A high-performance polypropylene masterbatch for ultrathin capacitor films and its preparation method
By synergistically modifying cyclic olefin copolymers with organic functional components, the problems of insufficient heat resistance and uncontrolled component distribution in ultrathin capacitor films were solved, achieving improved heat resistance and stable electrical performance at high temperatures, while avoiding the defects of introducing inorganic fillers.
Patent Information
- Application Number
- CN202611525735.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
In the production of ultrathin biaxially oriented polypropylene capacitor films, conventional homopolymer polypropylene has limited heat resistance, the introduction of inorganic heat-resistant fillers creates defects, the two-phase compatibility of polypropylene and cyclic olefin copolymers is limited, and the uncontrolled distribution of components responsible for carrier capture leads to batch-to-batch differences in electrical performance.
Synergistic modification with cyclic olefin copolymers and organic functional components is employed to introduce aromatic ring groups in an independent molecular form. The aromatic ring groups are homologous to the polypropylene matrix and are enriched in the amorphous region and at the interface between the two phases. Combined with reactive compatibilizers, the stable distribution of aromatic ring groups in the carrier transport channels is ensured, avoiding the introduction of inorganic rigid fillers.
It improves the heat resistance of the substrate at high temperatures, suppresses dielectric loss and leakage current, reduces interface polarization, avoids molding defects, and ensures stable electrical performance between batches.
Smart Images

Figure CN123062846A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polypropylene composition technology, specifically to a high-performance polypropylene masterbatch for ultrathin capacitor films and its preparation method. The masterbatch is used to prepare biaxially oriented polypropylene capacitor films with a thickness of 2μm to 3μm. The resulting capacitor films are suitable for thin-film capacitors in applications such as new energy power, photovoltaic inverters, and high-voltage energy storage. Background Technology
[0002] Biaxially oriented polypropylene (BOP) film is the primary insulating medium for film capacitors. As film capacitors evolve towards miniaturization, higher voltage, and higher temperature operation, ultra-thin BOP capacitor films with a thickness of 2μm to 3μm have become the standard for applications such as new energy power, photovoltaic inverters, and high-voltage energy storage, and their long-term operating temperature has also increased accordingly. Under these specifications and operating conditions, the following problems exist in the production and use of this type of film.
[0003] Firstly, conventional homopolymer polypropylene has limited heat resistance. When subjected to high-temperature conditions for extended periods, the molecular chain movement in the amorphous region of polypropylene intensifies, the structure of this region loosens, and the dielectric loss of the film increases accordingly, as does the leakage current, leading to a higher incidence of thermal breakdown failure during long-term operation.
[0004] Secondly, the practice of introducing inorganic heat-resistant fillers into polypropylene to improve heat resistance is limited at the aforementioned thickness. The particle size distribution and dispersion state of inorganic fillers are difficult to control. During the biaxial stretching process of films with a thickness of only 2μm to 3μm, their agglomerates become stress concentration points, forming pinholes, crystal points, and microcracks in the film, thus reducing the breakdown field strength of the film.
[0005] Third, when cyclic olefin copolymers are blended with polypropylene to improve heat resistance, the compatibility between the two is limited, and there are interface defects at the interface of the two phases. Interface polarization is prone to occur at this point, which affects the dielectric properties of the film under high frequency and high temperature conditions. Moreover, in the longitudinal and transverse stretching of biaxial stretching, the two phases separate and delaminate at the point where the interface bonding is insufficient.
[0006] To achieve a more consistent blending ratio and batch stability under the aforementioned operating conditions, the heat-resistant component, functional component, and polypropylene carrier can be first prepared into a concentrated masterbatch, which is then blended downstream at a certain ratio to form a film. This approach solves the problem of consistency in additive dosage between batches; however, the electrical properties of the film depend not only on the average content of the functional component in the film but also on the distribution of this component in each phase region within the film, and this distribution is not determined by the dosage.
[0007] Under this approach, the amounts that can be set in the masterbatch are typically determined by "what components to add and how much to add": what heat-resistant components to add to improve the dimensional and modulus retention of the matrix at high temperatures, and what functional components to add to affect the transport of charge carriers inside the film. However, under actual use conditions where the film thickness is reduced to 2μm to 3μm and the operating temperature is increased, what is needed in production is not only to determine the types and amounts of components, but also to ensure that the components that perform specific functions reach a set content in their actual functional phase region, and to keep this content within the allowable deviation when the crystallization state of the matrix fluctuates with the film formation conditions; otherwise, the electrical properties of the film will still differ between different batches of the same formulation.
[0008] To introduce functional units capable of trapping charge carriers into polypropylene, related technologies have begun to employ chemical grafting. For example, Chinese invention patent application CN120399353A, published on August 1, 2025, discloses an aromatic heterocyclic modified polypropylene composite material, its preparation method, and a capacitor film. The composite material comprises, by mass fraction, 70–98.89% polypropylene, 1–22.5% cyclic olefin copolymer, 0.1–5% aromatic heterocyclic modified polypropylene compound, 0–2% nucleating agent, and 0–0.5% antioxidant. The aromatic heterocyclic modified polypropylene compound is obtained by reacting polypropylene with an alkenyl aromatic heterocyclic compound, wherein the heteroatoms on the aromatic heterocycles are oxygen, sulfur, or selenium. This approach allows the aromatic heterocyclic units responsible for trapping charge carriers to be chemically bonded to the polypropylene backbone.
[0009] In this scheme, the amount of the aforementioned functional motif is determined by two parameters, the range of which is described in the literature as follows: graft unit content 0.1–40 wt%, and aromatic heterocyclic modified polypropylene compound content 0.1–5%. The composite material disclosed in this literature also contains two other components: a cyclic olefin copolymer and a nucleating agent. The literature does not describe the distribution of the aforementioned aromatic heterocyclic motif in the crystalline, amorphous, and two-phase interfaces of the composite material, nor does it describe the effect of the addition of the nucleating agent on this distribution. Since the aromatic heterocyclic motif is chemically bonded to the polypropylene backbone, its final location in the matrix tends to be determined along with the polypropylene crystallization process, rather than constituting an independently achievable quantity. Correspondingly, when the crystalline state of the matrix changes due to variations in the amount of crystallization-regulating components in the formulation or molding conditions, the relative content of this motif in each phase region also tends to change accordingly.
[0010] Chinese invention patent application CN122502763A, published on August 4, 2026, discloses a heat-resistant polypropylene capacitor film. Claim 1 describes a composition comprising 70-85 parts of highly crystalline homopolymer polypropylene, 8-12 parts of a cycloolefin copolymer, 0.5-2 parts of poly(3-hexylthiophene), and 0.1-0.6 parts of a nucleating agent. The specification states that the nucleating agent promotes the formation of a fine and uniform crystal structure in the highly crystalline homopolymer polypropylene, and that the poly(3-hexylthiophene) optimizes the dielectric properties of the film. This document describes these two as two parallel pathways, without describing the effect of the crystallization process on the distribution of poly(3-hexylthiophene) in different phase regions of the matrix.
[0011] Chinese invention patent application CN121271089A, published on January 6, 2026, discloses a polypropylene composite particle and a polypropylene capacitor film made therefrom. The raw materials for its preparation, by mass percentage, include 89%–98% polypropylene resin, 2%–10% high melt strength polypropylene, 0.03%–0.08% nucleating agent, 0.3%–0.5% antioxidant, and 0.03%–0.05% calcium stearate. This document states that capacitor film breakdown mainly occurs in the amorphous region; and based on this, by introducing a nucleating agent, the polypropylene achieves higher crystallinity under the same process parameters. Simultaneously, the long-branched structure of the high melt strength polypropylene is inserted into the amorphous region of the polypropylene to suppress the movement of molecular chains in that region. However, this document does not specify the required content of the component with charge carrier trapping function in the amorphous region.
[0012] Of the three documents mentioned above, the first document describes the chemical grafting of aromatic heterocyclic units onto the polypropylene backbone; the second document describes two pathways: nucleating agents and poly(3-hexylthiophene); and the third document describes that breakdown mainly occurs in the amorphous region, and accordingly introduces nucleating agents and high melt strength polypropylene. Regarding the components responsible for carrier capture in these three documents, the quantities described are the type and amount of the component; however, none of the three documents describe the proportion of this component in the crystalline region, the amorphous region, and at the interface with the heat-resistant second phase.
[0013] Therefore, in the production of ultrathin capacitor films with a thickness of 2μm to 3μm, what is actually needed is a masterbatch that can improve the heat resistance of the matrix at high temperatures without introducing inorganic rigid defect sources, improve the interfacial bonding between polypropylene and the heat-resistant second phase, and ensure that the basic units responsible for carrier capture reach a set content in the phase region through which the carriers actually pass inside the film, and that this content remains stable when the film crystallinity fluctuates within the range allowed by production. Summary of the Invention
[0014] Purpose of the invention The purpose of this invention is to address four problems existing in the production and use of ultrathin capacitor films: limited heat resistance of conventional homopolymer polypropylene, defects formed by inorganic heat-resistant fillers during ultrathin stretching, limited compatibility between polypropylene and cyclic olefin copolymers, and uncontrolled distribution of functional components within the membrane phase region leading to batch-to-batch variations in electrical performance. This invention provides a high-performance polypropylene masterbatch for ultrathin capacitor films and its preparation method. It does not introduce inorganic rigid fillers, but uses cyclic olefin copolymers and organic functional components for synergistic modification. This improves the heat resistance of the matrix at high temperatures, suppresses dielectric loss and leakage current under high-temperature conditions, and is compatible with existing biaxial stretching production lines, while also improving two-phase compatibility. Of the four issues mentioned above, the first three are directly achieved by the solution of this invention: no inorganic rigid fillers are introduced, thus avoiding molding defects during ultrathin stretching; the cyclic olefin copolymer improves the heat resistance of the matrix; and delivery in masterbatch form ensures compatibility with existing biaxial stretching production lines. The fourth issue lacks a solution in the prior art, and the effects corresponding to the first three issues can only be stably reproduced between batches using this method. Therefore, the technical problem to be solved by this invention is derived from the fourth item, the content of which is as follows.
[0015] The technical problem that the invention aims to solve The technical problem to be solved by this invention is as follows.
[0016] In a polypropylene functional masterbatch for capacitor films comprising a polypropylene matrix, a heat-resistant cyclic olefin copolymer dispersed phase, and an organic functional component, how can the organic functional component be made to: on the one hand, homologous with the polypropylene matrix through its olefin segments, thus preventing the formation of enriched domains in the composition with an equivalent diameter exceeding a given upper limit d_max; on the other hand, ensuring that the ratio of the mass fraction of its aromatic ring end groups in the amorphous region and at the interface between the polypropylene / cyclic olefin copolymer phases to the average mass fraction of the end groups in the masterbatch, i.e., the enrichment factor f, is not lower than a given lower limit f_min; and when the crystallinity of the composition varies within a given range [Xc1, Xc2], the relative change rate of f |Δf| / f does not exceed a given tolerance ε, so that the distribution of aromatic ring units responsible for carrier trapping in the actual carrier transport channels is no longer passively determined by the crystallization behavior of the matrix.
[0017] The symbols in the above technical problems are interpreted as follows in this invention. The upper limit d_max is taken as the equivalent diameter of the dispersed phase of the cyclic olefin copolymer, that is, the equivalent diameter of the enriched domains of the organic functional component shall not exceed the equivalent diameter of the dispersed phase of the cyclic olefin copolymer in the same composition. The lower limit f_min is taken as 1.5. The interval [Xc1, Xc2] is taken as 50% to 60% crystallinity. The tolerance ε is not given separately, and its meaning is embodied by the following condition: the enrichment factor f is not lower than the lower limit f_min at each point in the crystallinity interval, so the value of f in this interval is limited to f_min and the geometric upper bound corresponding to the interval, and its relative change is thus constrained by the condition itself. The above-mentioned d_max, f_min and [Xc1, Xc2] are the preferred landing points under the film-forming conditions described in this specification; the four conditions defined in claim 1 are the structural prerequisites for the landing points to be established, that is, the necessary technical features of the present invention, and are not limited to the specific values of the above-mentioned landing points.
[0018] Technical solution A first aspect of the present invention provides a high-performance polypropylene masterbatch for ultrathin capacitor films, comprising a polypropylene carrier resin, a cyclic olefin copolymer, and organic functional components.
[0019] The organic functional component is the component in this masterbatch that bears the electrical properties of the film. The organic functional component is an independent molecule that does not form chemical bonds with the molecular chains of the polypropylene carrier resin. This independent molecule consists of olefin segments homologous to the polypropylene carrier resin and aromatic ring groups attached to one end of the olefin segments. The aromatic ring groups are composed of carbon and hydrogen. Homologousity refers to the olefin segments being saturated polyolefin segments composed only of carbon and hydrogen, which are miscible with the polypropylene carrier resin in the melt and entangle with the molecular chains of the carrier resin. This homologousness allows the independent molecule to dissolve in polypropylene during the melt blending stage, thus dispersing the component in molecular form within the polypropylene in the masterbatch; the undissolved and aggregated portion is limited by the following mass fraction. The aromatic ring group is attached to only one end of the olefin segment, so the molecule has a free end homologous to the polypropylene carrier resin. When it is discharged from the crystallization front, it is anchored to the polypropylene matrix with the free end and the aromatic ring group points to the amorphous phase and the interface between the two phases. The group arrives at the molecule's landing point along with the entire molecule, and the phase region it is in is therefore the same as the molecule's landing point.
[0020] The aromatic ring groups function to capture charge carriers migrating in the amorphous phase, thereby suppressing dielectric loss and leakage current of the film under high-temperature conditions. Breakdown and charge carrier transport in polypropylene capacitor films mainly occur in the amorphous phase and at the two-phase interface. In the crystalline phase, the molecular chains are densely packed with small free volumes, making it difficult for charge carriers to pass through. Therefore, aromatic ring groups residing on lamellar folds or aggregated within enriched domains have a lower probability of encountering charge carriers than those located in the amorphous phase and at the two-phase interface. The actual capture contribution of the same number of aromatic ring groups varies depending on their location within the phase region. The limitations of this invention refer to the specific location, not the total number of these groups. Furthermore, when one end of the independent molecule is an olefin segment homologous to the polypropylene carrier resin and the other end is the aromatic ring group, and it resides at the interface between the polypropylene and cyclic olefin copolymers, the molecule spans both sides of the interface, forming a molecular-level connection. This reduces defects at the two-phase interface, and the interfacial polarization at the interface under high-frequency and high-temperature conditions is subsequently suppressed. Therefore, the organic functional component plays a dual role in this invention: it captures charge carriers at its landing point and improves the two-phase interface between polypropylene and cyclic olefin copolymer at the same landing point.
[0021] The offset is a factory acceptance indicator that can be measured in the laboratory after the masterbatch is manufactured. The offset of the differential scanning quanta (DSQ) melting peak temperature of the masterbatch relative to the DQ of the polypropylene carrier resin itself is within 1°C. This offset is a criterion for whether the aromatic ring groups participate in the polypropylene lattice construction: if the aromatic ring groups participate in the lattice construction, they act as defects in the lattice, reducing the perfection of the formed lamellar crystals, and the melting peak temperature of the polypropylene will shift accordingly; if the offset falls within the above range and is confirmed by differential verification of the following control masterbatch to be caused by the organic functional components, it can be determined that the independent molecules have not entered the growing lamellar crystals in a proportion sufficient to change the perfection of the lamellar crystals; those that have not entered the lamellar crystals are therefore discharged by the advancing crystallization front to the side of the uncrystallized melt, and their subsequent destination is determined and closed by the following remaining items. The 1℃ and 0.5℃ are set limits, and their values are significantly greater than the range of melting peak temperatures obtained by repeatedly measuring the same sample according to the measurement procedure described in this specification. Therefore, the offset exceeding these limits can be determined as a true shift in melting peak temperature rather than a measurement fluctuation. The cyclic olefin copolymer, the antioxidant system, the lubricant, and the compatibilizer when the masterbatch further includes the following reactive compatibilizer also contribute to the melting peak temperature. This contribution is measured by the difference in melting peak temperature between the control masterbatch with the same formulation but without the organic functional component and P. The offset is determined after deducting this contribution. If necessary, a control masterbatch with the same formulation but without the organic functional component can be prepared separately, and the above attribution can be verified by the difference in the differential scanning calorimetry melting peak temperature between the masterbatch and the control masterbatch. Thus, the distribution of the aromatic ring groups after film formation is no longer an average distribution result obtained by mass in each phase region. The mass fraction of this group at the interface between the amorphous phase and the polypropylene and cyclic olefin copolymer phases can be higher than its average mass fraction in the film.
[0022] The weight-average molecular weight range refers to the material selection requirements for this component before feeding. The weight-average molecular weight of the independent molecule is greater than the entanglement molecular weight of the polypropylene carrier resin, but less than the weight-average molecular weight of the polypropylene carrier resin. Each end of this range plays a specific role. The upper end is given by the weight-average molecular weight of the carrier resin: the self-diffusion coefficient of the molecule in the melt decreases as its weight-average molecular weight increases. Molecules with a weight-average molecular weight not less than that of the carrier resin are insufficient to leave the vicinity of the crystallization front during the time they take to advance at the crystallization front, and will be embedded in situ by the growing lamellar crystals, with their aromatic ring groups remaining on the lamellar fold surfaces. The lower end is given by the entanglement molecular weight of the carrier resin: molecules with a weight-average molecular weight not greater than this entanglement molecular weight do not form entanglements with the polypropylene molecular chains in the amorphous phase. Although these molecules are also expelled by the crystallization front, they can continue to migrate after expulsion. During the heat setting after biaxial stretching and the subsequent thermal process, the crystallinity of the matrix continues to increase, the volume of the amorphous phase continues to shrink, and the molecules that are not locked by entanglement will continue to be displaced until they aggregate into domains or migrate to the surface of the film. Molecules falling within the aforementioned range have a self-diffusion coefficient sufficient to complete migration within the timescale of the crystallization front advancement. Furthermore, upon reaching the amorphous phase between lamellar crystals and the two-phase interface, they are locked by entanglement and are no longer redistributed with changes in matrix crystallinity. The ratio of the mass fraction of the aromatic ring group in the amorphous phase and the two-phase interface to its average mass fraction in the film remains above a set lower limit when the matrix crystallinity varies within a certain range.
[0023] The mass fraction is the upper limit of the amount of this component in the formulation, which is determined by observing the cross-sectional morphology after the masterbatch is made. The mass fraction of the organic functional component ensures that the equivalent diameter of the enriched domains formed by the independent molecules in the masterbatch is smaller than the equivalent diameter of the dispersed phase of the cyclic olefin copolymer. The concentration of molecules discharged from the crystallization front in the amorphous phase increases proportionally to the shrinkage of the amorphous phase volume with the increase of matrix crystallinity; when this concentration exceeds the solubility limit of the molecule in amorphous polypropylene, the excess portion precipitates from the amorphous phase and aggregates into independent enriched domains, and the aromatic ring groups aggregated within these domains subsequently exit the carrier transport channels. The equivalent diameter of the dispersed phase of the cyclic olefin copolymer is used as the upper limit of the equivalent diameter of the enriched domains, making this upper limit a reference quantity inherent within the same composition that can be directly compared on the same sample under the same sample preparation conditions and the same magnification.
[0024] All the above limitations apply to the same independent molecule and share the same weight-average molecular weight: this weight-average molecular weight determines both the self-diffusion coefficient, thus determining the landing point of the molecule after it is expelled, and the solubility limit of the molecule in amorphous polypropylene, thus determining the upper limit of the mass fraction—the solubility limit of the same type of molecule decreases with increasing weight-average molecular weight because the entropy of mixing decreases with increasing chain length. The aromatic ring group reaches its landing point, determined by both the offset and the weight-average molecular weight; the group remains dispersed at the landing point, determined by the mass fraction. The two-end range of the weight-average molecular weight can be set independently on the masterbatch itself and is independent of downstream film-forming conditions; the landing point condition expressed below as the ratio of self-diffusion coefficient to crystal growth rate is a direct expression of this range under given cooling conditions. These are not two ways of writing the same condition; the latter further limits the former.
[0025] The mechanism by which the aromatic ring group reaches its destination is the crystallization growth front of the polypropylene matrix itself. The migration characteristic of this molecule after it is expelled is the ratio of its self-diffusion coefficient in the melt to the matrix crystallization growth rate; wherein the crystallization growth rate is given by the cooling and heat-setting conditions during film formation, and the self-diffusion coefficient is given by the weight-average molecular weight of the individual molecules. This invention sets the condition for achieving the above ratio on one side of the ratio that can be given by the masterbatch itself, namely the self-diffusion coefficient side; it does not limit the crystallization growth rate side, so that when the crystallization growth rate varies within the range given in the film formation process, the ratio still falls within the required range.
[0026] When the thickness of the thin film is on the order of several spherulite characteristic dimensions, the number of spherulite layers contained in the film thickness direction is limited. A single aggregation of functional components at the spherulite boundary can penetrate a considerable proportion of the film thickness in the thickness direction. The quantities defined in the above-mentioned limitations are the ratio of the mass fraction of the aromatic ring group in the phase region where the actual carrier transport channel is located to its average mass fraction in the film, rather than the average content of the component in the film itself.
[0027] The reactive compatibilizer is used to solve the practical problem of phase separation and delamination on the biaxial stretching production line. In a preferred embodiment, the masterbatch further includes a reactive compatibilizer, which is a polypropylene-grafted cyclic olefin copolymer. Its molecule contains both polypropylene segments homologous to the polypropylene carrier resin and cyclic olefin segments homologous to the cyclic olefin copolymer. During melt blending, the compatibilizer is enriched at the interface between the polypropylene and cyclic olefin copolymer phases. Its two types of segments extend into both phases and become entangled with the molecular chains of both phases, thus strengthening the interfacial bonding between the two phases. On the one hand, the dispersed phase of the cyclic olefin copolymer is refined during mixing, and its equivalent diameter decreases accordingly. On the other hand, during the longitudinal and transverse stretching of the biaxial stretching process, the two phases do not separate or delaminate due to insufficient interfacial bonding. After film formation, interfacial defects at the phase interface are reduced, and the interface can thus serve as a continuous phase region to support the aromatic ring groups.
[0028] The compatibilizer and the organic functional component complement each other at the interface between the two phases: the latter, with its polypropylene affinity at one end and an aromatic ring group at the other, spans both sides of the interface, forming a molecular-level connection; the former, with its two types of chain segments, extends into the two phases and entangles with the molecular chains of the two phases, further strengthening the bonding at the interface. The compatibilizer refines the dispersed phase of the cyclic olefin copolymer and reduces its equivalent diameter, which is precisely the upper limit of the equivalent diameter of the enriched domains. Therefore, the fourth limitation mentioned above becomes stricter after the addition of the compatibilizer; the present invention still makes the equivalent diameter of the enriched domains smaller than this upper limit even under this stricter reference amount. The compatibilizer does not change the mechanism by which the aromatic ring group is ejected and positioned by the crystallization front, so it is a preferred but not necessary technical feature.
[0029] A second aspect of the present invention provides a method for preparing the above-mentioned masterbatch, wherein each step corresponds to the above-described limitations, including: premixing a polypropylene carrier resin, a cyclic olefin copolymer, an organic functional component, and optionally a reactive compatibilizer, an antioxidant, and a lubricant, such that the components achieve macroscopic homogeneity before entering the melting section; melt extrusion, wherein the olefin segments of the individual molecules entangle with the molecular chains of the polypropylene carrier resin in the melt, thereby dispersing the component in molecular form within the polypropylene; the melt extrusion is performed in a mixture composed of a combination of weak shear elements and medium shear elements. The process is carried out in the refining stage, which fully plasticizes and disperses the material while preventing the cyclic olefin copolymer and the organic functional components from degrading due to shear heat, and allows the independent molecules to fully wet the interface between the polypropylene and the cyclic olefin copolymer in the melt; multi-stage vacuum devolatilization removes volatiles and low molecular weight substances that are not entangled with the matrix from the melt; cooling and pelletizing complete the crystallization of the masterbatch stage before the independent molecules aggregate; drying and curing release the residual stress and residual volatiles inside the pellets, and the offset and the equivalent diameter of the enriched domains are maintained during subsequent storage, transportation and blending.
[0030] A third aspect of the invention provides the application of the above-mentioned masterbatch in the preparation of biaxially oriented polypropylene capacitor films with a thickness of 2 μm to 3 μm, wherein the masterbatch is blended into a polypropylene matrix resin at a ratio of 2 wt% to 6 wt%, and the capacitor film is obtained by biaxial stretching. The masterbatch here serves as a concentrated delivery carrier: the individual molecules are already dispersed in the polypropylene in molecular form within the masterbatch, undergoing only one dilution during blending; the cooling crystallization during film formation constitutes another, and decisive, expulsion and placement of the individual molecules, where the final distribution of the aromatic ring groups is completed.
[0031] Based on this, the present invention may further include the following preferred technical solutions: the offset is within 0.5°C; the weight loss rate of the masterbatch after reflux extraction in n-heptane, minus the weight loss rate of a control masterbatch with the same formulation but without the organic functional component, whose reduced mass fraction is supplemented by the polypropylene carrier resin after reflux extraction under the same conditions, plus the product of the mass fraction of the organic functional component and the weight loss rate of the polypropylene carrier resin after reflux extraction under the same conditions, the resulting value is lower than the mass fraction of the organic functional component in the masterbatch, and the difference between this value and the mass fraction corresponds to the portion of the independent molecules that have formed entanglement with the polypropylene molecular chains and are therefore not extracted; the weight distribution of the independent molecules The ratio of the molecular weight to the weight-average molecular weight of the polypropylene carrier resin is such that the ratio of the self-diffusion coefficient of the individual molecule in the polypropylene carrier resin melt to the crystallization growth rate of the polypropylene carrier resin under the cooling conditions of the masterbatch blending film is greater than the lamellar length period of the polypropylene carrier resin under the cooling conditions, and less than the spherulite radius of the polypropylene carrier resin under the cooling conditions. The lamellar length period is determined by small-angle X-ray scattering, the spherulite radius is determined by polarized light microscopy, and the crystallization growth rate is determined by the growth rate of the spherulite radius over time under polarized light microscopy. When this ratio falls between the two, the expelled molecules cross the scale of the interlamellar amorphous phase but do not reach the scale of the spherulite boundary. The masterbatch is prepared at 2w After being blended into a polypropylene matrix resin at a ratio of t% to 6wt% and biaxially stretched to form a film, the ratio of the mass fraction of the aromatic ring groups at the amorphous phase and the interface between the polypropylene and cyclic olefin copolymer phases of the film to the average mass fraction of the aromatic ring groups in the film is 1.5 or more, and this ratio is 1.5 or more within the range when the crystallinity of the film varies within the range of 50% to 60%. The masterbatch contains, by mass fraction, 55% to 70% polypropylene carrier resin, 15% to 25% cyclic olefin copolymer, 3% to 8% organic functional components, 4% to 9% reactive compatibilizer, and the balance contains 0.8% to 1.8% of an antioxidant system composed of hindered phenolic antioxidants and phosphite antioxidants, as well as fatty acids. The masterbatch contains 0.5%–1.2% ester-based lubricant, and the sum of the mass fractions of all components is 100%; the glass transition temperature of the cyclic olefin copolymer is 130℃–180℃; the reactive compatibilizer is a polypropylene-grafted cyclic olefin copolymer; the polypropylene carrier resin is homopolymer polypropylene with a melt flow rate of 2.5–8 g / 10 min; the premixing is carried out at 60℃–80℃ for 8–12 min; the melt extrusion temperature is 180℃–230℃; the vacuum degree of the multi-stage vacuum devolatilization is below -0.09 MPa, and the relative content of fractions with a weight-average molecular weight lower than the entanglement molecular weight in the devolatilized material is lower than that before devolatilization; the drying and curing is carried out at 80℃ for more than 4 hours.
[0032] The polypropylene carrier resin is a high-crystallinity homopolymer polypropylene with low ash content and low catalyst residue. Its ash content is determined according to GB / T 9345, and it does not introduce migratable metal ions into the masterbatch. The antioxidant system does not contain metal elements. The fatty acid ester lubricant does not migrate or precipitate under the forming conditions of the capacitor film and subsequent vacuum metallization evaporation. The above three points address the same issue: the dielectric properties of the film are not contaminated by metal ions or precipitable substances introduced by the masterbatch. However, these three components themselves do not constitute the control of the endpoint of this invention.
[0033] The beneficial effects of this invention are as follows: Under the condition that the total amount of the organic functional components remains constant, the aromatic ring groups have five possible destinations after film formation: entering the growing lamellar crystals with the independent molecules or remaining on the folded surfaces of the lamellar crystals; entering the dispersed phase of the cyclic olefin copolymer; migrating to the surface of the film as the molecules are further displaced; agglomerating within the enrichment domains; or settling in the amorphous phase between the lamellar crystals and the interface between the two phases. The offset and the upper end of the weight-average molecular weight range close the first destination, the homology between the olefin segment and the polypropylene carrier resin closes the second destination, the lower end of the range closes the third destination, and the mass fraction closes the fourth destination. When all four conditions are met, the vast majority of the aromatic ring groups fall in the amorphous phase between the lamellar crystals and the interface between the two phases. The ratio of their mass fraction at these two locations to their average mass fraction in the film is therefore greater than one but not more than one divided by one minus the difference in crystallinity. This inequality holds true at all points within the crystallinity range. After the masterbatch is blended and formed into a film: the dielectric loss and leakage current of the film under high temperature conditions are suppressed; the presence of the aromatic ring groups at the interface between the two phases reduces the interface defects and suppresses the interface polarization, and the two phases do not separate or delaminate during biaxial stretching; the film does not produce pinholes, crystal points and microcracks due to inorganic rigid fillers; the components of the masterbatch do not migrate or precipitate under film formation and evaporation conditions; and the above properties are maintained when the crystallinity of the film fluctuates, thus reducing the difference in electrical properties between batches.
[0034] The above effects are not a superposition of the various limiting effects, but rather are established by closing one destination for each limiting effect: If the aromatic ring group participates in the lattice construction of polypropylene, or the weight-average molecular weight of the independent molecule is not less than the weight-average molecular weight of the carrier resin, then the first destination is open, and the molecule is in-situ embedded as the lamellar crystals grow, or its aromatic ring group is retained on the lamellar fold surface; if the olefin segment is not from the polypropylene carrier resin, then the second destination is open, and the molecule is instead distributed within the dispersed phase of the cyclic olefin copolymer; if the weight-average molecular weight is not greater than the entanglement molecular weight of the carrier resin, then the third destination is open, and the molecule does not entangle with the polypropylene molecular chains in the amorphous phase, and is subsequently displaced and migrates to the surface of the film during the thermal process; if the mass fraction causes the equivalent diameter of the enriched domain to exceed the equivalent diameter of the dispersed phase, then the fourth destination is open, and the component aggregates within the domain and exits the carrier transport channel. Each of the four destinations is closed by the limiting effect, and the closing methods are different for each other; therefore, the above effects are not a simple superposition of the various limiting effects.
[0035] In a preferred embodiment, the narrowing of the offset, the difference in extraction weight loss rate, the limitation of the migration characteristic scale, and the formulation and preparation conditions enable the above conditions to be repeatedly achieved within a conventional processing window.
[0036] The above effects shall be accepted according to the methods and criteria described in this instruction manual, and the actual measured values shall be determined. Attached Figure Description
[0037] Figure 1 This is a schematic diagram illustrating the mechanism by which the organic functional components of the present invention are sorted and positioned during the crystallization process of the polypropylene matrix; Figure 2 This is a schematic diagram of the molecular structure of the organic functional components of the present invention and the range of their weight-average molecular weights. Figure 3 This is a flowchart of the masterbatch preparation method and acceptance criteria of the present invention; Figure 4 The calculated curve shows the geometric upper bound of the enrichment factor as a function of crystallinity.
[0038] In the figure: 1—polypropylene matrix; 2—cyclic olefin copolymer dispersed phase; 21—two-phase interface between polypropylene and cyclic olefin copolymer; 3—individual molecules of organic functional components; 31—olefin segments; 32—aromatic ring groups; 4—lamellae; 5—amorphous phase between lamellar crystals; 6—spherulite boundary; 7—crystallization growth front; 8—enriched domains; 9—uncrystallized melt. Detailed Implementation
[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The following embodiments and comparative examples are used to illustrate the invention and are not intended to limit the scope of protection of the invention.
[0040] Terminology and Measurement Methods like Figure 2 As shown in this specification, the independent molecule 3 refers to a molecule that does not form chemical bonds with the polypropylene backbone. This molecule is composed of an olefin segment 31 and an aromatic ring group 32 attached to one end of the olefin segment 31. The aromatic ring group 32 is an aromatic ring group composed of carbon and hydrogen. For ease of description, the organic functional component will be referred to as S, and the polypropylene carrier resin as P.
[0041] The differential scanning calorimetry (DSC) melting peak temperature was determined according to GB / T 19466.3-2004. Weigh 5 mg to 10 mg of the sample and place it in an aluminum crucible. Under a nitrogen atmosphere, heat the sample from 40 °C to 200 °C at a rate of 10 °C / min, hold for 5 min to eliminate thermal history, then cool to 40 °C at a rate of 10 °C / min. Subsequently, heat the sample again to 200 °C at a rate of 10 °C / min. The peak temperature of the melting peak on the second heating curve is taken as the DSC melting peak temperature. The same sample is measured three times according to the above procedure, and the arithmetic mean of the three measurements is taken. The range of the three measurements should not exceed 0.2 °C; if it exceeds this range, the measurement should be repeated. The offset is the absolute value of the difference between the DSC melting peak temperature of the masterbatch and the DSC melting peak temperature of P itself, both measured on the same instrument using the same procedure. The boundaries between 1℃ and 0.5℃ are both more than twice the aforementioned range, so any offset falling outside these boundaries is a discernible real movement.
[0042] Crystallinity was determined separately from the determination of the melting peak temperature as described above: 5 mg to 10 mg of the sample was placed in an aluminum crucible and heated from 40 °C to 200 °C at a rate of 10 °C / min under a nitrogen atmosphere. The enthalpy of fusion of the melting peak on the first heating curve was recorded. Using the enthalpy of fusion of fully crystalline polypropylene (209 J / g) as a reference, the crystallinity was equal to the ratio of the sample's enthalpy of fusion to this reference value. This determination did not include a isothermal step to eliminate thermal history, thus the obtained crystallinity reflects the actual crystallization state of the sample after its thermal history. The determination of the melting peak temperature, however, used a second heating curve to compare the masterbatch with P in a comparable state after eliminating thermal history.
[0043] Weight-average molecular weight was determined by high-temperature gel permeation chromatography with 1,2,4-trichlorobenzene as the mobile phase and a column temperature of 150 °C. The column was calibrated using narrow-distribution polystyrene standard samples.
[0044] The entangled molecular weight was determined using the rheological plateau modulus method. A dynamic frequency scan of P was performed above its melting temperature. The storage modulus of the plateau region on the storage modulus versus frequency curve was taken as the plateau modulus. The entangled molecular weight was equal to the product of the density of P at that temperature, the gas constant, and the absolute temperature, divided by the plateau modulus.
[0045] Melt flow rate was determined according to GB / T 3682 at 230℃ and 2.16 kg. The glass transition temperature of the cyclic olefin copolymer was read by midpoint method on the double-heating curve according to the above differential scanning calorimetry program.
[0046] The weight loss rate of n-heptane reflux extraction was determined as follows. Approximately 2 g of the sample, accurate to 0.1 mg, was weighed and recorded as m0. It was placed in the filter paper thimble of a Soxhlet extractor and refluxed with n-heptane as solvent for 6 hours. After extraction, it was dried under vacuum at 105 °C to constant weight and recorded as m1. The weight loss rate was equal to the difference between m0 and m1 divided by m0. The weight loss rates of the following two samples were also measured using the same procedure: one was a control masterbatch, whose formulation and preparation conditions were the same as the tested masterbatch, except that it did not contain sulfur (S). The reduced mass fraction was compensated by phosphorus (P) to ensure that the sum of the mass fractions of all components remained 100%; the other was P itself. The weight loss rates of the tested masterbatch, control masterbatch, and P were recorded as L, L0, and Lp, respectively. The mass fraction of S in the tested masterbatch was wS. The corrected difference in weight loss rates ΔL = L - L0 + wS·Lp. The rationale for this correction is as follows: the contributions of the antioxidant system, lubricant, and reactive compatibilizer under these extraction conditions are the same in both the tested and control masterbatches, and thus cancel each other out when the difference is calculated; however, the control masterbatch contains more P than the tested masterbatch, and the contribution of the extractable portion of this P to L0 is wS·Lp, which must be added back. Therefore, ΔL is the mass fraction of S that has not yet been entangled and locked, and thus can be extracted.
[0047] The equivalent diameter of enriched domains and the equivalent diameter of the cyclic olefin copolymer dispersed phase were determined using the following method. The same sample was frozen in liquid nitrogen and then fractured to obtain two cross-sections. The first cross-section was immersed in n-heptane at 25°C for 30 min, dried, sputter-coated with gold, and imaged under a scanning electron microscope. This step selectively dissolved the S-enriched domains exposed on the cross-section, leaving pits in situ. The pits in the resulting image represent the morphology of the S-enriched domains. The second cross-section was immersed in cyclohexane at 60°C for 60 min, dried, sputter-coated with gold, and imaged at the same magnification. This step selectively dissolved the cyclic olefin copolymer dispersed phase exposed on the cross-section. The pits in the resulting image represent the morphology of the dispersed phase. Since both cross-sections were taken from the same sample, fractured in the same manner, and imaged at the same magnification, the equivalent diameters of the two types of domains could be directly compared. The selectivity of the above two steps should be determined first: The cross-section of a control masterbatch with the same formulation but without sulfur is treated in the second step; the resulting pits are purely cyclic olefin copolymer dispersed phase. The cross-section of a control masterbatch with the same formulation but without cyclic olefin copolymer is treated in the first step; the resulting pits are purely S-enriched domains. The equivalent diameter distribution of the pits obtained from the two controls is the interpretation criterion for this determination. The projected area of each domain is measured using image analysis software, and the diameter of the circle with the same area is taken as the equivalent diameter of that domain. For each sample and each type of domain, if the number of observed domains is not less than 200, the average number is taken as the equivalent diameter of that type of domain; if the number of observed domains is less than 200 but more than zero, the average number of all observed domains is taken as the equivalent diameter of that type of domain, and the number of observed domains is noted in the report. For samples with a total observed area of not less than 10 random fields of view and not less than 1000 μm... 2 If no S-enriched domains are observed within the specified range, it is denoted as "no S-enriched domains observed". In this case, S has not formed measurable enriched domains, and its equivalent diameter is considered to be zero, which is naturally smaller than the equivalent diameter of the cyclic olefin copolymer dispersed phase.
[0048] The long period of lamellar crystals is determined by small-angle X-ray scattering. The long period is equal to 2π divided by the value of q, which corresponds to the peak position on the one-dimensional correlation function or scattering intensity versus scattering vector curve. The spherulite radius and crystal growth rate are determined by a polarizing microscope hot stage: a thin sample is melted on a glass slide and then cooled and crystallized under orthogonal polarization at a cooling rate closest to the cooling rate of the film formation process within the controllable range of the hot stage. The radius of the same spherulite is recorded at equal time intervals. The radius is plotted against time, and the slope of the linear segment is taken as the crystal growth rate under the cooling condition. Half the diameter of the spherulite when it stops growing is taken as the spherulite radius. The cooling rate used should be noted when reporting the results. This cooling condition is an executable approximation of the cooling conditions of the film formation process in the laboratory. The crystal growth rate and spherulite radius used in the comparison according to claim 4 are all taken from the same measurement. The lamellar crystal long period, the spherulite radius, and the crystal growth rate are all measured on the sample under the same cooling condition. The self-diffusion coefficient of the independent molecule in the polypropylene carrier resin melt is determined by pulsed gradient field nuclear magnetic resonance at the same temperature used to determine the crystal growth rate; alternatively, it can be calculated from the weight-average molecular weight of the molecule according to the calibration relationship between the self-diffusion coefficient and weight-average molecular weight of similar molecules in the melt, which is obtained by actual measurement of a group of similar molecules with known weight-average molecular weights at the same temperature.
[0049] The enrichment factor f is defined and determined as follows. f is the ratio of the mass fraction of the aromatic ring group at the interface between the amorphous phase and the two phases in the film to its average mass fraction in the film. This quantity must be determined by a method that does not destroy the original phase morphology: any fractionation method that first dissolves the entire sample and then reprecipitates it will only reflect the solubility and crystallinity of each component, and is unrelated to the phase region in which the component is located in the original film, and is therefore not applicable to this invention. This invention uses the following selective etching method for determination. Three parallel samples are cut from the same film: the crystallinity of the first sample is determined by the above method and denoted as Xc; the second sample is dissolved in 1,2,4-trichlorobenzene at 135°C and its integrated area of aromatic hydrogens is determined by nuclear magnetic resonance hydrogen spectroscopy and its mass is normalized to obtain the mass fraction of aromatic hydrogens in the film, denoted as w0; the third sample is weighed and denoted as m0, for use in the following etching. A third sample was treated at room temperature with a permanent etchant (prepared from potassium permanganate dissolved in a mixture of concentrated sulfuric acid and orthophosphoric acid) used in the art for revealing the lamellar morphology of polypropylene. This etchant preferentially erodes the amorphous phase and the material at the phase interface of polypropylene while essentially not eroding the lamellar crystals. The sample was removed at regular intervals, washed sequentially with a dilute hydrogen peroxide-dilute sulfuric acid aqueous solution and deionized water, vacuum dried at 60°C to constant weight, and weighed. Etching was stopped when the cumulative weight loss of the sample equaled the product of m0 and (- minus Xc). The remaining solid was recorded as fraction B, with a mass of Xc·m0. The etchant erodes the amorphous phase and the material at the phase interface at a higher rate than it erodes the lamellar crystals; therefore, the removed material is mainly the amorphous phase of the film and the material at the two-phase interface. The obtained f is the apparent value under these etching conditions, and its endpoint must first be calibrated by treating a control film without S using the same method. Fraction B was dissolved in 1,2,4-trichlorobenzene at 135℃, and its integral area of aromatic hydrogens was determined by 1H NMR spectroscopy. The mass of aromatic hydrogens in fraction B was normalized to obtain the mass fraction of aromatic hydrogens, denoted as w2. The mass fraction of aromatic hydrogens removed by etching, w1, was obtained from the mass balance equation w0·m0 = w1·(1-Xc)·m0 + w2·Xc·m0. Therefore, the enrichment factor f = w1 / w0 = [1 - (w2 / w0)·Xc] ÷ (1 - Xc). The two limits of this equation can be used for verification: when the aromatic ring groups do not enter the crystalline phase at all, w2 = 0, f = 1 / (1 - Xc), i.e., the geometric upper bound; when the aromatic ring groups are uniformly distributed in each phase region, w2 = w0, f = 1. The above determination only quantifies the two complete samples, the original film and the etched residual solid, and does not require the recovery of the etched material. Whether the etching process affects the chemical structure of the removed material does not affect the determination result of f. However, if the aromatic ring in the residual solid is oxidized under the etching conditions, w2 will be lower and f will be higher. The obtained f is an upward biased estimate in this direction. This bias should be calibrated and deducted by treating the control film without S in the same way.If the mass fraction of aromatic hydrogens in the membrane is lower than the quantitative limit of 1H NMR spectroscopy, the above determination can be performed on a membrane prepared with the same masterbatch at a blending ratio of 6 wt% under the same film-forming conditions. The obtained f is applicable to the positional state of the same masterbatch at that crystallinity. The four conditions defined in claim 1 are accepted by criteria one to four on the masterbatch, independent of the determination of the enrichment factor. If it is necessary to convert to a number density ratio per unit volume, the number density ratio is equal to the mass fraction ratio multiplied by the ratio of the amorphous phase density to the average density of the membrane; since the amorphous phase density of semi-crystalline polypropylene is lower than its crystalline phase density, the multiplier is not greater than one, and the number density ratio per volume is not higher than the above ratio per mass. All limitations and acceptance criteria of this invention are based on the above ratios per mass.
[0050] The dielectric loss of the thin film was determined according to GB / T 1409 at the stated temperature and frequency. The leakage current of the thin film was determined according to GB / T 1410 at the stated temperature and electric field strength, and its volume current density was determined. The interfacial polarization of the thin film was characterized by dielectric spectrum, and the changes in dielectric constant and dielectric loss with frequency were measured at the stated temperature in the range of 0.1 Hz to 1 MHz. The peak height of the loss peak appearing in the low-frequency range was taken as a measure of the degree of interfacial polarization. The two-phase separation and delamination of the thin film were characterized by scanning electron microscopy observation of the cross-section of the film after biaxial stretching, and the value was taken per 1000 μm. 2 The number of two-phase delamination points appearing on the cross-section is used as its measurement. Pinholes, crystal points, and microcracks in the film are counted according to GB / T 13542.2, expressed as the number per square meter. The migration and precipitation of each component of the masterbatch are characterized by scanning electron microscopy counting of precipitates on the film surface after vacuum metallization deposition and coating adhesion. The breakdown field strength of the film is determined according to GB / T 1408.1 in power frequency AC, flat electrode, and transformer oil using a uniform voltage increase method, taking the ratio of breakdown voltage to sample thickness. At least 10 points are measured for each sample, and the median value is taken. The long-term safe operating temperature of the film is the upper limit corresponding to the temperature at which the film retains at least 80% of its initial breakdown field strength after 1000 hours of thermal aging. All samples used for the above measurements are biaxially oriented polypropylene capacitor films prepared according to the film formation conditions described in this specification.
[0051] Definition and acceptance of organic functional components like Figure 3 As shown, S is accepted according to the following four criteria in sequence. The specific chemical type and source of S are selected by the implementer according to the following criteria; the simultaneous satisfaction of the following four criteria is a condition for S to be used in this invention.
[0052] Criterion 1 is the structural criterion. Using 1H and 1C NMR spectra, it is confirmed that the molecule of S consists of an olefin segment and an aromatic ring group attached to one end of that olefin segment. It is confirmed that the aromatic ring group is composed only of carbon and hydrogen, and that no chemical shift signals characteristic of heteroatom-substituted aromatic rings appear in the spectra. Furthermore, it is confirmed that the olefin segment is a saturated polyolefin segment composed only of carbon and hydrogen. The aromatic ring group should only be attached to one end of the olefin segment; that is, the molecule should have one free end without an aromatic ring group. A molecule with aromatic ring groups at both ends does not meet this criterion. The requirement that S and P do not form a chemical bond is verified as follows: Dissolve the prepared masterbatch in 1,2,4-trichlorobenzene at 135°C, cool to 25°C, and then fractionate by precipitation with n-heptane. If S and P do not form a chemical bond, they can be separated into two fractions, and the 1H NMR spectra of the two fractions will only show the characteristic signals of P and S, respectively. If they have formed a chemical bond, they cannot be separated in this way. This fractionation is only used to determine whether a chemical bond exists and is not used to determine the enrichment factor described below. Regarding the requirement that the olefin segment is homologous to P, this is verified by the above-mentioned determination of the weight loss rate during n-heptane reflux extraction: If the corrected weight loss rate difference of the prepared masterbatch is lower than the mass fraction of S in the masterbatch, it indicates that a portion of S has dissolved in P and formed entanglement with the molecular chain of P.
[0053] Criterion two is the molecular weight criterion. The entangled molecular weight and weight-average molecular weight of P are determined using the method described above, and the weight-average molecular weight of S is also determined. The weight-average molecular weight of S should be greater than the entangled molecular weight of P and less than the weight-average molecular weight of P.
[0054] Criterion three is the lattice exclusion criterion. The differential scanning calorimetry melting peak temperature of the prepared masterbatch and P is measured using the method described above; the offset should be within 1°C. If necessary, a control masterbatch with the same formulation but without S is prepared using the method described above, and its melting peak temperature is measured. The difference between the prepared masterbatch and the control masterbatch is used to verify that the offset is indeed caused by S.
[0055] Criterion four is the dispersion criterion. The equivalent diameter of the S-enriched domains in the prepared masterbatch, measured using the above method, should be smaller than the equivalent diameter of the cyclic olefin copolymer dispersed phase. A result recorded as "no S-enriched domains observed" according to the above method is considered to satisfy this criterion. In the scheme using the aforementioned reactive compatibilizer, the cyclic olefin copolymer dispersed phase is refined due to the action of the compatibilizer, and its equivalent diameter is smaller than that without the compatibilizer; therefore, this criterion is correspondingly stricter in this scheme.
[0056] Criteria 1 and 2 are used to inspect the raw materials themselves before feeding, while Criteria 3 and 4 are used to inspect the masterbatch after it is made. If Criteria 3 or 4 fails to meet the requirements, the following adjustments should be made: If the deviation exceeds 1°C, it indicates that the aromatic ring group has participated in the lattice construction of polypropylene, and S should be replaced; if the equivalent diameter of the enriched domains is not less than the equivalent diameter of the dispersed phase of the cyclic olefin copolymer, it indicates that the mass fraction of S has exceeded its dispersion limit in the system, and the mass fraction of S should be reduced in increments of 1% from the current value, with the reduced mass fraction being made up by the polypropylene carrier resin. A new sample should be prepared and inspected, and the maximum value that still meets Criteria 4 should be taken as the upper limit of the mass fraction of S in the system.
[0057] Examples of available varieties of S are as follows. Any molecule that simultaneously meets the above four criteria can be used in this invention. One type that can be directly selected is a saturated polyolefin molecule with a single benzene ring or a fused aromatic ring attached to one end: the aromatic ring group consists only of carbon and hydrogen, and its volume is much smaller than the olefin chain segment to which it is attached. Therefore, the solubility limit of this molecule in amorphous polypropylene is relatively high, and the margin of criterion four is relatively large. This type of product can be obtained by anionic polymerization of conjugated dienes initiated by an organolithium initiator with the aromatic ring group, followed by selective hydrogenation of the diene segments. The aromatic ring group of the initiator is located at one end of the resulting molecule. Its number-average molecular weight is given by the molar ratio of monomer to initiator during polymerization. The weight-average molecular weight is determined by the above method and selected according to criterion two, with its weight-average molecular weight falling between the entangled molecular weight of P and the weight-average molecular weight of P. The hydrogenated polyisoprene segments obtained after hydrogenation are segments with alternating ethylene and propylene units, and the hydrogenated polybutadiene segments are segments with randomly connected ethylene and butene units. Both are saturated polyolefin segments composed only of carbon and hydrogen, and are homologous to homopolymer polypropylene, which is the carrier resin, i.e., the olefin segments. The residual hydrogenation catalyst used in the preparation of this type of product should be removed to prevent the introduction of migratable metal ions into the masterbatch. This type of molecule can also be prepared by adding a polyolefin with an unsaturated end group to a derivative of the aromatic ring via an addition reaction. Molecules with aromatic ring groups at both ends are not considered independent molecules as described in this invention, nor do they satisfy criterion one: the molecule lacks a free end without an aromatic ring group, and in the melt, it cannot be anchored at one end to the polypropylene matrix while the aromatic ring group points towards the amorphous phase and the interface between the two phases. The volume of the aromatic ring group should be much smaller than the olefin segment it is attached to; molecules containing a complete aromatic ring homopolymer segment have a significantly reduced solubility limit in amorphous polypropylene, making criterion four difficult to meet.
[0058] Example 1: Best Practice This embodiment is the best implementation of the present invention.
[0059] Raw materials: P is a high-crystallinity homopolymer polypropylene with low ash content and low catalyst residue, with a melt flow rate of 2.5 g / 10 min and ash content determined according to GB / T 9345; the glass transition temperature of the cyclic olefin copolymer is 155℃; the reactive compatibilizer is a polypropylene grafted cyclic olefin copolymer; S is an organic functional component selected according to the first category of "available varieties of S" above, i.e., a saturated polyolefin molecule with a single fused aromatic ring at one end, whose olefin segment is a saturated polyolefin segment composed only of carbon and hydrogen, and whose weight-average molecular weight is determined according to the above method and confirmed to fall between the entangled molecular weight of P and the weight-average molecular weight of P according to criterion two; the antioxidant system is composed of a hindered phenolic antioxidant without metal elements and a phosphite antioxidant in a mass ratio of 1:1; the lubricant is a low-precipitation fatty acid ester lubricant that does not migrate or precipitate under molding and vacuum metallization evaporation conditions.
[0060] Formula: Based on the total mass of the masterbatch, P is 64.0%, cyclic olefin copolymer is 20.0%, S is 6.0%, reactive compatibilizer is 8.0%, antioxidant system is 1.2%, lubricant is 0.8%, and the sum of the mass fractions of all components is 100.0%. This formula is taken from the optimal formula in the technical concept on which this invention is based.
[0061] Preparation: such as Figure 3 As shown, the above components are added to a high-speed mixer according to the specified ratio and premixed at 70°C for 10 minutes to obtain a premix. The premix is fed into a co-rotating twin-screw extruder with a screw length-to-diameter ratio of 44:1 to 56:1. The mixing section of the extruder consists of a combination of weak shear elements and medium shear elements. The temperature of each temperature zone is set sequentially from the feeding section to the die head within the range of 180°C to 230°C and increases along the screw direction. The screw speed is 300 r / min. A first-stage vacuum devolatilization is set in the middle section and at the end of the extruder, i.e., two-stage vacuum devolatilization, with the vacuum degree of each stage being less than -0.09 MPa. The devolatilized melt is extruded through the die head, water-cooled, and then pelletized to obtain granules. The granules are placed in an 80°C forced-air drying oven for 4 hours to dry and mature, obtaining the masterbatch.
[0062] In the above five processes, premixing ensures that the components achieve macroscopic uniformity before entering the melting section; melt extrusion causes the olefin segments of S to entangle with the molecular chains of P in the melt, and enriches the reactive compatibilizer at the interface between P and the cyclic olefin copolymer, thereby refining the dispersed phase; multi-stage vacuum devolatilization removes volatiles and low-molecular-weight substances that are not entangled with the molecular chains of P from the melt; water-cooled pelleting completes the crystallization of the masterbatch stage before S aggregates; drying and curing further promotes the crystallization of the pellets at 80°C and stabilizes them, thereby maintaining the offset and the equivalent diameter of the enriched domains during subsequent storage, transportation, and blending.
[0063] Acceptance of Masterbatch: According to criterion three, the deviation of the differential scanning calorimetry melting peak temperature between the masterbatch obtained in this embodiment and P is expected to be within 0.5℃. According to criterion four, the equivalent diameter of the S-enriched domains in the masterbatch obtained in this embodiment is expected to be smaller than the equivalent diameter of the cyclic olefin copolymer dispersed phase, or no S-enriched domains are observed; this embodiment contains the aforementioned reactive compatibilizer, and its cyclic olefin copolymer dispersed phase has a smaller equivalent diameter than that without the compatibilizer, therefore this criterion is stricter in this embodiment. The weight loss rates L, L0, and Lp of the masterbatch obtained in this embodiment, its control masterbatch, and P are measured according to the method for determining the weight loss rate by n-heptane reflux extraction. The corrected difference in weight loss rates is calculated using ΔL = L - L0 + 0.060·Lp, and ΔL is expected to be lower than the mass fraction of S in the masterbatch of this embodiment (6.0%). If all S is extracted, ΔL should be equal to 6.0%; the portion of ΔL below 6.0% corresponds to the portion of S that has formed entanglement with the molecular chains of P and is therefore not extracted.
[0064] Melt samples were taken once each from the inlet and outlet of the multi-stage vacuum devolatilization process, and their molecular weight distribution was determined by high-temperature gel permeation chromatography after cooling. After devolatilization, the relative content of the fraction with molecular weight lower than P is expected to decrease, while the relative content of the molecular weight range containing S is expected to remain basically unchanged.
[0065] Film Formation: The polypropylene matrix resin used is capacitor film-grade homopolymer polypropylene with a melt flow rate of 2 g / 10 min to 3 g / 10 min. The masterbatch obtained in this example is mixed into the polypropylene matrix resin at a ratio of 4 wt%, mixed by a twin-screw extruder, and then cast into a thick sheet. The cold roller temperature is 30°C, followed by longitudinal stretching of 5 times and transverse stretching of 9 times, and heat setting at 160°C for 15 s. The thickness of the cast sheet is adjusted to obtain a film thickness of 2.5 μm, thus obtaining a biaxially oriented polypropylene capacitor film. The polypropylene matrix resin and film forming equipment used in the following examples and comparative examples are the same as those in this example.
[0066] Membrane characterization: The crystallinity of the membrane was determined using the methods described above, and is expected to fall around 55%. The lamellar period and spherulite radius of the membrane were determined using the methods described above. The enrichment factor f of the membrane was determined using the methods described above, and is expected to be above 1.5. The dielectric loss of the membrane at 100℃ and 50Hz was determined using the methods described above, and is expected to be below 0.0004. The breakdown field strength of the membrane was determined using the methods described above, and is expected to be above 570kV / mm. The long-term safe operating temperature of the membrane was determined using the methods described above, and is expected to fall within the range of 115℃ to 125℃. The above three expected values are the indicators that can be accepted according to the methods described above, and the actual measured values are determined by the implementer according to the methods described above.
[0067] Example 2: Each parameter is taken at the lower end of the defined range. In this embodiment, the lower limit of the mass fraction of S, the lower limit of the glass transition temperature of the cyclic olefin copolymer, the upper limit of the melt flow rate of P, the lower limit of the preparation process parameters, and the lower limit of the blending ratio are taken.
[0068] Raw materials: P is homopolymer polypropylene with a melt flow rate of 8 g / 10 min; the glass transition temperature of the cyclic olefin copolymer is 130 °C; the rest is the same as in Example 1.
[0069] Formula: Based on the total mass of the masterbatch, P is 66.0%, cyclic olefin copolymer is 25.0%, S is 3.0%, reactive compatibilizer is 4.0%, antioxidant system is 1.2%, lubricant is 0.8%, and the sum of the mass fractions of all components is 100.0%.
[0070] Preparation: Premix at 60℃ for 8 min; set the temperature of each melt extrusion zone between 180℃ and 210℃, and the screw length-to-diameter ratio is 44:1; perform two-stage vacuum devolatilization with each stage vacuum degree below -0.09MPa; water-cooled pelletizing; dry and mature at 80℃ for 4 h.
[0071] Film formation: The obtained masterbatch was mixed into the polypropylene matrix resin at a ratio of 2wt%, and the thickness of the cast film was adjusted so that the thickness of the film was 2.0μm. The other film formation conditions were the same as in Example 1.
[0072] Acceptance and Characterization: Acceptance was conducted according to criteria three and four, and both were expected to be satisfactory. The enrichment factor f of the membrane was measured using the above method, and was expected to be above 1.5. The dielectric loss and breakdown field strength of the membrane at 100℃ and 50Hz were measured using the above method, and were expected to be below 0.0004 and above 570kV / mm, respectively. In this embodiment, the mass fraction of S in the masterbatch was taken as its lower limit of 3.0%, which is the lowest among all embodiments. The margin of S concentration in the masterbatch from its dispersion limit is the largest among all embodiments, so criterion four is the most lenient in this embodiment; correspondingly, the mass fraction of S in the membrane after film formation is 0.06%.
[0073] Example 3: Each parameter is taken at the upper end of the defined range. In this embodiment, the upper limit of the mass fraction of S, the upper limit of the glass transition temperature of the cyclic olefin copolymer, the lower limit of the melt flow rate of P, the upper limit of the preparation process parameters, and the upper limit of the blending ratio are taken.
[0074] Raw materials: P is homopolymer polypropylene with a melt flow rate of 2.5 g / 10 min; the glass transition temperature of the cyclic olefin copolymer is 180 °C; the rest is the same as in Example 1.
[0075] Formula: Based on the total mass of the masterbatch, P is 55.0%, cyclic olefin copolymer is 25.0%, S is 8.0%, reactive compatibilizer is 9.0%, antioxidant system is 1.8%, lubricant is 1.2%, and the sum of the mass fractions of all components is 100.0%.
[0076] Preparation: Premix at 80℃ for 12 min; set the temperature of each melt extrusion zone between 200℃ and 230℃, and the screw length-to-diameter ratio is 56:1; perform two-stage vacuum devolatilization with each stage vacuum degree below -0.09MPa; water-cooled pelletizing; dry and mature at 80℃ for 6 h.
[0077] Film formation: The obtained masterbatch was mixed into the polypropylene matrix resin at a ratio of 6 wt%, and the thickness of the cast film was adjusted so that the thickness of the film was 3.0 μm. The other film formation conditions were the same as in Example 1.
[0078] Acceptance and Characterization: Acceptance is conducted according to criteria three and four. In this embodiment, the mass fraction of S is taken as its upper limit of 8.0%, which is the highest among all embodiments. The margin of S concentration in the masterbatch from its dispersion limit is the smallest among all embodiments. At the same time, in this embodiment, the reactive compatibilizer is taken as its upper limit of 9.0%. Due to the action of this compatibilizer, the cyclic olefin copolymer dispersed phase is refined, and its equivalent diameter is smaller than that of Examples 1 and 2. The reference amount of criterion four is correspondingly tight. The above two items are superimposed in the same direction, so criterion four is relatively tight in this embodiment. If the acceptance according to criterion four is not qualified, the mass fraction of S is reduced from 8.0% in increments of 1% as described in Section 2, and the acceptance is repeated. The reduced mass fraction is made up by P to keep the sum of the proportions 100%. The enrichment factor f of the membrane was determined using the above method, and it is expected to be 1.5 or higher. The dielectric loss and breakdown field strength of the membrane at 100°C and 50Hz were determined using the above method, and they are expected to be less than 0.0004 and more than 570kV / mm, respectively.
[0079] Example 4: Investigation of Crystallinity Variation within a Defined Range In this embodiment, the same masterbatch obtained in Example 1 was mixed with the same polypropylene matrix resin at the same blending ratio of 4 wt%. The thickness of the resulting films was 2.5 μm. Only the cooling and heat setting conditions of the film formation were changed so that the crystallinity of the resulting films fell at the lower end, middle and upper end of the range, respectively, in order to examine the retention of the enrichment factor f when the crystallinity varied within this range.
[0080] Condition A: Cold roller temperature 20℃, heat setting temperature 150℃, heat setting time 10s. The crystallinity of the resulting film is expected to be around 50%.
[0081] Condition B: Cold roller temperature 30℃, heat setting temperature 160℃, heat setting time 15s. The crystallinity of the resulting film is expected to be around 55%.
[0082] Condition C: Cold roller temperature 40℃, heat setting temperature 168℃, heat setting time 20s. The crystallinity of the resulting film is expected to be around 60%.
[0083] Under all three conditions, the longitudinal stretching ratio was 5 times and the transverse stretching ratio was 9 times. The crystallinity and enrichment factor f of the films obtained under the three conditions were measured using the method described above. f was expected to be above 1.5 at all three points.
[0084] Example 5: The proportions are taken from the endpoint combinations within the defined range. This embodiment uses the upper limit of the mass fraction of the polypropylene carrier resin, the lower limit of the mass fraction of the cyclic olefin copolymer, and the lower limit of the mass fractions of the antioxidant system and the lubricant to examine the implementation of the above ratio at its endpoint combination. The raw materials are the same as in Example 1. Ratio: Based on the total mass of the masterbatch, P is 70.0%, the cyclic olefin copolymer is 15.0%, S is 4.7%, the reactive compatibilizer is 9.0%, the antioxidant system is 0.8%, and the lubricant is 0.5%, with the sum of the mass fractions of all components being 100.0%. The preparation and film-forming conditions are the same as in Example 1. The obtained masterbatch is blended into the polypropylene matrix resin at a ratio of 4 wt%, and the thickness of the cast film is adjusted to achieve a film thickness of 2.5 μm. Acceptance is performed according to criteria three and four, and both are expected to be qualified. The enrichment factor f of the film is measured according to the above method, and is expected to be above 1.5. In this embodiment, the cyclic olefin copolymer is taken at its lower limit and the reactive compatibilizer is taken at its upper limit. The compatibilizing dose per unit two-phase interface is higher than in other embodiments, and the equivalent diameter of the dispersed phase is correspondingly smaller, so the reference amount of criterion four is tighter; while the mass fraction of S is in the middle of the defined range, and its margin from the dispersion limit is larger than in embodiment three.
[0085] Comparative Examples 1 to 9 Comparative Example 1. Sa was used instead of S in Example 1, and all other components, proportions, preparation conditions, and film-forming conditions were the same as in Example 1. The Sa molecule is composed of olefin segments homologous to P, with both ends of the chain being end groups of the olefin segment itself, without aromatic ring groups. Since the entire Sa molecule can enter the polypropylene lattice and participate in lattice construction, the expected offset of the differential scanning calorimetry melting peak temperature of the resulting masterbatch from P exceeds 1°C, failing acceptance according to criterion three, and Sa is not discharged by the crystallization front. The aromatic ring groups are absent in the system of this comparative example, therefore the enrichment factor f is not measured; this illustrates that when the first limitation (aromatic ring end group) and the third limitation (offset) of claim 1 are missing, criterion three is failed.
[0086] Comparative Example 2. Sb was substituted for S in Example 1, with the rest remaining the same as in Example 1. The molecular structure of Sb is the same as S, but its weight-average molecular weight is not greater than the entanglement molecular weight of P. Sb does not form entanglements with the molecular chains of P in the amorphous phase, therefore it is preferentially removed along with low-molecular-weight substances during multi-stage vacuum devolatilization. The measured mass fraction of Sb in the resulting masterbatch is expected to be lower than 6.0% of the feed, denoted as wS-b′. Measured according to the above method and calculated using ΔL = L - L0 + wS-b′·Lp, ΔL is expected to be close to wS-b′, meaning that the remaining Sb is expected to be almost entirely extracted under these extraction conditions, which does not meet the conditions of claim 3; while the expected ΔL of the masterbatch obtained in Example 1 is significantly lower than its wS. Films were formed under the three film-forming conditions described in Example 4. Unentangled Sb continued to migrate during heat setting and subsequent thermal processes. As the matrix crystallinity increased from 50% to 60% and the amorphous phase volume continued to shrink, it was expected that Sb-enriched domains with an equivalent diameter exceeding the equivalent diameter of the cyclic olefin copolymer dispersion would appear, thus failing according to criterion four. This comparative example illustrates the consequences of the absence of the lower end (weight-average molecular weight greater than the entangled molecular weight) as defined in claim 1, paragraph 2.
[0087] Comparative Example 3. Sc is used instead of S in Example 1, with the rest remaining the same as in Example 1. The molecular structure of Sc is the same as S, but its weight-average molecular weight is not less than that of P. The self-diffusion coefficient of Sc in the polypropylene melt is too small; its self-diffusion coefficient to crystallization growth rate ratio is expected to be less than the lamellar length period of the film. The time Sc takes to advance at the crystallization front is insufficient to leave the adjacent region of that front, and it is in situ embedded by the growing lamellars, with its aromatic ring groups remaining on the lamellar fold surfaces. The enrichment factor f of the resulting film is expected to be no higher than one.
[0088] Comparative Example 4. The mass fraction of S in Example 1 was increased from 6.0% to 15.0%, and P was correspondingly reduced to 55.0%, with the rest remaining the same as in Example 1. The concentration of S in the amorphous phase of the masterbatch exceeded its dispersion limit in amorphous polypropylene. The excess portion precipitated from the amorphous phase and aggregated into independent enriched domains. The equivalent diameter of the S-enriched domains in the resulting masterbatch was expected to exceed the equivalent diameter of the dispersed phase of the cyclic olefin copolymer, which was deemed unacceptable according to criterion 4. The aromatic ring groups aggregated within the domains exited the carrier transport channels. It should be noted that the enrichment factor f, by its definition, only reflects the degree of enrichment of aromatic ring groups at the interface between the amorphous phase and the two phases relative to the entire film, and does not distinguish whether the aromatic ring groups are dispersed or aggregated within domains. Therefore, f in this comparative example may not be lower than that in Example 1—this precisely illustrates that the object constrained by the fourth claim of claim 1 (equivalent diameter of enriched domains) is different from the object measured by the enrichment factor f, and the two cannot be substituted for each other.
[0089] Comparative Example 5. The reactive compatibilizer was removed from the formulation of Example 1, and the resulting 8.0% reduction was made up by P, i.e., P was 72.0%. The remaining components, formulations, preparation conditions, and film-forming conditions were the same as in Example 1. In this comparative example system, there was no compatibilizer at the interface between P and the cyclic olefin copolymer, resulting in weaker interfacial bonding than in Example 1. This leads to two consequences: firstly, the dispersed phase of the cyclic olefin copolymer was not refined during mixing, and its equivalent diameter was larger than in Example 1, thus the reference amount for criterion four was less stringent than in Example 1; secondly, during biaxial stretching in both the longitudinal and transverse directions, the two phases easily separated and delaminated at this interface, resulting in more interfacial defects at this point after film formation than in Example 1, and the aromatic ring groups that had reached this point were no longer within a continuous phase region. This comparative example is used to illustrate the role of the reactive compatibilizer in the preferred embodiment; the resulting masterbatch still satisfies the four limitations described in claim 1, therefore this comparative example is not used to illustrate the necessity of these four limitations.
[0090] Comparative Example 6. Sd was used instead of S in Example 1, with all other components, proportions, preparation conditions, and film-forming conditions remaining the same as in Example 1. The Sd molecule consists of an olefin segment homologous to P and an aromatic heterocyclic group attached to one end of the olefin segment. This aromatic heterocyclic group contains heteroatoms, and its weight-average molecular weight is the same as S. According to criterion 1, its NMR spectrum shows the chemical shift signal characteristic of heteroatom substitution of the aromatic ring, and Sd does not meet criterion 1. This heteroatom gives the group a permanent dipole, causing orientation polarization under an alternating electric field and resulting in dielectric loss, contrary to the purpose of this invention to suppress dielectric loss in the film. Simultaneously, this polar group causes the solubility parameter of the molecule to deviate from that of amorphous polypropylene, thus decreasing its solubility limit in the amorphous phase. The equivalent diameter of the Sd-enriched domains in the masterbatch obtained at the same mass fraction is expected to be greater than that of Example 1. This comparative example illustrates the consequences of the omission of the first claim of claim 1, which specifies that "the aromatic ring group is an aromatic ring group composed of carbon and hydrogen."
[0091] Comparative Example 7. Se was substituted for S in Example 1, with the rest remaining the same as in Example 1. Se is a triblock molecule with aromatic ring segments at both ends and an olefin segment homologous to P in the middle. Its aromatic ring segments consist only of carbon and hydrogen, and its weight-average molecular weight is the same as S. Se does not have free ends without aromatic ring groups, and therefore fails acceptance according to criterion one. In the melt, this molecule cannot anchor one end to the polypropylene matrix while pointing the other end towards the amorphous phase and the interface between the two phases. After being expelled by the crystallization front, the tendency for the aromatic ring segments at both ends to aggregate is greater than that of the single-end molecule. The equivalent diameter of the Se-enriched domains in the resulting masterbatch is expected to be greater than that of Example 1, and therefore also fails acceptance according to criterion four. This comparative example illustrates the consequences of the absence of the phrase "connected to one end of the olefin segment" in the first claim of claim 1.
[0092] Comparative Example 8. Sf replaces S in Example 1, with the rest remaining the same as in Example 1. Sf is formed by grafting the same aromatic ring group as in Example 1 onto the polypropylene backbone via a grafting reaction. That is, the aromatic ring group forms a chemical bond with the molecular chain of the polypropylene carrier resin, and the grafting rate makes the total amount of aromatic ring groups in the system the same as in Example 1. According to criterion 1, the obtained masterbatch was dissolved in 1,2,4-trichlorobenzene at 135°C and precipitated and fractionated with n-heptane at 25°C. The characteristic signals of polypropylene and aromatic rings appeared simultaneously in the 1H NMR spectra of both fractions, indicating that they could not be separated. Therefore, Sf does not meet criterion 1. Since the aromatic ring group is already bonded to the polypropylene backbone, its destination during crystallization is no longer determined by its own self-diffusion coefficient, but by the polypropylene molecular chain segment to which it is bonded: those entering the lamellar crystals from the backbone carry their attached aromatic ring groups into the lamellar crystals. Therefore, the ratio in the obtained film is expected to be no higher than one, and this ratio varies with the crystallinity of the matrix. This comparative example illustrates the consequences of the omission of the first clause of claim 1, which states that the claim "does not form chemical bonds with the molecular chains of the polypropylene carrier resin" is missing.
[0093] Comparative Example 9. Sg was substituted for S in Example 1, with the rest remaining the same as in Example 1. The Sg molecule consists of an aromatic ring group and a chain segment attached to one end of the aromatic ring group. This chain segment is not homologous to P; it is a non-polyolefin chain segment containing polar units, with the same weight-average molecular weight as S. According to criterion one, this chain segment is not a saturated polyolefin chain segment composed solely of carbon and hydrogen, and Sg does not meet criterion one. During the melt blending stage, this molecule is insoluble in polypropylene and does not form entanglements with the molecular chains of P. According to the above-mentioned determination of the weight loss rate by reflux extraction with n-heptane, the corrected difference in its weight loss rate is expected to be close to the mass fraction of Sg in the masterbatch, meaning it can be essentially completely extracted. After film formation, this molecule is distributed within the cyclic olefin copolymer dispersion phase, which has a more similar solubility parameter, and the aromatic ring group it carries subsequently exits the intergranular amorphous phase and the two-phase interface. This comparative example illustrates the consequences of the absence of the "olefin segment homologous to the polypropylene carrier resin" in the first claim of claim 1, that is, the consequences of the second destination not being closed.
[0094] Results Comparison and Mechanism Explanation The above embodiments are compared with the comparative examples as follows. In Embodiments 1 to 5, the offset is within 1°C, the equivalent diameter of the enriched domain is smaller than the equivalent diameter of the cyclic olefin copolymer dispersed phase or the enriched domain is not observed, and the enrichment factor f is expected to be 1.5 or higher; while Comparative Examples 1 to 4 and Comparative Examples 6 to 9 each change one or a part of the four limitations described in claim 1, while keeping the other items unchanged, and the results are not expected to satisfy the above three conditions simultaneously: Comparative Example 1 fails to meet the offset, and Comparative Example 2 fails to meet the requirements of claim 3. The extraction conditions for Comparative Example 1 and Comparative Example 2 are as follows: Comparative Example 3 fails to meet the equivalent diameter of the enriched domain at the crystallinity level; Comparative Example 4 fails to meet the equivalent diameter of the enriched domain; Comparative Example 6 fails to meet the criterion that the aromatic ring group consists only of carbon and hydrogen; Comparative Example 7 fails to meet the criterion that the aromatic ring group is only attached to one end of the olefin chain; Comparative Example 8 fails to meet the criterion that the independent molecule does not form a chemical bond with the molecular chain of the polypropylene carrier resin; Comparative Example 9 fails to meet the criterion that the olefin chain is homologous to the polypropylene carrier resin. Each constraint has a different mode of failure, indicating that the objects constrained are different. The above effects are not the sum of the effects of each constraint; removing any one of them results in the failure of that corresponding condition. Comparative Example 5 does not change the four limitations described in claim 1. What it changes is the preferred technical feature of the reactive compatibilizer. Therefore, its comparison with Example 1 is used to illustrate the role of this preferred feature, not to illustrate the necessity of the above four limitations.
[0095] Regarding the migration characteristics of molecules after they are expelled. For example... Figure 1 As shown, after S is expelled from the crystal growth front 7, two processes occur simultaneously: its diffusion in the melt, characterized by the self-diffusion coefficient D, with the dimension of the square of length divided by time; and the advancement of the crystal growth front, characterized by the crystal growth rate G, with the dimension of length divided by time. The only combination of length that can be constructed from these two quantities is the ratio of D to G. Therefore, the characteristic scale that S can migrate after being expelled is this ratio. When this ratio is greater than the lamellar long period, S crosses the scale between lamellars 4 and falls into the amorphous phase 5 between lamellars and the two-phase interface 21; when it is less than the spherulite radius, S is already in place before reaching the spherulite boundary 6; those that are too small are buried in situ by the lamellars 4, while those that are too large are pushed to the spherulite boundary 6 and aggregate into enriched domains 8.
[0096] Regarding the function of multi-stage vacuum devolatilization: Molecules with a weight-average molecular weight lower than P, whose entanglement molecular weight is not entangled with the molecular chains of P, are removed first under vacuum devolatilization conditions; while molecules falling within the aforementioned range are already entangled and locked, and are retained under the same conditions. Therefore, multi-stage vacuum devolatilization not only removes volatiles, but also constitutes an online sieve at the lower end of the aforementioned molecular weight range.
[0097] Regarding the geometric upper bound of enrichment multiples. For example... Figure 4 As shown, when S does not enter the crystalline phase at all, its entire amount lies within the interface between the amorphous phase and the two phases. The mass fraction of this portion is one minus the crystallinity. Therefore, the geometric upper limit of the enrichment factor is equal to one divided by one minus the difference in crystallinity: for crystallinity of 50%, 55%, and 60%, this upper limit is 2.00, approximately 2.22, and 2.50, respectively. This upper limit monotonically increases with increasing crystallinity, so its minimum value appears at the lower end in the range of 50% to 60%. The 1.5 defined in this invention is 75% of the geometric upper limit at this lower end, and the margin relative to the upper limit is larger at other points. The above upper limit is a boundary given by geometric relationships; the actual value of the enrichment factor also depends on the degree to which S is expelled and placed.
[0098] The rationale for setting the criterion on the masterbatch: The mass fraction of sulfur (S) in the masterbatch is 3.0% to 8.0%. After being blended at 2 wt% to 6 wt%, its mass fraction in the film is 0.06% to 0.48%, and the concentration in the masterbatch stage is 16.7 to 50 times that in the film-forming stage. Therefore, the masterbatch has the highest S concentration throughout the process and is most likely to exceed its dispersion limit, leading to precipitation and aggregation. Setting the enriched domain equivalent diameter limit on the masterbatch sets the most stringent acceptance criteria. Regarding the function of the offset criterion: For molecules that pass acceptance according to criterion one, the volume of their aromatic ring groups is significantly larger than that that the polypropylene lattice can accommodate, and the structural condition that they do not participate in lattice construction is generally met. The function of the offset is to convert this structural condition into a batch-by-batch acceptance index that can be measured in the laboratory after the masterbatch is manufactured, so that this condition is not merely an inference about the raw material structure, but a measured verification of each batch of masterbatch.
[0099] Regarding the selection of n-heptane: n-Heptane has a boiling point lower than the melting point of polypropylene. Under reflux conditions, it is a selective solvent for polypropylene, dissolving fractions with low crystallinity and low molecular weight while retaining molecules already entangled and locked within the amorphous phase. The contribution of low molecular weight fractions that can be dissolved from P to the weight loss rate is subtracted from the wS·Lp term in the correction formula. If a solvent with a higher boiling point is used, the number of dissolved fractions increases, and the resolving power of this criterion decreases accordingly.
[0100] Regarding the effects of the various limitations in the preferred scheme: The offset is narrowed from 1°C to 0.5°C, increasing the margin for the condition that the aromatic ring groups do not participate in lattice construction; the difference in weight loss rate during heptane reflux extraction characterizes entanglement, making the entanglement a verifiable fact on the spot; the ratio of the self-diffusion coefficient to the crystal growth rate falls between the lamellar length period and the spherulite radius, allowing the migration characteristic scale to be directly compared with the matrix microstructure scale; the formulation and preparation conditions ensure that the above-mentioned items can be repeatedly achieved within the conventional processing window.
[0101] Regarding the effect of reactive compatibilizers on criterion four: This compatibilizer refines the dispersed phase of the cyclic olefin copolymer and reduces its equivalent diameter. Criterion four uses this equivalent diameter as the upper limit of the equivalent diameter of the enriched domains of S. Therefore, criterion four is stricter in the scheme containing this compatibilizer than in the scheme without it. Examples 1 to 3 and 5 meet criterion four under this stricter reference amount, and their dispersion margin comes from the molecular weight range and mass fraction of S itself.
[0102] Explanation of verification items and results In the embodiments described in this specification, all specific values relating to the offset, the equivalent diameter of the enriched domain and the cyclic olefin copolymer dispersed phase, the weight loss rate of the n-heptane reflux extraction, the crystallinity, the enrichment factor f, the dielectric loss of the membrane, the breakdown field strength, and the long-term safe operating temperature are values that can be measured according to the methods and criteria described in this specification. This specification provides measurement methods, criteria, and parameter boundaries for the above items, and the specific values shall be measured by the implementer according to the methods described above.
[0103] It is recommended that implementers perform verification in the following order: First, determine the entanglement molecular weight and weight-average molecular weight of P and the weight-average molecular weight of S according to criterion two, and confirm that S falls within the specified range. Second, after obtaining the masterbatch, determine the offset according to criterion three, and confirm that it is within 1°C. If necessary, verify with a control masterbatch that the offset is indeed caused by S. Third, determine and compare the equivalent diameters of the two types of domains according to criterion four, and confirm that the equivalent diameter of the enriched domains is smaller than the equivalent diameter of the dispersed phase of the cyclic olefin copolymer, or that no S-enriched domains are observed. Fourth, determine the weight loss rate of n-heptane reflux extraction of the obtained masterbatch, control masterbatch, and P, calculate ΔL = L - L0 + wS·Lp, and confirm that ΔL is lower than wS; at the same time, take samples before and after multi-stage vacuum devolatilization to determine the molecular weight distribution, and confirm that fractions below the entanglement molecular weight are removed while the range containing S is retained. Fifth, films were formed under the three film-forming conditions described in Example 4. The crystallinity and enrichment factor f of each film were measured using the selective etching method described above, confirming that f was above 1.5 within the crystallinity range. Sixth, the dielectric loss, breakdown field strength, and long-term safe operating temperature of the formed films were measured using the method described above, and compared with the corresponding expected values contained in this specification. Among these, the fifth item is the most critical at the upper limit of the S mass fraction corresponding to Example 3, and should be verified first. The etching endpoint is defined as the cumulative weight loss equal to the product of the sample mass and (subtracting the crystallinity). The practitioner should first calibrate the etching time required for this endpoint using a control film without S.
[0104] The expected values for dielectric loss, breakdown field strength, and long-term safe operating temperature of the membrane described in this specification are acceptance indicators that can be verified according to the methods described herein. Actual measured values in a real system depend on the polypropylene matrix resin used and the film-forming conditions, and must be determined by the practitioner using the methods described above. This specification does not assert any claims regarding the measured values. The leakage current of the membrane under high-temperature operating conditions is lower than the corresponding value of a control membrane prepared with the same formulation but without the aforementioned aromatic ring groups. The extent of this reduction must also be determined by actual measurement, and this specification does not assert any claims regarding this extent.
[0105] Other implementation methods and variations The embodiments described above are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of protection of the present invention. It should be noted that any equivalent substitutions and improvements made by those skilled in the art without departing from the concept and criteria of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-performance polypropylene masterbatch for ultrathin capacitor films, comprising polypropylene carrier resin, cyclic olefin copolymer, and organic functional components, characterized in that: The organic functional component is an independent molecule that does not form chemical bonds with the molecular chain of the polypropylene carrier resin. The independent molecule is composed of an olefin segment homologous to the polypropylene carrier resin and an aromatic ring group attached to one end of the olefin segment. The aromatic ring group is an aromatic ring group composed of carbon and hydrogen. The weight-average molecular weight of the individual molecules is greater than the entangled molecular weight of the polypropylene carrier resin, but less than the weight-average molecular weight of the polypropylene carrier resin. The differential scanning quanta melting peak temperature of the masterbatch is within 1°C offset from the differential scanning quanta melting peak temperature of the polypropylene carrier resin itself. The mass fraction of the organic functional component is such that the equivalent diameter of the enriched domains formed by the independent molecules in the masterbatch is smaller than the equivalent diameter of the dispersed phase of the cyclic olefin copolymer.
2. The high-performance polypropylene masterbatch for ultra-thin capacitor films according to claim 1, characterized in that, The offset is within 0.5°C.
3. The high-performance polypropylene masterbatch for ultra-thin capacitor films according to claim 1 or 2, characterized in that, The weight loss rate of the masterbatch after reflux extraction in n-heptane, minus the weight loss rate of the control masterbatch under the same conditions but without the organic functional component, whose reduced mass fraction is made up by the polypropylene carrier resin, plus the product of the mass fraction of the organic functional component and the weight loss rate of the polypropylene carrier resin under the same conditions, is lower than the mass fraction of the organic functional component in the masterbatch.
4. The high-performance polypropylene masterbatch for ultra-thin capacitor films according to claim 1 or 2, characterized in that, The ratio of the weight-average molecular weight of the independent molecule to the weight-average molecular weight of the polypropylene carrier resin is such that the ratio of the self-diffusion coefficient of the independent molecule in the polypropylene carrier resin melt to the crystallization growth rate of the polypropylene carrier resin under the cooling conditions of the masterbatch blending film is greater than the lamellar length period of the polypropylene carrier resin under the cooling conditions, and less than the spherulite radius of the polypropylene carrier resin under the cooling conditions.
5. The high-performance polypropylene masterbatch for ultra-thin capacitor films according to claim 1 or 2, characterized in that, After the masterbatch is blended into a polypropylene matrix resin at a ratio of 2wt% to 6wt% and biaxially stretched into a film, the ratio of the mass fraction of the aromatic ring groups at the amorphous phase and the interface between the polypropylene and cyclic olefin copolymer phases of the film to the average mass fraction of the aromatic ring groups in the film is 1.5 or more; and when the crystallinity of the film varies in the range of 50% to 60%, this ratio is 1.5 or more within this range.
6. The high-performance polypropylene masterbatch for ultrathin capacitor films according to claim 1 or 2, characterized in that, The masterbatch also contains a reactive compatibilizer; based on the total mass of the masterbatch, the polypropylene carrier resin accounts for 55% to 70%, the cyclic olefin copolymer accounts for 15% to 25%, the organic functional component accounts for 3% to 8%, the reactive compatibilizer accounts for 4% to 9%, and the balance includes an antioxidant system composed of hindered phenolic antioxidants and phosphite antioxidants (0.8% to 1.8%) and fatty acid ester lubricants (0.5% to 1.2%), and the sum of the mass fractions of all components in the masterbatch is 100%.
7. The high-performance polypropylene masterbatch for ultrathin capacitor films according to claim 6, characterized in that, The glass transition temperature of the cyclic olefin copolymer is 130℃~180℃; the reactive compatibilizer is a polypropylene-grafted cyclic olefin copolymer; the polypropylene carrier resin is homopolymer polypropylene with a melt flow rate of 2.5~8g / 10min; the antioxidant system is a compound system of hindered phenolic antioxidants and phosphite antioxidants without metal elements.
8. A method for preparing a high-performance polypropylene masterbatch for ultrathin capacitor films according to any one of claims 1 to 7, characterized in that, Includes the following steps: The polypropylene carrier resin, the cyclic olefin copolymer, the organic functional component, and optional reactive compatibilizers, antioxidants, and lubricants are premixed to obtain a premix; the premix is melt-extruded; the molten material is subjected to multi-stage vacuum devolatilization; the devolatilized material is cooled and pelletized to obtain pellets; the pellets are dried and matured to obtain the masterbatch.
9. The preparation method according to claim 8, characterized in that, The premixing is carried out at 60℃~80℃ for 8~12min; the melt extrusion processing temperature is 180℃~230℃, and the melt extrusion is carried out in a mixing section composed of a combination of weak shear elements and medium shear elements; the vacuum degree of the multi-stage vacuum devolatilization is below -0.09MPa; the drying and curing is carried out at 80℃ for more than 4h; the multi-stage vacuum devolatilization makes the relative content of fractions with weight average molecular weight lower than the entangled molecular weight of the polypropylene carrier resin in the devolatilized material lower than that before devolatilization.
10. The application of the high-performance polypropylene masterbatch for ultrathin capacitor films according to any one of claims 1 to 7 in the preparation of biaxially oriented polypropylene capacitor films with a thickness of 2 μm to 3 μm, characterized in that, The masterbatch is mixed into a polypropylene matrix resin at a ratio of 2wt% to 6wt%, and the capacitor film is obtained by biaxial stretching.
Citation Information
Patent Citations
Heteroaromatic ring-containing modified polypropylene composite material, preparation method thereof and capacitor film
CN120399353A
Polypropylene composite particle and preparation method thereof, and polypropylene capacitance film and preparation method thereof
CN121271089A
Heat-resistant polypropylene capacitor film and preparation method thereof
CN122502763A