A high-solids vinyl ester heavy-duty anti-corrosion coating and its preparation method
Modified wax was prepared by ring-opening reaction of oxidized paraffin with glycidyl methacrylate, which solved the problem of poor interlayer adhesion caused by the paraffin enrichment layer on the surface of high solids vinyl ester heavy-duty anti-corrosion coatings, and improved the corrosion resistance and interlayer adhesion of the coating.
Patent Information
- Application Number
- CN202611562990.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-10
AI Technical Summary
In existing high-solids vinyl ester heavy-duty anti-corrosion coatings, the paraffin-rich layer on the surface leads to poor interlayer adhesion, and existing grinding and solvent dewaxing methods are difficult to implement reliably in engineering practice, resulting in blistering and peeling under corrosive media immersion and temperature cycling.
Modified wax was prepared by ring-opening reaction of oxidized paraffin with glycidyl methacrylate, and then mixed with vinyl ester resin, styrene, anti-corrosion pigments and fillers, coating additives and cobalt isooctanoate solution to form separately packaged base component and initiator component, which improves interlayer adhesion.
It improves the interlayer adhesion of the coating, reduces the risk of corrosive media diffusion along the interlayer and coating blistering and peeling under temperature cycling, and improves the corrosion resistance of the coating.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of anti-corrosion coating technology, and relates to a high-solids vinyl ester heavy-duty anti-corrosion coating and its preparation method. Background Technology
[0002] Vinyl ester heavy-duty anti-corrosion coatings are commonly used for corrosion protection of metal equipment, storage tanks, pipelines, and concrete structures. Their high-solids composition reduces volatile matter release during application and facilitates the formation of a protective layer with a significant dry film thickness. Heavy-duty anti-corrosion projects typically require multiple coats applied consecutively to form a complete shielding system. Therefore, the surface curing state, wettability, and bonding strength of each coat directly affect the overall stability of the protective layer.
[0003] When vinyl ester resins undergo free radical curing, the active free radicals on the coating surface are easily quenched by oxygen in the air, leading to inhibited surface polymerization and a sticky appearance. Existing coatings can incorporate paraffin wax as an oxygen barrier. However, paraffin wax has limited compatibility with vinyl ester resins. During coating curing, it migrates to the air interface due to concentration changes, curing exothermics, and phase changes, and crystallizes upon cooling to form an enriched layer. This enriched layer reduces oxygen transfer to the reaction interface, but paraffin wax lacks functional groups that react with the vinyl ester resin crosslinking network, and after curing, it mainly exists as an independent wax phase. During subsequent coating processes, the surface-enriched paraffin wax has low surface energy, easily weakening the wetting and spreading of the previous coating by the subsequent coating, and hindering molecular contact, resin penetration, and interfacial co-curing between the two coatings, resulting in interlayer boundaries with low cohesive strength. High-solids thick-film systems have limited flow and penetration capabilities, making it difficult for subsequent coatings to re-dissolve or penetrate the wax layer, thus more easily preserving continuous or discontinuous weak interfaces. During construction, surface paraffin can be removed by grinding or solvent cleaning. However, it is difficult to achieve a consistent level of treatment for large equipment, complex curved surfaces, welds, and corner areas. Construction intervals, environmental pollution, and differences in manual operation can also cause wax film residue.
[0004] Therefore, the technical problem to be solved by the present invention is that the existing high-solids vinyl ester heavy-duty anti-corrosion coatings containing paraffin oxygen barrier have poor interlayer adhesion due to the paraffin enrichment layer on the surface. Furthermore, the existing grinding and solvent dewaxing methods are difficult to implement reliably in engineering practice, and the residual wax film causes immersion in corrosive media and blistering and peeling between layers under temperature cycling. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a high-solids vinyl ester heavy-duty anti-corrosion coating and its preparation method. Addressing the problem of poor interlayer adhesion caused by paraffin surface enrichment in high-solids vinyl ester heavy-duty anti-corrosion coatings, and blistering and peeling under corrosive medium immersion and temperature cycling, the present invention prepares a modified wax by ring-opening reaction of oxidized paraffin with glycidyl methacrylate. The modified wax is then made into a masterbatch, which is then mixed and dispersed with vinyl ester resin, styrene, anti-corrosion pigments and fillers, coating additives, and cobalt isooctanoate solution to obtain the base component, which is then packaged separately with methyl ethyl ketone peroxide solution.
[0006] To achieve this objective, the present invention adopts the following technical solution:
[0007] In a first aspect, the present invention provides a high-solids vinyl ester heavy-duty anti-corrosion coating, comprising a separately packaged base component and an initiator component, wherein the base component comprises vinyl ester resin, styrene, modified wax, anti-corrosion pigments and fillers, coating additives and cobalt isooctanoate solution, and the initiator component is methyl ethyl ketone peroxide solution;
[0008] The modified wax includes the structural unit shown: R-CO-O-CH2-CH(OH)-CH2-OCO-C(CH3)=CH2, where R-CO- represents the acyl group formed after removing the hydroxyl group from the carboxyl group contained in the oxidized paraffin.
[0009] Preferably, the anti-corrosion pigments and fillers include glass flakes, mica iron oxide, and barium sulfate, and the coating additives include hydrophobic fumed silica, polyester dispersant, and polyacrylate defoamer.
[0010] Preferably, the mass ratio of the vinyl ester resin, styrene, modified wax, glass flakes, mica iron oxide, barium sulfate, hydrophobic fumed silica, polyester dispersant and polyacrylate defoamer is (52-65):(3-10):(0.3-1.0):(15-25):(3-8):(5-12):(0.3-1.2):(0.2-0.8):(0.1-0.5).
[0011] Preferably, the mass ratio of the vinyl ester resin, cobalt isooctanoate solution and initiator component is 100:(1-4):(1-2.5).
[0012] Preferably, the modified wax has an acid value of 2-8 mg KOH / g, a dropping melting point of 52-65℃, and a methacrylate group content of 0.2-0.4 mmol / g.
[0013] Preferably, the vinyl ester resin is selected from at least one of bisphenol A type epoxy vinyl ester resin and phenolic epoxy vinyl ester resin.
[0014] Preferably, the D50 of the glass flakes is 60-180 μm; after the base material component and the initiator component are mixed according to the mass ratio described in claim 2, the mass fraction of non-volatile matter measured according to GB / T 34682-2017 is not less than 60 wt.%.
[0015] Preferably, the cobalt content in the cobalt isooctanoate solution is 0.7-0.9 wt.%; and the total active oxygen content in the methyl ethyl ketone peroxide solution is 8.5-10.0 wt.%.
[0016] In a second aspect, the present invention provides a method for preparing the high-solids vinyl ester heavy-duty anti-corrosion coating described in the first aspect, comprising the following steps:
[0017] S1, oxidized paraffin, glycidyl methacrylate, triphenylphosphine and p-methoxyphenol are mixed and subjected to a ring-opening reaction, wherein the carboxyl group in the oxidized paraffin reacts with the epoxy group in the glycidyl methacrylate to obtain a modified wax.
[0018] S2, the vinyl ester resin is divided into a first resin and a second resin, the styrene is divided into a first styrene and a second styrene, and the modified wax, the first resin and the first styrene are mixed to obtain a masterbatch;
[0019] S3, the second resin, second styrene, polyester dispersant, polyacrylate defoamer, hydrophobic fumed silica, mica iron oxide and barium sulfate are mixed and dispersed, then the masterbatch and cobalt isooctanoate solution are added, followed by glass flakes to obtain the base material component;
[0020] S4, the base material components and methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating.
[0021] Preferably, in S1, the acid value of the oxidized paraffin is 10-30 mg KOH / g, and the dropping melting point is 50-70℃; the molar ratio of the glycidyl methacrylate to the molar ratio of the carboxyl group in the oxidized paraffin is (0.7-0.95):1.
[0022] Preferably, the total mass ratio of the oxidized paraffin and the glycidyl methacrylate to the mass ratio of triphenylphosphine and p-methoxyphenol is 100:(0.10-0.20):(0.03-0.06).
[0023] Preferably, the ring-opening reaction is carried out in an argon atmosphere, the temperature of the reactants is 100-125℃, and the reaction time is 2-5 hours.
[0024] Preferably, in S2, the mass ratio of the modified wax, the first resin, and the first styrene is 1:(2-5):(0.5-2). When mixing, the temperature of the mixture is 60-75℃, the stirring speed is 300-800 r / min, and the stirring time is 20-60 min.
[0025] Preferably, in step S3, the second resin, second styrene, polyester dispersant, and polyacrylate defoamer are stirred at 400-800 r / min for 5-15 min. After adding hydrophobic fumed silica, mica iron oxide, and barium sulfate, the mixture is dispersed at 1200-1800 r / min for 20-40 min, with the material temperature at 25-50°C during dispersion. The material temperature is then adjusted to 25-40°C, and the masterbatch and cobalt isooctanoate solution are added. The mixture is stirred at 400-800 r / min for 10-30 min. After adding glass flakes, the mixture is stirred at 200-500 r / min for 10-30 min to obtain the base material component.
[0026] The carboxyl groups in oxidized paraffin and the epoxy groups in glycidyl methacrylate undergo ring-opening addition under the action of triphenylphosphine. The carboxyl group undergoes proton transfer to form a nucleophilic carboxylate group, which attacks the less sterically hindered carbon atom in the epoxy group. The carbon-oxygen bond in the epoxy ring breaks, and the resulting alkoxide anion is converted to a hydroxyl group via proton transfer. This forms a β-hydroxy ester linkage between the acyl group of oxidized paraffin and the glycidyl group of glycidyl methacrylate. This reaction consumes both the carboxyl and epoxy groups and does not use the carbon-carbon double bond of the methacrylate group as the reaction site; therefore, the methacrylate group can be retained until the subsequent curing stage.
[0027] The ring-opening reaction links the hydrocarbon wax segments of oxidized paraffin with the β-hydroxy ester structure and methacrylate groups in the same molecular structure. The hydrocarbon wax segments retain low polarity, crystallization tendency, and tendency to migrate towards the air interface. The β-hydroxy ester structure introduces hydroxyl and ester groups, increasing hydrogen bonding and dipole interactions between the modified wax and the polar segments of the vinyl ester resin. The methacrylate groups retain reaction sites for participating in free radical polymerization.
[0028] When the modified wax is mixed with the first resin and the first styrene, the modified wax melts upon heating, disrupting the original wax crystal lattice. The first styrene enters between the molten wax phase and the first resin, reducing the viscosity of the mixed phase. The first resin provides a carrier with the same composition as the subsequent base component's continuous phase. The shearing action generated by stirring reduces the size of the molten modified wax phase region. Hydroxyl and ester groups interact with the hydroxyl and ester groups in the first resin, allowing the modified wax to exist in the masterbatch in a dissolved state or as a finely dispersed phase. After the masterbatch cools or enters the second resin and the second styrene, there is no abrupt change in resin type between the first and second resins. The first and second styrene diffuse into each other, and the modified wax is distributed from the masterbatch to the continuous resin phase.
[0029] The second resin, second styrene, polyester dispersant, polyacrylate defoamer, hydrophobic fumed silica, mica iron oxide, and barium sulfate are first mixed and dispersed. The polyester dispersant adsorbs onto the surface of the inorganic particles and forms a spatial barrier, limiting direct particle contact and agglomeration. The masterbatch is added after the pigments and fillers are dispersed to reduce the embedding of modified wax by unwetted particle agglomerates, thus maintaining continuous contact with the vinyl ester resin and styrene. Glass flakes are added later and subjected to lower shear, limiting the fragmentation of their flake morphology.
[0030] After mixing, cobalt ions in cobalt isooctanoate undergo a redox reaction with methyl ethyl ketone peroxide, breaking the peroxide bond and generating free radicals that can initiate polymerization. Cobalt ions transform between different valence states and continue to promote the decomposition of the peroxide. The free radicals add to the unsaturated groups at the ends of the vinyl ester resin to form resin chain free radicals, which continue to grow with the vinyl groups of styrene. After the free radicals add to the methacrylate groups of the modified wax, the double bond transforms into a carbon-carbon single bond, and the modified wax forms a carbon-carbon bond with the growing resin chain. As styrene and unsaturated groups are consumed, the system viscosity increases, chain segment movement is restricted, and the vinyl ester resin, styrene, and modified wax all enter the crosslinked resin phase. The hydrocarbon wax segments in the modified wax exist as lateral wax segments connected to the resin chain segments; their overall diffusion requires the movement of the connected resin chain segments, thus the diffusion distance is less than that of unreacted paraffin molecules.
[0031] Oxygen on the coating surface can combine with carbon-centered free radicals to form peroxy free radicals with low reactivity, reducing the chain growth rate near the air interface and causing the surface layer to be less cured than the interior of the coating. As the curing reaction progresses, the molecular weight and degree of cross-linking of the resin increase, the compatibility between the hydrocarbon chain wax segments of the modified wax and the resin phase decreases, and wax segments with lower surface energy tend to migrate towards the air interface. Modified waxes that have not yet participated in polymerization can diffuse to the surface at this stage, and their methacrylate groups continue to participate in free radical polymerization during migration or after reaching the surface; modified waxes that have already formed carbon-carbon bonds are restrained by the resin chain segments and find it difficult to continue long-distance diffusion. The resulting surface enrichment region still contains hydrocarbon chain wax segments that can reduce the oxygen transfer rate, but the wax segments retain chemical bonds with the underlying cured resin, and the continuous migration of independent wax molecules, crystal growth, and crystal aggregation are restricted. The surface wax phase changes from a continuous free wax film to a wax-containing region dispersed on the surface of the cross-linked resin and constrained by the resin chain segments, and the continuous interfacial gaps and planar weak boundaries between the wax phase and the resin phase decrease accordingly.
[0032] The hydroxyl and ester groups formed by the ring-opening of the modified wax are distributed on the surface layer along with the wax segments, increasing the hydrogen bonding and dipole interactions between the surface layer and the polar segments of the subsequent vinyl ester resin, and reducing the barrier of the pure hydrocarbon wax film to the wetting and spreading of the subsequent coating. When the subsequent coating comes into contact with the previous coating, the styrene in it can enter the free volume of the resin phase of the previous surface layer and cause local swelling. The vinyl ester resin then approaches the exposed resin segments and wax-containing resin areas in the previous coating. The unsaturated groups in the previous surface layer that have not yet been consumed can continue to grow chains during the free radical curing process of the subsequent coating, forming resin connections across the original coating boundary on both sides of the interface. Areas where cross-interfacial polymerization has not occurred can still transfer interfacial shear stress through polar interactions, resin interpenetration, and mechanical interlocking generated by surface undulations. After the degree of abrupt change in interfacial composition and modulus is reduced, the stress generated by construction shrinkage and curing shrinkage is no longer concentrated at the boundary of the continuous free wax film, and the initiation sites and continuously propagating planar paths of interlayer cracks are reduced accordingly.
[0033] Corrosive media can enter multiple coating layers through pinholes, edges, local pores, or coating damage, and then diffuse laterally along low-cohesion regions between layers. The continuous wax film formed by free paraffin lacks chemical bonding with the resin, and the interfacial gaps can become areas for media accumulation. When media absorption causes volume changes in the resin phase, the wax film and resin phase cannot easily transmit the corresponding deformation, and localized debonding areas gradually transform into interlayer cavities storing the media. After modified wax forms carbon-carbon bonds with resin segments, the media must bypass the resin bonding areas when reaching the wax-containing surface. The continuous diffusion channel along the interlayer direction is segmented, thus reducing the media accumulation range and the area affected by liquid pressure.
[0034] Temperature cycling causes varying degrees of volume changes in the vinyl ester crosslinked resin, inorganic pigments and fillers, and wax segments. Free paraffin crystals can change their lattice size and crystallinity with temperature variations, repeatedly generating shear displacement at the boundary between the continuous wax film and the crosslinked resin. Existing pores and debonding zones at the interface become interconnected under repeated stress, leading to interlayer crack propagation along the low-cohesion wax film. When the modified wax connected to the resin segments undergoes volume changes, its displacement is limited by carbon-carbon bonds and surrounding crosslinked segments, making it difficult for the wax segments to shrink, slip, or detach from the resin phase. Local strain can be transmitted to surrounding areas via connected resin segments. Without a continuous free wax film between layers, crack propagation requires crossing the resin-bonded area or changing its direction, limiting the conditions for continuous propagation along the coating interface. The interfacial pressure generated by corrosive immersion and the shear stress generated by temperature cycling are therefore unlikely to jointly drive the continuous expansion of interlayer cavities, limiting the evolution of interfacial defects corresponding to blistering and peeling.
[0035] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention provides a modified wax obtained by the ring-opening reaction of the carboxyl groups of oxidized paraffin and the epoxy groups of glycidyl methacrylate. While retaining the migration and oxygen-barrier capabilities of the hydrocarbon chain wax segments, the modified wax introduces methacrylate groups that can participate in the curing of vinyl ester resin and styrene free radicals. After the modified wax migrates to the coating surface and participates in polymerization, the wax chain segments are constrained by the cross-linked resin chain segments, limiting the migration of free wax molecules, crystal aggregation, and the formation of a continuous wax film, thus reducing the interfacial gap between the independent wax phase and the resin phase. The hydroxyl and ester groups formed by ring opening increase the polar interaction and wetting contact between the surface of the previous coating and the subsequent coating. The unsaturated groups remaining on the surface can continue to participate in the reaction during the curing of the subsequent coating, reducing the weak continuous boundaries between layers and improving interlayer adhesion and adhesion retention after immersion. The channels through which corrosive media diffuse and accumulate laterally between layers are divided, and the interfacial shear stress generated by temperature cycling is less likely to concentrate at the boundary of the continuous wax film. The propagation of interfacial cavities and debonding cracks is restricted, and the degree of blistering and peeling of the coating is reduced under the conditions of immersion in corrosive media and temperature cycling. Detailed Implementation
[0036] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The embodiments described herein are specific implementations of the present invention and are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limiting the implementation of the present invention or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can also adopt other obvious technical solutions based on the content disclosed in the claims and the specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.
[0037] The chemical reagents used in the embodiments and comparative examples of this invention are all commercially available products and have not undergone any further purification treatment.
[0038] The vinyl ester resin used in the examples and comparative examples is TM-V211 high-toughness corrosion-resistant epoxy vinyl ester resin produced by Changzhou Tianma Group Co., Ltd. This resin belongs to the bisphenol A type epoxy vinyl ester resin. The solid content indicated in the product technical data is 58-64 wt.%, and the viscosity at 25°C is 300-500 mPa·s.
[0039] The paraffin oxide used in the examples and comparative examples was from the same batch, with an acid value of 25 mg KOH / g and a dropping melting point of 60°C. In the following examples and comparative examples, the amount of carboxyl groups in the paraffin oxide is calculated based on this acid value.
[0040] Example 1
[0041] This embodiment provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating, the preparation method specifically including the following steps:
[0042] S1, In an argon atmosphere, 47.60 g of oxidized paraffin, 2.29 g of glycidyl methacrylate, 0.09 g of triphenylphosphine, and 0.02 g of p-methoxyphenol were mixed; the molar ratio of glycidyl methacrylate to the molar ratio of carboxyl groups in the oxidized paraffin was 0.76:1. The temperature of the reactants was adjusted to 110 °C and the reaction was carried out for 5 h to obtain 50.00 g of modified wax; the modified wax had an acid value of 5.7 mg KOH / g, a dropping melting point of 58 °C, and a methacrylate group content of 0.32 mmol / g.
[0043] S2, 6100g of vinyl ester resin is divided into 150g of primary resin and 5950g of secondary resin, and 500g of styrene is divided into 50g of primary styrene and 450g of secondary styrene. 50.00g of modified wax, 150g of primary resin and 50g of primary styrene are mixed and stirred for 35 minutes at a mixture temperature of 68℃ and a stirring speed of 800r / min to obtain 250.00g of masterbatch.
[0044] S3, 5950g of secondary resin, 450g of secondary styrene, 20g of polyester dispersant, and 35g of polyacrylate defoamer were stirred at 700r / min for 5min. Then, 85g of hydrophobic fumed silica, 450g of mica iron oxide, and 950g of barium sulfate were added, and the mixture was dispersed at 1200r / min for 30min, with the material temperature at 45℃ during dispersion. The material temperature was adjusted to 40℃, and 250.00g of masterbatch and 183g of cobalt isooctanoate solution were added, and the mixture was stirred at 500r / min for 20min; the cobalt content in the cobalt isooctanoate solution was 0.84wt.%. After adding 2500g of glass flakes, the mixture was stirred at 350r / min for 30min to obtain 10873g of base material component; the D50 of the glass flakes was 140μm.
[0045] S4, 10873g of base material components and 61g of methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating; the total active oxygen content of the methyl ethyl ketone peroxide solution is 9.5wt.%.
[0046] Example 2
[0047] This embodiment provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating, the preparation method specifically including the following steps:
[0048] S1, In an argon atmosphere, 95.60 g of oxidized paraffin, 4.24 g of glycidyl methacrylate, 0.101 g of triphenylphosphine, and 0.059 g of p-methoxyphenol were mixed; the molar ratio of glycidyl methacrylate to the molar ratio of carboxyl groups in the oxidized paraffin was 0.70:1. The temperature of the reactants was adjusted to 125 °C and the reaction was carried out for 3 hours to obtain 100.00 g of modified wax; the modified wax had an acid value of 7.2 mg KOH / g, a dropping melting point of 59 °C, and a methacrylate group content of 0.30 mmol / g.
[0049] S2, 5200g of vinyl ester resin is divided into 500g of primary resin and 4700g of secondary resin, and 1000g of styrene is divided into 50g of primary styrene and 950g of secondary styrene. 100.00g of modified wax, 500g of primary resin and 50g of primary styrene are mixed and stirred for 60min at a mixture temperature of 60℃ and a stirring speed of 500r / min to obtain 650.00g of masterbatch.
[0050] S3, 4700g of the second resin, 950g of the second styrene, 60g of the polyester dispersant, and 10g of the polyacrylate defoamer were stirred at 400r / min for 12min. Then, 30g of hydrophobic fumed silica, 800g of mica iron oxide, and 500g of barium sulfate were added, and the mixture was dispersed at 1600r / min for 20min, with the material temperature at 35℃ during dispersion. The material temperature was adjusted to 30℃, and 650.00g of masterbatch and 52g of cobalt isooctanoate solution were added, and the mixture was stirred at 800r / min for 10min; the cobalt content in the cobalt isooctanoate solution was 0.70wt.%. After adding 1800g of glass flakes, the mixture was stirred at 500r / min for 15min to obtain 9552g of the base material component; the D50 of the glass flakes was 60μm.
[0051] S4, 9552g of base material component and 104g of methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating; the total active oxygen content of the methyl ethyl ketone peroxide solution is 8.5wt.%.
[0052] Example 3
[0053] This embodiment provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating, the preparation method specifically including the following steps:
[0054] S1, In an argon atmosphere, 28.24 g of oxidized paraffin, 1.70 g of glycidyl methacrylate, 0.05 g of triphenylphosphine, and 0.01 g of p-methoxyphenol were mixed; the molar ratio of glycidyl methacrylate to the molar ratio of carboxyl groups in the oxidized paraffin was 0.95:1. The temperature of the reactants was adjusted to 100°C and the reaction was carried out for 2 hours to obtain 30.00 g of modified wax; the modified wax had an acid value of 2.3 mg KOH / g, a dropping melting point of 54°C, and a methacrylate group content of 0.38 mmol / g.
[0055] S2, 6500g of vinyl ester resin is divided into 60g of primary resin and 6440g of secondary resin, and 300g of styrene is divided into 60g of primary styrene and 240g of secondary styrene. 30.00g of modified wax, 60g of primary resin and 60g of primary styrene are mixed and stirred for 45min at a mixture temperature of 75℃ and a stirring speed of 300r / min to obtain 150.00g of masterbatch.
[0056] S3, 6440g of the second resin, 240g of the second styrene, 35g of polyester dispersant, and 50g of polyacrylate defoamer were stirred at 800r / min for 8min. Then, 120g of hydrophobic fumed silica, 300g of mica iron oxide, and 1200g of barium sulfate were added, and the mixture was dispersed at 1400r / min for 40min, with the material temperature at 25℃ during dispersion. The material temperature was adjusted to 35℃, and 150.00g of masterbatch and 260g of cobalt isooctanoate solution were added, and the mixture was stirred at 400r / min for 30min; the cobalt content in the cobalt isooctanoate solution was 0.90wt.%. Finally, 2200g of glass flakes were added, and the mixture was stirred at 200r / min for 20min to obtain 10995g of the base material component; the D50 of the glass flakes was 180μm.
[0057] S4, 10995g of base material component and 97.5g of methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating; the total active oxygen content of the methyl ethyl ketone peroxide solution is 10.0 wt.%.
[0058] Example 4
[0059] This embodiment provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating, the preparation method specifically including the following steps:
[0060] S1, In an argon atmosphere, 71.08 g of oxidized paraffin, 3.78 g of glycidyl methacrylate, 0.10 g of triphenylphosphine, and 0.04 g of p-methoxyphenol were mixed; the molar ratio of glycidyl methacrylate to the molar ratio of carboxyl groups in the oxidized paraffin was 0.84:1. The temperature of the reactants was adjusted to 118 °C and the reaction was carried out for 4 hours to obtain 75.00 g of modified wax; the modified wax had an acid value of 3.8 mg KOH / g, a dropping melting point of 56 °C, and a methacrylate group content of 0.35 mmol / g.
[0061] S2, 5700g of vinyl ester resin was divided into 300g of primary resin and 5400g of secondary resin, and 750g of styrene was divided into 112.5g of primary styrene and 637.5g of secondary styrene. 75.00g of modified wax, 300g of primary resin and 112.5g of primary styrene were mixed and stirred for 20 minutes at a mixture temperature of 70℃ and a stirring speed of 650r / min to obtain 487.50g of masterbatch.
[0062] S3, 5400g of the second resin, 637.5g of the second styrene, 80g of polyester dispersant, and 20g of polyacrylate defoamer were stirred at 550r / min for 15min. Then, 55g of hydrophobic fumed silica, 650g of mica iron oxide, and 700g of barium sulfate were added, and the mixture was dispersed at 1800r / min for 25min, with the material temperature at 50℃ during dispersion. The material temperature was adjusted to 25℃, and 487.50g of masterbatch and 114g of cobalt isooctanoate solution were added, and the mixture was stirred at 650r / min for 15min; the cobalt content in the cobalt isooctanoate solution was 0.76wt.%. After adding 1500g of glass flakes, the mixture was stirred at 400r / min for 10min to obtain 9644g of the base material component; the D50 of the glass flakes was 100μm.
[0063] S4, 9644g of base material component and 142.5g of methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating; the total active oxygen content of the methyl ethyl ketone peroxide solution is 9.0 wt.%.
[0064] Comparative Example 1
[0065] This comparative example provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating. The difference between this method and Example 1 is that S1 is not performed, and an equal mass of paraffin wax is used to replace the modified wax. Other process parameters and operating conditions are exactly the same as in Example 1.
[0066] Comparative Example 2
[0067] This comparative example provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating. The difference between this method and Example 1 is that no ring-opening reaction is carried out in S1. Instead, oxidized paraffin, glycidyl methacrylate, triphenylphosphine and p-methoxyphenol are mixed at room temperature. Other process parameters and operating conditions are exactly the same as in Example 1.
[0068] Comparative Example 3
[0069] This comparative example provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating. The difference between this method and Example 1 is that the preparation of the masterbatch in S2 is omitted, and the modified wax, the first resin, and the first styrene are directly added to S3. Other process parameters and operating conditions are exactly the same as in Example 1.
[0070] Comparative Example 4
[0071] This comparative example provides a method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating. The difference between this method and Example 1 is that the ratio of the amount of glycidyl methacrylate to the amount of carboxyl groups in the oxidized paraffin in S1 is adjusted to 0.50:1. Other process parameters and operating conditions are exactly the same as in Example 1.
[0072] Test method:
[0073] Initial interlayer pull-off adhesion strength:
[0074] The tests were conducted according to GB / T 5210-2006 "Paints and Varnishes - Pull-off Adhesion Test". Q235 steel plates with dimensions of 150mm × 100mm × 3mm were prepared according to GB / T 9271-2008, with three test plates prepared for each example and comparative example. The coated surfaces of the steel plates were sandblasted to a surface roughness R. z The surface abrasive and dust were removed, and the sample was placed at 23±2℃ and 50±5%RH for 2 hours.
[0075] The base material components and initiator components of each embodiment or comparative example were mixed at the corresponding mass ratio, stirred at 300 r / min for 2 min, and immediately coated onto the front, back, and edges of a steel plate. The dry film thickness of the first coating was controlled at 350±25 μm, and cured for 24 h at 23±2℃ and 50±5%RH. The first coating was not sanded, wiped with solvent, or subjected to other dewaxing treatments; the second coating was directly applied, with a dry film thickness of 350±25 μm, resulting in a total dry film thickness of 700±50 μm. The coated test plates were cured for 7 days at 23±2℃ and 50±5%RH. The total dry film thickness was measured at five evenly selected locations on the front of the test plate, and the arithmetic mean of the five measurements was taken as the total dry film thickness of the test plate.
[0076] Three test positions were set on the front of each test plate, with the center of each test position no less than 30 mm from the edge of the test plate and the center-to-center distance between adjacent test positions no less than 40 mm. A 20 mm diameter steel test column and a room-temperature curing two-component epoxy adhesive were used. The tensile strength of the cured adhesive was no less than 20 MPa. The bonding surface of the test column and the test positions of the coating were sanded 10 times each in two mutually perpendicular directions using P240 sandpaper. After removing the sanding dust, the adhesive was applied, and the test column was vertically bonded to the coating surface. The coating was cured for 24 hours at 23±2℃ and 50±5%RH. A 20 mm inner diameter annular cutter was used to cut the coating down to the steel substrate along the perimeter of the test column.
[0077] A pull-off adhesion tester with a range of 0-20 MPa and an indication error not exceeding ±1% was used. Under conditions of 23±2℃ and 50±5%RH, a load was applied perpendicular to the test plate surface at a loading rate of 0.5 MPa / s, and a single pull-off test was completed within 90 seconds. The maximum tensile force F at failure of each test piece was recorded. The initial interlayer pull-off adhesion strength was calculated as P0 = F / A, where P0 is the initial interlayer pull-off adhesion strength at a single test location (in MPa); F is the maximum tensile force (in N); and A is the bonded area of the test piece (A = πd). 2 / 4, unit is mm 2 d represents the diameter of the test column, taken as 20 mm. Results showing detachment between the test column and the adhesive are considered invalid and retested at a spare location; other destructive results are not discarded. Nine valid results are obtained from each group, and the arithmetic mean is calculated. The arithmetic mean is retained to a value of 0.1 MPa and used as the initial interlayer tensile adhesion strength for this example or comparative example.
[0078] Adhesion strength retention rate after immersion in corrosive media:
[0079] Immersion in corrosive media was conducted according to GB / T 30648.1-2014 "Determination of resistance to liquids of paints and varnishes – Part 1: Immersion in liquids other than water". The pull-out adhesion strength after immersion was determined according to GB / T 5210-2006. For each example and comparative example, three Q235 steel plates with dimensions of 150mm × 100mm × 3mm were prepared. The surface treatment, mixing conditions of the base material and initiator components, the coating method of the two coatings, the interlayer curing time, the dry film thickness, and the final curing conditions were all the same as those for the initial interlayer pull-out adhesion strength test. No sanding, solvent wiping, or other dewaxing treatments were performed after the first coating had cured.
[0080] The corrosive medium was a 5.0 wt.% sodium chloride aqueous solution, prepared by mixing 50 g of analytical grade sodium chloride with 950 g of grade III water conforming to GB / T 6682. Each test plate was placed in an independent 5L polypropylene container, with 3.0 L of corrosive medium added to each container. The test plates were completely submerged vertically, with the upper edge of the plate at least 20 mm from the liquid surface and the plate at least 30 mm from the bottom and sidewalls of the container. The test plates were secured with insulating supports, the containers were covered, and the immersion temperature was 40 ± 2℃ for 720 hours. During the immersion period, all corrosive medium was replaced every 168 hours, with the newly prepared medium pre-adjusted to 40 ± 2℃.
[0081] After soaking, the test panels were removed and rinsed for 30 seconds under a three-stage water flow at 23±2℃. Surface water droplets were removed by pressing with a lint-free absorbent material, without wiping. The panels were then placed at 23±2℃ and 50±5%RH for 24 hours. The pull-out test was conducted according to the specified procedures for initial interlayer pull-out adhesion strength testing, including location arrangement, surface treatment, test column bonding, adhesive curing, ring cutting, and loading. Three locations were tested on each test panel, and nine valid results were obtained for each group. The arithmetic mean P1 of the interlayer pull-out adhesion strength after soaking was calculated, in MPa.
[0082] The adhesion strength retention rate after immersion in the corrosive medium is calculated as R1=P1 / P0×100%, where R1 is the adhesion strength retention rate after immersion in the corrosive medium, in %; P1 is the average interlayer pull-out adhesion strength after immersion in the embodiment or comparative example, in MPa; P0 is the average initial interlayer pull-out adhesion strength of the same embodiment or comparative example, in MPa, and the retention rate result is retained to 0.1%.
[0083] Adhesion strength retention rate after temperature cycling:
[0084] Temperature cycling was conducted according to Test Nb in GB / T 2423.22-2012 "Environmental Testing Part 2: Test Methods Test N: Temperature Change". The pull-out adhesion strength after cycling was determined according to GB / T 5210-2006. For each example and comparative example, three Q235 steel plates with dimensions of 150mm × 100mm × 3mm were prepared. The surface treatment, mixing conditions of the base material and initiator components, coating methods for the two coatings, interlayer curing time, dry film thickness, and final curing conditions were all the same as those for the initial interlayer pull-out adhesion strength test. No sanding, solvent wiping, or other dewaxing treatments were performed after the first coating layer cured.
[0085] A programmable temperature test chamber with a temperature range of -30 to 70℃, a temperature fluctuation of no more than ±1℃, and a temperature uniformity of no more than 2℃ is used. Three test plates are placed vertically inside the chamber, with a minimum distance of 50mm between the test plates and between the test plates and the chamber walls. The coating surfaces must not touch each other. A separate steel plate of the same size is used as a temperature monitoring plate, and a platinum resistance temperature sensor is fixed to the center of its surface. The measured temperature of the monitoring plate is used as the starting point for calculating the holding time. Dry air is circulated inside the test chamber without humidification, and the dew point of the air inside the chamber does not exceed -25℃.
[0086] The test plate was first held at 23±2℃ for 1 hour, then cooled to -20±2℃ at a rate of 2±0.2℃ / min; after reaching -20±2℃, the temperature monitoring plate was held for 2 hours; then the temperature was increased to 60±2℃ at a rate of 2±0.2℃ / min, and held for 2 hours; subsequently, it was cooled to -20±2℃ at a rate of 2±0.2℃ / min. One temperature cycle consisted of heating from -20℃, holding at 60℃, and then cooling back to -20℃. A total of 30 cycles were performed, with each cycle involving a 2-hour hold after cooling back to -20±2℃. After the 30th cycle, the temperature was increased to 23±2℃ at a rate of 2±0.2℃ / min, the test plate was removed, and placed at 23±2℃ and 50±5%RH for 24 hours.
[0087] The pull-out adhesion test was conducted according to the specified procedures, including location arrangement, surface treatment, test column bonding, adhesive curing, ring cutting, and loading. Three locations were tested on each test plate, and nine valid results were obtained for each group. The arithmetic mean P2 of the pull-out adhesion strength after temperature cycling was calculated, in MPa.
[0088] The adhesion strength retention rate after temperature cycling is calculated as R2 = P2 / P0 × 100%, where R2 is the adhesion strength retention rate after temperature cycling (in %), P2 is the average interlayer pull-out adhesion strength after temperature cycling in this embodiment or comparative example (in MPa), and P0 is the average initial interlayer pull-out adhesion strength in the same embodiment or comparative example (in MPa). The retention rate result is rounded down to 0.1%.
[0089] The test results are shown in Table 1.
[0090] Table 1. Test results of high-solids vinyl ester heavy-duty anti-corrosion coatings in Examples 1-4 and Comparative Examples 1-4
[0091]
[0092] As shown in Table 1, compared to Example 1, Comparative Example 1 showed a decrease in initial interlayer pull-out adhesion strength, adhesion strength retention rate after immersion in corrosive media, and adhesion strength retention rate after temperature cycling. Comparative Example 1 used an equal mass of paraffin wax instead of the modified wax; the paraffin wax did not contain methacrylate groups that could participate in the curing reaction of vinyl ester resin. After migrating to the surface of the first coating, the paraffin wax tended to form a low surface energy wax layer separated from the cured resin network, limiting the wetting and interfacial contact of the second coating on the first coating, forming weak interlayer boundaries, thus reducing the initial interlayer pull-out adhesion strength. Corrosive media could diffuse along local interfacial gaps, promoting interlayer debonding; temperature changes also caused differences in thermal deformation and interfacial shear stress between the paraffin phase and the cured resin, thus reducing the adhesion strength retention rate after both treatments.
[0093] As shown in Table 1, compared to Example 1, Comparative Example 2 exhibited decreased initial interlayer pull-out adhesion strength, adhesion strength retention rate after immersion in corrosive media, and adhesion strength retention rate after temperature cycling. Comparative Example 2 eliminated the ring-opening reaction between the carboxyl groups of paraffin oxide and the epoxy groups of glycidyl methacrylate, only physically mixing the raw materials. A stable grafting relationship did not form between glycidyl methacrylate and paraffin oxide. Even if free glycidyl methacrylate could participate in subsequent curing, paraffin oxide still lacked the reaction linkages to enter the curing network. After migrating to the coating surface, paraffin oxide could still form an independent wax phase, restricting wetting and stress transfer at the recoating interface, leading to a decrease in initial interlayer pull-out adhesion strength. This weak interface was more prone to expansion during immersion in corrosive media and temperature cycling, thus reducing the corresponding adhesion strength retention rates.
[0094] As shown in Table 1, compared to Example 1, Comparative Example 3 showed a decrease in initial interlayer pull-out adhesion strength, adhesion strength retention rate after immersion in corrosive media, and adhesion strength retention rate after temperature cycling. Comparative Example 3 retained the synthesis of the modified wax, but omitted the step of pre-preparing the masterbatch with the modified wax, the first resin, and the first styrene, directly adding all three to the subsequent system. Since the modified wax was not pre-wetted and dispersed, and the addition temperature was below its dropping point, the dispersion scale and distribution state of the wax phase in the resin were more difficult to maintain, potentially leading to local enrichment and local deficiencies. Locally enriched areas tend to form thicker surface wax phases, while locally deficient areas may be affected by oxygen inhibition, thereby increasing the discontinuity of the recoating interface and reducing the initial interlayer pull-out adhesion strength. Corrosive media and temperature cycling preferentially act on these local interface defects, causing the defects to expand and reducing the adhesion strength retention rate after treatment.
[0095] As shown in Table 1, compared to Example 1, Comparative Example 4 showed a decrease in initial interlayer pull-out adhesion strength, adhesion strength retention rate after immersion in corrosive media, and adhesion strength retention rate after temperature cycling. Comparative Example 4 reduced the molar ratio of glycidyl methacrylate to carboxyl groups in oxidized paraffin. With the reduced amount of glycidyl methacrylate, the ring-opening conversion degree of carboxyl groups in oxidized paraffin decreased, resulting in a decrease in the density of methacrylate groups in the modified wax. The number of sites for the modified wax to participate in the curing reaction of vinyl ester resin decreased, and the degree to which it was constrained by the curing network after surface migration was reduced. Unreacted wax segments were more likely to aggregate at the interlayer interface, thus reducing the initial interlayer pull-out adhesion strength. Immersion in corrosive media and temperature cycling further amplified the mass transfer channels and thermal deformation differences at this interface, thus reducing both adhesion strength retention rates.
[0096] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the scope of protection and disclosure of the present invention.
Claims
1. A high-solids vinyl ester heavy-duty anti-corrosion coating, characterized in that, It includes separately packaged base material components and initiator components. The base material components include vinyl ester resin, styrene, modified wax, anti-corrosion pigments and fillers, coating additives, and cobalt isooctanoate solution. The initiator component is methyl ethyl ketone peroxide solution. The modified wax includes the structural unit shown: R-CO-O-CH2-CH(OH)-CH2-OCO-C(CH3)=CH2, where R-CO- represents the acyl group formed after removing the hydroxyl group from the carboxyl group contained in the oxidized paraffin; The modified wax has an acid value of 2-8 mg KOH / g, a dropping melting point of 52-65℃, and a methacrylate content of 0.2-0.4 mmol / g.
2. The high-solids vinyl ester heavy-duty anti-corrosion coating according to claim 1, characterized in that, The anti-corrosion pigments and fillers include glass flakes, mica iron oxide and barium sulfate, and the coating additives include hydrophobic fumed silica, polyester dispersant and polyacrylate defoamer; The mass ratio of the vinyl ester resin, styrene, modified wax, glass flakes, mica iron oxide, barium sulfate, hydrophobic fumed silica, polyester dispersant, and polyacrylate defoamer is (52-65):(3-10):(0.3-1.0):(15-25):(3-8):(5-12):(0.3-1.2):(0.2-0.8):(0.1-0.5). The mass ratio of the vinyl ester resin, cobalt isooctanoate solution and initiator component is 100:(1-4):(1-2.5).
3. The high-solids vinyl ester heavy-duty anti-corrosion coating according to claim 2, characterized in that, The vinyl ester resin is selected from at least one of bisphenol A type epoxy vinyl ester resin and phenolic epoxy vinyl ester resin.
4. The high-solids vinyl ester heavy-duty anti-corrosion coating according to claim 2, characterized in that, The D50 of the glass flakes is 60-180 μm; after the base material component and the initiator component are mixed according to the mass ratio described in claim 2, the mass fraction of non-volatile matter measured according to GB / T 34682-2017 is not less than 60 wt.%.
5. The high-solids vinyl ester heavy-duty anti-corrosion coating according to claim 2, characterized in that, The cobalt content in the cobalt isooctanoate solution is 0.7-0.9 wt.%; the total active oxygen content in the methyl ethyl ketone peroxide solution is 8.5-10.0 wt.%.
6. A method for preparing a high-solids vinyl ester heavy-duty anti-corrosion coating as described in any one of claims 1-5, characterized in that, Includes the following steps: S1, oxidized paraffin, glycidyl methacrylate, triphenylphosphine and p-methoxyphenol are mixed and subjected to a ring-opening reaction, wherein the carboxyl group in the oxidized paraffin reacts with the epoxy group in the glycidyl methacrylate to obtain a modified wax. S2, the vinyl ester resin is divided into a first resin and a second resin, the styrene is divided into a first styrene and a second styrene, and the modified wax, the first resin and the first styrene are mixed to obtain a masterbatch; S3, the second resin, second styrene, polyester dispersant, polyacrylate defoamer, hydrophobic fumed silica, mica iron oxide and barium sulfate are mixed and dispersed, then the masterbatch and cobalt isooctanoate solution are added, followed by glass flakes to obtain the base material component; S4, the base material components and methyl ethyl ketone peroxide solution are packaged separately to obtain a high-solids vinyl ester heavy-duty anti-corrosion coating.
7. The preparation method according to claim 6, characterized in that, In S1, the acid value of the oxidized paraffin is 10-30 mg KOH / g, and the dropping melting point is 50-70℃; the molar ratio of the glycidyl methacrylate to the molar ratio of the carboxyl group in the oxidized paraffin is (0.7-0.95):
1. The total mass ratio of the oxidized paraffin and the glycidyl methacrylate to the mass ratio of triphenylphosphine and p-methoxyphenol is 100:(0.10-0.20):(0.03-0.06). The ring-opening reaction is carried out in an argon atmosphere, with the reactant temperature at 100-125℃ and the reaction time at 2-5 hours.
8. The preparation method according to claim 6, characterized in that, In S2, the mass ratio of the modified wax, the first resin and the first styrene is 1:(2-5):(0.5-2). When mixing, the temperature of the mixture is 60-75℃, the stirring speed is 300-800r / min, and the stirring time is 20-60min.
9. The preparation method according to claim 6, characterized in that, In step S3, the second resin, second styrene, polyester dispersant, and polyacrylate defoamer are stirred at 400-800 r / min for 5-15 min. After adding hydrophobic fumed silica, mica iron oxide, and barium sulfate, the mixture is dispersed at 1200-1800 r / min for 20-40 min, with the material temperature at 25-50℃ during dispersion. The material temperature is then adjusted to 25-40℃, and the masterbatch and cobalt isooctanoate solution are added. The mixture is stirred at 400-800 r / min for 10-30 min. After adding glass flakes, the mixture is stirred at 200-500 r / min for 10-30 min to obtain the base material composition.