A polypropylene composite material with low dielectric constant and low dielectric loss and its preparation method
A polypropylene interface layer was constructed on the surface of hollow glass microspheres by fluidized bed spray in-situ wetting-irradiation crosslinking process, which solved the problems of microsphere breakage and interface polarization, and realized a polypropylene composite material with low dielectric constant and low dielectric loss, which is suitable for high frequency communication.
Patent Information
- Application Number
- CN202611209645.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-10
AI Technical Summary
In the existing technology, hollow glass microspheres are easily broken during processing, which leads to an increase in dielectric constant and dielectric loss, and serious interface polarization problems, making it difficult to meet the requirements of high-frequency communication for low dielectric constant and low dielectric loss.
A fluidized bed spray in-situ impregnation-irradiation crosslinking process was used to construct a chemically bonded polypropylene interface layer on the surface of hollow glass microspheres. The three-dimensional network structure was formed by irradiation crosslinking, which protected the microspheres and improved the interfacial bonding force.
It effectively reduces dielectric constant and dielectric loss, protects microspheres from breakage, improves interfacial bonding, and enhances the performance of materials in high-frequency communication.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to a polypropylene composite material with low dielectric constant and low dielectric loss for use in high-frequency communication, and its preparation method. Background Technology
[0002] Polypropylene (PP), with its excellent comprehensive properties, has shown extremely broad application prospects in fields such as high-frequency electronic packaging and 5G / 6G radomes. However, the dielectric constant (Dk≈2.2–2.6) and dielectric loss (Df) of pure PP still need to be further reduced to meet the stringent requirements of low loss in high-speed signal transmission. While incorporating low-dielectric hollow glass microspheres (HGM) can effectively reduce the Dk value and density of composite materials, it faces two major technical bottlenecks: First, hollow glass microspheres are prone to breakage during processing. Thin-walled and brittle HGM is easily broken and fragmented during melt blending, screw shearing, and other processes. Excessive breakage weakens the Dk reduction effect, and the high surface energy fracture surfaces of these fragments become active sites for ion migration and partial discharge, thus introducing additional dielectric loss and deteriorating high-frequency performance. Second, significant interfacial polarization is a problem. Inorganic glass and organic PP differ significantly in polarity and coefficient of thermal expansion. Traditional blending or simple coupling agent treatment results in weak interfacial bonding, easily leading to defects and air gaps. These defects, under the influence of a high-frequency electric field, induce strong interfacial polarization, leading to a significant increase in the Df value, which in turn offsets the effect of reducing Dk.
[0003] Patent CN120157981A discloses a method for preparing polypropylene material, which reduces the breakage rate of microspheres during processing by introducing hollow glass microspheres grafted with polybutadiene or polypropylene. However, this preparation process does not adequately consider the potential agglomeration and grafting uniformity issues that may occur in the hollow glass microspheres during the polybutadiene / polypropylene grafting modification process. In the subsequent extrusion granulation stage, the melting of the surface resin weakens its protective effect on the hollow glass microspheres. Patent CN117757186A discloses a low dielectric constant polypropylene reinforced material and its preparation method. It adds sodium allyl sulfonate grafted and modified hollow glass microspheres. On one hand, by changing the surface properties of the hollow glass microspheres, the surface energy is reduced, improving the aggregation of the microspheres. On the other hand, by introducing functional groups on the surface of the microspheres, interaction forces are formed with the matrix, improving the compatibility between the microspheres and polypropylene. Simultaneously, the dielectric constant of the shell formed by the sodium allyl sulfonate is between the microspheres and the matrix, allowing the shell to act as a transition layer to reduce the degree of dielectric constant mismatch, resulting in a uniform electric field distribution. This reduces the dielectric constant and dielectric loss of the material without significantly reducing its mechanical properties. However, it does not consider the protection of the hollow glass microspheres. Patent CN114230916B discloses a polypropylene composite material, its preparation method, and its application. It uses low-specific polypropylene material to process and protect the hollow glass microspheres, but it does not adequately treat the interface. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a polypropylene composite material with low dielectric constant and low dielectric loss, as well as a method for its preparation. This method utilizes a fluidized bed spray in-situ wetting-irradiation crosslinking process to construct a chemically bonded and bulk-crosslinked polypropylene interface layer on the surface of hollow glass microspheres. This synergistically reduces the dielectric constant and dielectric loss by suppressing interfacial polarization and preventing microsphere breakage.
[0005] The technical solution of the present invention is as follows: A method for preparing a polypropylene composite material with low dielectric constant and low dielectric loss includes the following steps: Step 1: Preparation of irradiated crosslinked polypropylene emulsion: By weight, 100 parts of polypropylene emulsion, 1-2 parts of vinyl silane coupling agent, 2-5 parts of crosslinking aid, and 1.5-3 parts of emulsifier are mixed, and a pH stabilizer is added to adjust the pH value of the system and maintain it in a slightly alkaline range of 7.5-8 to obtain a stable irradiated crosslinked polypropylene emulsion. Preferably, the solid content of the polypropylene emulsion is 35-55%; Preferably, the vinyl silane coupling agent is one or both of vinyltrimethoxysilane or vinyltri(2-methoxyethoxy)silane; Preferably, the emulsifier is one or both of nonionic and anionic emulsifiers; Preferably, the pH stabilizer is ammonium bicarbonate; Preferably, the crosslinking agent is one or more of triallyl isocyanurate, trimethylolpropane trimethacrylate, and triallyl cyanurate; More preferably, the vinylsilane coupling agent is vinyltrimethylsilane (VTMO). More preferably, the emulsifier is a mixture of a nonionic emulsifier and anionic emulsifier; More preferably, the crosslinking agent is triallyl isocyanurate (TAIC).
[0006] Step 2: Surface coating treatment of hollow glass microspheres: Hollow glass microspheres are preheated to 80-100℃ and then fed into a fluidized bed reactor at a constant rate, forming a dynamic suspension under the action of hot air at 0.3-0.8 m / s. The emulsion obtained in step one is atomized through an atomizing nozzle at a pressure of 0.3-0.5 MPa and sprayed onto the surface of the fluidized microspheres at a mass ratio of emulsion solids to microspheres of 1:3 to 1:5. The microspheres are then held in a fluidized bed at 105-120℃ for 5-10 minutes to complete the processes of water evaporation, chemical bonding between silane and the glass surface, and film formation of polypropylene latex particles, resulting in pre-modified microspheres with a polypropylene interface layer coated on the surface. Preferably, the true density of the hollow microspheres is 0.2-0.6 g / cm³. 3 .
[0007] Step 3: Irradiation crosslinking enhancement of the coating layer: The pre-modified microspheres obtained in step two are placed under a nitrogen protective atmosphere and irradiated with an electron beam or gamma ray at a dose of 20-50 kGy. This initiates a free radical crosslinking reaction between the polypropylene in the coating layer and the crosslinking agent, forming a three-dimensional network structure, resulting in modified hollow glass microspheres with a crosslinked polymer interface layer on the surface.
[0008] Step 4: Composite material preparation The raw material composition, calculated by parts by weight, is as follows: Polypropylene: 45-87; Modified hollow glass microspheres: 10-50; Compatibilizer: 2-8; Antioxidant: 0.2-1; Lubricant: 0.1-0.8.
[0009] Preferably, the polypropylene has a melt index of 5-50 g / 10 min when tested at 230°C and 2.16 kg.
[0010] Preferably, the compatibilizer is maleic anhydride-grafted polypropylene.
[0011] Preferably, the antioxidant is a combination of a primary antioxidant and a secondary antioxidant. The primary antioxidant can be selected from one or more hindered phenolic antioxidants such as antioxidant 1010 and antioxidant 1076; the secondary antioxidant can be selected from one or more phosphite antioxidants such as antioxidant 168, triphenyl phosphite, and trinonylphenyl phosphite.
[0012] Preferably, the lubricant is one or more of calcium stearate, magnesium stearate, zinc stearate, and vinyl bis-stearate.
[0013] More preferably, the raw material composition of the composite material, calculated by mass parts, is as follows: Polypropylene: 60-80; Modified hollow glass microspheres: 15-35; Maleic anhydride-grafted polypropylene: 3-6; Antioxidant: 0.2-0.6; Lubricant: 0.2-0.6.
[0014] More preferably, the lubricant is calcium stearate.
[0015] The modified hollow glass microspheres obtained in step three are melt-blended and granulated with polypropylene resin in a predetermined ratio to obtain the polypropylene composite material with low dielectric constant and low dielectric loss.
[0016] The polypropylene composite material with low dielectric constant and low dielectric loss obtained by this invention can be applied in the field of high-frequency communication, high-frequency electronic packaging, and 5G / 6G radome. The material composition, by weight, includes: 45-87 parts of polypropylene, 10-50 parts of modified hollow glass microspheres, 2-8 parts of compatibilizer, 0.2-1 parts of antioxidant, and 0.1-0.8 parts of lubricant.
[0017] Modified hollow glass microspheres are produced by fluidized spraying followed by irradiation, which can suppress interfacial polarization and prevent microsphere breakage.
[0018] A polypropylene composite material with low dielectric constant and low dielectric loss prepared according to the above method is characterized in that the composite material comprises a polypropylene resin matrix and surface-modified hollow glass microspheres uniformly dispersed therein; the density of the surface-modified hollow glass microspheres is 0.20-0.60 g / cm³, and the surface of the microspheres is chemically bonded to a polypropylene-based polymer interface layer, which is a three-dimensional network structure formed by radiation crosslinking.
[0019] Compared with the prior art, the present invention has the following characteristics: (1) Through silane chemical bonding, a robust, dense, and low-polarity ideal interface was constructed, reducing polarization loss caused by interface defects.
[0020] (2) The three-dimensional network coating layer formed by irradiation crosslinking has excellent toughness and strength. In subsequent high-shear processing such as mixing and extrusion, it can act as a "buffer armor" to effectively protect the brittle hollow glass microspheres.
[0021] (3) The introduction of low-density hollow microspheres and low-polarity polymer coating layer synergistically reduces the effective dielectric constant of composite material and significantly reduces material density. Detailed Implementation
[0022] The present invention will be further illustrated below with reference to specific embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified, all raw materials used in the following embodiments and comparative examples are commercially available.
[0023] Polypropylene material: SP179 Qilu Petrochemical Polypropylene emulsion: 43040 Michael Men Hollow glass microspheres: K46 3M Maleic anhydride-grafted polypropylene: CMG5701 Jia Yi Rong Material characterization methods: Density was tested according to GB / T 1033.1-2008, and dielectric properties were tested according to GB / T 5594.4-2015. Example 1 Step 1: Take 250g of maleic anhydride-grafted polypropylene emulsion 43040 (40% solids content) and dilute it with 200g of deionized water. Pre-emulsify 5g of TAIC with an emulsifier solution prepared from 2g of nonionic emulsifier TX-10 and 1g of anionic emulsifier SDS to obtain a stable pre-emulsion. Slowly add this pre-emulsion to the diluted PP emulsion. Adjust the pH of the system to 7.8 with 1% ammonium bicarbonate aqueous solution. At this pH, slowly add 2g of VTMO silane and stir for 1 hour. Add water to bring the total volume to 35% and allow it to mature to obtain the working emulsion.
[0024] Step 2: Preheat K46 to 90°C and feed it into the fluidized bed at a rate of 9 kg / h. The hot air velocity is 0.6 m / s, and the bed temperature is 110°C. Spray the emulsion at a rate of 3 kg / h (atomization pressure 0.4 MPa). The average residence time of the microspheres is approximately 7 minutes.
[0025] Step 3: Collect the modified hollow glass microspheres and irradiate them with an electron accelerator under N2 protection at a dose of 30 kGy.
[0026] Step 4: By weight, add 71 parts SP179, 25 parts modified hollow glass microspheres, 0.3 parts 1010, 0.3 parts 168, 3 parts CMG5701 and 0.4 parts calcium stearate into a high-speed mixing pot. After stirring for 3 minutes, feed the mixture into the main feed loss-in-weight scale of a twin-screw extruder for melt blending, cooling and pelletizing to obtain the corresponding material. The twin-screw extrusion temperature is 180-220℃.
[0027] Example 2 Except for step four, where the SP179 content is changed to 81 parts and the modified hollow glass microsphere content is changed to 15 parts, the other steps are the same as in Example 1.
[0028] Example 3
[0029] Except for step four, where the SP179 content is changed to 61 parts and the modified hollow glass microsphere content is changed to 35 parts, the remaining steps are the same as in Example 1.
[0030] Comparative Example 1 Except for step one, which does not use VTMO silane, the other steps are the same as in Example 1.
[0031] Comparative Example 2 Except for step one, which does not use VTMO silane and TAIC, but only uses pure PP emulsion for coating, the remaining steps are the same as in Example 1.
[0032] Comparative Example 3 Except for omitting the irradiation crosslinking treatment in step three, the remaining steps are the same as in Example 1.
[0033] Comparative Example 4 Replace the modified hollow glass microspheres with untreated hollow glass microspheres K46, and perform the remaining steps as in step four of Example 1.
[0034] Table 1 shows the test results of Examples 1-3 and Comparative Examples 1-4. Table 1. Test results of Examples 1-3 and Comparative Examples 1-4 Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 <![CDATA[Density, g / cm 3 > 0.74 0.80 0.67 0.76 0.79 0.78 0.81 Dielectric constant @ 10 GHz 1.91 2.01 1.80 1.93 2.02 2.01 2.04 Dielectric loss @10GHz 0.0010 0.0009 0.0013 0.0016 0.0019 0.0014 0.0022 As can be seen from the results of Examples 1-3 and Comparative Examples 1-4 in Table 1, after the hollow glass microspheres are treated by fluidized bed spray in-situ impregnation-irradiation crosslinking process, adding them to polypropylene can effectively reduce the dielectric constant of the composite material, and the dielectric loss is not significantly increased. With the increase of the content of modified hollow glass microspheres, the dielectric loss will increase, and the preferred content is 15-35%.
[0035] The above description of the embodiments is provided to enable those skilled in the art to understand and apply the present invention. It will be apparent to those skilled in the art that various modifications can be easily made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the embodiments described herein, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a polypropylene composite material with low dielectric constant and low dielectric loss, comprising the following steps: Step 1: Preparation of irradiated crosslinked polypropylene emulsion: By weight, 100 parts of polypropylene emulsion, 1-2 parts of vinyl silane coupling agent, 2-5 parts of crosslinking aid, and 1.5-3 parts of emulsifier are mixed, and a pH stabilizer is added to adjust the pH value of the system and maintain it in a slightly alkaline range of 7.5-8 to obtain a stable irradiated crosslinked polypropylene emulsion. Step 2: Surface coating treatment of hollow glass microspheres: Hollow glass microspheres are preheated to 80-100℃ and then fed into a fluidized bed reactor at a constant rate, forming a dynamic suspension under the action of hot air at 0.3-0.8 m / s. The emulsion obtained in step one is atomized through an atomizing nozzle at a pressure of 0.3-0.5 MPa and sprayed onto the surface of the fluidized microspheres at a mass ratio of emulsion solids to microspheres of 1:3 to 1:
5. The microspheres are then held in a fluidized bed at 105-120℃ for 5-10 minutes to complete the processes of water evaporation, chemical bonding between silane and the glass surface, and film formation of polypropylene latex particles, resulting in pre-modified microspheres with a polypropylene interface layer coated on the surface. Step 3: Irradiation crosslinking enhancement of the coating layer: The pre-modified microspheres obtained in step two are placed under a nitrogen protective atmosphere and irradiated with an electron beam or gamma ray at a dose of 20-50 kGy to initiate a free radical crosslinking reaction between the polypropylene in the coating layer and the crosslinking agent, forming a three-dimensional network structure, and obtaining modified hollow glass microspheres with a crosslinked polymer interface layer on the surface. Step 4: Composite material preparation The raw material composition, calculated by parts by weight, is as follows: Polypropylene: 45-87 Modified hollow glass microspheres: 10-50 Compatibilizer: 2-8 Antioxidant: 0.2-1 Lubricant: 0.1-0.8; The modified hollow glass microspheres obtained in step three are melt-blended and granulated with polypropylene resin in a predetermined ratio to obtain the polypropylene composite material with low dielectric constant and low dielectric loss.
2. The low dielectric constant and low dielectric loss polypropylene composite material obtained by the preparation method according to claim 1, by mass parts, has the following raw material composition: Polypropylene: 45-87 Modified hollow glass microspheres: 10-50 Compatibilizer: 2-8 Antioxidant: 0.2-1 Lubricant: 0.1-0.
8.
3. The low dielectric constant and low dielectric loss polypropylene composite material obtained by the preparation method according to claim 1, with the following raw material composition by mass parts: Polypropylene: 60-80; Modified hollow glass microspheres: 15-35; Maleic anhydride-grafted polypropylene: 3-6; Antioxidant: 0.2-0.6; Lubricant: 0.2-0.
6.
4. The low dielectric constant and low dielectric loss polypropylene composite material according to claims 2 and 3, characterized in that, The polypropylene tested at 230℃ and 2.16 kg had a melt flow index of 5-50 g / 10 min.
5. The low dielectric constant and low dielectric loss polypropylene composite material according to claims 2 and 3, characterized in that... The compatibilizer is maleic anhydride-grafted polypropylene.
6. The low dielectric constant and low dielectric loss polypropylene composite material according to claims 2 and 3, characterized in that... The antioxidant is a combination of primary and secondary antioxidants. The primary antioxidant can be selected from one or more hindered phenolic antioxidants such as antioxidant 1010 and antioxidant 1076; the secondary antioxidant can be selected from one or more phosphite antioxidants such as antioxidant 168, triphenyl phosphite, and trinonylphenyl phosphite.
7. The low dielectric constant and low dielectric loss polypropylene composite material according to claims 2 and 3, characterized in that, The lubricant is one or more of calcium stearate, magnesium stearate, zinc stearate, and vinyl bis-stearate.
8. The low dielectric constant and low dielectric loss polypropylene composite material obtained by the preparation method according to claim 1 is applied to the fields of high frequency communication, high frequency electronic packaging, and 5G / 6G antenna radomes.
Citation Information
Patent Citations
A polypropylene composite material, its preparation method and application
CN114230916B
Low-dielectric-constant polypropylene reinforced material and preparation method thereof
CN117757186A
Polypropylene material and preparation method thereof