A bio-based oil-resistant and moisture-proof coating agent for cardboard surfaces and its preparation method

By constructing a bimodal hydrophobic dispersion system and an environmentally responsive network, the problems of oil and moisture resistance and crease damage during the use of cardboard surface coatings were solved, achieving efficient oil and moisture resistance and crease repair for cardboard, while also taking into account alkaline pulp recycling performance, thus improving the stability and adaptability of the coating.

CN123063006APending Publication Date: 2026-11-10JIANGXI SANHE PAPER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448780.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing bio-based coatings on cardboard surfaces struggle to simultaneously achieve planar oil and moisture resistance, barrier retention after crease damage, and alkaline pulp recycling performance. Furthermore, these coatings are prone to developing through-cracks and reduced continuity during use.

Method used

A bimodal hydrophobic dispersion system with different particle sizes, softening temperatures, and interfacial affinity was constructed by using a fibrous film-forming component in an aqueous dispersion medium, first and second bio-based hydrophobic dispersion phases, an interface-modifying component, and an environmentally responsive network component. This system forms a thickness-direction gradient coating. The first hydrophobic phase is enriched on the air side, while the second hydrophobic phase is retained in the continuous phase and dissociated under alkaline conditions through the environmentally responsive network.

Benefits of technology

It improves the planar oil and moisture resistance of cardboard, enhances the barrier retention of crease areas, and can effectively dissociate during alkaline pulping, while taking into account both usage stability and recyclability. The coating agent remains stable during storage and coating processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063006A_ABST
    Figure CN123063006A_ABST
Patent Text Reader

Abstract

This application relates to the field of paperboard barrier coating technology, and in particular to a bio-based oil-blocking and moisture-proof coating agent for paperboard surfaces and its preparation method. The agent comprises a fibrous film-forming component, a first bio-based hydrophobic dispersed phase, a second bio-based hydrophobic dispersed phase, an interface-modifying component, and an environmentally responsive network component. The two hydrophobic dispersed phases have different particle sizes, softening temperatures, and interfacial affinity, forming a bimodal dispersion system. During preparation, two hydrophobic emulsions are prepared separately, compounded under medium-low shear conditions, and then amino- and carboxyl-containing biopolymers are added to form a reversible ion-associative network. After coating and drying, the first hydrophobic phase is enriched towards the air side, while the second hydrophobic phase remains inside the coating, improving planar oil-blocking and moisture-proof performance and crease / crack sealing capabilities. Under alkaline pulping conditions, the network weakens and promotes coating dissociation and paper fiber recycling. This application achieves a balance between planar oil-blocking and moisture-proofing, barrier retention after crease damage, and alkaline pulping recycling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of paperboard barrier coating technology, and in particular to a bio-based oil-blocking and moisture-proof coating agent for paperboard surface and its preparation method. Background Technology

[0002] Cardboard is formed from interwoven plant fibers, and its surface contains hydrophilic groups and inter-fiber pores, allowing oils and moisture to easily penetrate along capillary channels. Therefore, when used for food and other protective packaging, it usually requires oil-blocking and moisture-proofing treatment. Existing bio-based coatings mostly utilize hydrophilic polymers such as starch, cellulose derivatives, and chitosan to form a continuous film to seal the pores on the cardboard surface. However, the barrier stability of such coatings tends to decrease after moisture absorption. Using plant waxes or plant lipids can improve surface hydrophobicity, but if the particle size, content, and spatial distribution of the wax phase are not properly controlled, the continuity of the hydrophilic polymer film can be easily disrupted, or the wax can enter the pores of the cardboard along with the aqueous phase, making it difficult to form an effective surface hydrophobic enrichment layer.

[0003] Furthermore, during the creasing, folding, and boxing processes of cardboard, the outer surface of the coating is subjected to tensile forces, which easily leads to the formation of through-cracks, significantly reducing the oil and moisture barrier performance in the crease area. While increasing the cross-linking strength of the coating may maintain stability during use, it could hinder coating swelling and dissociation during waste paper pulping, increasing screen residue and affecting paper fiber recycling. Therefore, how to achieve planar oil and moisture barrier performance, barrier retention after crease damage, and alkaline pulping recycling performance using the same water-based bio-based coating system is a problem that existing technologies need to address. Summary of the Invention

[0004] This application provides a bio-based oil-resistant and moisture-proof coating agent for cardboard surfaces and its preparation method, in order to solve the above-mentioned problems.

[0005] In a first aspect, this application provides a bio-based oil-blocking and moisture-proof coating agent for cardboard surfaces, comprising an aqueous dispersion medium and a fibrophilic film-forming component, a first bio-based hydrophobic dispersion phase, a second bio-based hydrophobic dispersion phase, an interface-modifying component, and an environmentally responsive network component dispersed in the aqueous dispersion medium. The fibrous film-forming component includes at least one bio-based polysaccharide with a hydrophilic group, used to form a continuous coating phase and penetrate into the inter-fiber pores of the paperboard surface; The first bio-based hydrophobic dispersion phase comprises plant waxes and / or hydrogenated plant lipids, and the median volumetric particle size D50 of the dispersed droplets is 0.8–4.0 μm; The second bio-based hydrophobic dispersion phase includes plant-derived lipids with plastic flow capability, the median volumetric particle size D50 of the dispersed droplets is 0.10 to 0.80 μm, and the softening temperature of the second bio-based hydrophobic dispersion phase is lower than that of the first bio-based hydrophobic dispersion phase. The interface-modifying component is at least coated on the microdroplet surface of the second bio-based hydrophobic dispersion phase, such that the interfacial affinity between the second bio-based hydrophobic dispersion phase and the fibrophilic film-forming component is higher than the interfacial affinity between the first bio-based hydrophobic dispersion phase and the fibrophilic film-forming component. The environmentally responsive network components include amino-containing biopolymers and carboxyl-containing biopolymers. The amino-containing biopolymers and the carboxyl-containing biopolymers form an ion-association network under the weakly acidic to near-neutral conditions of the coating agent. Under alkaline conditions, the ion-association network is weakened due to the reduced protonation degree of the amino-containing biopolymers. The first bio-based hydrophobic dispersion phase and the second bio-based hydrophobic dispersion phase constitute a bimodal hydrophobic dispersion system with different particle sizes, so that when the coating agent is coated on the paperboard and dried, the first bio-based hydrophobic dispersion phase is enriched relative to the second bio-based hydrophobic dispersion phase towards the air side of the coating, and the second bio-based hydrophobic dispersion phase is retained in the continuous phase formed by the fibrous film-forming component.

[0006] Optionally, the fibroblastic film-forming component includes modified starch and auxiliary polysaccharides. The modified starch is selected from at least one of oxidized starch, hydroxypropyl starch, carboxymethyl starch, and cationic starch. The auxiliary polysaccharides are selected from at least one of carboxymethyl cellulose, pectin, alginate, microfibrillated cellulose, and carboxymethyl chitosan. The modified starch accounts for 60-90% of the mass of the fibroblastic film-forming component, and the auxiliary polysaccharides account for 10-40% of the mass of the fibroblastic film-forming component.

[0007] Optionally, the first bio-based hydrophobic dispersed phase comprises a high-melting-point plant wax and a medium-melting-point plant lipid, wherein the high-melting-point plant wax is selected from at least one of carnauba wax, rice bran wax, sugarcane wax, and candelilla wax, and the medium-melting-point plant lipid is selected from at least one of soybean wax, hydrogenated vegetable oil, and plant-derived long-chain fatty acid esters; the high-melting-point plant wax accounts for 50-85% of the mass of the first bio-based hydrophobic dispersed phase, and the medium-melting-point plant lipid accounts for 15-50%.

[0008] Optionally, the second bio-based hydrophobic dispersion phase is selected from at least one of partially hydrogenated vegetable oil products, vegetable fatty acid glycerides, fatty acid monoglycerides, fatty acid diglycerides, and plant-derived soft waxes. The softening temperature of the second bio-based hydrophobic dispersion phase is 25–50°C, and its softening temperature is 10–45°C lower than that of the first bio-based hydrophobic dispersion phase.

[0009] Optionally, the median volumetric size (D50) of the dispersed droplets in the first bio-based hydrophobic dispersed phase is 1.2–3.0 μm, the median volumetric size (D50) of the dispersed droplets in the second bio-based hydrophobic dispersed phase is 0.20–0.60 μm, and the ratio of the D50 of the first bio-based hydrophobic dispersed phase to that of the second bio-based hydrophobic dispersed phase is 2.5–12.

[0010] Optionally, the interface-modifying component is selected from at least one of lecithin, sucrose fatty acid ester, protein emulsifier, amphiphilic chitosan derivative, and amphiphilic starch derivative; the interface-modifying component is at least distributed on the microdroplet surface of the second bio-based hydrophobic dispersion phase and binds to the fibrophilic film-forming component through hydrogen bonding and / or electrostatic interactions, so that the second bio-based hydrophobic dispersion phase is retained in the continuous phase formed by the fibrophilic film-forming component during the coating drying process.

[0011] Optionally, based on 100 parts of total solids excluding water in the coating agent, it includes: 40-70 parts of a fibrous film-forming component, 10-30 parts of a first bio-based hydrophobic dispersed phase, 5-20 parts of a second bio-based hydrophobic dispersed phase, 3-15 parts of an environmentally responsive network component, 1-5 parts of an interface-modifying component, and 2-10 parts of a bio-based plasticizer; the coating agent has a solid content of 15-35 wt% and a pH of 4.5-6.8.

[0012] Secondly, this application provides a method for preparing a bio-based oil-resistant and moisture-proof coating agent for cardboard surfaces, the preparation method comprising: S1. Add bio-based polysaccharides to water for dissolution and / or gelatinization to obtain an aqueous continuous phase containing the fibrous film-forming component; S2. Heat the plant wax and / or hydrogenated plant lipids to a molten state, and disperse the molten plant wax and / or hydrogenated plant lipids in the aqueous phase under the first emulsification condition, controlling the median particle size D50 of the resulting dispersed droplets to be 0.8-4.0 μm, to obtain the first hydrophobic emulsion. S3. Plant-derived lipids with a softening temperature lower than that of the hydrophobic component in the first hydrophobic emulsion are heated to a molten state, an interface conditioning component is added, and emulsification is carried out under the second emulsification conditions. The median particle size D50 of the resulting dispersed droplets is controlled to be 0.10-0.80 μm, so that a hydrophilic interface layer capable of interacting with the fibrous film-forming component is formed on the surface of the dispersed droplets, thereby obtaining the second hydrophobic emulsion. S4. Under the condition that the temperature of the aqueous continuous phase is 35-55°C, the first hydrophobic emulsion and the second hydrophobic emulsion are added to the aqueous continuous phase, and mixed under shear conditions that do not refine the dispersed droplets of the first hydrophobic emulsion to the particle size range of the second hydrophobic emulsion, to form a bimodal hydrophobic dispersion system containing a large-particle-size first bio-based hydrophobic dispersion phase and a small-particle-size second bio-based hydrophobic dispersion phase. S5. Add amino-containing biopolymers and carboxyl-containing biopolymers to the system obtained in step S4, and adjust the pH of the system to 4.5-6.8, so that the amino-containing biopolymers and the carboxyl-containing biopolymers undergo partial ion association, forming an environmentally responsive network that can limit the migration of the second bio-based hydrophobic dispersed phase without producing macroscopic flocculation, to obtain the bio-based oil-resistant and moisture-proof coating agent for the paperboard surface.

[0013] Optionally, in step S2, the plant wax and / or hydrogenated plant lipids are heated to 5-20°C above their highest melting point and then subjected to a first emulsification, controlling the D50 of the resulting first hydrophobic emulsion to be 1.2-3.0 μm. In step S3, the plant-derived lipids are melted and mixed with the interface regulation component, and emulsified under a second emulsification condition with a shear strength higher than the first emulsification condition in step S2, so that the D50 of the resulting second hydrophobic emulsion is controlled to be 0.20-0.60 μm.

[0014] Optionally, in step S4, the temperature of the aqueous continuous phase is controlled at 35-55°C. The first hydrophobic emulsion is added and dispersed first, and then the second hydrophobic emulsion is added. The mixture is compounded under mixing conditions with a shear strength lower than the second emulsification conditions in step S3, so that the ratio of the D50 of the compounded first bio-based hydrophobic dispersed phase to the second bio-based hydrophobic dispersed phase is maintained at 2.5-12. In step S5, after the bimodal hydrophobic dispersion system is formed, the amino-containing biopolymer and the carboxyl-containing biopolymer are added, and the pH of the system is adjusted to 4.5-6.8 so that the two form partial ion association without macroscopic flocculation, thereby obtaining the coating agent.

[0015] Through the above technical solution, this application has the following beneficial effects: A thickness-direction gradient barrier structure is formed. This application involves preparing a large-particle-size first hydrophobic emulsion and a small-particle-size second hydrophobic emulsion separately, and then compounding them under medium-to-low shear conditions to maintain a bimodal particle size structure. During the coating and drying process, the first hydrophobic phase accumulates towards the air side, while the second hydrophobic phase is confined within the coating by interface-modified components and an environmentally responsive network, thus forming a gradient coating with surface moisture resistance, continuous oil blocking, and internal flexible lipid dispersion characteristics under a single coating condition.

[0016] It balances the planar oil-resistant and moisture-proof properties of the paperboard. The fibrous film-forming component can penetrate and seal the pores between fibers on the surface of the paperboard, while the first hydrophobic phase enriched on the air side reduces the moisture transport rate. The paperboards obtained in Examples 1-3 all achieved a Kit grade of 12, with a Cobb 60 water absorption of less than 10.5 g / m² and a water vapor transmission rate of less than 95 g·m². - 24h - ¹, which can avoid the decrease in film continuity caused by simply increasing plant wax.

[0017] It improves the barrier retention and recovery capabilities of the crease area. The second hydrophobic phase has a lower softening temperature and smaller particle size, which can deform and redistribute when local stress is generated during cardboard folding, filling the micro-cracks in the crease and reducing the width and penetration of the cracks. In Example 2, the Kit grade can be restored from 8 to 12 after one fold, and the crack width reduction rate reaches 70.4%. After 5 folds and resting, the Kit grade is still maintained at 10.

[0018] A switching between stable operation under normal use and alkaline pulping dissociation is achieved. Amino-containing and carboxyl-containing biopolymers form a reversible ionic association network under weakly acidic to near-neutral conditions, improving coating cohesion and limiting the migration of the second hydrophobic phase. Under alkaline pulping conditions, the protonation degree of the amino-containing component decreases, and the network swells and weakens. In Example 3, the fiber dissociation rate reached 96.2% at pH 10.5, the slag rate was 2.4%, and the recoverable fiber yield reached 95.1%.

[0019] It exhibits good adaptability in preparation and storage stability. The two hydrophobic emulsions are emulsified separately and compounded using a low-shear process. The proportions of the first hydrophobic phase, the second hydrophobic phase, and the environmentally responsive network component can be adjusted according to the intended use of the paperboard, achieving an adaptive balance between moisture resistance, crease repair performance, and pulp recovery performance. In Examples 1-3, the viscosity change rate after standing at 25°C for 7 days was less than 6%, and no significant irreversible stratification or block flocculation was observed, which is beneficial for the storage and continuous coating of the water-based coating agent. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 A flowchart illustrating the preparation method of a bio-based oil-resistant and moisture-proof coating agent for cardboard surface according to an embodiment of this application; Figure 2This is a schematic diagram of the particle size distribution of a bimodal hydrophobic dispersion system provided in an embodiment of this application; Figure 3 This is a schematic diagram of a thickness direction gradient structure of coated paperboard provided in an embodiment of this application; Figure 4 This is a schematic diagram illustrating the formation and sealing process of coating creases and cracks, provided in an embodiment of this application. Figure 5 This is a schematic diagram of an environment-responsive network state switching provided in an embodiment of this application. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0023] Furthermore, the term "and / or" in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character " / " in this article, unless otherwise specified, generally indicates that the preceding and following related objects have an "or" relationship.

[0024] The embodiments of this application will now be described in further detail with reference to the accompanying drawings.

[0025] General Implementation This application provides a bio-based oil-blocking and moisture-proof coating agent for cardboard surfaces. The coating agent uses water as a dispersion medium and includes a fibrous film-forming component, a first bio-based hydrophobic dispersed phase, a second bio-based hydrophobic dispersed phase, an interface regulating component, and an environmentally responsive network component. Bio-based plasticizers, rheology modifiers, and defoamers can also be added according to actual coating needs.

[0026] This application does not achieve hydrophobic properties by simply increasing the content of plant waxes. Instead, it constructs two types of hydrophobic dispersed phases with different particle sizes, different softening temperatures, and different interfacial affinities in the same water-based coating agent. This allows the first bio-based hydrophobic dispersed phase to preferentially migrate to the air side of the coating during the paperboard coating and drying process, while the second bio-based hydrophobic dispersed phase remains more in the continuous phase formed by the fibrous film-forming components, thereby forming an oil-resistant and moisture-proof coating with a compositional gradient in the thickness direction.

[0027] Meanwhile, the second bio-based hydrophobic dispersion phase uses plant-derived lipids with low softening temperature and plastic flow capability. This allows the second bio-based hydrophobic dispersion phase to deform and redistribute to the crack area under local stress after microcracks are generated during the creasing and folding process of the cardboard. This reduces the possibility of forming continuous oil and moisture transport channels at the crease.

[0028] In addition, an environmentally responsive network is constructed through ion association between amino-containing biopolymers and carboxyl-containing biopolymers, which enables the coating to maintain structural stability under normal use conditions, while swelling and dissociation occur due to the weakening of ion association under alkaline pulping conditions of waste paper, thereby improving the redispersibility of paper fibers.

[0029] I. Fiber-loving film-forming components The fibrous film-forming component is used to form the continuous phase of the coating and wets the surface of the paperboard and partially penetrates the interfiber pores of the paperboard surface during the coating process.

[0030] The fibrous film-forming component includes at least one bio-based polysaccharide having hydroxyl, carboxyl, and / or other hydrophilic groups.

[0031] Preferably, the fibroblastic film-forming component includes modified starch and auxiliary polysaccharides.

[0032] The modified starch may be selected from at least one of oxidized starch, hydroxypropyl starch, carboxymethyl starch and cationic starch; the auxiliary polysaccharide may be selected from at least one of carboxymethyl cellulose, pectin, alginate, microfibrillated cellulose and carboxymethyl chitosan.

[0033] Preferably, the modified starch accounts for 60-90% of the mass of the fiber-forming film-forming component, and the auxiliary polysaccharide accounts for 10-40%.

[0034] Modified starch has good paper fiber wetting and film-forming ability, and can enter some of the inter-fiber pores on the surface of paperboard under the action of moisture, thereby reducing the number of through capillary channels inside the paperboard; auxiliary polysaccharides are used to improve the integrity, cohesive strength and interaction with environmentally responsive network components of continuous films.

[0035] The fiber-forming component is not required to completely penetrate the interior of the paperboard. Instead, it forms a gradually decreasing penetration distribution from the interior to the exterior during coating and initial drying, giving the area near the paperboard better pore-sealing ability.

[0036] II. First Bio-based Hydrophobic Dispersion Phase The first bio-based hydrophobic dispersion phase is mainly used to form a hydrophobic enrichment structure in the region of the coating near the air side.

[0037] The first bio-based hydrophobic dispersion phase includes plant waxes and / or hydrogenated plant lipids.

[0038] The plant wax can be selected from at least one of carnauba wax, rice bran wax, sugarcane wax, and candelilla wax; it can also be further combined with soybean wax, hydrogenated vegetable oil, or plant-derived long-chain fatty acid esters.

[0039] The preferred method is to use a combination of high-melting-point plant wax and medium-melting-point plant lipids, with the high-melting-point plant wax accounting for 50-85% of the mass of the first bio-based hydrophobic dispersed phase and the medium-melting-point plant lipids accounting for 15-50%.

[0040] The first bio-based hydrophobic dispersion exists in the coating agent in the form of microdroplets, with its volume median particle size D50 controlled to be 0.8–4.0 μm, preferably 1.2–3.0 μm.

[0041] The first bio-based hydrophobic dispersion is not intended to obtain the smallest possible emulsion particle size.

[0042] By maintaining it at a relatively large micron-sized particle size, on the one hand, the extent to which it enters the tiny capillaries of the cardboard with the aqueous phase is reduced, and on the other hand, it is easier for it to be relatively enriched on the upper part of the coating during the process of the coating moisture evaporating from the air side.

[0043] If the particle size of the first bio-based hydrophobic dispersed phase is too small, it is easy for it to migrate into the interior of the paperboard together with the fiber-friendly film-forming component, weakening the moisture-proof enrichment effect on the outer surface; if the particle size is too large, it is easy to cause a decrease in the stability of the coating liquid and a rough coating surface.

[0044] Therefore, this application controls the emulsification strength of the first bio-based hydrophobic dispersed phase to ensure that it is within a particle size range that allows for stable coating but does not easily penetrate into the micropores of the cardboard.

[0045] III. Second Bio-based Hydrophobic Dispersion Phase The second bio-based hydrophobic dispersion phase is mainly used to form flexible lipid microdomains dispersed within the continuous phase.

[0046] The second bio-based hydrophobic dispersion phase may be selected from at least one of partially hydrogenated vegetable oil products, vegetable fatty acid glycerides, fatty acid monoglycerides, fatty acid diglycerides, and plant-derived soft waxes.

[0047] Preferably, the softening temperature of the second bio-based hydrophobic dispersion is 25–50°C, and more preferably 30–45°C.

[0048] The softening temperature of the second bio-based hydrophobic dispersion is lower than that of the first bio-based hydrophobic dispersion, and preferably the difference between the two softening temperatures is 10–45 °C.

[0049] The volume median particle size D50 of the second bio-based hydrophobic dispersion is 0.10–0.80 μm, preferably 0.20–0.60 μm.

[0050] The D50 ratio of the first bio-based hydrophobic dispersion to the second bio-based hydrophobic dispersion is preferably 2.5 to 12.

[0051] This results in the formation of a bimodal hydrophobic dispersion system in the coated agent that can be distinguished from each other on the particle size scale.

[0052] The second bio-based hydrophobic dispersion phase not only achieves retention by having a smaller particle size than the first bio-based hydrophobic dispersion phase, but also enhances its interaction with the fibrous film-forming components through interface-modifying components.

[0053] IV. Interface Modulation of the Second Bio-based Hydrophobic Dispersion Phase The interface-modifying component used for the second bio-based hydrophobic dispersion phase may be selected from at least one of lecithin, sucrose fatty acid esters, protein emulsifiers, amphiphilic chitosan derivatives, and amphiphilic starch derivatives.

[0054] During emulsification, the interface-modifying components are distributed on the surface of lipid droplets in the second bio-based hydrophobic dispersion phase.

[0055] The hydrophilic groups in the interface regulating component are oriented towards the aqueous phase and can form hydrogen bonds, electrostatic interactions, and / or intermolecular associations with fibrous film-forming components such as modified starch, carboxymethyl cellulose, and pectin.

[0056] Therefore, compared with the first bio-based hydrophobic dispersion phase, the second bio-based hydrophobic dispersion phase has a higher degree of interfacial compatibility with the fibrophilic film-forming continuous phase.

[0057] As moisture gradually evaporates and the concentration of the continuous phase increases, the droplets of the second bio-based hydrophobic dispersion are more easily confined by the continuous phase network, rather than migrating entirely to the air side.

[0058] The first and second bio-based hydrophobic dispersed phases thus produce different thickness orientation distributions.

[0059] It should be noted that the second bio-based hydrophobic dispersed phase in this application is "retained within the continuous phase" and does not require it to be completely and uniformly fixed at a certain depth of the coating. Rather, it means that, relative to the first bio-based hydrophobic dispersed phase, it has a higher degree of relative retention in the middle of the coating and in the area near the cardboard.

[0060] V. Environmentally Responsive Networks The environmentally responsive network components include amino-containing biopolymers and carboxyl-containing biopolymers.

[0061] The amino-containing biopolymer is preferably chitosan and / or chitosan derivatives.

[0062] Carboxyl-containing biopolymers can be at least one of pectin, alginate, carboxymethyl cellulose, and carboxymethyl starch.

[0063] Under weakly acidic to near-neutral conditions of the coating agent, some amino groups of amino-containing biopolymers undergo protonation and can form ion associations with carboxyl groups in carboxyl-containing biopolymers.

[0064] This forms reversible network nodes dispersed in the fibrous continuous phase.

[0065] The environmentally responsive network does not form a completely solidified, permanent cross-linked structure.

[0066] The network strength should be such that it can enhance the cohesiveness of the continuous phase and limit the excessive migration of the second bio-based hydrophobic dispersed phase, while not causing macroscopic flocculation of the coated agent.

[0067] The determination can be made by observing the flow state and static stability of the reagent during the preparation process.

[0068] Under suitable conditions, the coating agent maintains continuous fluidity and does not produce large, visible flocculent aggregates; after a short period of standing, no significant aqueous phase precipitation occurs, and normal roller coating, bar coating, or scraper coating can be performed.

[0069] Preferably, the pH of the coating agent is controlled at 4.5 to 6.8.

[0070] If the pH is too low, the protonation degree of amino-containing biopolymers will be too high, which will easily lead to excessive ion association and cause local flocculation; if the pH is too high, the protonation degree of amino-containing biopolymers will be insufficient, which is not conducive to the formation of an ion network for fixing the second hydrophobic dispersed phase.

[0071] VI. Composition range of coating agents Based on a total solid mass excluding water of 100 parts, the coating agent preferably includes: 40-70 parts of a fibrous film-forming component; 10-30 parts of a first bio-based hydrophobic dispersed phase; 5-20 parts of a second bio-based hydrophobic dispersed phase; 3-15 parts of an environmentally responsive network component; 1-5 parts of an interface modifier component; and 2-10 parts of a bio-based plasticizer. A small amount of rheology modifier and defoamer may also be added as needed.

[0072] The bio-based plasticizer can be one or more of glycerol, sorbitol, and xylitol, used to reduce the brittleness of the fibrous continuous phase after drying.

[0073] The solid content of the final coating agent is preferably 15-35 wt%, and more preferably 20-30 wt%.

[0074] At 25°C, the viscosity of the coating agent is preferably controlled at 300–2500 mPa·s, and more preferably at 500–1800 mPa·s, in order to balance the storage stability of the emulsion, the leveling properties of the paperboard surface, and the control of the coating amount.

[0075] VII. General Preparation Methods for Coating Agents The coating agent described in this application can be prepared in the following manner.

[0076] S1. Preparation of fibrous aqueous continuous phase Add the prescribed amount of water to the reaction vessel and heat to 70–90°C.

[0077] Add the modified starch slowly while stirring to ensure it is evenly dispersed and gelatinized and / or fully swollen, avoiding powder agglomeration caused by adding it all at once.

[0078] After maintaining the above temperature for 10–40 minutes, gradually cool down to 40–65°C.

[0079] Add carboxymethyl cellulose, pectin, or other auxiliary polysaccharides, and continue stirring for 20–60 minutes to fully hydrate the auxiliary polysaccharides.

[0080] If necessary, filter out large particles that are not fully dissolved to obtain a homogeneous aqueous continuous phase.

[0081] S2, Preparation of the first hydrophobic emulsion Add plant waxes and / or hydrogenated plant lipids to a heating container and heat to 5–20°C above their highest melting point until the hydrophobic components are completely melted.

[0082] Add an appropriate amount of emulsifying component in the molten state and mix thoroughly.

[0083] The molten hydrophobic phase is gradually added to the aqueous phase at a similar temperature, and shear emulsification is performed under the first emulsification conditions.

[0084] During the first emulsification process, the shearing time and shearing intensity are adjusted according to the equipment used to control the median particle size D50 of the dispersed droplets in the resulting emulsion to be 0.8–4.0 μm, preferably 1.2–3.0 μm.

[0085] After emulsification, a sample is taken to measure the particle size. Once the target particle size range is reached, high-intensity shearing is stopped to obtain the first hydrophobic emulsion.

[0086] S3, Preparation of the second hydrophobic emulsion Plant-derived lipids with low softening temperatures are heated to a molten state, and interface-modifying components are added.

[0087] The resulting lipid phase was added to the aqueous phase and then emulsified using a high shear strength.

[0088] The second emulsification conditions are higher than the effective emulsification strength during the preparation of the first hydrophobic emulsion, so that the second hydrophobic emulsion forms smaller lipid droplets.

[0089] By adjusting the shear speed, homogenization pressure, number of homogenization cycles and / or processing time, the D50 of the second hydrophobic emulsion is controlled to be 0.10–0.80 μm, preferably 0.20–0.60 μm.

[0090] During emulsification, the interface-modifying components adsorb onto the lipid droplet interface, forming an interface layer containing hydrophilic groups on the outer side of the resulting droplets.

[0091] After emulsification, the particle size was measured to obtain the second hydrophobic emulsion.

[0092] S4, Construction of a Bimodal Hydrophobic Dispersion System Adjust the temperature of the aqueous continuous phase obtained in step S1 to 35-55℃.

[0093] The first hydrophobic emulsion obtained in step S2 is added under medium-low shear conditions to make it uniformly dispersed in the continuous phase.

[0094] Then add the second hydrophobic emulsion obtained in step S3 and continue mixing.

[0095] The shear strength of the compound in this step is lower than that used in step S3 to prepare the second hydrophobic emulsion, and the mixing time is controlled to prevent the first hydrophobic emulsion from being further refined to the particle size range of the second hydrophobic emulsion.

[0096] Particle size distribution was tested after the compounding was completed.

[0097] If two main particle size distribution regions corresponding to the smaller second hydrophobic dispersed phase and the larger first hydrophobic dispersed phase can be identified in the particle size distribution, and the D50 relationship between the two meets the preset requirements, it indicates that the bimodal hydrophobic dispersion system is maintained.

[0098] S5, Construction of Environmentally Responsive Networks Add amino-containing biopolymers and carboxyl-containing biopolymers to the bimodal dispersion system obtained in step S4.

[0099] The order of addition can be adjusted according to the solubility state of the selected components.

[0100] Amino-containing biopolymers are preferably prepared in advance as a homogeneous aqueous solution or dispersion and then added slowly to avoid excessive local concentrations that may cause significant flocculation.

[0101] The final pH was adjusted to 4.5–6.8 using a weak acid and / or buffer system.

[0102] Under these conditions, partial ion association occurs between the amino-containing component and the carboxyl-containing component.

[0103] Then add plasticizer, rheology modifier and defoamer, and mix evenly under low speed conditions.

[0104] After standing and degassing, the surface of the cardboard is coated with a bio-based oil-blocking and moisture-proofing agent.

[0105] VIII. Detection of Bimodal Hydrophobic Dispersion Systems The particle size distribution of the first hydrophobic emulsion, the second hydrophobic emulsion, and the coating agent after the two emulsions are combined can all be detected by laser particle size analysis.

[0106] The volume median particle size D50 of the first and second hydrophobic emulsions were recorded respectively.

[0107] After compounding, the coating agent should be observed to determine whether it still retains two distinguishable main particle size distribution regions.

[0108] The term "bimodal hydrophobic dispersion system" as used in this application does not require the formation of two completely separate and non-overlapping sharp peaks in the particle size distribution curve. Rather, it refers to two main particle size groups of two types of hydrophobic dispersed phases that can maintain their respective differences in migration and interfacial behavior at the particle size scale.

[0109] IX. Paperboard Coating Method The resulting coating agent can be applied to food packaging paperboard, kraft paperboard, white cardboard, or other paper-based materials mainly composed of plant fibers.

[0110] To reduce the impact of differences in base paper on barrier performance evaluation, the same batch, same basis weight, and same surface treatment state of the same set of examples and comparative examples are preferred.

[0111] Before coating, the cardboard is equilibrated in a constant temperature and humidity environment.

[0112] The agent is applied to the surface of the cardboard to be treated in one pass using rod coating, doctor blade coating, roller coating, or other water-based coating equipment.

[0113] The dry coating amount can be controlled to be 4–18 g / m², preferably 6–14 g / m².

[0114] In the same test group, it is preferable to control the actual dry coating amount of each sample to be at a similar level, so as to avoid the difference in coating amount from masking the technical effects brought by the bimodal structure and environmental response network.

[0115] 10. Formation of Gradient Structures After coating, a two-stage drying method is preferred.

[0116] The first stage is the migration orientation stage.

[0117] The drying temperature in the first stage can be controlled at 40-70℃, so that the moisture in the coating gradually evaporates, but the fiber-friendly continuous phase has not yet been cured quickly and completely.

[0118] During this stage, some of the fiber-friendly film-forming components permeate into the pores of the paperboard surface under the capillary action of the paper fibers.

[0119] The migration of the first bio-based hydrophobic dispersion phase into the paperboard is limited due to its large particle size and low interfacial affinity with the continuous phase.

[0120] As moisture on the air side continues to evaporate, the first bio-based hydrophobic dispersed phase gradually accumulates on the air side of the coating relative to the fiber-friendly continuous phase.

[0121] Meanwhile, the second bio-based hydrophobic dispersed phase, due to its smaller particle size and the fact that its surface interface conditioning layer can interact strongly with the continuous phase, is mostly retained in the middle and upper regions of the coating.

[0122] The drying time for the first stage can be controlled to be 10–120 seconds, depending on the coating amount and the heat exchange capacity of the equipment.

[0123] The second stage is the structural locking stage.

[0124] Raising the temperature to 75–110°C further removes residual moisture, allowing the fibrous film-forming components to form a continuous membrane and strengthening hydrogen bonding and environmentally responsive ion-associated networks.

[0125] The first bio-based hydrophobic dispersed phase undergoes moderate contact and aggregation in the surface region, thereby forming a relatively continuous surface hydrophobic enrichment structure.

[0126] This results in a gradient coating that exhibits characteristics of permeation sealing, continuous oil blocking, flexible lipid dispersion, and surface hydrophobic enrichment from the cardboard side to the air side.

[0127] The aforementioned functional areas are not a multi-layered structure with clear, independent interfaces, but rather a continuously changing compositional gradient.

[0128] XI. Verification Methods for Gradient Distribution To verify that the first and second bio-based hydrophobic dispersed phases exhibit different migration behaviors within the coating, cross-sectional microanalysis can be used for characterization.

[0129] For example, two types of hydrophobic phases can be pre-labeled using fluorescent substances with different tracer properties, and coatings can be prepared without significantly altering the emulsification and migration behavior of the two types of hydrophobic phases.

[0130] A cross-section was prepared along the thickness direction of the dried coating, and the relative signal distribution of the two hydrophobic phases on the air side, the middle region, and the paperboard side was obtained by fluorescence microscopy.

[0131] If the relative signal intensity of the first bio-based hydrophobic dispersed phase is significantly higher on the air-side region than on the cardboard side, while the second bio-based hydrophobic dispersed phase still maintains a clear distribution in the middle region, it can be demonstrated that there is differential migration between the two types of hydrophobic phases.

[0132] The thickness distribution can also be further verified by using cross-sectional SEM combined with appropriate component analysis, infrared spectroscopy layer testing, or other methods that can distinguish the content of organic hydrophobic components.

[0133] 12. Crease Treatment and Crack Sealing Cut the coated and fully dried cardboard into the specified size.

[0134] Fold the coating surface along the set fold line so that it is outside the fold line, and then fold it 180°.

[0135] Hold the folded cardboard for a short time before unfolding it.

[0136] Tensile strain is generated on the outer side of the coating during the folding process.

[0137] When the local strain of a continuous film phase exceeds its bearing capacity, microcracks may occur near the crease.

[0138] The second bio-based hydrophobic dispersion phase of this application has a low softening temperature, and its droplets are dispersed inside the continuous phase.

[0139] During the folding process, local compression, tension and shear stress are generated near the crack tip, causing plastic deformation of the flexible lipid micro-regions and redistribution of some lipids to the vicinity of the crack.

[0140] After the cardboard is unfolded and left to stand, the flexible lipids can fill some of the crack gaps.

[0141] At the same time, some hydrogen bonds can be reformed between starch, cellulose or other polysaccharide chains that re-contact on both sides of the crack.

[0142] Therefore, the originally continuous through crack at the crease can be transformed into a tortuous mass transfer channel with reduced width, local discontinuity, or separation by hydrophobic lipids.

[0143] It should be noted that the "crack sealing" or "repair" referred to in this application does not require the coating after crease to be completely restored to the state before crease in terms of microstructure. Rather, it refers to reducing the penetration degree of crease cracks through the deformation and redistribution of the second bio-based hydrophobic dispersed phase, so that the oil-blocking performance after folding and standing is higher than that of the control coating without the second bio-based hydrophobic dispersed phase.

[0144] If necessary, the cardboard can be subjected to a short-term, mild heat treatment at 30–55°C after folding to improve the local flowability of the second hydrophobic dispersed phase, thereby further improving the degree of crack filling.

[0145] XIII. Evaluation of Crease Repair Performance Oil-blocking performance can be evaluated using the grease barrier rating test methods commonly used for paper and paperboard.

[0146] The coating area without folding, the crease area tested immediately after folding, and the crease area tested after folding and leaving it to stand for a certain period of time were measured respectively.

[0147] in: The oil resistance rating before folding is denoted as K0; The immediate oil resistance rating after folding is denoted as K1. The oil resistance rating after folding and resting is recorded as K2.

[0148] The degree of crease barrier recovery of different systems can be compared based on K0, K1 and K2.

[0149] When it is necessary to normalize the evaluation of the recovery ability of different samples, the recovery rate R can be used to represent it: R=(K2-K1) / (K0-K1)×100%.

[0150] When K0 and K1 are the same, the above recovery rate is not used for evaluation; instead, the oil resistance rating before and after folding is directly compared.

[0151] In addition, the same crease location can be observed immediately after folding and observed again after standing, and the changes in typical crack width, crack continuity or number of through cracks per unit length can be recorded to help verify the crack-sealing effect of the second bio-based hydrophobic dispersed phase.

[0152] XIV. Evaluation of Oil Repellency and Moisture Proof Performance The oil-blocking performance of the flat area of ​​the cardboard can be evaluated using the Kit grade and verified by combining it with the edible oil static penetration test.

[0153] The water absorption performance can be determined by the Cobb method, which measures the amount of water absorbed per unit area of ​​cardboard over a certain period of time.

[0154] The moisture-proof performance is further evaluated by water vapor transmission rate.

[0155] This application does not use simply increasing the static contact angle of water droplets as the sole criterion for judging moisture resistance performance. Instead, it combines the evaluation of Cobb water absorption, water vapor transmission rate and actual oil resistance performance to reflect the overall barrier capability of the coating.

[0156] 15. Alkaline pulping response After the cardboard is used, it can be put into the waste paper pulping system.

[0157] To evaluate the impact of environmentally responsive networks on repulping performance, coated paperboard was cut to specified dimensions and pulping media were added at the same solid-liquid ratio.

[0158] Near-neutral pulping conditions and alkaline pulping conditions were set up separately.

[0159] The pH of near-neutral pulping conditions can be controlled between 6.5 and 7.5.

[0160] The pH of alkaline pulping conditions can be controlled at 9–12, preferably 10–11, while the pulping temperature is controlled at 30–60°C.

[0161] Under alkaline conditions, the protonation degree of amino-containing biopolymers decreases, and their electrostatic association with carboxyl-containing biopolymers weakens.

[0162] The original continuous network absorbs water and swells.

[0163] As the coating is mechanically agitated and sheared, it gradually breaks down, allowing water to penetrate further into the surface fibers of the cardboard and the areas where the fibers intersect.

[0164] The paperboard fibers gradually disperse from a sheet-like bonded state to a single fiber or small bundle state.

[0165] By comparing the degree of fiber dissociation under near-neutral and alkaline conditions, it can be used to determine whether an environmental response network has pH-triggered characteristics.

[0166] XVI. Evaluation of Pulping Performance After the specified pulping time is completed, the pulp is sieved through a specified sieve.

[0167] Collect unseparated paper scraps, larger coating fragments, and other sieve residues, dry them, and weigh them.

[0168] The slag rate is calculated based on the dry mass of the feed and the dry mass of the slag.

[0169] Simultaneously, the fiber pulp after passing through the screen can be filtered, dried, and weighed to evaluate the yield of recyclable fibers.

[0170] The degree of fiber dissociation can be characterized by the mass ratio of fibers that have dispersed into single fibers or small fiber bundles within a specified time.

[0171] The examples and comparative examples used the same pulping equipment, solid-liquid ratio, temperature, rotation speed and processing time to eliminate the influence of different mechanical processing conditions.

[0172] This application focuses on the following comparisons: First, the coating can maintain its oil-blocking and moisture-proof structure under normal or near-neutral conditions; Secondly, in an alkaline pulping environment, the network interaction between amino-containing and carboxyl-containing components is reduced, making the coating more prone to dissociation than coatings without the aforementioned environmentally responsive network.

[0173] 17. Synergistic Relationships Among Various Technical Features The bimodal hydrophobic dispersion system, environmentally responsive network, and staged drying in this application are not independent technical measures.

[0174] The first bio-based hydrophobic dispersion has a large particle size and low affinity for the continuous phase, which makes it suitable for enrichment on the air side of the coating.

[0175] The second bio-based hydrophobic dispersion has a smaller particle size and enhances its interaction with the fiber-loving continuous phase through interface-modulating components, allowing it to remain more within the coating.

[0176] The environmentally responsive network further restricts the migration of the second bio-based hydrophobic dispersed phase during the drying process, resulting in different spatial distributions of the first and second bio-based hydrophobic dispersed phases.

[0177] The first stage of the two-stage drying process provides a time window for the aforementioned migration, and the second stage then fixes the resulting gradient structure.

[0178] Therefore, this application is ultimately formed as follows: The paperboard side is mainly filled with a fibrous film-forming component that permeates and seals the pores, the middle of the coating contains a flexible second bio-based hydrophobic dispersion phase, and the air side of the coating is enriched with a first bio-based hydrophobic dispersion phase, forming a continuous gradient structure.

[0179] Under normal planar conditions, the fibrous film-forming component provides continuous oil-blocking capability, while the first bio-based hydrophobic dispersion phase on the surface provides moisture-proof capability; In the folded state of the cardboard, the second bio-based hydrophobic dispersion phase provides crack sealing capability; In the alkaline pulping state of waste paper, the environmentally responsive network weakens and promotes coating dissociation.

[0180] This allows the same coating to exhibit corresponding structural and functional states at different stages, including film formation, packaging, folding, and pulp recycling.

[0181] Example 1 This embodiment is used to illustrate the specific composition, preparation method, and coating film formation process of the bio-based oil-blocking and moisture-proof coating agent of this application on the surface of paperboard, and to verify the bimodal particle size structure, hydrophobic component distribution in the thickness direction, oil-blocking and moisture-proof performance, crease repair performance, and alkaline pulping performance of the obtained coating.

[0182] 1. Raw material composition Based on 100 parts of the total solids (excluding water) in the coating agent, the following formulation is used in this embodiment: Table 1 Formulation Information for Example 1

[0183] The melting point of the carnauba wax is approximately 82°C, and the melting point of the soybean wax is approximately 51°C; the softening temperature of the vegetable fatty acid glycerides used is approximately 38°C.

[0184] Therefore, the softening temperature of the second bio-based hydrophobic dispersion is significantly lower than that of the main high-melting-point plant wax in the first bio-based hydrophobic dispersion.

[0185] The oxidized starch and sodium carboxymethyl cellulose constitute a fibrophilic film-forming continuous phase; the carnauba wax and soybean wax constitute a first bio-based hydrophobic dispersion phase; the plant fatty acid glycerides constitute a second bio-based hydrophobic dispersion phase; and chitosan and pectin are used to form an environmentally responsive ion-associated network.

[0186] In this embodiment, the target solid content of the final coating agent is set at 25 wt%.

[0187] The preparation process of the bio-based oil-resistant and moisture-proof coating agent for the cardboard surface in this embodiment is as follows: Figure 1 As shown, a fibrophilic aqueous continuous phase was first prepared, and a first hydrophobic emulsion with a larger particle size and a second hydrophobic emulsion with a smaller particle size and containing interface-modifying components were prepared separately. Then, the two hydrophobic emulsions were compounded under medium-low shear conditions to maintain two different particle size groups and construct a bimodal hydrophobic dispersion system. Finally, amino-containing biopolymers and carboxyl-containing biopolymers were added to adjust the pH of the system, causing partial ion association between the two to construct an environmentally responsive network, thus obtaining the coating agent.

[0188] 2. Preparation of fibrous aqueous continuous phase Add 420 parts of deionized water to a reaction vessel equipped with a mechanical stirrer and temperature control device, and heat to 82℃ under stirring at 300 r / min. Slowly add 46 parts of oxidized starch to the reaction vessel over 8 min. After the addition is complete, increase the stirring speed to 500 r / min and keep at 82±2℃ for 25 min to allow the oxidized starch to gelatinize completely.

[0189] The obtained system was cooled to 58℃. Ten parts of sodium carboxymethyl cellulose were taken and dispersed in 100 parts of deionized water. Then, under continuous stirring, the mixture was slowly added to the gelatinized oxidized starch system, and stirring was continued at 450 r / min for 35 min. The resulting system was a uniform, semi-transparent, viscous state, with no obvious agglomerates, yielding a cellulose-loving aqueous continuous phase.

[0190] 3. Preparation of the first hydrophobic emulsion Weigh 14 parts carnauba wax and 6 parts soybean wax, add them to the oil phase container and heat to 95°C. Stir at 300 rpm until both waxes are completely melted. Add 0.6 parts sucrose fatty acid ester to the molten wax phase and continue stirring for 5 minutes.

[0191] Take another 120 parts of deionized water and preheat it to 90℃. Under the condition of 90±3℃, slowly add the molten wax phase to the preheated hot water phase, while simultaneously shearing at 6000 r / min for 3 min using a high-speed shear emulsifier, and then reduce the speed to 3000 r / min and continue shearing for 2 min. After emulsification is completed, stop the high-speed shearing and cool down under low-speed stirring conditions to obtain the first hydrophobic emulsion.

[0192] The volumetric median particle size (D50) of the first hydrophobic emulsion, measured using a laser particle size analyzer, was 2.16 μm, with the main particle size distribution ranging from 1.10 to 3.80 μm. High-pressure homogenization was not performed in this step to avoid over-refining of the first bio-based hydrophobic dispersed phase.

[0193] 4. Preparation of the second hydrophobic emulsion Weigh 10 parts of vegetable fatty acid glycerides and heat to 65℃ until completely melted. Add 1.5 parts of lecithin and 0.9 parts of sucrose fatty acid esters to the molten lipids and stir for 5 minutes to ensure uniform dispersion of the interface modifiers.

[0194] Take another 100 parts of deionized water and preheat it to 60°C. Slowly add the molten lipid to the deionized water and shear at 9000 r / min for 4 min to form a pre-emulsion; then perform two high-pressure homogenizations, the first at 35 MPa and the second at 45 MPa. After homogenization, cool to below 40°C to obtain the second hydrophobic emulsion.

[0195] The D50 of the second hydrophobic emulsion was 0.39 μm, with the main particle size distribution ranging from 0.18 to 0.72 μm. The D50 ratio of the first to the second hydrophobic emulsion was 5.54. The second hydrophobic emulsion was uniformly milky white, and no obvious oil layer precipitation or emulsion stratification was observed after standing at room temperature for 24 hours.

[0196] 5. Construction of a bimodal hydrophobic dispersion system The temperature of the fibrophilic aqueous continuous phase was adjusted to 45℃, and the mixture was stirred at 350 rpm. The first hydrophobic emulsion was slowly added to the fibrophilic aqueous continuous phase, and stirring was continued for 8 minutes after the addition was complete. Then the second hydrophobic emulsion was added, the stirring speed was adjusted to 400 rpm, and the mixture was continued to mix for 10 minutes at 45±2℃. High-speed shearing or high-pressure homogenization was not performed during the compounding process.

[0197] The particle size distribution of the compounded system was analyzed, revealing two main particle size groups: a small particle size group mainly distributed between 0.20 and 0.75 μm, corresponding to a D50 of approximately 0.43 μm; and a large particle size group mainly distributed between 1.15 and 3.70 μm, corresponding to a D50 of approximately 2.05 μm. The particle size distribution of the resulting bimodal hydrophobic dispersion system is shown in the figure below. Figure 2 As shown, the first and second bio-based hydrophobic dispersed phases still maintain distinguishable particle size distributions after being compounded.

[0198] 6. Construction of Environmentally Responsive Networks Four parts of chitosan were added to an aqueous solution of acetic acid with a mass concentration of 1.0 wt%, and stirred at room temperature until a homogeneous chitosan solution was formed; four parts of pectin were added to an appropriate amount of deionized water and fully hydrated.

[0199] Under the condition of stirring at 400 rpm in a bimodal hydrophobic dispersion system, pectin solution was first slowly added and stirring continued for 10 min. Then, chitosan solution was slowly added in a thin stream and mixing continued for 15 min. The pH of the system was adjusted to 5.8 using dilute acetic acid solution and dilute sodium hydroxide solution. 3 parts of glycerol were added, the stirring speed was reduced to 250 rpm and stirring continued for 15 min. After standing for degassing for 30 min, the coating agent was obtained.

[0200] The obtained reagent is a uniform milky white viscous liquid, without any visible lumps or flocs, and no obvious aqueous phase precipitation occurred after standing for 2 hours.

[0201] Table 2 Basic properties of the coating agent in Example 1

[0202] The above results indicate that chitosan and pectin partially associated with each other, but did not form a macroscopic gel or flocculent structure that would affect the flowability and spreadability of the drug.

[0203] 7. Paperboard coating and two-stage drying White cardboard for food packaging with a basis weight of 300 g / m² was selected as the coating substrate, and all samples were taken from the same batch of cardboard. Before coating, the cardboard was placed in an environment with a temperature of 23±2℃ and a relative humidity of 50±5% for 24 hours to equilibrate.

[0204] A laboratory-grade automated bar coater was used for single-sided, one-pass coating at a speed of 10 m / min. By adjusting the coating bar specifications and the amount of reagent fed, the actual dry-once coating weight was 9.8 ± 0.3 g / m².

[0205] After coating, the cardboard was first dried in 60℃ hot air for 45 seconds as the first stage of migration drying; then immediately transferred to 95℃ hot air for another 90 seconds as the second stage of structure-locking drying. After drying, it was allowed to cool naturally and equilibrate for 24 hours in an environment of 23±2℃ and 50±5% relative humidity. The resulting coating surface was continuous and smooth, and no obvious shrinkage craters, large-area cracks, or wax precipitation were observed.

[0206] 8. Distribution of hydrophobic dispersed phase in the thickness direction To verify the differential migration behavior of the two types of hydrophobic dispersed phases, a separate fluorescent tracer sample identical to that in this embodiment was prepared. The first and second hydrophobic phases were labeled, and the amount of tracer added was less than 0.05% of the mass of the corresponding hydrophobic phase. A cross-section of the dried coating was prepared and divided into an air-side region, an intermediate region, and a cardboard-side region along the thickness direction.

[0207] Table 3. Distribution of hydrophobic phase thickness in Example 1

[0208] The relative signal of the first hydrophobic phase in the air-side region is 5.72 times that in the paperboard-side region, indicating that the first bio-based hydrophobic dispersed phase is mainly enriched in the air side of the coating. The second hydrophobic phase is mainly distributed in the middle region of the coating and retains a certain proportion in the paperboard side, indicating that the second bio-based hydrophobic dispersed phase regulated by the interface is more retained in the fibrophilic film-forming continuous phase.

[0209] Based on the above thickness direction distribution results, the gradient structure of the coated paperboard obtained in this embodiment is as follows: Figure 3 As shown, the fibrous film-forming continuous phase permeates and seals the inter-fiber pores on the surface of the paperboard near the paperboard substrate; the first bio-based hydrophobic dispersed phase is relatively enriched on the air side of the coating; the second bio-based hydrophobic dispersed phase is mainly retained in the middle of the coating; and an environmentally responsive network is distributed within the fibrous film-forming continuous phase and restricts the excessive migration of the second bio-based hydrophobic dispersed phase. The regions described above exhibit a continuous compositional gradient rather than independent layered structures with clear interfaces.

[0210] 9. Oil-repellent, moisture-proof, and water-absorbing properties Table 4 Planar barrier properties of the coated paperboard in Example 1

[0211] As shown in Table 4, the coating obtained in Example 1 significantly improved the oil-blocking performance of the paperboard and reduced its water absorption and water vapor transmission rate. Specifically, the fibrous film-forming continuous phase blocked the capillary channels on the surface of the paperboard, and the first hydrophobic dispersed phase enriched on the air side further reduced the moisture transport rate.

[0212] 10. Crease barrier recovery performance The coated paperboard was cut into 100mm × 50mm samples. The samples were folded 180° along the center line with the coated side facing outwards and held in the folded state for 10 seconds before being unfolded. The Kit rating of the folded area was measured as follows: K0 for the folded area, K1 for the crease area within 5 minutes after folding, and K2 for the crease area after standing at 23°C for 2 hours.

[0213] Table 5. Crease Barrier Recovery Results in Example 1

[0214] According to the calculation based on R = (K2 - K1) / (K0 - K1) × 100%, the crease oil-resistant performance recovery rate of Example 1 is 75.0%.

[0215] Optical microscopy revealed that, immediately after folding, the typical crack opening width was 11–19 μm. After standing for 2 hours, some crack edges showed lipid-like filling structures, and the typical effective opening width decreased to 4–9 μm. Some continuous cracks transformed into intermittent cracks. These results indicate that the second bio-based hydrophobic dispersed phase can deform and locally redistribute under folding stress, forming partial physical filling of the fold crack.

[0216] 11. Alkaline pulping performance The coated paperboard obtained in Example 1 was cut into 20mm × 20mm pieces, with each sample having an oven-dry weight of 50g. The solid-liquid ratio of the paperboard to the pulp water was 1:20, the pulping temperature was 45℃, the stirring speed was 1000r / min, and the pulping time was 20min. Near-neutral group (pH 7.0 ± 0.2) and alkaline group (pH 10.5 ± 0.2) were set up respectively.

[0217] Table 6 Pulping performance of Example 1

[0218] At pH 10.5, the fiber dissociation rate was significantly increased and the slag rate was significantly reduced. This is because the alkaline environment reduces the protonation degree of the amino groups in chitosan, weakens the ionic association between chitosan and pectin, causes the fibrous film-forming network to absorb water and swell, and further breaks down under mechanical shearing.

[0219] 12. Results Analysis In this embodiment, a first hydrophobic emulsion with a D50 of 2.16 μm and a second hydrophobic emulsion with a D50 of 0.39 μm were prepared, and medium-low shear mixing was used in the compounding stage to ensure that the two hydrophobic phases still maintain two different particle size groups in the final drug.

[0220] During the single coating and two-stage drying process of the paperboard, the first hydrophobic dispersed phase, with larger particle size and lower interfacial affinity with the fiber-loving continuous phase, is more concentrated on the air side of the coating; the second hydrophobic dispersed phase, with smaller particle size and a hydrophilic interfacial layer on its surface, is more retained in the middle of the coating. The resulting gradient coating has both oil-blocking and moisture-proof properties in a planar state. After folding, it can seal creases and cracks through the local migration of the second hydrophobic phase, and can undergo network weakening and paper fiber release under alkaline pulping conditions.

[0221] Example 2 This example illustrates the effect of increasing the content of the second bio-based hydrophobic dispersed phase and lowering its softening temperature on the sealing of creases and cracks in cardboard and its barrier retention performance after repeated folding. Except for the differences described below, the preparation, coating, and drying conditions are the same as in Example 1.

[0222] 1. Raw material composition Table 7 Formulation Information for Example 2

[0223] In this embodiment, the total amount of the first bio-based hydrophobic dispersed phase is 17 parts, and the total amount of the second bio-based hydrophobic dispersed phase is 16 parts. The overall softening temperature range of the partially hydrogenated soybean oil and vegetable fatty acid monoglycerides is approximately 33–39°C, which is lower than the softening temperature of the first hydrophobic phase.

[0224] 2. Preparation of hydrophobic emulsions and coating agents The first hydrophobic emulsion was prepared according to the emulsification conditions of Example 1, and the D50 was measured to be 2.21 μm, with the main particle size distribution range being 1.16–3.91 μm.

[0225] Twelve parts of partially hydrogenated soybean oil and four parts of vegetable fatty acid monoglycerides were melted at 65°C. Two parts of lecithin and one part of sucrose fatty acid ester were added, and the mixture was sheared at 9500 r / min for 5 min to form a pre-emulsion. The pre-emulsion was then subjected to two high-pressure homogenization processes at 40 MPa and 50 MPa, respectively. The resulting second hydrophobic emulsion had a D50 of 0.31 μm and a main particle size distribution range of 0.14–0.61 μm.

[0226] The two emulsions were compounded according to the low-to-medium shear method described in Example 1. After compounding, the D50 of the small particle size group was approximately 0.34 μm, and the D50 of the large particle size group was approximately 2.11 μm. Chitosan, pectin, and glycerol were added, and the pH was adjusted to 5.8 to obtain the coating agent of Example 2.

[0227] Table 8 Basic properties of the coating agent in Example 2

[0228] 3. Coating, drying, and thickness distribution Using the same batch of 300g / m² white cardboard as in Example 1, a single-sided one-time coating was applied, with a dry coating amount of 10.0±0.3g / m². The cardboard was first dried at 60°C for 45s, and then dried at 95°C for 90s.

[0229] Table 9. Hydrophobic phase thickness distribution in Example 2

[0230] The first hydrophobic phase can still be enriched on the air side, and the relative signal of the second hydrophobic phase in the middle region increases to 48.9%, indicating that increasing the content of the second hydrophobic phase and reducing its particle size can form more flexible lipid microdomains in the middle of the coating.

[0231] 4. Flat surface oil-resistant and moisture-proof performance Table 10 Planar Barrier Performance of Example 2

[0232] In Example 2, due to the appropriate reduction in the proportion of the first hydrophobic phase, the water absorption capacity and WVTR of Cobb60 were slightly higher than in Example 1, but the Kit grade of 12 was still maintained, indicating that increasing the content of the second hydrophobic phase did not significantly damage the continuous oil-blocking film.

[0233] 5. Single folding and crack sealing performance Table 11 Crease Barrier Recovery Dynamics in Example 2

[0234] Example 2: The oil-resistant performance recovery rate of the crease was 100%. Microscopic observation showed that the typical crack opening width after folding was 10-18 μm, which decreased to 6-11 μm after standing for 30 min, and further decreased to 2-6 μm after standing for 2 h; some continuous cracks were separated into multiple discontinuous crack segments.

[0235] The process of crease crack formation and sealing of the coating obtained in Example 2 is as follows: Figure 4 As shown. Before folding, the second bio-based hydrophobic dispersed phase is dispersed in the form of flexible lipid microdomains within the fibrophilic film-forming continuous phase. When the paperboard is folded, the outer side of the coating is stretched and cracks are formed. The second bio-based hydrophobic dispersed phase at the crack tip and on both sides of the crack undergoes plastic deformation. After the paperboard is unfolded and left to stand, some of the second bio-based hydrophobic dispersed phase redistributes to the crack opening area and forms local filling, which reduces the crack width and penetration, and some continuous cracks are transformed into discontinuous crack segments.

[0236] 6. Performance under multiple folding and mild heat activation Table 12 Barrier performance after multiple folds in Example 2

[0237] After five folds, the sample was placed in a 40°C hot air environment for 5 minutes, and then left to stand at 23°C for 30 minutes. The Kit grade of the crease area was measured to be 11, which is higher than the Kit grade of 10 for the untreated sample. This result indicates that 40°C is close to the softening temperature of the second hydrophobic phase, which can promote the migration of flexible lipids into the crack.

[0238] 7. Alkaline pulping performance Table 13 Pulping performance of Example 2

[0239] Example 2 has a higher content of the second hydrophobic phase, and its pulping performance is slightly lower than that of Example 1. However, the fiber dissociation rate is still significantly improved under alkaline conditions, indicating that the environmentally responsive network can still promote coating breakage and fiber release.

[0240] 8. Results Analysis In Example 2, the amount of the second bio-based hydrophobic dispersed phase was increased from 10 parts to 16 parts, and its overall softening temperature range was lowered to 33–39°C. Simultaneously, the D50 of the second hydrophobic emulsion was reduced to 0.31 μm through higher homogeneity. These adjustments resulted in the formation of more numerous and more uniformly distributed flexible lipid microdomains in the central region of the coating.

[0241] When the cardboard is folded, the flexible lipid micro-regions can deform under the local stress at the crack tip and on both sides of the crack and redistribute to the crack opening, so that the Kit grade after a single fold is restored from 8 to 12; after 5 folds and standing for 2 hours, it still maintains a Kit grade of 10, which shows good crease repair and repeated folding durability.

[0242] Example 3 This example illustrates how adjusting the ratio of amino-containing biopolymers to carboxyl-containing biopolymers and increasing the total amount of environmentally responsive network components can maintain the oil-blocking and moisture-proof properties of the coating under normal use conditions, while simultaneously producing more pronounced network swelling, structural dissociation, and paper fiber release effects in an alkaline pulping environment. Except for the differences described below, the preparation, coating, and drying conditions are the same as in Example 1.

[0243] 1. Raw material composition Table 14 Formulation Information for Example 3

[0244] In this embodiment, the total amount of chitosan and pectin is 12.5 parts, which is higher than the 8 parts in Example 1. The amount of pectin is higher than the amount of chitosan, so as to form more reversible ion association nodes under weakly acidic conditions and enhance the network's water absorption and swelling tendency under alkaline conditions.

[0245] 2. Preparation of coating agent A fibrophilic aqueous continuous phase, a first hydrophobic emulsion, and a second hydrophobic emulsion were prepared according to the method in Example 1. The D50 of the first hydrophobic emulsion was 2.12 μm, and the D50 of the second hydrophobic emulsion was 0.38 μm, with a D50 ratio of 5.58. After blending, the D50 of the small particle size group was approximately 0.42 μm, and the D50 of the large particle size group was approximately 2.03 μm.

[0246] Seven parts of pectin were fully hydrated at 50°C, and 5.5 parts of chitosan were prepared into a 1.0 wt% aqueous solution of acetic acid. At 42±2°C and 350–400 rpm, the pectin solution was slowly added and stirred for 15 min, followed by the chitosan solution added in a thin stream over 20 min, with stirring continued for another 20 min. The pH was adjusted to 5.6, and 3.5 parts of glycerol were added. The mixture was stirred at low speed and allowed to stand to remove bubbles, yielding the coating agent of Example 3.

[0247] Table 15 Basic Properties of the Coating Agent in Example 3

[0248] Compared with Example 1, the viscosity of this example is increased, indicating that more ion-associated nodes are formed in the continuous phase, but the agent still maintains continuous fluidity and can be coated normally.

[0249] 3. Coating, drying, and thickness distribution Using the same white cardstock and coating and drying conditions as in Example 1, the dry coating amount was 10.1 ± 0.3 g / m². The resulting coating surface was continuous and smooth, without obvious pinholes, large-area cracks, or coating peeling.

[0250] Table 16 Distribution of hydrophobic phase thickness in Example 3

[0251] Even after increasing the amount of environmentally responsive network, the first hydrophobic phase can still accumulate towards the air side, while the second hydrophobic phase is mainly distributed in the middle region of the coating. This indicates that a higher density reversible network can effectively limit the excessive migration of the small-particle-size second hydrophobic phase.

[0252] 4. Flat surface with oil-repellent, moisture-proof, and crease-resistant properties. Table 17 Barrier and Crease Performance of Example 3

[0253] Example 3 has a planar oil-blocking and moisture-proof performance similar to that of Example 1; its crease oil-blocking performance recovery rate is 50.0%, which is lower than that of Example 1. The main reason is that the higher network density restricts the migration of flexible lipid micro-regions to a certain extent, but still retains a certain crease-blocking ability.

[0254] 5. Coating swelling and mass loss under different pH conditions The coated paperboard was cut into 50mm × 50mm samples, dried to constant weight, and then immersed in aqueous solutions with pH values ​​of 7.0, 9.0, 10.5, and 11.5, respectively, and treated at 45℃ for 30 minutes. The overall water absorption and swelling rate was calculated based on the mass before and after treatment.

[0255] Table 18 Swelling behavior under different pH conditions in Example 3

[0256] Table 19 Mass loss rate after static treatment in Example 3

[0257] As pH increases, the degree of amino protonation of chitosan decreases, the number of ion association nodes between chitosan and pectin decreases, and pectin and other hydrophilic segments absorb water and unfold, causing the coating to exhibit obvious alkali-triggered swelling and mass loss.

[0258] The state switching of an environmentally responsive network under normal operating conditions and alkaline pulping conditions, such as... Figure 5 As shown. Under weakly acidic to near-neutral operating conditions, some amino groups of the amino-containing biopolymers undergo protonation and form ion-association nodes with the carboxyl groups of the carboxyl-containing biopolymers, maintaining a relatively stable network structure in the coating and limiting the excessive migration of the second bio-based hydrophobic dispersed phase within the continuous phase. When the coated paperboard enters an alkaline pulping environment, the degree of protonation of the amino-containing biopolymers decreases, the number of ion-association nodes decreases, and the environmentally responsive network absorbs water, swells, and weakens. Under mechanical stirring and shearing, it gradually dissociates, promoting the redispersibility of the paperboard fibers.

[0259] 6. Pulping performance at different pH levels and time periods Table 20 Pulping performance under different pH conditions in Example 3

[0260] Table 21 Pulping time response of Example 3 at pH 10.5

[0261] When the pH was increased from 7.0 to 10.5, the fiber dissociation rate increased from 69.4% to 96.2%, and the slag rate decreased from 13.1% to 2.4%. The improvement rate tended to decrease after the pH was further increased to 11.5, indicating that the pH of around 10.5 can effectively weaken most environmentally responsive networks.

[0262] 7. Recycled paper sheet forming verification The fiber pulp obtained from Example 3, which was pulped for 20 minutes at pH 10.5, was collected, diluted, and then papered into laboratory recycled paper sheets according to the same basis weight. An uncoated original paperboard from the same batch was pulped and papered under the same conditions as a reference.

[0263] Table 22 Performance of Recycled Paper in Example 3

[0264] In Example 3, the tensile index of the recycled paper was about 95.0% of that of the control group, and no large-area waxy patches or obvious uneven forming were observed, indicating that the coating residues after alkaline pulping could be dispersed to a smaller size and had little impact on the reforming of recycled fibers.

[0265] 8. Results Analysis In Example 3, the total amount of chitosan and pectin was increased from 8 parts to 12.5 parts, with the pectin content exceeding that of chitosan. In the reagent at pH 5.6, the increased number of reversible ionic association nodes improved the system viscosity and network stability under normal operating conditions.

[0266] In an alkaline environment, the degree of amino protonation of chitosan decreases, and the ion association nodes between chitosan and pectin weaken. Higher pectin content provides more hydrophilic carboxyl sites, promoting the penetration of alkaline water into the coating. Therefore, Example 3, while maintaining Kit grade 12 and lower Cobb60 and WVTR, achieved a fiber dissociation rate of 96.2% and a sieve residue rate of 2.4% at pH 10.5.

[0267] Comparative Example 1 This comparative example illustrates the effect of co-emulsifying all hydrophobic raw materials to form a single-particle-size system on surface hydrophobic enrichment, planar barrier properties, and crease repair performance. The raw material composition is the same as in Example 1, but the first and second hydrophobic emulsions are not prepared separately.

[0268] 1. Preparation of single hydrophobic emulsions and coating agents Fourteen parts of carnauba wax, six parts of soybean wax, and ten parts of vegetable fatty acid glycerides were heated together to 95°C. Then, 1.5 parts of lecithin and 1.5 parts of sucrose fatty acid esters were added. The mixture was sheared at 9000 r / min for 5 min, followed by two high-pressure homogenization processes at 40 MPa and 50 MPa, respectively. The resulting emulsion exhibited a single dominant particle size distribution, with a D50 of 0.47 μm and a dominant particle size range of 0.19–0.93 μm.

[0269] The single hydrophobic emulsion was added to the same fibrous aqueous continuous phase as in Example 1, followed by the addition of pectin, chitosan, and glycerol, and the pH was adjusted to 5.8 to obtain the coating agent for Comparative Example 1. Its solid content was 25.2 wt%, and its viscosity was 1120 mPa·s. Coated paperboard was prepared using the same paperboard, coating amount, and two-stage drying conditions as in Example 1.

[0270] Table 23 Main Detection Results of Comparative Example 1

[0271] After all hydrophobic components are refined together, the small-particle-size wax phase is more likely to enter the middle of the coating and the pores of the cardboard surface along with the aqueous continuous phase, reducing the degree of hydrophobic enrichment on the air side; the low-softening lipids are also difficult to migrate effectively at the cracks as relatively independent flexible micro-regions. Therefore, the moisture-proof and crease-recovery performance of Comparative Example 1 is lower than that of Example 1.

[0272] Comparative Example 2 This comparative example is used to illustrate the effect of the second bio-based hydrophobic dispersion on the sealing of creases and cracks in cardboard and the recovery of barrier properties after folding.

[0273] 1. Raw material composition and preparation Table 24 Formulation Information for Comparative Example 2

[0274] Compared to Example 1, this comparative example omits 10 parts of vegetable fatty acid glycerides and adds the same mass to the first hydrophobic phase, maintaining the total amount of hydrophobic raw materials at 30 parts. 21 parts of carnauba wax and 9 parts of soybean wax were emulsified under the first hydrophobic emulsion conditions of Example 1, and the D50 was measured to be 2.28 μm. The remaining preparation, coating, and drying conditions were the same as in Example 1.

[0275] Table 25 Main Detection Results of Comparative Example 2

[0276] The high proportion of the first hydrophobic phase in Comparative Example 2 improved the moisture-proof performance of the planar material, but it was in a hard crystalline state at room temperature and could not effectively plastically fill creases and cracks. The Kit grade of the cardboard dropped significantly after folding and did not recover after standing, indicating that setting a second hydrophobic phase with small particle size and low softening temperature is the key to obtaining crease repair effect.

[0277] Comparative Example 3 This comparative example illustrates the effect of environmentally responsive ion-associated networks on the retention of the second hydrophobic phase, planar film stability, and alkaline pulping response.

[0278] 1. Raw material composition and preparation Table 26 Comparative Example 3 Formulation Information

[0279] In this comparative example, chitosan and pectin were omitted, and their corresponding masses were added to oxidized starch and sodium carboxymethyl cellulose. The first and second hydrophobic emulsions were prepared according to Example 1, with D50 values ​​of 2.14 μm and 0.40 μm, respectively. After compounding, no environmentally responsive network components were added; only glycerol was added and the pH was adjusted to 5.8. The resulting reagent had a viscosity of 820 mPa·s and exhibited slight redispersibility and stratification after standing for 24 hours.

[0280] Table 27 Main Detection Results of Comparative Example 3

[0281] In the absence of an environmentally responsive network, the second hydrophobic phase is more likely to migrate towards the air side with moisture evaporation, reducing the flexible micro-regions in the center of the coating and decreasing planar barrier and crease recovery properties. More importantly, the fiber dissociation rate only increased by 5.3 percentage points after the pH was increased from 7.0 to 10.5, indicating that the system does not exhibit significant alkali-triggered network weakening characteristics.

[0282] Comparative Example 4 This comparative example illustrates the effect of continuing high-intensity shearing and high-pressure homogenization to disrupt the bimodal particle size structure during the compounding stage after the two hydrophobic emulsions have been prepared independently. The raw material composition and the initial emulsification process are the same as in Example 1.

[0283] 1. High-strength compounding treatment The first and second hydrophobic emulsions were sequentially added to a fibrous aqueous continuous phase at 45°C, followed by high-speed shearing at 9000 r / min for 5 min, and then high-pressure homogenization at 35 MPa. After treatment, the overall D50 of the system was 0.58 μm, with the main particle size distribution range of 0.21–1.16 μm. The original large particle size group basically disappeared, and the bimodal structure was transformed into a broad unimodal distribution with highly overlapping particles.

[0284] Subsequently, pectin, chitosan, and glycerol were added according to the method in Example 1, the pH was adjusted to 5.8, and coated paperboard was prepared using the same paperboard, coating amount, and two-stage drying conditions.

[0285] Table 28 Main Detection Results of Comparative Example 4

[0286] Comparative Example 4 and Example 1 have the same raw material formulation; the main difference lies in the compounding step. High-intensity homogenization reduces the particle size of the first hydrophobic phase and disrupts the bimodal structure, resulting in an increased proportion of it entering the middle of the coating and the cardboard side. The surface moisture-proof enrichment, planar barrier, and crease recovery performance are all lower than those of Example 1, indicating that low-shear compounding to maintain the bimodal particle size structure is not a common process choice.

[0287] Comprehensive performance test To further verify the synergistic effect of the bimodal hydrophobic dispersion system, the environmentally responsive network, and the two-stage drying process, a comprehensive comparison was made between the reagents obtained in Examples 1-3 and Comparative Examples 1-4 and the coated paperboards. Unless otherwise specified, all tests were conducted in an environment with a temperature of 23±2℃ and a relative humidity of 50±5%. Five samples were prepared in parallel for each group, and the data in the table are average values.

[0288] 1. Basic properties and particle size structure of coating agents Table 29 Basic Properties of Coating Agents in Each Group

[0289] Table 30 Particle size structure of each group of hydrophobic dispersed phases

[0290] Examples 1-3, after compounding, still retained distinct small-particle-size and large-particle-size groups. Comparative Example 1 formed a single peak due to the co-emulsification of all hydrophobic components, while Comparative Example 4 formed a broad single peak due to high-intensity homogenization after compounding. Although Comparative Example 3 maintained bimodal peaks, it lacked network constraint and showed slight wax enrichment in the upper layer after standing.

[0291] 2. Coating thickness distribution Table 31 Thickness distribution of the first hydrophobic phase

[0292] Table 32 Thickness distribution of the second hydrophobic phase

[0293] In Examples 1-3, the signal on the air side of the first hydrophobic phase all exceeded 58%, and the signal ratio between the air side and the cardboard side was greater than 5; the signal of the second hydrophobic phase in the intermediate region was all above 45%. In Comparative Example 4, due to the refinement of the first hydrophobic phase, the signal ratio between the air side and the cardboard side decreased to 2.16; in Comparative Example 3, lacking an environmentally responsive network, the proportion of the second hydrophobic phase on the air side increased to 43.9%. The above results demonstrate that particle size differences, interfacial affinity differences, network confinement, and two-stage drying collectively contribute to the gradient structure.

[0294] 3. Flat surface oil-resistant and moisture-proof performance Table 33 Planar barrier properties of each group of coated paperboard

[0295] Examples 1-3 all achieved Kit grade 12, Cobb 60 water absorption of less than 10.5 g / m², and water absorption of less than 95 g·m². - 24h -¹WVTR. Comparative Example 2 has the best planar moisture-proof performance due to its higher content of the first hydrophobic phase, but its crease resistance is significantly reduced; Comparative Examples 1 and 4 have the same total amount of hydrophobic raw materials, but their moisture-proof performance is significantly lower than that of Example 1 due to insufficient surface enrichment.

[0296] 4. Crease Barrier Recovery Dynamics Table 34: Kit grade changes after one fold for each group

[0297] Table 35 Changes in the Morphology of Each Group of Fold Cracks

[0298] Example 2 has a higher content of the second hydrophobic phase and a lower softening temperature, resulting in the highest crease recovery rate and crack width reduction rate. Comparative Example 2 does not contain the second hydrophobic phase, and the Kit grade and crack width after folding hardly recover with resting time, further proving that the second hydrophobic phase is the main functional component for crease and crack sealing.

[0299] 5. Durability after multiple folds Table 36 Kit grades after multiple folds and 2 hours of rest for each group

[0300] Examples 1-3 maintained a Kit grade of 8 or higher after 5 folds, with Example 2 reaching 10; Comparative Example 2 only reached 3, indicating that the high-melting-point surface wax phase cannot replace the internal low-softening-temperature flexible lipid microregions.

[0301] 6. pH-responsive swelling and pulping performance Table 37 pH-responsive swelling rates of each coating group

[0302] Table 38 Pulping performance of each group of paperboards at pH 10.5

[0303] Example 3 exhibits the largest pH-responsive swelling increment and the best alkaline pulping performance. Comparative Example 3 lacks an environmentally responsive network; its swelling rate increment due to pH changes is only 10.3 percentage points, and its fiber dissociation rate at pH 10.5 is only 82.1%, indicating that ordinary hydrophilic polymers cannot replace the network state switching caused by changes in the protonation degree of amino-containing components.

[0304] 7. Drug storage stability Table 39 Stability of each group of coating agents after standing at 25℃ for 7 days.

[0305] The viscosity change rate of Examples 1-3 after standing for 7 days was less than 6%, and no obvious irreversible stratification or block flocculation was observed. Comparative Example 3 lacked an environmentally responsive network and showed a slight wax enrichment in the upper layer after standing, indicating that the reversible network can improve the storage stability of the drug without causing macroscopic gelation.

[0306] 8. Comprehensive Analysis Comprehensive experiments show that preparing first and second hydrophobic emulsions with different particle sizes, and maintaining a bimodal structure under medium-low shear conditions during the compounding process, is the basis for achieving differential migration of the two hydrophobic phases. Comparative Examples 1 and 4 demonstrate that high-intensity homogenization after co-emulsification or compounding leads to a more uniform particle size distribution, weakening the surface enrichment of the first hydrophobic phase and the independent flexible micro-region effect of the second hydrophobic phase.

[0307] The first hydrophobic phase mainly accumulates towards the air side and assumes the function of moisture protection; the second hydrophobic phase is retained inside the continuous phase through its smaller particle size and hydrophilic interface layer, reducing the degree of crack penetration during cardboard folding through deformation and redistribution. Comparative Example 2 shows that simply increasing the surface wax phase with a high melting point can improve the moisture protection performance of the planar surface, but it cannot solve the barrier failure in the crease area.

[0308] The environmentally responsive network formed by chitosan and pectin, on the one hand, restricts the migration of the second hydrophobic phase and enhances the cohesion of the continuous phase during agent storage and coating drying; on the other hand, it weakens under alkaline pulping conditions due to the reduced protonation degree of chitosan amino groups. Comparative Example 3 demonstrates that, in the absence of this network, the coating no longer exhibits significant alkali-triggered swelling and pulping response.

[0309] Example 1 achieves a good overall balance between planar oil and moisture resistance, crease recovery, and alkaline pulping performance; Example 2 exhibits superior crease repair and multiple folding durability; Example 3 exhibits superior alkaline pulping dissociation performance. Therefore, the proportions of the first hydrophobic phase, the second hydrophobic phase, and the environmentally responsive network component can be adjusted within the scope defined in the claims, depending on the intended use of the paperboard product.

Claims

1. A bio-based oil-resistant and moisture-proof coating agent for cardboard surfaces, characterized in that, It includes an aqueous dispersion medium and a fibrophilic film-forming component dispersed in the aqueous dispersion medium, a first bio-based hydrophobic dispersion phase, a second bio-based hydrophobic dispersion phase, an interface modulation component, and an environmentally responsive network component; The fibrous film-forming component includes at least one bio-based polysaccharide with a hydrophilic group, used to form a continuous coating phase and penetrate into the inter-fiber pores of the paperboard surface; The first bio-based hydrophobic dispersion phase comprises plant waxes and / or hydrogenated plant lipids, and the median volumetric particle size D50 of the dispersed droplets is 0.8–4.0 μm; The second bio-based hydrophobic dispersion phase includes plant-derived lipids with plastic flow capability, the median volumetric particle size D50 of the dispersed droplets is 0.10 to 0.80 μm, and the softening temperature of the second bio-based hydrophobic dispersion phase is lower than that of the first bio-based hydrophobic dispersion phase. The interface-modifying component is at least coated on the microdroplet surface of the second bio-based hydrophobic dispersion phase, such that the interfacial affinity between the second bio-based hydrophobic dispersion phase and the fibrophilic film-forming component is higher than the interfacial affinity between the first bio-based hydrophobic dispersion phase and the fibrophilic film-forming component. The environmentally responsive network components include amino-containing biopolymers and carboxyl-containing biopolymers. The amino-containing biopolymers and the carboxyl-containing biopolymers form an ion-association network under the weakly acidic to near-neutral conditions of the coating agent. Under alkaline conditions, the ion-association network is weakened due to the reduced protonation degree of the amino-containing biopolymers. The first bio-based hydrophobic dispersion phase and the second bio-based hydrophobic dispersion phase constitute a bimodal hydrophobic dispersion system with different particle sizes, so that when the coating agent is coated on the paperboard and dried, the first bio-based hydrophobic dispersion phase is enriched relative to the second bio-based hydrophobic dispersion phase towards the air side of the coating, and the second bio-based hydrophobic dispersion phase is retained in the continuous phase formed by the fibrous film-forming component.

2. The coating agent according to claim 1, characterized in that, The fibroblastic film-forming component includes modified starch and auxiliary polysaccharides. The modified starch is selected from at least one of oxidized starch, hydroxypropyl starch, carboxymethyl starch, and cationic starch. The auxiliary polysaccharides are selected from at least one of carboxymethyl cellulose, pectin, alginate, microfibrillated cellulose, and carboxymethyl chitosan. The modified starch accounts for 60-90% of the mass of the fibroblastic film-forming component, and the auxiliary polysaccharides account for 10-40% of the mass of the fibroblastic film-forming component.

3. The coating agent according to claim 1, characterized in that, The first bio-based hydrophobic dispersion phase comprises high-melting-point plant wax and medium-melting-point plant lipids. The high-melting-point plant wax is selected from at least one of carnauba wax, rice bran wax, sugarcane wax, and candelilla wax. The medium-melting-point plant lipids are selected from at least one of soybean wax, hydrogenated vegetable oil, and plant-derived long-chain fatty acid esters. The high-melting-point plant wax accounts for 50-85% of the mass of the first bio-based hydrophobic dispersion phase, and the medium-melting-point plant lipids account for 15-50%.

4. The coating agent according to claim 1, characterized in that, The second bio-based hydrophobic dispersion phase is selected from at least one of partially hydrogenated vegetable oil products, vegetable fatty acid glycerides, fatty acid monoglycerides, fatty acid diglycerides, and plant-derived soft waxes. The softening temperature of the second bio-based hydrophobic dispersion phase is 25-50°C, and its softening temperature is 10-45°C lower than that of the first bio-based hydrophobic dispersion phase.

5. The coating agent according to claim 1, characterized in that, The median volumetric particle size (D50) of the dispersed droplets in the first bio-based hydrophobic dispersion phase is 1.2–3.0 μm, the median volumetric particle size (D50) of the dispersed droplets in the second bio-based hydrophobic dispersion phase is 0.20–0.60 μm, and the ratio of the D50 of the first bio-based hydrophobic dispersion phase to that of the second bio-based hydrophobic dispersion phase is 2.5–12.

6. The coating agent according to claim 1, characterized in that, The interface modulating component is selected from at least one of lecithin, sucrose fatty acid ester, protein emulsifier, amphiphilic chitosan derivative and amphiphilic starch derivative; the interface modulating component is at least distributed on the microdroplet surface of the second bio-based hydrophobic dispersion phase and binds to the fibrophilic film-forming component through hydrogen bonding and / or electrostatic interaction, so that the second bio-based hydrophobic dispersion phase is retained in the continuous phase formed by the fibrophilic film-forming component during the coating drying process.

7. The coating agent according to claim 1, characterized in that, The coating agent comprises, based on 100 parts of total solids excluding water, the following components: 40-70 parts of a fibrous film-forming component, 10-30 parts of a first bio-based hydrophobic dispersed phase, 5-20 parts of a second bio-based hydrophobic dispersed phase, 3-15 parts of an environmentally responsive network component, 1-5 parts of an interface-modifying component, and 2-10 parts of a bio-based plasticizer; the coating agent has a solid content of 15-35 wt% and a pH of 4.5-6.

8.

8. A method for preparing a bio-based oil-resistant and moisture-proof coating agent for cardboard surfaces, characterized in that, include: S1. Add bio-based polysaccharides to water for dissolution and / or gelatinization to obtain an aqueous continuous phase containing the fibrous film-forming component; S2. Heat the plant wax and / or hydrogenated plant lipids to a molten state, and disperse the molten plant wax and / or hydrogenated plant lipids in the aqueous phase under the first emulsification condition, controlling the median particle size D50 of the resulting dispersed droplets to be 0.8-4.0 μm, to obtain the first hydrophobic emulsion. S3. Plant-derived lipids with a softening temperature lower than that of the hydrophobic component in the first hydrophobic emulsion are heated to a molten state, an interface conditioning component is added, and emulsification is carried out under the second emulsification conditions. The median particle size D50 of the resulting dispersed droplets is controlled to be 0.10-0.80 μm, so that a hydrophilic interface layer capable of interacting with the fibrous film-forming component is formed on the surface of the dispersed droplets, thereby obtaining the second hydrophobic emulsion. S4. Under the condition that the temperature of the aqueous continuous phase is 35-55°C, the first hydrophobic emulsion and the second hydrophobic emulsion are added to the aqueous continuous phase, and mixed under shear conditions that do not refine the dispersed droplets of the first hydrophobic emulsion to the particle size range of the second hydrophobic emulsion, to form a bimodal hydrophobic dispersion system containing a large-particle-size first bio-based hydrophobic dispersion phase and a small-particle-size second bio-based hydrophobic dispersion phase. S5. Add amino-containing biopolymers and carboxyl-containing biopolymers to the system obtained in step S4, and adjust the pH of the system to 4.5-6.8, so that the amino-containing biopolymers and the carboxyl-containing biopolymers undergo partial ion association, forming an environmentally responsive network that can limit the migration of the second bio-based hydrophobic dispersed phase without producing macroscopic flocculation, to obtain the bio-based oil-resistant and moisture-proof coating agent for the paperboard surface.

9. The preparation method according to claim 8, characterized in that, In step S2, the plant wax and / or hydrogenated plant lipids are heated to 5-20°C above their highest melting point for the first emulsification, and the D50 of the resulting first hydrophobic emulsion is controlled to be 1.2-3.0 μm. In step S3, the plant-derived lipids are melted and mixed with the interface regulation component, and emulsified under a second emulsification condition with a shear strength higher than the first emulsification condition in step S2, so that the D50 of the resulting second hydrophobic emulsion is controlled to be 0.20-0.60 μm.

10. The preparation method according to claim 8, characterized in that, In step S4, the temperature of the aqueous continuous phase is controlled at 35-55°C. The first hydrophobic emulsion is added and dispersed first, and then the second hydrophobic emulsion is added. The mixture is compounded under mixing conditions with a shear strength lower than the second emulsification conditions in step S3, so that the ratio of the D50 of the compounded first bio-based hydrophobic dispersed phase to the second bio-based hydrophobic dispersed phase is maintained at 2.5-12. In step S5, after the bimodal hydrophobic dispersion system is formed, the amino-containing biopolymer and the carboxyl-containing biopolymer are added, and the pH of the system is adjusted to 4.5-6.8 so that the two form partial ion association without macroscopic flocculation, thereby obtaining the coating agent.