicate for 10 min, then add POCl3 at a mass ratio of 1:8 to acidified BCN-GNTs, stir at room temperature for 1 h, heat to 55 °C and react for 3.5 h, then vacuum dry at 80 °C for 12 h to obtain phosphorus-modified boron-nitrogen-doped carbon nanotubes, namely P-BCN-GNTs, or P-BCN for short.

[0049] S4: P-BCN was dissolved in deionized water at a mass-to-volume ratio of 1 g:50 mL. The mixture was sonicated for 20 min, and then La(NO3)3•6H2O was added at a mass ratio of 1:0.03. The mixture was stirred at room temperature for 1 h, heated to 75 °C and reacted for 3.5 h. The mixture was then vacuum dried at 80 °C for 12 h to obtain a black powder product, namely the lanthanum-supported phosphorus-modified boron nitrogen-doped carbon nanotube La@P-BCN-GNTs (LPBN) composite flame retardant system.

[0050] Example 5: This embodiment provides a method for preparing a composite flame retardant for TPU, comprising the following steps: S1: Urea, boric acid, and polyethylene glycol 2000 were mixed in deionized water at a mass ratio of 40:1 (urea to boric acid), 1:12 (polyethylene glycol to urea), and 1 g:50 mL (polyethylene glycol 2000 to deionized water). The mixture was stirred at room temperature for 30 min. Then, it was dried at 110 °C for 12 h. The dried product was placed at the bottom of a quartz tube and pyrolyzed in a tube furnace at 950 °C for 5 h under a nitrogen atmosphere to obtain boron-nitrogen-doped carbon nanotubes, i.e., BCN-GNTs.

[0051] S2: Add BCN-GNTs to a 30wt% nitric acid solution, stir at room temperature for 2.5h, filter, wash, and dry to obtain acidified BCN-GNTs.

[0052] S3: Dissolve acidified BCN-GNTs in anhydrous ethanol at a mass-to-volume ratio of 1 g: 20 mL, sonicate for 24 min, then add POCl3 at a mass ratio of 1:12 to acidified BCN-GNTs, stir at room temperature for 1 h, heat to 65 °C and react for 4.5 h, then vacuum dry at 80 °C for 12 h to obtain phosphorus-modified boron-nitrogen-doped carbon nanotubes, namely P-BCN-GNTs, or P-BCN for short.

[0053] S4: P-BCN was dissolved in deionized water at a mass-to-volume ratio of 1 g:50 mL. The mixture was sonicated for 25 min, and then La(NO3)3•6H2O was added at a mass ratio of 1:0.03. The mixture was stirred at room temperature for 1 h, heated to 85 °C and reacted for 4.5 h. The mixture was then vacuum dried at 80 °C for 12 h to obtain a black powder product, namely the lanthanum-supported phosphorus-modified boron nitrogen-doped carbon nanotube La@P-BCN-GNTs (LPBN) composite flame retardant system.

[0054] Example 6: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN added accounted for 0.1 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)0.1.

[0055] Example 7: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN added accounted for 0.5 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)0.5.

[0056] Example 8: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN added accounted for 1 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)1.

[0057] Example 9: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN added accounted for 5 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)5.

[0058] Example 10: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 180°C for 8 min, with a rotor speed of 50 rpm. The amount of LPBN added accounted for 10 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 180°C for 5 min, and hot-pressed at 10 MPa for 10 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)10.

[0059] Example 11: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system prepared in Example 1 was melt-blended with TPU granules at 170°C for 12 min, with a rotor speed of 70 rpm. The amount of LPBN added accounted for 15 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 170°C for 10 min, and hot-pressed at 15 MPa for 5 min. After cooling, a TPU / LPBN composite material sample was obtained, denoted as TPU / (LPBN0.03)15.

[0060] Example 12: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system (i.e., LPBN0.01) prepared in Example 2 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN0.01 added accounted for 1 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / (LPBN0.01)1 composite material sample was obtained.

[0061] Example 13: This embodiment provides a method for preparing TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the LPBN composite flame-retardant system (i.e., LPBN0.05) prepared in Example 3 was melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of LPBN0.05 added accounted for 1 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / (LPBN0.05)1 composite material sample was obtained.

[0062] Comparative Example 1: This comparative example provides a method for preparing pure TPU samples. Specifically, using a Thermo HAAKE rheometer, TPU granules are melt-blended at 175°C for 10 minutes with a rotor speed of 60 rpm. After blending, the TPU is placed in a mold, preheated at 175°C for 6 minutes, and hot-pressed at 12 MPa for 8 minutes. After cooling, a pure TPU sample is obtained, denoted as TPU.

[0063] Comparative Example 2: This comparative example provides a method for preparing a TPU composite material. The difference from Example 8 is that unmodified BCN-GNTs are used instead of LPBN, and the amount of BCN-GNTs added in the TPU composite material is 1 wt%, resulting in a TPU / BCN composite material sample.

[0064] Comparative Example 3: This comparative example provides a method for preparing a TPU composite material. The difference from Example 8 is that P-BCN is used instead of LPBN, and the amount of P-BCN added in the TPU composite material is 1 wt%, resulting in a TPU / P-BCN composite material sample.

[0065] Comparative Example 4: This comparative example provides a method for preparing a TPU composite material, including the following steps: Using a Thermo HAAKE rheometer, the BCN-GNTs prepared in step S1 of Example 1 were melt-blended with TPU granules at 175°C for 10 min, with a rotor speed of 60 rpm. The amount of BCN-GNTs added accounted for 10 wt% of the total mass of the TPU composite material. After blending, the composite material was placed in a mold, preheated at 175°C for 6 min, and hot-pressed at 12 MPa for 8 min. After cooling, a TPU / BCN10 composite material sample was obtained.

[0066] Testing and Characterization: 1. Structural characterization of flame retardants: The structure of the LPBN0.03 composite flame retardant system prepared in Example 1, as well as its intermediate products BCN-GNTs and P-BCN-GNTs, was characterized.

[0067] Figure 2 a and Figure 2 b shows the FTIR and XRD spectra of BCN, P-BCN, and LPBN0.03. Figure 2 As shown in figure a, BCN is at 1400cm -1 The presence of characteristic absorption peaks for BN bonds nearby indicates the successful formation of the boron-nitrogen structure. Compared to BCN, P-BCN exhibits a higher absorption peak in the 1000-1200 cm⁻¹ range. -1 The presence of absorption peaks for phosphorus-containing groups such as PO, POC, and P=O in the region indicates the successful introduction of phosphorus onto the BCN surface. LPBN0.03 shows absorption changes in the low wavenumber region related to La-O or La coordination, while still retaining characteristic peaks for BN and PO, indicating successful La loading onto the P-BCN surface. Figure 2 As shown in b, BCN exhibits broad peaks at approximately 26° and 43° of 2θ, corresponding to the (002) and (100) crystal planes of the graphitic carbon structure, respectively. P-BCN and LPBN0.03 retain the main diffraction peaks of BCN, indicating that phosphorus modification and La loading did not disrupt the main structure of BCN. Meanwhile, no obvious lanthanum-based crystal diffraction peaks were observed in LPBN, suggesting that La may exist in a highly dispersed or amorphous state. Combining the FTIR and XRD results, the LPBN composite flame-retardant system was successfully prepared.

[0068] Figure 3 XPS spectra of BCN, P-BCN, and LPBN0.03. Full spectrum scans show that... Figure 3 (a) It can be seen that C, N, O, and B elements were mainly detected in BCN; after POCl3 modification, a P2p characteristic peak appeared in P-BCN, indicating that phosphorus was successfully introduced into the BCN surface. Further loading with La resulted in a significant La3d characteristic peak in LPBN0.03, while still retaining C1s, N1s, O1s, B1s, and P2p signals, indicating that La was successfully loaded onto the P-BCN surface. Figure 3 As shown in (b), the C1s peaks in LPBN0.03 are 283.5, 284.6, 285.6, and 288.4 eV, corresponding to structures such as CB, CC / C=C, CN / CO, and C=O, respectively. This indicates that the BCN surface contains various carbon-containing functional groups, providing active sites for subsequent phosphorus modification and La loading. Figure 3As shown in (c), the N1s peaks are mainly located at 397.6, 399.6 and 401.7 eV, which can be attributed to BN, CN and graphitic N or oxidized N, respectively, indicating that nitrogen was successfully doped into the carbon framework. Figure 3 (d) is the B1s spectrum. LPBN0.03 shows characteristic peaks near 190.2, 191.4, and 192.5 eV, which can be attributed to BN, BCN, and BO bonding structures, indicating chemical bonding between B and C, N, and O elements. Figure 3 As shown in (e), the O1s spectrum peaks can be divided into 530.9, 531.7 and 533.0 eV, which correspond to oxygen-containing structures such as La-O, PO / C=O and CO or adsorbed oxygen, respectively. This indicates that there are abundant oxygen-containing functional groups in LPBN0.03, which is conducive to the coordination of La with the P-BCN surface. Figure 3 (f) shows the P2p spectrum. Both P-BCN and LPBN0.03 exhibit a characteristic P2p peak around 134 eV, which can be attributed to phosphorus-containing structures such as PO, P=O, or POC, indicating that phosphorus was successfully modified on the BCN surface. Compared to P-BCN, the position of the P2p peak in LPBN0.03 changes, suggesting that the introduction of La may involve coordination or interaction with phosphorus-containing functional groups. Figure 3 As shown in (g), the La3d spectral peaks are located at 836.2, 839.5, 852.7, and 856.1 eV, indicating that La mainly exists as La3d eV. 3+ The form exists in LPBN0.03. In summary, the XPS results further prove that P and La elements were successfully introduced into the BCN surface, forming a multi-element composite structure containing C, B, N, O, P and La.

[0069] Figure 4 This section presents SEM, TEM, and STEM-HAADF images of BCN and LPBN 0.03, along with corresponding EDS element distribution maps for the regions. Figure 4 As shown in (a) and (b), BCN exhibits a tubular structure, but the nanotubes are entangled and densely packed, with localized bundle-like aggregation. EDS elemental distribution results show that C, B, N, and O elements are evenly distributed, indicating that B and N elements were successfully introduced into the BCN framework. After P modification and La loading, LPBN0.03 still maintains its tubular morphology, but its structure is more loosely disordered than BCN, and the bundle-like aggregation phenomenon is weakened, indicating that the dispersibility of BCN is improved after modification. Figure 4 (f) shows that C, B, O, P and La elements are evenly distributed. The above results prove that phosphorus-containing functional groups were successfully introduced into the BCN surface, and La element was further effectively loaded on the P-BCN surface, providing a structural basis for the subsequent synergistic flame retardant effect of La / P / B / N multi-element.

[0070] 2. Structure and dispersibility of TPU composite materials: The TPU / (LPBN0.03) composite materials prepared in Examples 8-11 and Comparative Examples 1-4 were characterized by XRD and TEM.

[0071] Figure 5 XRD patterns of TPU and its various composite materials. Figure 5 It can be seen that pure TPU exhibits a relatively broad diffraction peak at approximately 20° 2θ, indicating that TPU mainly has an amorphous structure with a certain degree of ordered aggregation of soft and hard segments. After adding BCN, P-BCN, and different contents of LPBN0.03, the composite material still retains the main characteristic peaks of TPU, and the peak positions do not shift significantly, indicating that the introduction of the flame retardant did not significantly damage the main structure of TPU. Simultaneously, no obvious new crystal diffraction peaks appeared in the figure, indicating that LPBN0.03 did not form significant large-sized crystal aggregations in the TPU matrix.

[0072] Figure 6 TEM images of TPU / BCN10 and TPU / LPBN10 composite materials. Figure 6 (a, b) It is evident that BCN exhibits significant aggregation within the TPU matrix, forming locally larger aggregates. This indicates poor interfacial compatibility between unmodified BCN and the TPU matrix, with nanotubes easily entangled and stacked due to van der Waals interactions. In contrast, as... Figure 6 As shown in (c) and (d), the filler distribution of TPU / LPBN10 is more uniform, and the agglomerate size is significantly reduced. LPBN0.03 exhibits better dispersion in the TPU matrix. This is mainly attributed to the increased surface polar groups and active sites of BCN after P modification and La loading, which improves the interfacial interaction between the filler and TPU molecular chains, thereby weakening the self-aggregation tendency between fillers. The above results indicate that LPBN0.03 can be relatively uniformly dispersed in the TPU matrix, which is beneficial for forming a continuous physical barrier network.

[0073] 3. Mechanical property testing: Tensile properties of the specimens prepared in Examples 6-13 and Comparative Examples 1-3 were tested using an AG-IS universal testing machine according to DIN 53504 standard. S1 type dumbbell-shaped specimens were used, with narrow parallel section dimensions of 33 mm × 6 mm × 2 mm, an initial gauge length of 25 mm, and a tensile rate of 500 mm / min. Five parallel specimens were tested for each group, and the average value was taken.

[0074] Table 1 shows the tensile data of TPU composites with different LPBN ratios at a 1 wt% addition amount. Figure 7 The stress-strain curves for the corresponding TPU and TPU / LPBN composites are shown. Figure 7As shown in Table 1, the tensile strength of pure TPU is 31.4 MPa, and the elongation at break is 618.9%. After adding BCN, the tensile strength of TPU / BCN decreased to 29.3 MPa, possibly due to BCN agglomeration in the TPU matrix, resulting in poor interfacial compatibility. The tensile strength of TPU / P-BCN was 30.5 MPa, higher than that of TPU / BCN, indicating that P modification improved the interaction between the filler and the TPU matrix. Compared with TPU, the tensile strengths of TPU / (LPBN0.01)1 and TPU / (LPBN0.03)1 increased to 32.2 MPa and 33.1 MPa, respectively, representing increases of 2.5% and 5.4% compared to pure TPU. Among them, TPU / (LPBN0.03)1 exhibited the highest tensile strength, indicating that appropriate La loading and phosphorus modification can improve the dispersibility of LPBN in the TPU matrix and enhance the interfacial interaction between the filler and the matrix. The tensile strength of TPU / (LPBN0.05)1 was 31.3 MPa, indicating a decrease in reinforcement, possibly related to localized agglomeration caused by excessive La loading. Simultaneously, the elongation at break of the composite material was lower than that of pure TPU, suggesting that the addition of filler restricted the movement of TPU molecular chains. Considering both tensile strength and elongation at break, the composite flame retardant with an LPBN0.03 ratio showed the best mechanical reinforcement effect on TPU when 1 wt% flame retardant was added simultaneously.

[0075] Table 1. Statistical table of tensile data for TPU / LPBN composite materials.

[0076] Table 2 shows the cone calorimetric data for different LPBN ratios at the same 1wt% addition amount. Figure 8 HRR and SPR curves for TPU and TPU / LPBN composites are shown in Table 2. Figure 8 It can be seen that the PHRR of pure TPU is 881 kW / m. 2 THR is 97 MJ / m 2 PSPR and TSP are 0.086m. 2 / s and 9.17m 2 After adding BCN, the PHRR of TPU / BCN decreased to 733 kW / m. 2 The PHRR was reduced by 16.8% compared to TPU, indicating that the tubular structure of BCN can play a certain physical barrier role during combustion. The PHRR of TPU / P-BCN was further reduced to 657 kW / m³. 2The flame retardancy was reduced by 25.4% compared to TPU, indicating that P modification helps promote char formation in the condensed phase and improves the flame retardant effect of the composite material. Compared with TPU / BCN and TPU / P-BCN, the TPU / LPBN composite material exhibited lower heat release and smoke release. Specifically, the PHRR of TPU / LPBN 0.03 was reduced to 583 kW / m³. 2 It is 33.8% lower than TPU; PSPR and TSP are reduced to 0.061m. 2 / s and 8.31m 2 The results indicate that LPBN0.03 has a good flame retardant and smoke-suppressing effect on TPU. This may be due to the synergistic effect between the appropriate La loading and phosphorus-modified BCN, which promotes the formation of a more stable char layer during combustion, thereby inhibiting heat and smoke release. Combined data on PHRR, THR, PSPR, and TSP show that the composite flame retardant with LPBN0.03 ratio has the best flame retardant and smoke-suppressing effect on TPU.

[0077] Table 2. Statistical Table of Conical Calorific Data for TPU and TPU / LPBN Composite Materials

[0078] In Table 2, the meanings of each parameter are as follows: TTI: ignition time, PHRR: peak heat release rate, THR: total heat release, AMLR: average mass loss rate, PSPR: peak smoke release rate, TSP: total smoke release.

[0079] 4. Thermal stability test: Thermogravimetric analysis was performed on the samples prepared in Examples 6-11 and Comparative Example 1 using a STA449F3 thermal analyzer under air conditions, heating from 30°C to 800°C at a heating rate of 10°C / min. The TG curves and DTG curves were recorded.

[0080] Figure 9 The TG(a) and DTG(b) curves of TPU and TPU / LPBN0.03 composite material in air atmosphere are shown in Table 3. The relevant thermogravimetric data are also presented. Figure 9As shown in Table 3, the Ti and Tmax of pure TPU are 304℃ and 416℃, respectively. With the increase of LPBN0.03 addition, the Ti of the TPU / LPBN0.03 composite material generally shows a decreasing trend. The Ti values ​​for TPU / (LPBN0.03)1, TPU / (LPBN0.03)10, and TPU / (LPBN0.03)15 are 299℃, 284℃, and 278℃, respectively, indicating that LPBN0.03 may promote the premature decomposition and dehydration of TPU into carbon at lower temperatures. The residual carbon content of pure TPU at 500℃ and 700℃ are 15.7wt% and 0.07wt%, respectively. The addition of LPBN0.03 significantly increased the char content of the composite materials. The char content of TPU / (LPBN0.03)5, TPU / (LPBN0.03)10, and TPU / (LPBN0.03)15 increased to 25.9 wt%, 28.2 wt%, and 29.1 wt% at 500 °C, respectively, and to 1.97 wt%, 6.05 wt%, and 8.02 wt% at 700 °C, respectively. DTG curves showed that the composite materials still exhibited the main thermal degradation process of TPU, but the intensity of the maximum thermogravimetric peak decreased. These results indicate that LPBN0.03 improved the thermal stability and char-forming ability of the TPU composites to a certain extent.

[0081] Table 3. Statistical table of thermogravimetric data for TPU and TPU / LPBN0.03 composite materials.

[0082] In Table 3, T i and T max These refer to the temperature at which a 5% mass loss occurs and the temperature at which the decomposition rate reaches its maximum value, respectively.

[0083] 5. Flame retardant performance test: Using an FTT cone calorimeter, with an external heat flux of 35 kW / m² 2 Under the conditions, the flame retardant and smoke suppression performance of the samples (100mm×100mm×3mm in size, wrapped in aluminum foil) prepared in Examples 6-11 and Comparative Example 1 were tested. Figure 10 The HRR and SPR curves for TPU and the TPU / LPBN0.03 composite material are shown in Table 4, along with relevant cone calorimetric data. The HRR of pure TPU is 881 kW / m³. 2 THR is 97 MJ / m 2 PSPR and TSP are 0.086m. 2 / s and 9.17m 2With increasing LPBN0.03 content, the pHRR of the TPU / LPBN0.03 composite material showed a significant decreasing trend. The pHRRs of TPU / (LPBN0.03)1, TPU / (LPBN0.03)5, TPU / (LPBN0.03)10, and TPU / (LPBN0.03)15 were 583, 496, 394, and 304 kW / m², respectively. 2 Compared to pure TPU, LPBN0.03 reduced heat release by 33.8%, 43.7%, 55.3%, and 65.5%, respectively, indicating that LPBN0.03 can effectively suppress heat release during TPU combustion. Simultaneously, the addition of LPBN0.03 also reduced TPU smoke release. Specifically, the PSPR and TSP of TPU / (LPBN0.03)15 decreased to 0.034 m³ / s. 2 / s and 5.42m 2 Compared to pure TPU, the content of LPBN0.03 decreased by approximately 60.5% and 40.9%, respectively. Furthermore, with increasing LPBN0.03 content, the TTI of the composite material increased from 56 s to 73 s, and the AMLR decreased from 0.056 g / s to 0.033 g / s, indicating that LPBN0.03 can delay ignition and reduce the mass loss rate during combustion. These results demonstrate that LPBN0.03 can effectively suppress the release of heat, combustible volatiles, and smoke by promoting char formation and forming a barrier layer, thereby improving the flame retardant and smoke-suppressing properties of TPU.

[0084] Table 4. Statistical Table of Conical Calorimetric Data for TPU and TPU / LPBN0.03 Composite Materials

[0085] The combined effect of different LPBN ratios on the mechanical and flame retardant properties of TPU composites shows that LPBN0.03 exhibits superior overall performance. In terms of mechanical properties, the tensile strength of TPU / (LPBN0.03)1 reaches 33.1 MPa, which is 5.4% higher than pure TPU and higher than TPU / (LPBN0.01)1 and TPU / (LPBN0.05)1, indicating that an appropriate La loading is beneficial for improving the interfacial interaction between LPBN and the TPU matrix, thereby increasing stress transfer efficiency. Regarding flame retardant properties, the PHRR of TPU / LPBN0.03 decreases to 583 kW / m³. 2 Compared to pure TPU, it reduced by 33.8%, while PSPR and TSP decreased to 0.061m. 2 / s and 8.31m 2The TPU / LPBN composite exhibited good flame retardant and smoke suppression effects. In contrast, LPBN0.01 had a lower La content, resulting in relatively insufficient synergistic flame retardant and reinforcing effects; while LPBN0.05 had a higher La content, which may lead to localized filler agglomeration, affecting its dispersibility and interfacial interaction in the TPU matrix. Therefore, LPBN0.03 showed a better balance between mechanical properties, heat release suppression, and smoke release suppression, making it the optimal formulation and used in subsequent performance studies of TPU / LPBN composites with different addition amounts.

[0086] Figure 11 The stress-strain curves and related tensile property data for TPU and TPU / LPBN0.03 composite materials are shown in Table 5. Figure 11 As shown in Table 5, the tensile strength and elongation at break of pure TPU are 31.4 MPa and 618.9%, respectively. When the LPBN0.03 addition amount is 0.1 wt% and 0.5 wt%, the tensile strength of the composite material is 30.6 MPa and 30.8 MPa, respectively, showing little change compared to pure TPU. As the LPBN0.03 addition amount increases to 1 wt%, 5 wt%, and 10 wt%, the tensile strength increases to 33.1 MPa, 34.3 MPa, and 34.9 MPa, respectively, indicating that an appropriate amount of LPBN0.03 can enhance the interfacial interaction between the filler and the TPU matrix and improve stress transfer efficiency. When the LPBN0.03 addition amount further increases to 15 wt%, the tensile strength decreases to 28.2 MPa, which may be related to local agglomeration and stress concentration caused by excessive filler. Meanwhile, the elongation at break of the composite material decreased overall with increasing addition amount, from 618.9% for pure TPU to 213.7% for TPU / (LPBN0.03)15, indicating that LPBN0.03 restricts the movement of TPU molecular chains to some extent, thus reducing the material's flexibility. In summary, an appropriate amount of LPBN0.03 is beneficial for improving the tensile strength of TPU, but excessive addition will weaken the material's mechanical properties.

[0087] Table 5. Statistical table of tensile data for TPU and TPU / LPBN0.03 composite materials.

[0088] 6. Carbon residue analysis: Digital photographs, SEM, EDX, FTIR, and Raman analyses were performed on the carbon residues of Examples 8-11 and Comparative Example 1 after cone calorimetry testing.

[0089] Figure 12Digital photographs of the char residue after combustion of TPU and TPU / LPBN0.03 composite materials are shown. As can be seen from the figures, pure TPU produces less char residue after combustion, and the char layer is thin and discontinuous, indicating that TPU itself has a weak char-forming ability. After adding LPBN0.03, the char residue of the composite material increases significantly, the char layer coverage area increases, and cracks and pores decrease. With increasing LPBN0.03 addition, the char structure gradually becomes more continuous and thicker, with TPU / (LPBN0.03)10 and TPU / (LPBN0.03)15 showing more complete char coverage.

[0090] Figure 13 SEM images of the char residues of TPU and TPU / LPBN0.03 composite materials are shown in Table 6, and EDX data of the corresponding char residues are also presented. As can be seen from the images, the surface of the pure TPU char residue is relatively smooth, but there are obvious cracks, and the continuity of the char layer is poor. After adding LPBN0.03, the surface of the char residue gradually changes from a smooth structure to a rough granular and lamellar structure, indicating that LPBN0.03 participates in the char formation process of the TPU condensed phase. With the increase of LPBN0.03 addition, the char structure becomes more complete. Among them, the char residue of TPU / (LPBN0.03)15 exhibits a significant expansion morphology, forming a thicker expanded char layer, which is beneficial for blocking the transfer of heat, oxygen, and combustible volatiles. As shown in Table 6, only C and O elements were detected in the pure TPU char residue, while N, B, P, and La elements were present in the TPU / LPBN0.03 composite material char residue, indicating that LPBN0.03 is retained in the condensed phase after combustion and participates in the construction of the composite char layer. The presence of P and La indicates that LPBN0.03 can catalyze char formation during combustion, promoting the formation of a stable char layer containing B, N, P, and La. In summary, LPBN0.03 can significantly improve the char formation ability of TPU and enhance the flame retardant and smoke-suppressing properties of the composite material by forming a continuous, expanded, and element-rich protective char layer.

[0091] Table 6. Statistical table of EDX data for carbon residue in TPU composite materials.

[0092] Figure 14 FTIR and Raman spectra of residual carbon from TPU and TPU / LPBN0.03 composite materials. Figure 14 (a) FTIR spectra of TPU and TPU / LPBN0.03 composite char. Pure TPU char mainly shows absorption peaks of oxygen-containing groups such as C=O, indicating a relatively simple char structure after combustion. After adding LPBN0.03, the composite char showed a higher absorption peak at 3400 cm⁻¹. -1 An NH-related absorption peak appears nearby, at 1000-1100 cm⁻¹. -1Characteristic absorption peaks such as COC / PO were observed nearby, and La-O related absorption peaks appeared in the low wavenumber region, indicating that N, P, and La elements in LPBN0.03 participated in the formation of the residual char structure. With increasing LPBN0.03 addition, these characteristic peaks became more pronounced, indicating that LPBN0.03 can promote the formation of a composite char layer containing nitrogen, phosphorus, and lanthanum during combustion. Figure 14 (b) It can be seen that each sample is at approximately 1350 cm. -1 and 1580cm -1 D and G peaks appeared at the point. The ID / IG value of pure TPU char was 3.27. With the increase of LPBN0.03 addition, this value gradually decreased to 0.71 of TPU / (LPBN0.03)15, indicating that the degree of ordering and graphitization of the char was improved. Combined with the char morphology and FTIR analysis, it can be seen that LPBN0.03 participates in the condensed phase char formation during combustion, promoting the formation of a continuous and stable char layer containing N, P and La, thereby effectively blocking the transfer of heat, oxygen and combustible volatiles, and improving the flame retardant and smoke suppression performance of TPU composite materials.

[0093] The above tests, including FTIR, XRD, XPS, SEM, TEM, and EDS results, demonstrate that this invention successfully modifies the BCN surface with P and further loads La onto the P-BCN surface, successfully constructing an LPBN composite flame-retardant system. Compared to BCN, LPBN0.03 exhibits reduced bundle aggregation and improved dispersibility, which is beneficial for its formation of a barrier network within the TPU matrix.

[0094] Mechanical and flame retardant performance tests showed that adding the composite flame retardant of this invention to the TPU matrix improved the tensile strength of the composite material compared to pure TPU at an appropriate addition amount, while significantly reducing the peak heat release rate and smoke release rate, demonstrating good flame retardant and smoke suppression effects. Specifically, the LPBN0.03 ratio at 1 wt% showed superior overall performance, with the tensile strength of TPU / (LPBN0.03)1 reaching 33.1 MPa, a 5.4% increase compared to pure TPU, and the PHRR decreasing to 583 kW / m². 2 Compared to pure TPU, it reduced by 33.8%, with PSPR and TSP decreasing to 0.061m. 2 / s and 8.31m 2 Within the range of P-BCN to lanthanum nitrate mass ratio of 1:0.01 to 1:0.05 as defined in this invention, other ratios of LPBN can also impart significant flame retardant and smoke-suppressing properties to the TPU matrix.

[0095] To investigate the effect of lanthanum loading on the overall performance of composite flame retardants, this invention prepared LPBN composite flame retardants with different lanthanum loadings by setting the mass ratio of phosphorus-modified boron-nitrogen-doped carbon nanotubes to lanthanum nitrate hexahydrate to 1:0.01, 1:0.03, and 1:0.05. Through comprehensive analysis of mechanical properties, flame retardant properties, and smoke suppression properties, all three lanthanum loading ratios improved the overall performance of TPU composites to a certain extent. Among these, the mass ratio of 1:0.03 achieved a better balance between the catalytic char formation and smoke suppression effects of lanthanum, the dispersion of the flame retardant in the TPU matrix, and the interfacial interaction between the filler and the matrix. The resulting composite exhibited the best flame retardant, smoke suppression, and mechanical properties; therefore, 1:0.03 was determined as the preferred ratio. Meanwhile, the composite flame retardants prepared with mass ratios of 1:0.01 and 1:0.05 still exhibited good flame retardant, smoke suppression, and mechanical properties, meeting the performance control requirements of different application scenarios and serving as a basis for further optimization research in this invention.

[0096] Furthermore, performance tests at the same addition amount for different lanthanum loading ratios revealed that when the addition amount of LPBN0.01 and LPBN0.05 composite flame retardants in TPU composites is between 0.1% and 15 wt%, both can exert the physical barrier effect of boron-nitrogen-doped carbon nanotubes, the char-promoting effect of phosphorus-containing groups, and the catalytic char formation and smoke suppression effect of lanthanum, thereby improving the thermal stability, flame retardant performance, and smoke suppression performance of TPU composites. With the increase in the addition amount of the composite flame retardant, its role in forming a physical barrier network and promoting the construction of condensed phase char layer in the TPU matrix is ​​expected to gradually increase. Therefore, both LPBN0.01 and LPBN0.05 can achieve good comprehensive performance within the addition range of 0.1% to 15 wt%. Lower addition amounts are beneficial in reducing the impact of the flame retardant on the molecular chain movement and mechanical properties of TPU, while higher addition amounts are beneficial in increasing char formation and barrier effect. However, excessively high addition amounts may increase the tendency for local filler agglomeration and stress concentration. Therefore, the addition amounts of LPBN0.01 and LPBN0.05 can be selected and optimized according to the specific requirements of different application scenarios for flame retardant performance, smoke suppression performance, mechanical properties, and processing performance. Although LPBN0.03 exhibits superior overall performance under existing testing conditions, LPBN0.01 and LPBN0.05 still have good potential for performance adjustment.

[0097] Furthermore, for the LPBN0.01 composite flame retardant of Example 2 and the LPBN0.05 composite flame retardant of Example 3, when they were added to the TPU matrix at different amounts to prepare composite materials, the trends of the mechanical properties, thermal stability, flame retardant properties, and smoke suppression properties of the resulting composite materials were basically consistent with the trends of the LPBN0.03 system in Examples 6-11. That is, as the amount of flame retardant added increased, the heat release rate and smoke release rate of the composite material gradually decreased, while the char residue and char layer integrity gradually increased. Among them, the LPBN0.01 system, due to its relatively low lanthanum loading, had a slightly higher peak heat release rate (PHRR) than the LPBN0.03 system at the same addition amount, and its tensile strength was slightly lower than that of the LPBN0.03 system, but still significantly better than Comparative Examples 1-4. The LPBN0.05 system, due to its relatively high lanthanum loading, had a PHRR that was basically equivalent to that of the LPBN0.03 system at the same addition amount, but its tensile strength was lower than that of the LPBN0.03 system.

[0098] For Comparative Example 4, the flame retardant performance of TPU / BCN10 is improved compared to that of Comparative Example 2, but due to the obvious aggregation of unmodified BCN in the TPU matrix, the flame retardant effect and mechanical properties of Comparative Example 4 are significantly inferior to the system using the LPBN composite flame retardant of this invention at the same addition amount. This further confirms the necessity of phosphorus modification and lanthanum loading for improving the dispersibility of carbon nanotubes and enhancing the overall flame retardant performance.

[0099] With increasing LPBN content, the tensile strength of the TPU composite material initially increases and then decreases, achieving a good balance between mechanical properties and flame retardant properties within an appropriate addition range. When the addition amount is too high, the tensile strength decreases, which is related to localized agglomeration and stress concentration caused by excessive filler. Simultaneously, the elongation at break of the composite material decreases with increasing addition amount, indicating that LPBN restricts the movement of TPU molecular chains to some extent.

[0100] Thermogravimetric analysis showed that although the addition of LPBN reduced the initial decomposition temperature of TPU, it significantly increased the amount of char residue, indicating that LPBN can promote the early cracking and dehydration of TPU to form char and improve the char formation ability of the condensed phase.

[0101] Cone calorimetry results show that LPBN can significantly reduce the heat and smoke release of TPU. Taking TPU / (LPBN0.03)15 as an example, its PHRR decreased to 304 kW / m³. 2 Compared to pure TPU, it reduced by 65.5%, with PSPR and TSP decreasing to 0.034m. 2 / s and 5.42m 2 Compared with pure TPU, the flame retardant content was reduced by approximately 60.5% and 40.9%, respectively, indicating that the composite flame retardant of the present invention has excellent flame retardant and smoke suppression effects.

[0102] Digital photographs, SEM, EDX, FTIR, and Raman results of the char residue showed that LPBN promotes the formation of a continuous, expanded, and stable composite char layer after TPU combustion. The presence of B, N, P, and La elements in the char residue, as well as the decrease in the ID / IG value, indicate that LPBN0.03 participates in the char layer construction and improves the degree of char layer ordering. This char layer can effectively block the transfer of heat, oxygen, and combustible volatiles, thereby improving the flame retardant and smoke-suppressing properties of the TPU composite material.

[0103] In summary, LPBN effectively enhances the flame retardant and smoke-suppressing properties of TPU through the physical barrier effect of its tubular carbon-based structure, the catalytic carbonization effect of phosphorus (P), the carbon layer stabilization effect of boron / nitrogen (B / N), and the synergistic catalytic effect of la. Within the mass ratio of phosphorus-modified boron-nitrogen-doped carbon nanotubes to lanthanum nitrate or lanthanum nitrate hexahydrate (as defined in this invention) of 1:0.01-1:0.05, the resulting composite flame retardants significantly improve the flame retardant and smoke-suppressing properties of the TPU matrix. Furthermore, the effective control between flame retardant and smoke-suppressing effects and mechanical properties can be achieved within the range of 0.1-15 wt% of the flame retardant addition.

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite flame retardant for TPU, characterized in that, The invention includes boron-nitrogen-doped carbon nanotubes, the surface of which is modified with phosphorus, and lanthanum is also loaded onto the boron-nitrogen-doped carbon nanotubes.

2. A method for preparing the composite flame retardant for TPU according to claim 1, characterized in that, Includes the following steps: S1: Dissolve urea, boric acid and polyethylene glycol in water, dry them and then pyrolyze them under an inert atmosphere to obtain boron-nitrogen-doped carbon nanotubes. S2: Acidification treatment of boron-nitrogen-doped carbon nanotubes to obtain acidified boron-nitrogen-doped carbon nanotubes; S3: React acidified boron nitrogen-doped carbon nanotubes with a phosphorus source to obtain phosphorus-modified boron nitrogen-doped carbon nanotubes; S4: React phosphorus-modified boron-nitrogen-doped carbon nanotubes with lanthanum ions to obtain a composite flame retardant for TPU.

3. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S1, the mass ratio of urea to boric acid is 35:1-40:1, and the mass ratio of polyethylene glycol to urea is 1:10-1:

12.

4. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S1, the pyrolysis treatment temperature is 850-950℃, the time is 3-5h, and the inert atmosphere is nitrogen atmosphere.

5. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S2, boron-nitrogen-doped carbon nanotubes are added to a nitric acid solution and acidified for 1.5-2.5 hours. The concentration of the nitric acid solution is 20-30 wt%.

6. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S3, boron nitrogen-doped carbon nanotubes are dispersed in anhydrous ethanol, ultrasonically treated, and then a phosphorus source is added. After stirring, the mixture is heated to 55-65℃ and reacted for 3.5-4.5 hours to obtain phosphorus-modified boron nitrogen-doped carbon nanotubes. The phosphorus source is phosphorus oxychloride, and the mass ratio of the phosphorus source to the boron nitrogen-doped carbon nanotubes is 1:8-1:

12.

7. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S4, phosphorus-modified boron-nitrogen-doped carbon nanotubes are dispersed in water, ultrasonically treated, and then lanthanum nitrate or lanthanum nitrate hexahydrate is added. After stirring, the mixture is heated to 75-85℃ and reacted for 3.5-4.5 hours. After drying, a composite flame retardant for TPU is obtained.

8. The method for preparing the composite flame retardant for TPU according to claim 2, characterized in that, In step S4, the mass ratio of phosphorus-modified boron-nitrogen-doped carbon nanotubes to lanthanum nitrate or lanthanum nitrate hexahydrate is 1:0.01-1:0.

05.

9. A TPU composite material, characterized in that, It includes a TPU matrix, and a TPU composite flame retardant as described in claim 1 or a TPU composite flame retardant prepared by any one of the preparation methods described in claims 2-8; the mass of the TPU composite flame retardant accounts for 0.1-15% of the mass of the TPU composite material.

10. A method for preparing the TPU composite material according to claim 9, characterized in that, TPU composite material is prepared by melt blending TPU with the TPU using a composite flame retardant.