A highly branched polyolefin cable sheath and its preparation method

By using materials such as furan-side linear polyethylene and single-end maleimide-modified partially hydrogenated polyolefin long-chain arms, a highly branched polyolefin cable sheath with reversible comb-like long-chain branching is formed, solving the problem of irreversible branching and achieving reversible recycling and good dispersibility of the material.

CN123062889APending Publication Date: 2026-11-10SHANDONG LINGHANGYUAN ELECTRIC POWER EQUIPMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611532269.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, the branching bonds of highly branched polyolefin cable sheaths are irreversible, which means that waste cannot be 100% recycled and its performance cannot be maintained. It is difficult to balance high branching degree, molding precision, flame retardancy and recyclability.

Method used

Using furan-containing linear polyethylene, single-end maleimide-modified partially hydrogenated polyolefin long chain arms, unmodified polyethylene, non-reactive polar compatibilizer, and double-layer passivated halogen-free flame retardant filler, comb-like long chain branches with reversible grafting of single-end long chain arms are formed through annular die extrusion and low-temperature branching conditioning, thus avoiding permanent cross-linking networks.

Benefits of technology

It achieves low stress difference and low mold expansion during the melting process. The pipe has environmental stress cracking resistance and melt recovery capability under service conditions. It also has good filler dispersion and can be 100% recycled for reprocessing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062889A_ABST
    Figure CN123062889A_ABST
Patent Text Reader

Abstract

This invention proposes a highly branched polyolefin cable sheath and its preparation method, belonging to the technical field of highly branched polyolefin materials. The invention uses furan-containing side-based linear polyethylene, single-end maleimide-modified partially hydrogenated polyolefin long-chain arms, unmodified polyethylene, non-reactive polar compatibilizer, and double-layer passivated halogen-free flame-retardant filler as raw materials. These materials are first melt-mixed and extruded through an annular die to maintain a low reversible cycloaddition conversion rate. Then, through crystallization lock-type molding and low-temperature branching conditioning, comb-like long-chain branching with reversible grafting of single-end long-chain arms is formed, avoiding permanent cross-linking networks and ensuring that the filler interface and branching chemistry are independent, resulting in a highly branched polyolefin cable sheath. This invention solves technical problems such as excessive melt elasticity leading to uncontrolled single-layer extrusion molding precision and poor interfacial compatibility between highly branched polyolefin and halogen-free flame-retardant filler leading to deterioration of mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of highly branched polyolefin materials technology, specifically to a highly branched polyolefin cable sheath and its preparation method. Background Technology

[0002] Currently, polyolefin cable sheaths are often manufactured by introducing long-chain branched or cross-linked structures to improve melt strength, resistance to environmental stress cracking, and creep resistance. However, traditional linear polyolefin melt strength is relatively low, and while permanent cross-linking or irreversible branching can improve strength, it is prone to gelation, deterioration of processing fluidity, and the inability to remelt and recycle waste materials. It is difficult to achieve a balance between high branching degree, molding accuracy, flame retardancy, and recyclability.

[0003] To address the aforementioned problems, CN122381251A discloses a highly branched polyolefin plastic granule and its preparation method. This method employs a stepwise reactive extrusion process of "grafting followed by chain extension," where maleic anhydride free radical grafting is completed in the front section of a twin-screw extruder, while a trifunctional branching agent is fed in the middle and rear sections. This allows the epoxy or isocyanate groups to undergo ring-opening reactions with the anhydride, forming a star-shaped or dendritic highly branched structure and inhibiting cross-linking gelation, thereby improving melt strength. However, the ester or imide bonds formed by this method are permanent covalent bonds, and the branched structure cannot dissociate during secondary melting, failing to restore the linear topology. When waste is recycled, the branched network remains, leading to a decrease in the flowability and mechanical properties of the recycled material, making it difficult to achieve 100% recycling. Furthermore, the multifunctional branching agent connects multiple polyolefin chains, essentially remaining an irreversible network, making it impossible to simultaneously achieve high branching and reprocessability.

[0004] CN122645697A discloses a weather-resistant highly branched polyolefin protective film and its preparation process. The highly branched polyolefin resin is prepared by polymerization or reactive extrusion of long-chain branching and used in a three-layer co-extrusion blown film protective film. The high degree of branching improves melt strength and film thickness uniformity. However, its long-chain branching is also a permanent covalent bond, which cannot be dissociated by heating. The branching structure is irreversible during recycling and reprocessing, making it impossible to achieve 100% recycling of waste film while maintaining performance. The reactive extrusion long-chain branching process is also prone to gelation. Although the gel content is controlled below 2.0%, there is still a risk of irreversible crosslinking.

[0005] In summary, while existing technologies can improve melt strength or weather resistance through permanent covalent branching, the branching bonds are irreversible and cannot be dissociated to restore the linear topology during secondary melting. This results in the inability to achieve 100% recycling of waste materials while maintaining performance. Therefore, there is an urgent need to develop a high-branching polyolefin cable sheath that maintains a low melt elastic linear topology in the processing state, forms reversible comb-like long-chain branching in the service state, and allows for 100% recycling and re-extrusion of waste materials, along with its preparation method. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a highly branched polyolefin cable sheath and its preparation method. The invention uses furan-containing linear polyethylene, single-ended maleimide-modified partially hydrogenated polyolefin long-chain arms, unmodified polyethylene, non-reactive polar compatibilizer, and double-layer passivated halogen-free flame-retardant filler as raw materials. These materials are first melt-mixed and extruded through an annular die to maintain a low reversible cycloaddition conversion rate. Then, through crystallization lock-type molding and low-temperature branching conditioning, a comb-like long-chain branched structure with reversible grafting of single-ended long-chain arms is formed, avoiding permanent cross-linking networks and ensuring that the filler interface and branching chemistry are independent, resulting in a highly branched polyolefin cable sheath.

[0007] This invention proposes a highly branched polyolefin cable sheath. Based on 100 parts by weight of the total polyolefin resin, the composition includes 44.00-55.00 parts of component A, 11.00-14.00 parts of component B, 18.00-23.00 parts of HDPE, 2.00-6.00 parts of LLDPE, 1.00-10.00 parts of resin compatibilizer, and the balance being hydrogenated polybutadiene with inert end caps. The total amount of the above resin components is 1... 00 parts; in addition, it includes 70.00~120.00 parts of passivated magnesium hydroxide, 0.50~8.00 parts of zinc borate and 3.50~5.50 parts of processing stabilizers, wherein the processing stabilizers include 1.50~2.20 parts of antioxidant 1010 (excluding components A and B), 1.00~1.50 parts of phosphite antioxidant 168, 0.70~1.20 parts of hindered amine light stabilizer 622, and the balance is phenothiazine.

[0008] This invention also proposes a method for preparing a highly branched polyolefin cable sheath, the specific technical solution of which is as follows: Step 1: Add furfurylamine to molten maleic anhydride-grafted polyethylene, heat and react, then apply vacuum and maintain the reaction. Subsequently, add n-octylamine and antioxidant, mix and use as component A. Mix hydrogenated polybutadiene with one end amino and the other end hydrogen-capped with maleic anhydride, heat and react, then apply vacuum. Add acetic anhydride and antioxidant and continue the vacuum reaction. Mix and use as component B.

[0009] Step 2: Heat and dry magnesium hydroxide in a high-speed mixer, then spray octadecylphosphonic acid solution into it, keep it at a certain temperature and recover the solvent, then add polyethylene wax and continue mixing, and then vacuum dry to obtain passivated magnesium hydroxide.

[0010] Step 3: After drying zinc borate and resin particles, mix component A, polyethylene, compatibilizer and stabilizer, then add component B and hydrogenated polybutadiene with inert ends. Add the mixture to a twin-screw extruder, and simultaneously add passivated magnesium hydroxide and zinc borate through a side feeder. Then melt-blend and extrude under vacuum conditions and pelletize underwater. After drying, obtain the pellets.

[0011] Step 4: The granules are added to a single-screw pipe extruder and melted, then extruded through a die to form a pipe blank. The pipe blank then stays in a vacuum sizing sleeve heated by a jacket, and then enters a hot air tunnel. After exiting the tunnel, it is cooled by spraying, traction and cut, and after being placed, the desired high-branched polyolefin cable sheath pipe is obtained.

[0012] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. During the melting process, the single-end long chain arm can be detached from the main chain, thereby reducing the first normal stress difference and mold expansion. After the tube body is sized, the comb-like long chain branching is formed, avoiding the branching reaction from interfering with the flow distribution in the annular die.

[0013] 2. The branched arm can only be connected at one end and cannot bridge two main chains, so that the pipe can obtain long chain drag and topological constraint in service, without forming a permanent cross-linked network, thus taking into account both environmental stress cracking resistance and melt recovery capability.

[0014] 3. Neither the phosphonate inner layer nor the polyolefin wax outer layer of the flame-retardant filler participates in the reaction, so that the filler dispersion, interface compatibilization and dynamic branching are achieved through independent mechanisms, reducing the consumption of branching sites and interface voids. Attached Figure Description

[0015] Figure 1 The images show the FTIR spectra of the sample from Example 1 at different process stages. Detailed Implementation

[0016] Obviously, based on the above description of the present invention, and in accordance with common technical knowledge and conventional methods in the field, various other modifications, substitutions, or alterations can be made without departing from the basic technical concept of the present invention.

[0017] This invention proposes a method for preparing a highly branched polyolefin cable sheath, the specific technical solution of which is as follows: 1. Functionalization and Endcapping Maleic anhydride-grafted polyethylene and mono-amino-terminated hydrogenated polybutadiene were functionalized and capped, respectively, following reaction, vacuum desaturation, capping, and the addition of antioxidants. The anhydride groups of the maleic anhydride-grafted polyethylene underwent ring-opening amidation with furfurylamine to form ammonium acid. Under heating and vacuum conditions, the ammonium acid underwent dehydration and cyclization to form N-furfuryl succinimide side groups, allowing the furan ring to be linked to the imide nitrogen via a methylene group. The imide ring was then attached to the polyethylene backbone through the grafting point. Subsequently, reaction water and excess furfurylamine were removed under vacuum. The residual anhydride reacted with n-octylamine, undergoing ammonium acid dehydration and imidization to form an N-octyl succinimide capped structure, which passivated the residual anhydride side group sites, preventing their retention. The added antioxidants inhibited molten thermal oxidation and free radical chain scission.

[0018] Hydrogenated polybutadiene with one amino terminus and the other hydrogen-capped is mixed with maleic anhydride. The primary amine reacts with the anhydride to form an ammonium acid through ring-opening. Heating causes the ammonium acid to dehydrate and form maleimide end groups, while the hydrogen-capped end group does not participate in the reaction. Acetic anhydride reacts with the residual primary amine to form acetamide end groups, reducing the free primary amine content and inhibiting the thermal oxidation of the polyolefin chain through antioxidants. Product B is predominantly a single-terminated maleimide functional structure, with controlled double-terminated impurities. Therefore, the long chain arms mainly form single-point grafted comb-like long chain branching, with only a very small amount of double-terminated impurities potentially forming interchain connections, but their content is controlled and insufficient to form a permanent cross-linked network.

[0019] 2. Flame-retardant filler double-layer passivation After drying, magnesium hydroxide is sprayed with octadecylphosphonic acid, kept at a constant temperature, and the solvent is recovered. Polyethylene wax is then added and vacuum dried. The magnesium hydroxide surface contains hydroxyl groups. The phosphonic acid groups in the octadecylphosphonic acid coordinate or condense with these surface hydroxyl groups, forming a phosphonate anchoring layer. This causes the long-chain alkyl groups to extend outward, reducing surface polarity. Isopropanol is used as a solvent to carry the octadecylphosphonic acid dispersed on the magnesium hydroxide surface. Temperature control allows the phosphonic acid groups to fully interact with the surface hydroxyl groups. Meanwhile, the polyethylene wax melts under heating conditions, partially coating the surface of the anchored alkyl chains, forming a low surface energy outer layer. This polyethylene wax outer layer provides a low surface energy similar to polyolefins, thus improving wetting. The outer and inner layers are mainly bonded through van der Waals forces, hydrophobic interactions, and physical coating, possibly accompanied by local co-crystallization, but without covalent reactions.

[0020] Residual solvents and moisture are removed by vacuum drying, reducing interparticle hydrogen bond aggregation. The inner phosphonate layer bonds to the magnesium hydroxide surface, while the outer polyethylene wax layer adheres partially, forming a non-reactive bilayer structure. This reduces filler aggregation and improves wetting and dispersion with the polyolefin matrix. It is not designed to consume furan or maleimide groups, and due to the low organic coating, some polar sites remain on the particle surface that are not obscured by the polyethylene wax, facilitating subsequent dipole adsorption with compatibilizer ester groups. This structure reduces surface hydroxyl density, decreases interparticle hydrogen bonds, and improves wetting and dispersion with polyolefins. Neither the inner nor outer layers contain reactive groups such as amino, mercapto, furan, or maleimide groups, and therefore do not participate in dynamic covalent reactions.

[0021] 3. Twin-screw melt granulation Resin, additives, component B, and inert long-chain arms are mixed sequentially, and flame-retardant filler is added via a side feeder. The mixture is then vacuum melt-blended using a twin-screw extruder, underwater pelletized, and dried to obtain granules. First, moisture is removed from zinc borate and resin particles under heating and vacuum conditions. Component A, polyethylene, compatibilizer, and stabilizer are then mixed and dispersed under the shear and heat action of the twin-screw extruder. Component B and hydrogenated polybutadiene with inert end caps are added and dispersed in the resin phase. Passivated magnesium hydroxide and zinc borate are added directly to the twin-screw extruder via a side feeder without premixing, avoiding mechanical shearing damage to the phosphonate inner layer and polyethylene wax outer layer on the surface of magnesium hydroxide during the premixing stage.

[0022] When the temperature inside the twin-screw extruder reaches the set range, the reversible cycloaddition equilibrium of furan-maleimide shifts towards the reverse Diels-Alder reaction, causing reversible bond dissociation. The long-chain polyolefin arms of component B dissociate from the main chain, resulting in a low melt elasticity linear topology in the polymer phase, thus reducing melt elasticity. Passivated magnesium hydroxide particles disperse in the low-elasticity melt, and their phosphonate inner layer no longer undergoes new coordination reactions, while the polyethylene wax outer layer does not participate in coordination reactions. Interfacial compatibilization is achieved through the wetting of the polyethylene wax outer layer with the polyolefin and the dipole adsorption and chain entanglement of the compatibilizer. Specifically, the ethylene segments of the compatibilizer entangle with the matrix, and the ester groups undergo dipole adsorption with the partially covered local polar sites of the polyethylene wax outer layer. These two processes synergistically disperse the filler in the low-elasticity melt. After vacuum degassing to remove moisture, volatiles, and bubbles, the melt is extruded through a die and underwater pelletized. Cooling allows the polymer to crystallize and solidify, and then drying removes surface moisture from the pellets to obtain pellets for subsequent extrusion.

[0023] 4. Extrusion sizing and post-branching molding The granules are melted and extruded into a tube blank, which is then vacuum sizing, hot air holding, spray cooling, traction cutting, and placement to produce a sheathed tube. The granules are heated, melted, and plasticized in a single-screw pipe extruder. The melt is extruded through a die to form a tube blank. When the tube blank enters the jacketed, heated vacuum sizing sleeve, the vacuum negative pressure keeps the outer wall of the tube blank tightly against the inner wall of the sizing sleeve. The heat from the jacket keeps the temperature of the tube blank uniform. The tube blank completes dimensional calibration and crystallization locking in the vacuum sizing sleeve, and the outer diameter and wall thickness are fixed. After leaving the sizing sleeve, the tube blank enters the hot air tunnel. The hot air maintains the temperature of the tube blank within a range that allows the polymer chain segments to move. In the amorphous region, furan groups and maleimide groups undergo reversible cycloaddition to form long-chain branching points. Since the long chain arms are single-end reactions, each long chain arm can connect to at most one main chain, thus forming a side-connected long-chain branching point rather than a permanent cross-linked network. After exiting the tunnel, spray cooling rapidly reduces the temperature of the tube blank, and the crystalline structure stabilizes, thus shaping the tube body. Then, the continuous tube body is segmented by traction and cutting.

[0024] During placement, reversible cycloaddition continues in the amorphous region, and the density of reversible long-chain branching points, calculated based on the main chain carbon atoms of component A, gradually increases to 0.2~1.2 per 1000 main carbon chain atoms. This density is significantly higher than the near-zero long-chain branching point density of linear polyolefins. The number-average molecular weight of each long chain arm is much greater than that of polyethylene entanglement, and it is dominated by a single-terminal maleimide functional structure. The double-terminal reaction impurities are controlled. Therefore, when branching points connect to long chain arms, they mainly form side-connected long-chain branching points. Only a very small amount of double-terminal impurities may generate inter-chain connections, and their content is insufficient to form a permanent cross-linked network. This results in a tube with low irreversible gel content and melt flow rate. As a result, a relatively high branching degree structure is formed in the tube, with long chain arms as branching units, a branching point density significantly higher than that of linear polyolefins, and each branching point connecting to a long chain.

[0025] To further illustrate the highly branched polyolefin cable sheath proposed in this invention, specific embodiments and comparative examples are given below. Table 1 shows the information of each raw material used in the embodiments.

[0026] Table 1 Raw Material Information Table ; ; Example 1 The feed amount in this embodiment is based on a total dry weight of 100 parts by weight of the non-volatile components of the resin phase, including 54.00 parts of component A, 13.50 parts of component B, 21.00 parts of HDPE, 5.00 parts of LLDPE, 1.50 parts of hydrogenated polybutadiene with inert ends, and 5.00 parts of ethylene-butyl acrylate copolymer, totaling 100 parts of the resin phase; in addition, 90.00 parts of sequentially surface-treated passivated magnesium hydroxide, 4.00 parts of zinc borate, and 4.72 parts of... Processing stabilizers include 2.00 parts of antioxidant 1010, 1.20 parts of phosphite antioxidant 168, 1.00 parts of hindered amine light stabilizer 622, and 0.52 parts of phenothiazine. The antioxidant 1010 contained in the preparation of components A and B is included in the dry mass of components A and B respectively, and is not repeatedly deducted or added from the above-mentioned additional 2.00 parts of antioxidant. The actual weight of each commercial raw material is determined by dividing the corresponding dry basis target mass by the measured non-volatile matter mass fraction of the batch.

[0027] S1: In a closed system equipped with high-torque mixing, nitrogen protection, controlled liquid feeding, condensation recovery, and vacuum devolatilization functions, 1000.00g of maleic anhydride-grafted high-density polyethylene and 0.200g of antioxidant 1010 are added. Under nitrogen protection, the temperature is raised to 170°C to melt the resin. Then, 5.3815g of furfurylamine is added at a 0.98 equivalent. A controlled nitrogen atmosphere is maintained during the feeding stage. The temperature is then raised to 180°C for mixing, and samples are taken periodically to assess the furfurylamine binding and imidization process. Once the binding reaches stability, the absolute pressure is gradually reduced to 20kPa to remove water and free low-molecular-weight substances. Finally, 0.1g of maleic anhydride-grafted high-density polyethylene and 0.200g of antioxidant 1010 are added at a 1.05 equivalent of the residual anhydride. 535g of n-octylamine was further vacuum-mixed and devolatilized to complete the imidization and end-capping of residual anhydride with n-octylamine until the residual anhydride on a dry basis was no higher than 0.001 mmol / g. The mixture was then discharged and cooled to obtain component A, which appeared as grayish-white granules. Component A had a solid content of 99.75%–99.90%, a furanyl content of 0.05–0.06 mmol / g, a melt flow rate of 0.55–0.75 g / 10 min, a residual anhydride on a dry basis of <0.001 mmol / g, free furfurylamine not exceeding 0.002 mmol / g, free n-octylamine not exceeding 0.003 mmol / g, and a weight-average molecular weight of (1.0–1.4) × 10⁻⁶. 5 g / mol, with a molecular weight distribution of 4.0–5.0; In another closed apparatus equipped with high-torque mixing, nitrogen protection, controlled liquid feeding, condensation recovery, and vacuum devolatilization functions, 250.00 g of hydrogenated polybutadiene with one amino terminus and the other hydrogen end capped was used as a calculation unit, with a dry polymer mass of 248.25 g. 4.8474 g of maleic anhydride and 0.050 g of antioxidant 1010 were added. The reaction was first carried out under nitrogen at 105 °C for 10 min to open the ring, followed by the addition of 0.1087 g of acetic anhydride. The temperature was raised to 175 °C and a vacuum was applied to -0.085 MPa for 10 min. The mixture was then mechanically stirred at 120 r / min for 3 min at 175 °C. The material was then discharged and cooled to obtain component B, which was a pale yellow, viscous, blocky substance. The solid content of component B was 99.65%–99.75%, the number average molecular weight was 4400–4800 g / mol, the weight average molecular weight was 5000–5300 g / mol, the molecular weight distribution was 1.05–1.15, the maleimide group content was 0.190–0.200 mmol / g, the average maleimide functionality was 0.90–0.93, the proportion of long chain arms with only a single maleimide end group was ≥90.0 mol%, the proportion of double-terminated amino chains was ≤0.3 mol%, and the residual free primary amine was <0.001 mmol / g.

[0028] S2: Add 1653.40g of magnesium hydroxide to a high-speed mixer and dry at 105℃ for 30min until the moisture content does not exceed 0.01wt%. Then transfer the dried magnesium hydroxide powder to a processing device with a closed, precipitated, electrostatically controlled, and appropriately explosion-proof design. Reduce the temperature to the spraying temperature confirmed by a safety assessment. Dissolve 13.23g of octadecylphosphonic acid in 250.00g of isopropanol to obtain a dispersion. Then slowly spray the dispersion into the high-speed mixer and keep it at 105℃ for 15min. Simultaneously, the condensation recovery device connected to the exhaust port of the high-speed mixer is turned on. Isopropanol vapor is condensed by the condenser and collected in the recovery tank until no obvious distillation is observed, thus completing solvent recovery. 8.27g of polyethylene wax is added to the system and melt-coated at 105℃ for 8 minutes, followed by drying at 105℃ and 40kPa absolute pressure for 2 hours. The resulting material is a white powder of passivated magnesium hydroxide with a D50 of 1.2~1.6μm and a BET specific surface area of ​​6.0~7.0m². 2 / g, with an organic coating content of 1.21~1.31wt%, an inner phosphonate content of 0.4~1.2wt%, an outer polyethylene wax content of 0.2~0.8wt%, and a water contact angle ≥105°.

[0029] S3: 74.27g of zinc borate was dried in a vacuum drying oven at 105℃ and -0.06MPa for 2 hours. HDPE and LLDPE were dried at 70℃ for 2 hours. 1002.65g of component A prepared from S1, 389.92g of HDPE, 92.84g of LLDPE, 92.84g of ethylene-butyl acrylate copolymer, 37.14g of antioxidant 1010, and 22.28g of phosphite antioxidants 168 and 18 were added. 57g of hindered amine light stabilizer 622 and 9.65g of phenothiazine were added to a high-speed mixer and mixed for 3 minutes. Then, 250.66g of component B prepared from S1 and 27.85g of hydrogenated polybutadiene with inert ends were added and mixed for 2 minutes to obtain a mixture. The mixture was then fed into the main feed port of a co-rotating twin-screw extruder. Simultaneously, 1671.08g of passivated magnesium hydroxide and 74.27g of dried zinc borate were fed into the twin-screw extruder via side feeders. In this process, the temperatures of each zone of the extruder are set as follows: 150℃, 165℃, 175℃, 185℃, 192℃, 195℃, 195℃, 190℃, and 185℃, respectively. The screw speed is 260 rpm, and a vacuum of -0.085 MPa is maintained inside the screw. The material is held in the zone ≥175℃ for 95 seconds. The exhaust pressure is 20 kPa. After the melt is extruded through the die, it is pelletized underwater and then dehumidified and dried at 50℃ until the moisture content is ≤0.15 wt%. % Obtain uncolored granules with an MFR of 0.5~0.8 g / 10 min and irreversible gel ≤2.0%; the reversible cycloaddition conversion rate at the die exit is defined as the percentage of maleimide moles that have undergone Diels-Alder cycloaddition at the die exit relative to the initial maleimide moles, and R is the percentage of maleimide moles that have undergone Diels-Alder cycloaddition at the die exit relative to the initial maleimide moles. t And compared with the initial area ratio R0 before mixing components A and B, the conversion rate is calculated according to the formula = Calculations show that the reversible cycloaddition conversion rate at the die outlet is ≤10.0%.

[0030] S4: The granules obtained in S3 are added to a single-screw pipe extruder equipped with a melt gear pump. The screw diameter is 65mm, the length-to-diameter ratio is 33, and the temperatures of each zone of the single screw are set as follows: 170℃, 180℃, 188℃, 194℃, 196℃, the die head temperature is 195℃, and the die temperature is 195℃. The melt pressure is 15MPa, the screw speed is 38rpm, and the traction speed is 0.25m / min. The melt is extruded through an annular die with a nominal outer diameter of 110mm and a die gap of 5.2mm to form a pipe blank. The target finished pipe blank has an outer diameter of 110mm and a wall thickness of 5.0mm. Subsequently, the pipe blank enters the vacuum sizing section with a jacket temperature of 102℃ and a vacuum degree of -0.035MPa and stays for a maximum of 300s, with an effective length of 1.25m, to complete dimensional calibration and crystallization locking. The pipe blank then leaves the sizing section. After being fitted, the cable sheath is placed in a hot air tunnel for 30 minutes. The effective length of the tunnel is 7.5m, the temperature is 70℃, and the wind speed is 1m / s. The outer circumference is continuously supported by low-friction rollers. After exiting the tunnel, it is cooled by water spray at 20℃ until the surface temperature does not exceed 35℃. It is then pulled by a double-track traction machine at a traction speed of 0.25m / min, cut into sections, and then placed at 23℃ and 50% relative humidity for 24 hours to obtain a highly branched polyolefin cable sheath with an outer diameter of 110mm and a nominal wall thickness of 5.0mm.

[0031] Example 2 The difference from the preparation method in Example 1 is as follows: S1: The reaction temperature of component A is 175℃, the heating temperature of component B is 170℃, the reaction time is 3min, the vacuum reaction time is 4min, and the remaining steps are the same.

[0032] Example 3 The difference from the preparation method in Example 1 is as follows: S1: The reaction temperature of component A is 182℃, the heating temperature of component B is 185℃, the reaction time is 6min, the vacuum reaction time is 10min, and the remaining steps are the same.

[0033] Example 4 The difference from the preparation method in Example 1 is as follows: S3: The temperatures of each zone of the extruder are 145℃, 160℃, 170℃, 180℃, 190℃, 190℃, 190℃, 185℃, and 180℃; the material residence time in the zone ≥175℃ is 75s, and the other steps are the same.

[0034] Example 5 The difference from the preparation method in Example 1 is as follows: S3: The temperatures of each zone of the extruder are 155℃, 170℃, 180℃, 190℃, 195℃, 200℃, 200℃, 195℃, and 190℃; the residence time of the material in the zone ≥175℃ is 180s, and the other steps are the same.

[0035] Example 6 The difference from the preparation method in Example 1 is as follows: S4: The jacket temperature of the vacuum sizing sleeve is 95℃, the residence time of the billet in the sizing sleeve is 20s, the hot air tunnel temperature is 60℃, and the rest of the steps are the same.

[0036] Example 7 The difference from the preparation method in Example 1 is as follows: S4: The jacket temperature of the vacuum sizing sleeve is 110℃, the residence time of the billet in the sizing sleeve is 60s, the hot air tunnel temperature is 75℃, and the remaining steps are the same.

[0037] Example 8 The difference from the preparation method in Example 1 is as follows: The amount of materials used in this embodiment is based on a total of 100 parts by weight of the resin phase, including 44.00 parts of component A, 11.00 parts of component B, 18.00 parts of HDPE, 2.00 parts of LLDPE, 15.00 parts of hydrogenated polybutadiene with inert ends, and 10.00 parts of ethylene-butyl acrylate copolymer, totaling 100 parts of the resin phase. In addition, it includes 70.00 parts of passivated magnesium hydroxide, 0.50 parts of zinc borate, and 3.5 parts of processing stabilizers. The processing stabilizers include 1.50 parts of antioxidant 1010, 1.00 part of phosphite antioxidant 168, 0.70 parts of hindered amine light stabilizer 622, and 0.30 parts of phenothiazine. The antioxidant 1010 mentioned here does not include the antioxidant 1010 added during the preparation of components A and B. All other steps are the same.

[0038] Example 9 The difference from the preparation method in Example 1 is as follows: The amount of materials used in this embodiment is based on a total of 100 parts by weight of the resin phase, including 55.00 parts of component A, 14.00 parts of component B, 23.00 parts of HDPE, 6.00 parts of LLDPE, 0.50 parts of hydrogenated polybutadiene with inert ends, and 1.50 parts of ethylene-butyl acrylate copolymer, totaling 100 parts of the resin phase. In addition, it includes 120.00 parts of passivated magnesium hydroxide, 8.00 parts of zinc borate, and 5.5 parts of processing stabilizers. The processing stabilizers include 2.20 parts of antioxidant 1010, 1.50 parts of phosphite antioxidant 168, 1.20 parts of hindered amine light stabilizer 622, and 0.60 parts of phenothiazine. The antioxidant 1010 mentioned here does not include the antioxidant 1010 added during the preparation of components A and B. All other steps are the same.

[0039] Example 10 The difference from the preparation method in Example 1 is as follows: S3: Replace the ethylene-butyl acrylate copolymer with the ethylene-ethyl acrylate copolymer, and the remaining steps are the same.

[0040] Comparative Example 1 The difference from the preparation method in Example 1 is as follows: S1: Component B is not prepared; S3: Replace component B with an equal mass of hydrogenated polybutadiene with inert ends.

[0041] This comparative example prepares a cable sheath without reversible long-chain branching points.

[0042] Comparative Example 2 The difference from the preparation method in Example 1 is as follows: S1: Component A is not prepared; S3: Replace component A with an equal mass of linear polyethylene containing an equal amount of N-butylsuccinimide but without furan.

[0043] This comparative example prepares a cable sheath without furan reaction sites.

[0044] Comparative Example 3 The difference from the preparation method in Example 1 is as follows: S1: Component B is not prepared; S3: Replace component B with 4,4'-diphenylmethane bismaleimide containing an equal amount of maleimide groups, and make up the mass part with hydrogenated polybutadiene with inert ends capped at both ends.

[0045] This comparative example prepares a cable sheath using a reversible cross-linked network constructed with a bifunctional cross-linking agent.

[0046] Comparative Example 4 The difference from the preparation method in Example 1 is as follows: Cancel S2; S3: Replace passivated magnesium hydroxide with an equal mass of unmodified magnesium hydroxide.

[0047] This comparative example shows the preparation of cable sheaths without magnesium hydroxide filling.

[0048] Comparative Example 5 The difference from the preparation method in Example 1 is as follows: S3: Replace the ethylene-butyl acrylate copolymer with an equal part by mass of HDPE.

[0049] This comparative example prepares cable sheaths without non-reactive compatibilizers.

[0050] Comparative Example 6 The difference from the preparation method in Example 1 is as follows: S4: After the tube blank is sized, it does not enter the hot air tunnel, but directly enters the water tank for cooling.

[0051] This comparative example shows the preparation of a cable sheath without post-branching conditioning sections.

[0052] Comparative Example 7 The difference from the preparation method in Example 1 is as follows: S4: The die temperature is 155℃, and the material stays in the front section of the die for 6 minutes.

[0053] This comparative example shows the pre-formed branched cable sheath inside the die.

[0054] Experimental Example 1 Thin slices containing 1.000 g of organic phase were cut from the cable sheaths prepared in Examples 1-10 and Comparative Examples 1-7, respectively, and refluxed in xylene at 140±2℃ for 24 h, with the solvent being replaced every 6 h. After reflux, the slices were filtered through a 100 μm metal mesh, washed three times with hot xylene, and then vacuum dried at 80℃ to constant weight. The inorganic filler was first deducted by ash content test, and then the mass percentage of insoluble organic matter in the initial organic phase was calculated. Three parallel samples were taken from each group as the irreversible gel content of the sample.

[0055] Take about 1g of the pipe slices prepared in the examples and comparative examples, press them into thin sheets at 190°C, and observe whether the resulting thin sheets can form a continuous and particle-free film. If a continuous particle-free film can be formed, it is determined that there is no permanent network.

[0056] Samples of the pipes prepared in the examples and comparative examples were taken from the pipe wall and crushed. Referring to GB / T3682.1-2018 "Determination of melt mass flow rate (MFR) and melt volumetric flow rate (MVR) of thermoplastics – Part 1: Standard methods", the samples were preheated at 190°C for 4 minutes, a 5 kg weight was applied, and timing began when the piston descended under gravity until the lower reference mark reached the top surface of the barrel. Every 40 seconds, the extruded melt strips were cut with a cutter and collected one by one. After cooling, the remaining strips were weighed individually, and the average mass of the strips was calculated. The melt mass flow rate was then calculated. Five parallel samples were taken for each sample, and the average value of all parallel samples was taken. The test results are shown in Table 2.

[0057] Table 2. Characterization results of reversible long-chain branching and non-permanent networks in the samples. ; As can be seen from Table 2, the irreversible gel content, meltability and MFR of the sample of the example are better than those of the comparative example. The irreversible gel content of Example 1 is the lowest, the MFR is in the preferred range and the meltability is "yes". This shows that the single-end long chain arm reversible comb-shaped long chain branching design of the present invention can effectively avoid permanent cross-linking network, ensure that the material can be repeatedly melted and processed and has suitable melt flowability.

[0058] In Comparative Example 1, component B was not prepared and was replaced with hydrogenated polybutadiene with inert ends. The system lacked single-ended maleimide long chain arms, and the furan group could not undergo a reversible Diels-Alder reaction with the maleimide group, thus failing to form reversible long chain branching points. The polymer phase lacked topological constraints, and the molecular chains were prone to irreversible thermal oxidation and free radical side reactions during processing, leading to an increase in irreversible gel content and a deviation of the MFR from the preferred range. Therefore, both the irreversible gel content and MFR were worse than those of the example.

[0059] In Comparative Example 2, component A was not prepared and was replaced with linear polyethylene containing an equal amount of N-butylsuccinimide but without furan. Since component A does not have furan side groups, it cannot undergo reversible cycloaddition with the maleimide group of component B, and cannot form reversible comb-like long chain branching. The melt lacks dynamic dissociation-bonding equilibrium at high temperature, and the processing heat history leads to the accumulation of irreversible side reactions. Therefore, the irreversible gel content increases, and the MFR deviates from the preferred range.

[0060] Comparative Example 3 replaced component B with 4,4'-diphenylmethane bismaleimide containing an equal amount of maleimide groups. Bismaleimide is a bifunctional crosslinking agent that can bridge two polyethylene backbones to form a reversible crosslinking network, rather than comb-like branching with single-end long chain arms. Although the DA bond can dissociate at 190°C, the bifunctional crosslinking agent causes multiple connection points between molecular chains. After dissociation, the flowable linear topology cannot be completely restored, resulting in an extremely high irreversible gel content and the inability to form a continuous particle-free film. The MFR is significantly low, so the meltability is "no". Both the irreversible gel content and MFR are significantly worse than those of the example.

[0061] In Comparative Example 4, S2 was removed, and an equal mass of unmodified magnesium hydroxide was used to replace passivated magnesium hydroxide. Unmodified magnesium hydroxide has high surface polarity and high hydroxyl density, making it prone to agglomeration and the formation of interfacial voids. During processing, stress concentration and local overheating occur around the filler agglomerates, inducing irreversible thermal oxidation and side reactions in the polymer, resulting in an increase in irreversible gel content.

[0062] Comparative Example 5 replaced the ethylene-butyl acrylate copolymer with an equal mass of HDPE. The lack of non-reactive polar compatibilizer resulted in the absence of ester group dipole adsorption anchoring at the local polar sites not covered by polyethylene wax. The interfacial wetting and dipole adsorption between magnesium hydroxide and the polyolefin matrix were insufficient, leading to poor filler dispersion. The local shear heat increased during processing, triggering irreversible side reactions in the polymer. Therefore, the irreversible gel content increased, and the MFR was high.

[0063] After the billet in Comparative Example 6 was sized, it did not enter the hot air tunnel but went directly into the water tank for cooling. The lack of a post-branching conditioning section meant that the reversible cycloaddition of furan-maleimide failed to form sufficient bonds in the intergranular amorphous region, resulting in insufficient density of long-chain branching points. At the same time, rapid cooling caused the chain segments in the amorphous region to freeze, and the residual stress could not be released. During the processing of recycled materials, stress release and side reactions led to an increase in irreversible gel content and a high MFR.

[0064] Comparative Example 7 set the die temperature to 155°C, with the material held in the die for 6 minutes. Although the reverse Diels-Alder reaction can occur at 155°C, the dissociation rate is lower than the dominant dissociation range above 175°C. During the longer holding time of 6 minutes, the melt temperature inside the die is insufficient to fully dissociate the furan-maleimide adduct, and the reversible cycloaddition equilibrium still leans towards the bonding direction. This leads to premature branching within the die, increased melt elasticity, and a higher die exit conversion rate than in the example. By the time the billet is shaped, the branched network has partially formed, resulting in localized stress concentration and irreversible side reactions. Consequently, the irreversible gel content increases, and the MFR is lower.

[0065] Experiment Example 2 The same formula and process as the examples and comparative examples were scaled up to continuous production scale. 20m sections were cut from the cable sheaths prepared in the scaled-up production. 8 points were measured at equal angles for each 1m section using an 8-channel ultrasonic thickness gauge, resulting in a total of 160 wall thickness values. The coefficient of variation (CV) of the wall thickness of the samples was calculated based on the data.

[0066] Take the pipes prepared in the examples and comparative examples, and measure the maximum and minimum outer diameters of the same cross section every 1m using a circumferential coordinate instrument. Calculate the roundness deviation of the sample according to the formula: roundness deviation = (maximum outer diameter - minimum outer diameter) / nominal outer diameter × 100%.

[0067] Table 3. Characterization results of sample tubing ; As can be seen from Table 3, the wall thickness variation coefficient and roundness deviation of the sample in the example are better than those of the comparative example. The wall thickness variation coefficient and roundness deviation of Example 1 are the lowest, indicating that the process of the present invention can effectively fix the tube blank size and release stress.

[0068] In Comparative Example 1, the system lacks single-ended maleimide long-chain arms, so the furan group cannot undergo a reversible Diels-Alder reaction with the maleimide group, and cannot form reversible long-chain branching points. The melt lacks dynamic dissociation-bonding equilibrium at the die exit, resulting in higher melt elasticity. After the billet enters the sizing sleeve, the dimensional fluctuation increases, thus the wall thickness variation coefficient and roundness deviation are higher than those in the Example.

[0069] In Comparative Example 2, component A lacks furan side groups and cannot undergo reversible cycloaddition with the maleimide group of component B. Similarly, it cannot form reversible comb-like long chain branching, resulting in higher melt elasticity, poor dimensional stability of the tube blank at the die exit, and uneven local cooling and shrinkage during shaping. Therefore, the coefficient of variation of wall thickness and roundness deviation are higher than those of the Example.

[0070] In Comparative Example 3, bismaleimide is a bifunctional crosslinking agent that can bridge two polyethylene backbones to form a reversible crosslinked network, rather than a comb-like branching of single-ended long chain arms. The bifunctional crosslinking agent creates multiple connection points between molecular chains. Although the DA bonds can dissociate at 190°C, the flowable linear topology cannot be completely restored after dissociation, resulting in the highest melt elasticity, severe extrusion swell, and the largest dimensional fluctuations in the billet after entering the sizing sleeve. Therefore, the wall thickness variation coefficient and roundness deviation are significantly higher than in the examples.

[0071] In Comparative Example 4, the unmodified magnesium hydroxide has high surface polarity and high hydroxyl density, making it prone to agglomeration and the formation of interfacial voids. During processing, local overheating and uneven cooling occur around the filler agglomerates, and the local shrinkage difference increases when the tube blank is shaped. Therefore, the wall thickness variation coefficient and roundness deviation are higher than those of the Example.

[0072] Comparative Example 5 lacks a non-reactive polar compatibilizer. Although the outer layer of polyethylene wax provides partial surface passivation, the local polar sites not covered by polyethylene wax lack ester dipolar adsorption anchoring. The wetting and dipolar adsorption at the interface between magnesium hydroxide and the polyolefin matrix are insufficient, the filler dispersion is poor, the melt viscosity fluctuation is increased, the flow distribution is uneven during tube blank extrusion, and the dimensional stability decreases during shaping. Therefore, the wall thickness variation coefficient and roundness deviation are higher than those of the Example.

[0073] Comparative Example 6 lacks a branching conditioning section at 60-75°C. The reversible cycloaddition of furan-maleimide fails to fully bond in the intergranular amorphous region, resulting in insufficient density of long-chain branching points. Simultaneously, rapid cooling freezes the chain segments in the amorphous region, preventing the release of residual stress. Consequently, the dimensional springback and shrinkage are uneven after the billet is shaped, leading to higher wall thickness variation coefficient and roundness deviation compared to the Example.

[0074] In Comparative Example 7, the die temperature was too low and the dwell time at the front of the die was too long, resulting in insufficient dissociation of DA bonds and premature formation of branches within the die. This led to increased melt elasticity and higher die exit conversion rate. By the time the billet was shaped, the branched network had already partially formed, causing localized stress concentration and disordered shrinkage sequence. Consequently, the wall thickness variation coefficient and roundness deviation were significantly higher than those of the Example.

[0075] Experimental Example 3 The flat surface of the cable sheath prepared in the examples and comparative examples was cut off. The surface was wiped with anhydrous ethanol and allowed to dry naturally. In an environment of 23±2℃ and 50±10% relative humidity, 5μL of deionized water was dropped onto the sample surface using a microsyringe. After the droplet stabilized on the surface for 30s, the water contact angle was read and recorded. Five positions were tested for each sample and the average value was taken.

[0076] 100mm×10mm×3mm specimens were prepared by molding using the same batch of granules and process as those used in the examples and comparative examples of cable sheathing pipes. Referring to GB / T2406.2-2009 "Determination of Combustion Behavior by Oxygen Index Method for Plastics - Part 2: Room Temperature Test", five specimens were prepared in each group. The specimens were vertically fixed in the combustion chamber, and an oxygen-nitrogen mixture was introduced. The top of the specimen was ignited with an igniter, and the combustion time and length of the specimen were recorded. The minimum oxygen concentration required to maintain combustion was determined by changing the oxygen concentration, and the average value of the five specimens was taken as the oxygen index of the sample.

[0077] 125mm×13mm×3mm specimens were prepared using the same batch of granules and process molding of the cable sheaths prepared in the examples and comparative examples. Vertical combustion tests were conducted in accordance with GB / T2408-2021 "Determination of Burning Performance of Plastics - Horizontal and Vertical Methods". Five specimens were prepared in each group. The specimens were vertically fixed on the support, and a standard flame was applied for 10 seconds before being removed. The afterflame time, afterglow time and whether the degreased cotton was ignited were recorded. The flammability rating was determined according to the standard.

[0078] 75mm × 75mm × 3mm specimens were prepared by molding using the same batch of granules and process as those used in the examples and comparative examples of cable sheathing. Referring to GB / T8323.2-2008 "Plastics Smoke Generation Part 2: Test Method for Determination of Smoke Density by Single Chamber Method", a 25kW / m³ pressure was used. 2 In flame mode, the sample was placed horizontally under the radiation cone inside the smoke density chamber. After the chamber door was closed, the sample was ignited. The light beam passed through the smoke inside the chamber and irradiated the photodetector. The attenuation of the light flux during the test was recorded and converted into specific optical density according to the standard formula. The maximum value during the entire test was taken as the maximum specific optical density of the sample. The test results are shown in Table 4.

[0079] Table 4. Characterization results of flame-retardant interface properties of samples ; As can be seen from Table 4, the water contact angle, oxygen index, vertical combustion rating and maximum specific optical density of the sample of the embodiment are better than those of the comparative example. The sample of embodiment 1 has the highest water contact angle, the highest oxygen index, the vertical combustion rating of V-0 and the lowest maximum specific optical density. This shows that the non-reactive double-layer passivated flame retardant filler system of the present invention can effectively reduce the surface polarity of the filler, improve the interface wetting and dispersion, and achieve a synergistic improvement in flame retardancy and smoke suppression.

[0080] In Comparative Example 1, the system lacks single-ended maleimide long-chain arms, so the furan group cannot undergo a reversible Diels-Alder reaction with the maleimide group, and cannot form reversible long-chain branching points. The polymer phase lacks topological constraints, resulting in increased melt viscosity fluctuations during processing and decreased uniformity of filler dispersion in the matrix. Although the phosphonate inner layer of passivated magnesium hydroxide and the polyethylene wax outer layer are present, the lack of a low-elasticity melt environment due to reversible branching leads to an increased tendency for filler agglomeration and an increase in interfacial voids. Consequently, the water contact angle decreases, the oxygen index decreases, the vertical combustion rating drops to V-1, and the maximum specific optical density increases.

[0081] Comparative Example 2: Component A has no furan side group and cannot undergo reversible cycloaddition with the maleimide group of Component B. Similarly, it cannot form reversible comb-like long chain branching. The melt lacks dynamic dissociation-bonding equilibrium at high temperature. The processing heat history leads to an increase in local shear heat around the filler, which may destroy the passivation layer. The polar hydroxyl groups on the filler surface are re-exposed, resulting in poor interfacial wetting. Therefore, the water contact angle decreases, the oxygen index decreases, the vertical combustion rating drops to V-1, and the maximum specific optical density increases.

[0082] In Comparative Example 3, bismaleimide is a bifunctional crosslinking agent that can bridge two polyethylene main chains to form a reversible crosslinking network, rather than a comb-like branching of single-end long chain arms. The bifunctional crosslinking agent causes multiple connection points between molecular chains. Although the DA bond can dissociate at the processing temperature, it still cannot completely restore the flowable linear topology after dissociation. This makes it difficult for the filler to be uniformly dispersed in the high-viscosity network, resulting in interfacial voids and stress concentration around the agglomerates. During combustion, heat transfer is uneven, and the char structure is discontinuous. Therefore, the water contact angle is the lowest, the oxygen index is the lowest, the vertical combustion rating drops to V-2, and the maximum specific optical density is the highest.

[0083] In Comparative Example 4, the unmodified magnesium hydroxide has high surface polarity and high hydroxyl density, making it prone to agglomeration and the formation of interfacial voids. During combustion, the surface hydroxyl groups promote the release of flammable volatiles, resulting in a decrease in flame retardant efficiency. At the same time, the uncoated filler has poor wettability with the polyolefin matrix and uneven dispersion during processing. Therefore, the water contact angle is significantly reduced, the oxygen index decreases, the vertical burning rating drops to V-1, and the maximum specific optical density increases.

[0084] In Comparative Example 5, a non-reactive polar compatibilizer was lacking. Although the outer layer of polyethylene wax provided some surface passivation, the local polar sites not covered by polyethylene wax lacked ester dipolar adsorption anchoring. The wetting and dipolar adsorption at the interface between magnesium hydroxide and the polyolefin matrix were insufficient, resulting in poor filler dispersion, increased agglomerates, and the filler's inability to effectively isolate heat and oxygen during combustion. The char layer was incomplete, thus reducing the water contact angle, decreasing the oxygen index, lowering the vertical combustion rating to V-1, and increasing the maximum specific optical density.

[0085] Comparative Example 6 lacked a branching conditioning section at 60-75℃. The reversible cycloaddition of furan-maleimide failed to fully bond in the intercrystalline amorphous region, resulting in insufficient density of long-chain branching points, inadequate stress release inside the tube, freezing of chain segments in the amorphous region, and poor bonding between the filler and the matrix. During combustion, interface debonding and voids increased, thus reducing the water contact angle, decreasing the oxygen index, lowering the vertical combustion rating to V-1, and increasing the maximum specific optical density.

[0086] In Comparative Example 7, the die temperature was too low and the dwell time at the front of the die was too long, resulting in insufficient dissociation of DA bonds and premature formation of branching within the die. This increased melt elasticity and die exit conversion rate. By the time the tube blank was shaped, the branched network had already partially formed, leading to uneven distribution of filler in the tube wall, increased local agglomeration and interface defects, and uneven release of heat and smoke during combustion. Consequently, the water contact angle decreased, the oxygen index dropped, the vertical combustion rating decreased to V-2, and the maximum specific optical density increased.

[0087] Experiment Example 4 Fourier transform infrared spectrometer equipped with a single-reflection diamond ATR accessory and an MCT detector was used to perform in-situ FTIR tests on the sample of Example 1 (denoted as A1) at four process stages: pre-conditioned, high-temperature state, re-conditioned, and secondary high-temperature. The spectral acquisition range was 4000~600 cm⁻¹. -1 4cm resolution -1 A single spectral scan consisted of 16 scans, with dry nitrogen purging throughout the test. The ATR clamping stroke was kept constant to ensure consistent contact conditions between the sample and the diamond crystal. Wavenumber calibration was performed daily using a polystyrene standard film, and the actual sample temperature was recorded using a calibration thermocouple placed close to the crystal. Atmospheric correction and measurements were performed at 710~650 cm⁻¹ before testing. -1 Local baseline correction within the interval, selecting 690cm. -1 The characteristic absorption peaks of maleimide in the vicinity were normalized using the inert characteristic bands of polyethylene to obtain the normalized absorbance of the characteristic peaks of maleimide under different conditions. A zero-conversion reference baseline was determined using the spectrum of the comparative C1 sample to characterize the dynamic changes in the reversible cycloaddition reaction of furan-maleimide DA. The results are as follows: Figure 1 As shown.

[0088] Figure 1 The following are FTIR spectra of the sample from Example 1 at different process stages. It can be seen that at 690 cm⁻¹... -1 The area near the peak represents the characteristic absorption of free maleimide. In the conditioned state, the furan group undergoes a DA cycloaddition reaction with the maleimide group, resulting in a significant consumption of free maleimide. Therefore, this characteristic peak exhibits the lowest normalized absorbance. When the sample is heated to a high temperature, the reversible DA cycloaddition product undergoes reverse DA dissociation, and the DA adduct cleaves, releasing free maleimide again. (690 cm⁻¹) -1 The absorbance of the characteristic peak increased significantly. Subsequently, the sample was subjected to hot air conditioning at 70°C again, allowing the free maleimide to undergo a renewed DA addition reaction with the furan group, causing the absorbance of the characteristic peak to drop again. A second heating triggered the reverse DA reaction, causing the concentration of free maleimide to rise again, and the absorbance of the characteristic peak to increase again. This spectral change confirms that the furan-maleimide DA covalent bond in this system possesses thermal reversibility, providing a molecular-level reaction basis for achieving controllable transformation of the topological structure of polyolefin molecules, while considering pipe forming accuracy, service mechanical properties, and melt recovery performance, in accordance with the specific raw material structure and step-by-step processing sequence of this invention.

Claims

1. A highly branched polyolefin cable sheath, made from a polyolefin composition by extrusion molding and heat conditioning, characterized in that: Based on a total resin phase dry basis mass of 100 parts by weight, the resin phase comprises 44.00-55.00 parts of component A, 11.00-14.00 parts of component B, 18.00-23.00 parts of high-density polyethylene, 2.00-6.00 parts of linear low-density polyethylene, 1.00-10.00 parts of resin compatibilizer, and 0.50-15.00 parts of hydrogenated polybutadiene with inert ends, totaling 100 parts by weight; relative to the... The composition comprises 100 parts by weight of resin phase, and further comprises 70.00-120.00 parts of passivated magnesium hydroxide, 0.50-8.00 parts of zinc borate, and 3.50-5.50 parts of processing stabilizer, wherein the processing stabilizer comprises 1.50-2.20 parts of antioxidant 1010 (excluding components A and B), 1.00-1.50 parts of phosphite antioxidant 168, 0.70-1.20 parts of hindered amine light stabilizer 622, and the balance being phenothiazine.

2. The highly branched polyolefin cable sheath according to claim 1, characterized in that: Component A is linear polyethylene containing furan side groups, with a solid content of 99.75%~99.90%, a furan group content of 0.05~0.06 mmol / g, a melt flow rate of 0.55~0.75 g / 10 min, a dry basis residual anhydride of <0.001 mmol / g, free furfurylamine not exceeding 0.002 mmol / g, free n-octylamine not exceeding 0.003 mmol / g, and a weight-average molecular weight of (1.0~1.4)×10⁻⁶. 5 g / mol, with a molecular weight distribution of 4.0~5.

0.

3. The highly branched polyolefin cable sheath according to claim 1, characterized in that: Component B is a single-terminal maleimide-terminated linear partially hydrogenated polyolefin long-chain arm with a solid content of 99.65%~99.75%, a number-average molecular weight of 4400~4800 g / mol, a weight-average molecular weight of 5000~5300 g / mol, a molecular weight distribution of 1.05~1.15, a maleimide group content of 0.190~0.200 mmol / g, an average maleimide functionality of 0.90~0.93, a long-chain arm with only a single maleimide end group of ≥90.0 mol%, a double-terminal amino chain of ≤0.3 mol%, and residual free primary amine <0.001 mmol / g.

4. The highly branched polyolefin cable sheath according to claim 1, characterized in that: The composition has an MFR of 0.5~0.8 g / 10 min and an irreversible gel content of ≤2.0%.

5. A method for preparing a highly branched polyolefin cable sheath as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1: Add furfurylamine to molten maleic anhydride-grafted polyethylene, heat and react, then apply vacuum and maintain the reaction. Add n-octylamine and antioxidant, mix and use as component A. Mix hydrogenated polybutadiene with one amino end and the other hydrogen end capped with maleic anhydride, heat and react, then apply vacuum and maintain the reaction. Add acetic anhydride and antioxidant and continue the vacuum reaction. Mix and use as component B. S2: Magnesium hydroxide is heated and dried in a high-speed mixer, then octadecylphosphonic acid solution is sprayed into it, the solvent is recovered after heat preservation, polyethylene wax is added to it and mixing is continued, and then vacuum drying is performed to obtain passivated magnesium hydroxide. S3: After drying zinc borate and resin particles, mix component A, polyethylene, resin compatibilizer and processing stabilizer, then add component B and hydrogenated polybutadiene with inert ends. Add the mixture to a twin-screw extruder, and simultaneously add passivated magnesium hydroxide and zinc borate through a side feeder. Then melt-blend and extrude under vacuum conditions and pelletize underwater. After drying, obtain the pellets. S4: The granules are added to a single-screw pipe extruder and melted, then extruded through a die to form a pipe blank. The pipe blank then stays in a vacuum sizing sleeve heated by a jacket to complete dimensional calibration and crystallization locking. It then enters a hot air tunnel and stays there. After exiting the tunnel, it is cooled by spraying, traction and cut, and after being placed, the required high-branched polyolefin cable sheath pipe is obtained.

6. The method for preparing a highly branched polyolefin cable sheath according to claim 5, characterized in that: The heating reaction temperature in S1 is 175~182℃; the temperature of the heating reaction is 170~185℃, and the reaction time is 3~6min; the vacuum reaction time is 4~10min.

7. The method for preparing a highly branched polyolefin cable sheath according to claim 5, characterized in that: The passivated magnesium hydroxide described in S2 has a D50 of 1.2~1.6 μm and a BET specific surface area of ​​6.0~7.0 m². 2 / g, with an organic coating content of 1.21~1.31wt%, an inner phosphonate content of 0.4~1.2wt%, an outer polyethylene wax content of 0.2~0.8wt%, and a water contact angle ≥105°.

8. The method for preparing a highly branched polyolefin cable sheath according to claim 5, characterized in that: The resin compatibilizer described in S3 is an ethylene-butyl acrylate copolymer, an ethylene-ethyl acrylate copolymer, or a mixture thereof.

9. The method for preparing a highly branched polyolefin cable sheath according to claim 5, characterized in that: The twin-screw extruder described in S3 has temperature zones of 145~155℃, 160~170℃, 170~180℃, 180~190℃, 190~195℃, 190~200℃, 190~200℃, 185~195℃, and 180~190℃, respectively, and the material stays in the zone ≥175℃ for 75~180s.

10. The method for preparing a highly branched polyolefin cable sheath according to claim 5, characterized in that: The temperature of the jacket heating in S4 is 95~110℃; the time the tube blank stays in the vacuum sizing sleeve of the jacket heating is 20~60s; the temperature of the hot air tunnel is 60~75℃.

Citation Information

Patent Citations

  • Weather-resistant highly-branched polyolefin protective film and preparation process thereof