A corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound and its preparation method

By adding fluorinated dienes and conductive fillers to fluororubber, a tight cross-linked network and conductive pathways are constructed, solving the problems of static electricity accumulation and mechanical property degradation in fluororubber. This results in highly efficient antistatic and corrosion-resistant fluororubber compounds suitable for fields such as electronics, semiconductors, and aerospace.

CN123062877APending Publication Date: 2026-11-10ZHONGHAO CHENGUANG RES INST OF CHEMICALINDUSTRY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611473745.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing fluororubber is prone to static electricity accumulation due to friction during use, which affects product cleanliness and safety. Furthermore, the addition of conductive fillers can lead to a decrease in mechanical properties and resistance to media.

Method used

By adding fluorinated dienes and conductive fillers to fluorinated rubber compounds and employing special mixing methods and vulcanization processes, a tight cross-linked network and conductive pathways are constructed, thereby improving antistatic and mechanical properties.

Benefits of technology

It achieves stable antistatic properties of fluororubber, improves tensile strength and elongation at break, reduces compression set, and maintains high temperature resistance and chemical corrosion resistance, making it suitable for sealing applications in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a corrosion-resistant, antistatic, and low-voltage-deformation fluoropolymer compound and its preparation method, relating to the field of fluororubber technology. The fluoropolymer compound, by weight, comprises the following raw materials: 100 parts of high-fluorine peroxyfluororubber raw rubber, 0.5-3.0 parts of fluorinated diene, 1.0-4.5 parts of peroxy vulcanizing agent, 2.0-5.5 parts of peroxy vulcanization accelerator, 0-5.0 parts of acid scavenger, 0.5-3.0 parts of processing aid, 5.0-25.0 parts of conductive filler, 0.5-5.0 parts of coupling agent, and 5.0-10.0 parts of reinforcing carbon black. The fluoropolymer compound of this invention retains the excellent high and low temperature resistance and chemical corrosion resistance of fluororubber, while also possessing stable and long-lasting antistatic properties and good physical and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fluororubber technology, specifically to a corrosion-resistant, antistatic, low-pressure-change fluororubber compound and its preparation method. Background Technology

[0002] Fluororubber possesses excellent resistance to high and low temperatures (-40℃ to 320℃ or even higher), chemical corrosion resistance, ozone resistance, weather resistance, and good mechanical properties, making it widely used in high-end fields such as aerospace, automotive, petrochemical, and electronics. However, pure fluororubber itself is an excellent insulator, with a surface resistivity typically around 10 Ω·cm. 12 With a static electricity level above Ω·cm, fluororubber is highly susceptible to static electricity buildup during use due to friction and other factors. This buildup not only attracts dust, affecting product cleanliness and performance, but more seriously, in certain situations (such as electronic semiconductor manufacturing or flammable and explosive environments), it can trigger electrostatic discharge, causing equipment damage, product scrapping, or even serious accidents like fires and explosions. Therefore, endowing fluororubber with excellent antistatic properties and expanding its application in fields with high antistatic requirements is of significant practical importance.

[0003] Currently, the main methods for preparing antistatic rubber include adding conductive fillers, surface coating with antistatic agents, and blending with antistatic polymers. Among these, adding conductive fillers is the most commonly used and provides the most lasting effect. Commonly used conductive fillers include conductive carbon black, metal powders, carbon fibers, carbon nanotubes, and graphene. However, fluororubber has a regular molecular chain structure and low polarity, resulting in poor compatibility with inorganic conductive fillers. Directly adding large amounts of conductive fillers to achieve an antistatic effect often leads to a significant decrease in the processing and mechanical properties of fluororubber, and also affects its resistance to dielectrics.

[0004] Therefore, how to make fluororubber possess good antistatic ability, mechanical properties and resistance to media corrosion at the same time, so as to meet the requirements of antistatic and sealing materials in special application scenarios, is an urgent problem to be solved in this field. Summary of the Invention

[0005] This invention aims to solve the technical problem that existing fluororubber cannot simultaneously possess good antistatic ability, mechanical properties, and resistance to media corrosion. The purpose is to provide a corrosion-resistant, antistatic, and low-pressure-transformation fluororubber compound and its preparation method. This fluororubber compound retains the excellent high and low temperature resistance and chemical corrosion resistance of fluororubber, while also possessing stable and long-lasting antistatic function and good physical and mechanical properties.

[0006] This invention is achieved through the following technical solution:

[0007] This invention provides a corrosion-resistant, antistatic, and low-pressure-change fluoropolymer compound composition, comprising the following raw materials by weight:

[0008] 100 parts of high-fluorine peroxidized fluororubber raw rubber, 0.5-3.0 parts of fluorinated diene, 1.0-4.5 parts of peroxidized vulcanizing agent, 2.0-5.5 parts of peroxidized vulcanization accelerator, 0-5.0 parts of acid scavenger, 0.5-3.0 parts of processing aid, 5.0-25.0 parts of conductive filler, 0.5-5.0 parts of coupling agent, and 5.0-10.0 parts of reinforcing carbon black.

[0009] This invention adds a fluorinated diene, a diene vulcanization point monomer, to a fluorinated compound composition, which can be used as an auxiliary crosslinking accelerator for peroxide vulcanizing agents. Specifically:

[0010] In peroxide vulcanization, fluorinated dienes act as active additives. The two double bonds (-C=C-) on their molecules can quickly react with the free radicals generated by the decomposition of peroxides. The resulting active sites then combine with the fluororubber molecular chains, acting as a "bridge" to connect different molecular chains. Compared to simple crosslinking that only forms "point" connections, this can construct a denser and more uniform three-dimensional network structure, achieving a tight combination of longitudinal and transverse structures. Therefore, the addition of fluorinated dienes deeply participates in and optimizes the peroxide vulcanization process, achieving an efficient bridge and optimizing the crosslinking network. This can improve the mechanical properties and resilience of the product. The more uniform and dense crosslinking network significantly improves the tensile strength and tear strength of the rubber compound. At the same time, the introduced flexible segments prevent the network from being too rigid, allowing the vulcanized rubber to recover quickly after being stressed, possessing reliable resilience and ensuring long-term sealing reliability.

[0011] Fluorinated dienes contain both reactive double bonds and flexible fluorinated segments in their molecular structure. They not only participate in crosslinking but also "anchor" the flexible segments in the crosslinking network. At the same time, their fluorinated properties make them highly compatible with high-fluorine-content fluororubber matrices, allowing them to disperse uniformly and providing more and more stable binding sites for conductive fillers. Therefore, the addition of fluorinated dienes can improve the dispersion and binding efficiency of conductive fillers (such as conductive carbon black) in fluororubber matrices. More stable binding helps to form more complete conductive pathways and optimizes the conductivity of the material.

[0012] Furthermore, the molecular formula of the fluorinated diene is C0. n H 2n-2-m F m n and m are both positive integers, and 8≤n≤12, m≤2n-2.

[0013] Furthermore, the high-fluorine peroxyfluorinated rubber raw rubber is selected from one or more of vinylidene fluoride-hexafluoropropylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene-CSM, tetrafluoroethylene-perfluoroalkyl vinyl ether, and tetrafluoroethylene-perfluoroalkyl vinyl ether-CSM.

[0014] Furthermore, the high-fluorine peroxidized fluororubber raw rubber is selected from the high-fluorine peroxidized raw rubber FKM-GB506 independently developed by Chenguang Institute. The fluorine content of FKM-GB506 raw rubber is about 70.0%, and the Mooney viscosity is in the Mooney range of 45 to 65 MU.

[0015] This invention preferentially utilizes the high-fluorine peroxide raw rubber FKM-GB506 independently developed by Chenguang Institute. Compared to conventional raw rubber structures, this raw rubber structure introduces a sulfurization point monomer (primarily iodoalkane monomers, supplemented by other iodides or sulfurization point monomers, collectively introducing the sulfurization point). The primary monomer refers to sulfurization point monomers containing iodoalkane structures (such as perfluoroiodoalkyl vinyl ethers). The supplementary iodides or sulfurization point monomers include other iodine-containing monomers (such as trifluoroiodoethylene, other varieties of perfluoroiodoalkyl vinyl ethers, and iodoolefins), or bromine-containing monomers (such as trifluorobromoethylene, bromoethylene, and vinylidene fluoride). The primary and auxiliary monomers enter the polymer chain through emulsion polymerization. Using an iodine transfer agent, the corresponding structures are generated during polymerization, allowing iodine atoms to efficiently and stably bond to the ends or side chains of the molecular chain. The typical addition amount is 0.06%-6% of the monomer dosage.

[0016] Compared to conventional fluororubbers such as FKM-246, this invention uses FKM-GB506 raw rubber containing iodine-containing monomers with high vulcanization points. This fundamentally improves the crosslinking efficiency and final properties of fluororubber. Synergistically acting with fluorinated dienes, it transforms passive crosslinking into active crosslinking, thereby enhancing crosslinking efficiency. The CF bonds in the fluororubber backbone are very stable, and relying solely on free radicals generated by peroxides for attack is inefficient and uncontrollable. Introducing highly reactive CI bonds into the raw rubber allows for active, rapid, and targeted reactions with free radicals, achieving highly efficient crosslinking, significantly increasing vulcanization speed, reducing compression set, and improving overall performance.

[0017] Furthermore, the peroxide vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butylperoxyhexane (commonly known as bis2.5), and the vulcanization accelerator is TAIC (triallyl triisocyanurate).

[0018] Furthermore, the acid absorbent is selected from one or more of neutral magnesium oxide, highly active magnesium oxide, zinc oxide, and nano zinc oxide, preferably domestically produced Zhongke nano zinc oxide; the processing aid is selected from one or more of Struktol HT290, Moken FK101, Ws280, and palm wax; the reinforcing carbon black filler is selected from one or more of thermal cracking carbon black, spray carbon black, semi-reinforcing carbon black, light carbon black, high-reinforcing carbon black, furnace black, and precipitated silica.

[0019] Furthermore, the conductive filler is selected from one or more of conductive carbon black, graphene, and carbon nanotubes. The conductive carbon black has a particle size of 10–50 nm and a specific surface area of ​​80–1500 m². 2 / g; the graphene is single-layer or multi-layer graphene with a sheet diameter of 0.5-10μm; the carbon nanotube is single-walled or multi-walled carbon nanotube with a diameter of 1-50nm and a length of 1-50μm.

[0020] Furthermore, the conductive filler is a compound of conductive carbon black and carbon nanotubes, with a weight ratio of (3-5):1. The compound conductive filler used in this invention can exert a synergistic effect: conductive carbon black can fill the gaps between carbon nanotubes, while carbon nanotubes can form a more effective conductive network with a lower addition amount. Thus, while ensuring antistatic properties, the total amount of filler is reduced, which is beneficial to improving the processing and mechanical properties of the compound.

[0021] Furthermore, the coupling agent is selected as a silane coupling agent. The silane coupling agent is at least one selected from γ-aminopropyltriethoxysilane (KH550) and γ-glycidoxypropyltrimethoxysilane (KH560). This invention treats the inorganic filler with a silane coupling agent, which improves the interfacial bonding force between the inorganic conductive filler and the organic fluororubber matrix through a chemical reaction, increasing the coupling structure on the surface of the inorganic filler. Then, through the shearing action of the two rollers of an open mill, the inorganic filler and the fluororubber structure are effectively encapsulated together, enhancing their compatibility.

[0022] The second objective of this invention is to provide a method for preparing a corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound, comprising the following steps:

[0023] (1) Mix the dried conductive filler and coupling agent at 80-100℃ for 10-30 minutes to fully coat the surface of the conductive filler with the coupling agent and obtain the surface modified conductive filler.

[0024] (2) Put the high-fluorine peroxy fluorinated rubber raw rubber into a two-roll mill, add surface-modified conductive filler and other raw materials, mix and then extrude into sheets;

[0025] (3) The mixed rubber compound is re-rolled through a thin pass at least 15 times;

[0026] (4) The recycled rubber compound is subjected to a first-stage vulcanization at a temperature of 165-175℃ and a pressure of 15-30MPa for 10-35 minutes to allow the rubber compound to undergo preliminary cross-linking and shaping. Then, a second-stage vulcanization is carried out at 230-290℃ for 12-24 hours to obtain the product.

[0027] In the preparation process of this invention, the coupling agent is directly dry-mixed at a high temperature of 80-100℃. Compared with conventional coupling agent modification, which is mostly used for solvent (wet method) assisted dispersion, this invention has no risk of solvent residue. Moreover, by using high temperature to melt and vaporize the coupling agent for adsorption, and precisely determining within a certain temperature range, it can effectively ensure that the coupling agent uniformly coats the conductive filler.

[0028] Meanwhile, the pretreated conductive filler is recycled and passed through the same material as other raw materials, with the number of passes increased to at least 15 (5-10 passes for ordinary rubber). The purpose is to use strong shear force to break up the conductive filler agglomerates, forcing the high-viscosity fluororubber to penetrate into the filler voids and build a stable conductive network.

[0029] Finally, an ultra-high temperature and ultra-long duration two-stage vulcanization process is performed. Unlike the conventional two-stage vulcanization process for fluororubber, this application raises the temperature to 230-290℃ for 12-24 hours. This high-temperature and long-term treatment is not only for continued cross-linking, but also for high-temperature aging and shaping, allowing the conductive filler to undergo microscopic rearrangement at high temperature, eliminating internal stress, thereby obtaining an extremely low and stable volume resistivity, ensuring that the resistance does not drift under extreme high-temperature conditions, thus achieving excellent comprehensive performance.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] 1. This invention designs the composition of the compound and adds a fluorinated diene. Using a special mixing method and vulcanization process, a medium-hardness peroxyfluorinated compound is obtained. This ensures the excellent mechanical properties of the peroxyfluorinated compound while improving the surface resistance of the fluororubber. It also meets the requirements for sealing applications in harsh chemical environments and can replace foreign products. Therefore, the peroxyfluorinated compound obtained according to this invention not only possesses excellent physical and mechanical properties but also improves the surface resistance of the fluororubber, achieving excellent antistatic effects. Through a specific vulcanization process, a vulcanized product is obtained, which can be applied in sealing fields such as electronics, semiconductors, aerospace, and petrochemicals where high antistatic and corrosion resistance of materials are required.

[0032] 2. The surface resistivity of the fluoropolymer compound product of the present invention can be stably controlled at 10 Ω·cm. 6 -10 9 Within the Ω·cm range, it achieves excellent antistatic effect. At the same time, its tensile strength can reach more than 21MPa, its elongation at break can reach more than 210%, and its compression set at 200℃ for 70h can be as low as 17%. It has good mechanical properties and retains the original high temperature resistance and chemical corrosion resistance of fluororubber, which meets the requirements of high antistatic performance of fluororubber materials in fields such as electronics, semiconductors, aerospace, and petrochemicals. Detailed Implementation

[0033] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the illustrative embodiments and descriptions of the present invention are only used to explain the present invention and are not intended to limit the present invention.

[0034] The embodiments of the present invention will be described in detail below. However, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art.

[0035] The "scope" disclosed in this invention is defined in the form of a lower limit and an upper limit. A given scope is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific scope. The scope defined in this way can include or exclude end values, and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a scope.

[0036] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0037] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.

[0038] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other substances not listed may also be included, or that only the listed substances may be included.

[0039] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0040] The technical solution of the present invention will be further described in detail below with reference to the embodiments.

[0041] It should be noted that, unless otherwise specified, the experimental methods used in the embodiments are conventional methods. Unless otherwise specified, the materials, reagents, methods, and instruments used are all conventional materials, reagents, methods, and instruments in the art, and can be obtained commercially by those skilled in the art.

[0042] Example 1

[0043] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0044] Fluororubber FKM-GB506 100

[0045] Double 2.5 1.5

[0046] TAIC 2.5

[0047] 0.5% perfluoromethylene diene

[0048] Zinc oxide 3

[0049] Conductive carbon black 25

[0050] Multi-walled carbon nanotubes 5

[0051] 10g of precipitated silica filler

[0052] Silane coupling agent KH550 0.5

[0053] HT290 1.0

[0054] The preparation method of the above-mentioned fluororubber compound is as follows:

[0055] (1) Pretreatment: The conductive carbon black and multi-walled carbon nanotubes are mixed evenly and vacuum dried at 80-120℃ for 2-4 hours. Then, the dried mixed conductive filler is mixed with KH550 silane coupling agent in a high-speed mixer at 80-100℃ for 10-30 minutes to fully coat the surface of the conductive filler with silane coupling agent, thus obtaining the surface-modified conductive filler.

[0056] (2) Mixing: Put the raw fluororubber into a two-roll mill and plasticize for 1-2 minutes. The roller temperature should not exceed 45°C to soften the raw rubber, which will facilitate the addition and dispersion of subsequent fillers. Then add the conductive filler treated in step (1) and continue mixing for 5-15 minutes to make the material evenly mixed. After mixing, sheet out to obtain a pre-mixed fluororubber containing conductive filler. Then seal it for 24-48 hours (preferably 48 hours) at a constant temperature.

[0057] (3) Preparation of other formulation additives: Pre-mix other additives according to the proportion of formulation components and mix them in a closed system to prevent the additives from becoming ineffective.

[0058] (4) The premixed fluoropolymer rubber is first plasticized on an XK160 open mill for 1-2 minutes. The roll gap is adjusted to 0.8-1.0 mm, and other pre-formulated additives are added in sequence. The mixture is mixed for 3-5 minutes, then sheeted and cooled for more than 12 hours.

[0059] (5) Re-rolling: The peroxyfluorinated rubber compound after being left to stand is re-rolled 15 times in the form of a triangular bag on an XK160 two-roll mill, and finally sheeted out for testing and vulcanization.

[0060] (6) Vulcanization: The fluorinated compound, after being stored and recycled, is placed in a mold and vulcanized on a 50-ton flat vulcanizing machine at a temperature of 165–175℃, a vulcanization pressure of 15–30 MPa (pressure vulcanization), and a vulcanization time of 10–35 min to allow the compound to initially crosslink and solidify. Then, a second stage of vulcanization is carried out in a forced-air drying oven at 230–290℃ for 12–24 h to remove volatiles generated during vulcanization, further improve the crosslinking structure, and enhance the overall performance of the vulcanized rubber. After the above steps, a corrosion-resistant, antistatic, low-pressure-deformation fluorinated compound product is obtained.

[0061] Example 2

[0062] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0063] Fluororubber FKM-GB506 100

[0064] Double 2.5 1.5

[0065] TAIC 2.5

[0066] 0.5% perfluoromethylene diene

[0067] Zinc oxide 3

[0068] Conductive carbon black 20

[0069] Multi-walled carbon nanotubes 5

[0070] 10g of precipitated silica filler

[0071] Silane coupling agent KH550 0.5

[0072] HT290 1.0

[0073] The preparation method is the same as in Example 1.

[0074] Example 3

[0075] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0076] Fluororubber FKM-GB506 100

[0077] Double 2.5 1.5

[0078] TAIC 2.5

[0079] 0.5% perfluoromethylene diene

[0080] Zinc oxide 3

[0081] Conductive carbon black 15

[0082] Multi-walled carbon nanotubes 5

[0083] 10g of precipitated silica filler

[0084] Silane coupling agent KH550 0.5

[0085] HT290 1.0

[0086] The preparation method is the same as in Example 1.

[0087] Example 4

[0088] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0089] Fluororubber FKM-GB506 100

[0090] Double 2.5 1.5

[0091] TAIC 2.5

[0092] Perfluoromethylene diene 1.0

[0093] Zinc oxide 3

[0094] Conductive carbon black 15

[0095] Multi-walled carbon nanotubes 5

[0096] 10g of precipitated silica filler

[0097] Silane coupling agent KH550 0.5

[0098] HT290 1.0

[0099] The preparation method is the same as in Example 1.

[0100] Example 5

[0101] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0102] Fluororubber FKM-GB506 100

[0103] Double 2.5 1.5

[0104] TAIC 2.5

[0105] Perfluoromethylene diene 1.5

[0106] Zinc oxide 3

[0107] Conductive carbon black 15

[0108] Multi-walled carbon nanotubes 5

[0109] 10g of precipitated silica filler

[0110] Silane coupling agent KH550 0.5

[0111] HT290 1.0

[0112] The preparation method is the same as in Example 1.

[0113] Example 6

[0114] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0115] Fluororubber FKM-GB506 100

[0116] Double 2.5 1.5

[0117] TAIC 2.5

[0118] Perfluoromethylene diene 2.0

[0119] Zinc oxide 3

[0120] Conductive carbon black 15

[0121] Multi-walled carbon nanotubes 5

[0122] 10g of precipitated silica filler

[0123] Silane coupling agent KH550 0.5

[0124] HT290 1.0

[0125] The preparation method is the same as in Example 1.

[0126] Example 7

[0127] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0128] Fluororubber FKM-GB506 100

[0129] Double 2.5 1.5

[0130] TAIC 2.5

[0131] Perfluoromethylene diene 1.5

[0132] Zinc oxide 3

[0133] Conductive carbon black 15

[0134] Multi-walled carbon nanotubes 5

[0135] 10g of precipitated silica filler

[0136] Silane coupling agent KH550 1.0

[0137] HT290 1.0

[0138] The preparation method is the same as in Example 1.

[0139] Example 8

[0140] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0141] Fluororubber FKM-GB506 100

[0142] Double 2.5 1.5

[0143] TAIC 2.5

[0144] Perfluoromethylene diene 1.5

[0145] Zinc oxide 3

[0146] Conductive carbon black 15

[0147] Multi-walled carbon nanotubes 5

[0148] 10g of precipitated silica filler

[0149] Silane coupling agent KH550 1.5

[0150] HT290 1.0

[0151] The preparation method is the same as in Example 1.

[0152] Example 9

[0153] A corrosion-resistant, antistatic, low-pressure transformer fluoropolymer compound composition, with the following formulation (by weight):

[0154] Fluororubber FKM-GB506 100

[0155] Double 2.5 1.5

[0156] TAIC 2.5

[0157] Perfluoromethylene diene 1.5

[0158] Zinc oxide 3

[0159] Conductive carbon black 15

[0160] Multi-walled carbon nanotubes 5

[0161] 10g of precipitated silica filler

[0162] Silane coupling agent KH550 2.0

[0163] HT290 1.0

[0164] The preparation method is the same as in Example 1.

[0165] Comparative Example 1

[0166] The difference from Example 5 is that no fluorinated diene is added; the specific formulation is as follows:

[0167] Fluororubber FKM-GB506 100

[0168] Double 2.5 1.5

[0169] TAIC 2.5

[0170] Zinc oxide 3

[0171] Conductive carbon black 15

[0172] Multi-walled carbon nanotubes 5

[0173] 10g of precipitated silica filler

[0174] Silane coupling agent KH550 0.5

[0175] HT290 1.0

[0176] Comparative Example 2

[0177] The difference between this comparative example and Example 5 is that only conductive carbon black is used as the conductive filler, while the weight percentage remains the same. The specific formulation is as follows:

[0178] Fluororubber FKM-GB506 100

[0179] Double 2.5 1.5

[0180] TAIC 2.5

[0181] Perfluoromethylene diene 1.5

[0182] Zinc oxide 3

[0183] Conductive carbon black 20

[0184] 10g of precipitated silica filler

[0185] Silane coupling agent KH550 0.5

[0186] HT290 1.0

[0187] Comparative Example 3

[0188] The difference between this comparative example and Example 5 is that no vulcanization crosslinking point is introduced into the raw rubber structure (since raw rubber FKM-GB506 is a raw rubber containing four monomers including a vulcanization point monomer, without the addition of a vulcanization point monomer, it is a raw rubber polymerized from three monomers, such as FKM-246). The specific formulation is as follows:

[0189] Fluororubber FKM-246 100

[0190] Double 2.5 1.5

[0191] TAIC 2.5

[0192] Fluorinated diene (perfluoromethylene diene) 1.5

[0193] Zinc oxide 3

[0194] Conductive carbon black 15

[0195] Multi-walled carbon nanotubes 5

[0196] 10g of precipitated silica filler

[0197] Silane coupling agent KH550 0.5

[0198] HT290 1.0.

[0199] The properties of the fluororubber compound compositions prepared in the embodiments and comparative examples of the present invention were tested. The tensile strength and elongation at break were determined according to GB / T 528-2009; the hardness was determined according to GB / T 531.1-2008; the compression set (200℃×70h) was determined according to GB / T 7759—1996; the surface resistivity was determined according to GB / T 40719—2021; and the chemical resistance (lithium electrolyte 23℃×70h) was determined according to GB / T 1690—2010. The results are shown in Table 1.

[0200] Table 1. Performance test data of the fluororubber compound compositions prepared in the examples and comparative examples.

[0201]

[0202] As can be seen from the data in Table 1:

[0203] The tensile strength of the product in the embodiment can reach over 21 MPa, and the surface resistivity can be controlled within 10. 6 -10 9 It has excellent pressure transformation properties and resistance to harsh chemical media, improves the electrical properties of fluororubber, achieves good antistatic properties, and improves the overall performance of fluororubber. Among them, the overall performance of Example 5 is better.

[0204] Compared to Example 5, Comparative Example 1, without the addition of fluorinated diene, showed a decline in all properties. This is because the absence of fluorinated diene in Comparative Example 1 reduced the crosslinking density and network integrity (resulting in a significant decrease in mechanical properties). In the crosslinking process using peroxide (double 2.5) and co-crosslinking agent (TAIC), the number of crosslinking bonds formed solely by TAIC was small and rigid, leading to insufficient crosslinking density and uneven crosslinking structure in the vulcanizate, thus causing a decrease in mechanical properties. In contrast, the formulation in Example 5, containing fluorinated diene, extended the crosslinking bonds, allowing them to insert between fluororubber molecular chains and form a longer, more flexible, and denser CC crosslinking network, resulting in superior mechanical properties. Simultaneously, the lack of interfacial bridging by fluorinated segments increased the contact resistance between conductive fillers, raising the volume resistivity and degrading the antistatic effect.

[0205] In Comparative Example 2, the compounded conductive filler was replaced with pure conductive carbon black. Under the same mass fraction, all properties of Comparative Example 2 decreased, proving that the compounded conductive filler used in this invention has a synergistic effect. This is because conductive carbon black can fill the gaps between carbon nanotubes, and carbon nanotubes can form a more effective conductive network with a lower addition amount. Thus, while ensuring antistatic properties, the total amount of filler is reduced, which is beneficial to improving the processing and mechanical properties of the compound.

[0206] In the comparative example, the raw rubber structure of fluororubber did not introduce vulcanization crosslinking points. When FKM-246 was used to replace the raw rubber FKM-GB506 and peroxide vulcanization was used, incomplete vulcanization and weak crosslinking occurred. Because the molecular chains did not have clear reaction points, they could not form a three-dimensional crosslinking network smoothly, which led to a sharp decline in the mechanical properties of the crosslinking. At the same time, the volume resistivity also increased, and the effect did not meet the expectations at all.

[0207] Finally, it should be noted that the above specific embodiments are only used to describe the purpose, technical solution, and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation of the present invention and is not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the foregoing specific embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions or improvements can be made to some or all of the technical features. These modifications, equivalent substitutions, and improvements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.

Claims

1. A corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition, characterized in that, By weight, it includes the following ingredients: 100 parts of high-fluorine peroxidized fluororubber raw rubber, 0.5-3.0 parts of fluorinated diene, 1.0-4.5 parts of peroxidized vulcanizing agent, 2.0-5.5 parts of peroxidized vulcanization accelerator, 0-5.0 parts of acid scavenger, 0.5-3.0 parts of processing aid, 5.0-25.0 parts of conductive filler, 0.5-5.0 parts of coupling agent, and 5.0-10.0 parts of reinforcing carbon black.

2. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The molecular formula of the fluorinated diene is C n H 2n-2-m F m n and m are both positive integers, and 8≤n≤12, m≤2n-2.

3. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The high-fluorine peroxy fluororubber raw rubber is selected from one or more of vinylidene fluoride-hexafluoropropylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene, high-fluorine peroxy raw rubber FKM-GB506, tetrafluoroethylene-perfluoroalkyl vinyl ether, and tetrafluoroethylene-perfluoroalkyl vinyl ether-CSM.

4. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The high-fluorine peroxidized fluororubber raw rubber is selected from high-fluorine peroxidized raw rubber FKM-GB506.

5. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The peroxy vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, and the vulcanization accelerator is TAIC.

6. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The acid absorbent is selected from one or more of neutral magnesium oxide, highly active magnesium oxide, zinc oxide, and nano zinc oxide; the processing aid is selected from one or more of Struktol HT290, Moken FK101, Ws280, and carnauba wax.

7. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The conductive filler is selected from one or more of conductive carbon black, graphene, and carbon nanotubes.

8. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 7, characterized in that, The conductive filler is a compound of conductive carbon black and carbon nanotubes, with a weight ratio of (3-5):

1.

9. The corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition according to claim 1, characterized in that, The coupling agent is selected from silane coupling agents.

10. The method for preparing a corrosion-resistant, antistatic, low-pressure-change fluoropolymer compound composition as described in claim 1, characterized in that, Includes the following steps: (1) Mix the dried conductive filler and coupling agent at 80-100℃ for 10-30 minutes to fully coat the surface of the conductive filler with the coupling agent and obtain the surface modified conductive filler. (2) Put the high-fluorine peroxy fluorinated rubber raw rubber into a two-roll mill, add surface-modified conductive filler and other raw materials, mix and then extrude sheets; (3) The mixed rubber compound is re-rolled through a thin pass at least 15 times; (4) The recycled rubber compound is subjected to a first-stage vulcanization at a temperature of 165-175℃ and a pressure of 15-30MPa for 10-35 minutes to allow the rubber compound to undergo preliminary cross-linking and shaping. Then, a second-stage vulcanization is carried out at 230-290℃ for 12-24 hours to obtain the product.